Acid sulfate electronic copper electroplating solution and application thereof in dense filling of high-aspect-ratio silicon through hole metal

By using surfactant and brightener in acid sulfate electronic electroplating copper plating solution, combined with vertical plating and cutting rod technology, the dense filling problem of high-deep and aspect ratio TSV is solved, and the uniform dense filling of the copper layer and the brightness of the plating layer are achieved. Improved, suitable for aspect ratio TSVs from 20:1 to 5:1.

CN118932439APending Publication Date: 2024-11-12XIAMEN UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410981113.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

In three-dimensional integrated packages, dense filling of high-deep-to-depth ratio through-silicon holes (TSVs) is more difficult to fill, and the complex composition of existing electroplating solution additives is not conducive to maintenance, and it is difficult to achieve dense and uniform filling of high-deep-to-depth ratio TSVs.

Method used

Using an acid sulfate electronic electroplating copper plating solution composed of surfactant and brightener, combined with vertical plating method and uniform supplementation technology of non-conductive cutting rods, ensures timely replenishment of the plating solution components and uniform distribution of power lines, and use specific surfactivity The agent and sulfonic acid sodium salt act as inhibitors and brighteners to promote the formation of copper crystal nuclei and the density of the coating.

Benefits of technology

Achieve dense copper filling with high-deep aspect ratio TSV, preventing sealing effect, improving the copper deposition rate in the hole and the brightness of the plating layer, ensuring the consistency of the thickness of the plating, and suitable for 20:1 to 5:1 aspect ratio TSV ( Pore ​​size 0.5 to 20 μm) filled.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118932439A_ABST
    Figure CN118932439A_ABST
Patent Text Reader

Abstract

The invention discloses an acid sulfate electronic copper electroplating solution and application thereof in dense filling of high aspect ratio silicon through hole metal, the acid sulfate electronic copper electroplating solution is composed of a basic solution and a combined additive, the basic solution takes water as a solvent and contains 100-250 g / L of copper sulfate pentahydrate, 5-30 g / L of sulfuric acid and 40-80 mg / L of chloride ions, and the combined additive is composed of a surfactant and a brightener. According to the invention, the copper compact filling of the TSV (the aperture is 0.5-20 microns) with a high aspect ratio (20: 1-5: 1) can be realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of electronic electroplating for three-dimensional integrated packaging of chips, and in particular relates to an acidic sulfate electronic copper electroplating solution and an application thereof in dense metal filling of through-silicon vias with a high aspect ratio. Background Art

[0002] As the demand for miniaturization, intelligence and functionality of electronic products continues to increase, the process reduction method that follows Moore's Law in traditional chip manufacturing has begun to encounter bottlenecks. Three-dimensional packaging integration technology, as an important development direction that goes beyond Moore's Law, is increasingly valued. Through-silicon via (TSV) technology, as a core component of three-dimensional integrated packaging, can achieve "vertical" interconnection between chips, which not only speeds up signal transmission speed, but also reduces the package size, thereby improving the performance and function of future electronic products. TSV is a sub-μm pore structure with one end open and the other end closed. Its interior usually needs to be densely filled with metal copper to achieve multi-layer interconnection between chips. Electronic electroplating of copper is the key technology for metal filling in TSV, and achieving dense filling of TSV is the main challenge in TSV manufacturing.

[0003] Due to the unique porous structure of TSV, there is inconsistency in the copper ion mass transfer rate and the distribution density of electric lines at the hole mouth and inside the hole during its electronic electroplating filling process, which can easily lead to the copper layer growing too fast at the hole mouth, forming a void, and the internal copper layer is sealed in advance before it is filled. By adding a specific combination of additives to the acid copper electroplating solution, the electrodeposition behavior of metal copper in TSV can be orderly regulated to achieve dense filling of TSV. However, as the aspect ratio of TSV increases to more than 10:1 (for example, the aperture is 10μm and the hole depth is 100μm), its dense filling becomes more difficult. In addition, ensuring the dense uniformity of the overall coating of large wafers is also a technical challenge. Therefore, the development of electroplating solutions and electroplating methods for electronic electroplating copper of TSV (aperture 0.5 to 20μm) with high aspect ratios (20:1 to 5:1) has important industrial application value for promoting the further development of chip three-dimensional packaging technology.

[0004] CN103361681A discloses an additive combination that can change the copper plating filling mode of TSV microvias and an electroplating solution containing the additive combination, the additive combination includes an inhibitor S, an accelerator A, a leveler L and a special additive C. The combination can achieve dense filling of TSVs with a hole diameter of 10μm and a hole depth of 100μm, but the additive composition is relatively complex. In addition to the inhibitor, accelerator and leveler, it also contains a special additive C, which is not conducive to the maintenance of the plating solution. CN115354369A discloses an ultra-deep hole TSV electroplating solution for MEMS device packaging, the additives in the electroplating solution are composed of a composite accelerator, a composite wetting agent, a composite leveler, an auxiliary agent and a complexing agent. The additive combination achieves void-free filling of ultra-deep TSV holes with a maximum depth of 700μm, but it is also not conducive to the maintenance of the plating solution because the additive composition is extremely complex. Summary of the invention

[0005] The present invention aims to overcome the defects of the prior art and provide an acid sulfate electronic copper electroplating solution.

[0006] Another object of the present invention is to provide a high aspect ratio through silicon via metal dense filling electronic electroplating method using the above acidic sulfate electronic electroplating copper electroplating solution.

[0007] The technical solution of the present invention is as follows:

[0008] An acid sulfate electronic copper electroplating solution is composed of a base solution and a combination of additives, wherein:

[0009] The base liquid uses water as solvent and contains 100-250 g / L copper sulfate pentahydrate, 5-30 g / L sulfuric acid and 40-80 mg / L chloride ions.

[0010] The combined additive consists of a surfactant and a brightener.

[0011] The surfactant is selected from at least one of polyethylene glycol, polyvinyl alcohol, polyvinyl pyrrolidone, polyoxyethylene ether, behenamide, triglyceride, pentaerythritol stearate, alkylphenol polyoxyethylene ether, alkyl glycoside, myristyl myristate, triglycerol monooleate, hexadecyl stearate, triisohexadecyl citrate, stearyl stearate, coconut fatty acid diethanolamide, lauroyl monoethanolamine, linoleyl diethanolamine, emulsifier OP-40, lauryl glycol ether, polythiocyanate chloride, 4-piperidinyl propionate hydrochloride, octadecyl trimethyl ammonium bromide, dioctadecyl dimethyl ammonium chloride, octadecyl trimethyl ammonium chloride, benzalkonium chloride, octadecyl dimethyl benzyl ammonium chloride and tetraethyl ammonium bromide, and the concentration of the surfactant in the acid sulfate electronic electroplating copper plating solution is 1-500 mg / L.

[0012] The brightener is selected from at least one of sodium polydisulfide propane sulfonate, sodium 3-mercaptopropane sulfonate, sodium 2,7-dihydroxynaphthalene-3,6-disulfonate, sodium anisole sulfonate, sodium dodecylbenzene sulfonate, sodium benzene sulfinate, sodium saccharin, xylose, chitosan, xylan, hydroxypropyl cellulose, trehalose, sucralose, xylitol, sorbitol, maltitol, lactobionic acid and glucose, and the concentration of the brightener in the acid sulfate electronic electroplating copper plating solution is 0.1-200 mg / L.

[0013] In a preferred embodiment of the present invention, the surfactant is selected from at least one of alkylphenol polyoxyethylene ether, polyvinyl alcohol, polyvinyl pyrrolidone, polythiophene chloride, octadecyltrimethylammonium chloride and octadecyldimethylbenzylammonium chloride.

[0014] Further preferably, the surfactant is alkylphenol polyoxyethylene ether, polyvinyl alcohol, polyvinyl pyrrolidone+polythiophene chloride or octadecyltrimethylammonium chloride+octadecyldimethylbenzylammonium chloride.

[0015] In a preferred embodiment of the present invention, the brightener is at least one selected from sodium anisole sulfonate, sodium 3-mercaptopropane sulfonate, sodium 2,7-dihydroxynaphthalene-3,6-disulfonate, sodium saccharin, trehalose and glucose.

[0016] More preferably, the brightener is sodium anisole sulfonate, sodium 3-mercaptopropane sulfonate + sodium 2,7-dihydroxynaphthalene-3,6-disulfonate, sodium saccharin or trehalose + glucose.

[0017] In a preferred embodiment of the present invention, the surfactant is alkylphenol polyoxyethylene ether, polyvinyl alcohol, polyvinyl pyrrolidone + polythiophene chloride or octadecyltrimethylammonium chloride + octadecyldimethylbenzylammonium chloride; the brightener is sodium anisole sulfonate, sodium 3-mercaptopropane sulfonate + sodium 2,7-dihydroxynaphthalene-3,6-disulfonate, sodium saccharin or trehalose + glucose.

[0018] Further preferably, the surfactant is alkylphenol polyoxyethylene ether, and the brightener is sodium anisole sulfonate;

[0019] Or the surfactant is polyvinyl alcohol, and the brightener is sodium 3-mercaptopropane sulfonate + sodium 2,7-dihydroxynaphthalene-3,6-disulfonate;

[0020] Or the surfactant is polyvinyl pyrrolidone + polythiophene chloride, and the brightener is saccharin sodium;

[0021] Or the surfactant is octadecyltrimethylammonium chloride+octadecyldimethylbenzylammonium chloride, and the brightener is trehalose+glucose.

[0022] A high aspect ratio through silicon via (TSV) metal dense filling electronic electroplating method adopts the acid sulfate electronic electroplating copper electroplating solution.

[0023] In a preferred embodiment of the present invention, vertical electroplating is adopted, and a flow pump is used to ensure that the components of the acid sulfate electronic copper electroplating solution are replenished to the cathode in time; a non-conductive cutting rod is placed about 1 to 5 mm close to the cathode surface, and the cutting rod can move back and forth horizontally along the surface of the cathode and the wafer connected to it to ensure uniform replenishment of the cathode plating solution and uniform distribution of the power lines, so that the coating thickness is uniform; square wave pulse current electroplating or direct current electroplating is adopted; the temperature of the acid sulfate electronic copper electroplating solution is 15-30°C.

[0024] Further preferably, the horizontal reciprocating speed of the non-conductive cutting rod is 60-500 r / min; the cathode current in the square wave pulse current electroplating is 0.2-0.3 A / dm 2 , 50~100ms, anode current 0.5~0.8A / dm 2 , 5 to 10 ms, pause time 50 to 100 ms; in the DC electroplating, the constant current density is: 0.15 / 0.2 / 0.25A / dm 2, Or segment current density: 0.1-0.3A / dm 2 .

[0025] The beneficial effects of the present invention are:

[0026] 1. The present invention uses a specific surfactant to significantly reduce the surface tension of the plating solution, which is beneficial for the plating solution components to penetrate into the TSV with a high aspect ratio. As an inhibitor, the surfactant ensures a strong inhibitory effect on copper deposition at the TSV hole mouth, preventing the sealing effect, thereby facilitating the growth of the copper layer in the TSV hole with a high aspect ratio. At the same time, the surfactant also serves as an adsorption carrier for the brightener, which is beneficial for the brightener to play a role in the deep hole.

[0027] 2. The present invention uses specific sodium salts of sulfonic acid and carbohydrates as brighteners, which can effectively promote the formation of copper nuclei and make the coating more dense and bright. Without destroying the strong inhibition ability of the plating solution at the opening of the high aspect ratio TSV, they greatly increase the deposition rate of copper in the hole, which is conducive to achieving dense metal filling of the high aspect ratio TSV.

[0028] 3. The present invention combines an efficient electroplating method: vertical electroplating is adopted, and a flow pump is used to ensure that the plating solution components can be replenished to the cathode in time (the flow rate is controlled at 1-10L / min). A non-conductive cutting rod is placed about 1-5mm from the cathode surface (see Figure 1In the figure, a non-conductive cutting rod is placed about 1 mm away from the cathode surface. The cutting rod can move back and forth horizontally along the surface of the cathode and the wafer connected to it, driven by the moving rod (the moving rate is 60 to 500 rpm) parallel to the surface, to ensure uniform replenishment of the cathode plating solution and uniform distribution of the electric lines, thereby ensuring the consistency of the coating thickness.

[0029] 4. Within the range of use conditions, the present invention can achieve dense copper filling of TSV (aperture 0.5 to 20 μm) with a high aspect ratio (20:1 to 5:1). BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 Schematic diagram of the electroplating method used in Examples 1 to 4 of the present invention.

[0031] Figure 2 It shows that the surfactant concentration is too high, the copper layer at the bottom of the TSV grows slowly, and the hole cannot be completely filled.

[0032] Figure 3 It shows that the brightener concentration is too high, TSV is sealed prematurely, and holes appear in the hole.

[0033] Figure 4 It shows that the surfactant concentration is too low, the growth rate of the TSV bottom is lower than that at the hole mouth, and the hole is sealed prematurely.

[0034] Figure 5 It shows that the brightener concentration is too low, the growth rate of the TSV bottom is slow, and the hole cannot be completely filled.

[0035] Figure 6 This is a metallographic microscope image of the TSV electroplated copper layer in Example 1 of the present invention.

[0036] Figure 7 This is a metallographic microscope image of the TSV electroplated copper layer in Example 2 of the present invention.

[0037] Figure 8 This is a metallographic microscope image of the TSV electroplated copper layer in Example 3 of the present invention.

[0038] Fig. 9 This is a metallographic microscope image of the TSV electroplated copper layer in Example 4 of the present invention. DETAILED DESCRIPTION

[0039] The technical solution of the present invention is further illustrated and described below through specific implementation modes in combination with the accompanying drawings.

[0040] Examples 1 to 4

[0041] Take the preparation of 1L of concentrate as an example:

[0042] ① Accurately weigh 20g of surfactant and 2g of brightener, respectively, and adjust the volume to 1L to prepare additive concentrate; according to the different contents of additives, combined additives with different content ratios can be prepared.

[0043] ② During electroplating, a quantitative concentrated solution is added to the electroplating copper base solution, which uses water as a solvent and contains 100-250 g / L copper sulfate pentahydrate, 5-30 g / L sulfuric acid and 40-80 mg / L chloride ions.

[0044] ③ The sample board containing the TSV array is pre-treated with acetone and ethanol, then washed with ultrapure water, and then vacuum infiltrated in a deionized water solution, and finally directly placed in an acidic electronic plating solution for TSV copper electroplating; after the electroplating is completed, the cathode is removed from the electroplating solution, the surface is cleaned with distilled water, and dried with cold air. The electroplating method is as follows: vertical electroplating is adopted, and a flow pump is used to ensure that the plating solution components are replenished to the cathode in time (the flow rate is 1 to 10 L / min); a non-conductive cutting rod (such as Figure 1 As shown in the figure, a non-conductive cutting rod is placed about 1mm away from the cathode surface. The cutting rod can move back and forth horizontally along the surface of the cathode and the wafer connected to it, driven by the moving rod (moving speed: 60-500r / min) parallel to the surface, to ensure uniform replenishment of the cathode plating solution and uniform distribution of the power lines, so that the coating thickness is uniform; a square wave pulse current (cathode current 0.2-0.3A / dm 2 , 50~100ms, anode current 0.5~0.8A / dm 2 , 5~10ms, pause time 50~100ms) or DC plating (constant current density: 0.15 / 0.2 / 0.25A / dm 2 Or segment current density: 0.1-0.3A / dm 2 ); the plating solution temperature is 15-30°C.

[0045] Taking 1L of electroplating solution, TSV aperture of 10μm and hole depth of 100μm as an example, the acid sulfate electronic electroplating copper electroplating solution of the present invention can obtain an ideal TSV copper dense electroplating filling effect. The specific embodiment of the acid sulfate electronic electroplating copper electroplating solution is shown in Table 1 below:

[0046] Table 1 Example - Different acid sulfate electronic copper electroplating combination additive combinations and corresponding electroplating parameters

[0047]

[0048]

[0049] When the combination of additives for electronic copper electroplating is not suitable, a comparison example of a specific acid sulfate electronic copper electroplating solution is shown in Table 2 below:

[0050] Table 2 Comparative Examples - Combinations of additives and corresponding electroplating parameters for different acid sulfate electronic copper plating

[0051]

[0052]

[0053] like Figure 2 As shown, in Comparative Example 1, the concentration of the surfactant in the acidic sulfate electronic copper plating solution is higher than 500 mg / L, which will strongly inhibit the deposition of copper ions at the bottom of the TSV and slow the growth of the bottom copper layer; Figure 4 As shown, in Comparative Example 2, the surfactant concentration is lower than 1 mg / L, the copper ion deposition inhibition effect on the top of the TSV hole is weak, and the hole mouth is sealed in advance; Figure 3 As shown, in Comparative Example 3, the concentration of the brightener in the acid sulfate electronic copper plating solution is higher than 200 mg / L, which will cause the pore deposition rate to be too fast, the pores to be sealed in advance, and the brightness of the coating to be reduced; Figure 5 As shown, in Comparative Example 4, the brightener concentration is lower than 0.1 mg / L, which will result in a slower copper deposition rate inside the hole and poor brightness of the coating.

[0054] like Figures 6 to 9 As shown, it can be seen that the acid sulfate electronic electroplating copper combination additives of Examples 1 to 4 of the present invention can successfully achieve dense electroplating filling of TSV. It should be noted that when the TSV aperture is 0.5-20 μm and the aspect ratio is 20-5:1, the results obtained are the same or similar to those of the above examples.

[0055] The above description is only a preferred embodiment of the present invention, and therefore cannot be used to limit the scope of the present invention. That is, equivalent changes and modifications made according to the patent scope of the present invention and the contents of the specification should still fall within the scope of the present invention.

Claims

1. An acid sulfate electronic copper electroplating solution, characterized in that: It is composed of a base liquid and a combination of additives, wherein the base liquid, with water as solvent, contains 100-250 g / L of copper sulfate pentahydrate, 5-30 g / L of sulfuric acid and 40-80 mg / L of chloride ions. The combined additive consists of a surfactant and a brightener. The surfactant is selected from at least one of polyethylene glycol, polyvinyl alcohol, polyvinyl pyrrolidone, polyoxyethylene ether, behenamide, triglyceride, pentaerythritol stearate, alkylphenol polyoxyethylene ether, alkyl glycoside, myristyl myristate, triglycerol monooleate, hexadecyl stearate, triisohexadecyl citrate, stearyl stearate, coconut fatty acid diethanolamide, lauroyl monoethanolamine, linoleyl diethanolamine, emulsifier OP-40, lauryl glycol ether, polythiocyanate chloride, 4-piperidinyl propionate hydrochloride, octadecyl trimethyl ammonium bromide, dioctadecyl dimethyl ammonium chloride, octadecyl trimethyl ammonium chloride, benzalkonium chloride, octadecyl dimethyl benzyl ammonium chloride and tetraethyl ammonium bromide, and the concentration of the surfactant in the acid sulfate electronic electroplating copper plating solution is 1-500 mg / L. The brightener is selected from at least one of sodium polydisulfide propane sulfonate, sodium 3-mercaptopropane sulfonate, sodium 2,7-dihydroxynaphthalene-3,6-disulfonate, sodium anisole sulfonate, sodium dodecylbenzene sulfonate, sodium benzene sulfinate, sodium saccharin, xylose, chitosan, xylan, hydroxypropyl cellulose, trehalose, sucralose, xylitol, sorbitol, maltitol, lactobionic acid and glucose, and the concentration of the brightener in the acid sulfate electronic electroplating copper plating solution is 0.1-200 mg / L.

2. The acidic sulfate electronic copper electroplating solution according to claim 1, characterized in that: The surfactant is selected from at least one of alkylphenol polyoxyethylene ether, polyvinyl alcohol, polyvinyl pyrrolidone, polythiocyanate chloride, octadecyltrimethylammonium chloride and octadecyldimethylbenzylammonium chloride.

3. The acidic sulfate electronic copper electroplating solution according to claim 2, characterized in that: The surfactant is alkylphenol polyoxyethylene ether, polyvinyl alcohol, polyvinyl pyrrolidone+polythiophene chloride or octadecyl trimethyl ammonium chloride+octadecyl dimethyl benzyl ammonium chloride.

4. The acidic sulfate electronic copper electroplating solution according to claim 1, characterized in that: The brightener is selected from at least one of sodium anisole sulfonate, sodium 3-mercaptopropane sulfonate, sodium 2,7-dihydroxynaphthalene-3,6-disulfonate, sodium saccharin, trehalose and glucose.

5. The acidic sulfate electronic copper electroplating solution according to claim 4, characterized in that: The brightener is sodium anisole sulfonate, sodium 3-mercaptopropane sulfonate+sodium 2,7-dihydroxynaphthalene-3,6-disulfonate, sodium saccharin or trehalose+glucose.

6. The acidic sulfate electronic copper electroplating solution according to claim 1, characterized in that: The surfactant is alkylphenol polyoxyethylene ether, polyvinyl alcohol, polyvinyl pyrrolidone+polythiocyanate or octadecyltrimethylammonium chloride+octadecyldimethylbenzylammonium chloride; the brightener is sodium anisole sulfonate, sodium 3-mercaptopropane sulfonate+sodium 2,7-dihydroxynaphthalene-3,6-disulfonate, sodium saccharin or trehalose+glucose.

7. The acidic sulfate electronic copper electroplating solution according to claim 6, characterized in that: The surfactant is alkylphenol polyoxyethylene ether, and the brightener is sodium anisole sulfonate; Or the surfactant is polyvinyl alcohol, and the brightener is sodium 3-mercaptopropane sulfonate + sodium 2,7-dihydroxynaphthalene-3,6-disulfonate; Or the surfactant is polyvinyl pyrrolidone + polythiophene chloride, and the brightener is saccharin sodium; Or the surfactant is octadecyltrimethylammonium chloride+octadecyldimethylbenzylammonium chloride, and the brightener is trehalose+glucose.

8. A method for densely filling high aspect ratio through silicon via metal with electronic electroplating, characterized in that: An acid sulfate electronic copper electroplating solution as claimed in any one of claims 1 to 7 is used.

9. A method for densely filling high aspect ratio through silicon via metal with electronic electroplating as claimed in claim 8, characterized in that: The method adopts a vertical electroplating method, and a flow pump is used to ensure that the components of the acid sulfate electronic copper electroplating solution are replenished to the cathode in time; a non-conductive cutting rod is placed about 1 to 5 mm close to the cathode surface, and the cutting rod can move back and forth horizontally along the surface of the cathode and the wafer connected thereto to ensure uniform replenishment of the cathode plating solution and uniform distribution of the power lines, so that the plating thickness is uniform; square wave pulse current electroplating or direct current electroplating is adopted; the temperature of the acid sulfate electronic copper electroplating solution is 15-30°C.

10. The method for densely filling high aspect ratio through silicon via metal with electronic electroplating according to claim 9, characterized in that: The horizontal reciprocating speed of the non-conductive cutting rod is 60-500 r / min; the cathode current in the square wave pulse current electroplating is 0.2-0.3 A / dm 2 , 50~100ms, anode current 0.5~0.8A / dm 2 , 5 to 10 ms, pause time 50 to 100 ms; in the DC electroplating, the constant current density is: 0.15 / 0.2 / 0.25A / dm 2, Or segment current density: 0.1-0.3A / dm 2 .