Water-borne epoxy resin and preparation method thereof

The preparation of non-ionic emulsifiers through composite acid anhydrides and compounded with Sipan and Tween has solved the problem of poor compatibility with epoxy resin and water, significantly improved the stability and dispersion of the aqueous epoxy resin emulsion, and achieved environmental protection. Paint application.

CN119039615APending Publication Date: 2024-11-29GUANGDONG MECHANICAL & ELECTRICAL COLLEGE
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411189736.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-11-29

AI Technical Summary

Technical Problem

Traditional epoxy resins have high emissions of volatile organic compounds due to the use of organic solvents, which is harmful to the environment and the human body, and have poor compatibility with water, resulting in unstable emulsion system and difficult to disperse stably.

Method used

Nonionic emulsifiers are prepared by composite anhydrides and combined with Sipan and Tween. Through specific molar ratios and process conditions, the compatibility and stability of epoxy resin with water are improved, and high solid content and An aqueous epoxy resin emulsion with excellent dispersion stability.

Benefits of technology

It significantly improves the water-based effect and dispersion stability of the epoxy resin emulsion, reduces the surface tension of the emulsion, improves the adhesion and permeability of the paint, avoids the emulsion demulsification phenomenon, and meets modern environmental protection requirements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005014737680000091
    Figure BDA0005014737680000091
Patent Text Reader

Abstract

The invention discloses a water-borne epoxy resin and a preparation method thereof, and relates to the field of epoxy resin preparation, the preparation method of the water-borne epoxy resin comprises the following steps: mixing polyethylene glycol and methoxypolyethylene glycol, and removing water to obtain a mixture; mixing and reacting the mixture with composite anhydride to obtain an intermediate product; mixing the intermediate product with epoxy resin and a catalyst, stirring and heating to obtain a nonionic emulsifier; mixing the nonionic emulsifier with Tween and Span to obtain a nonionic compound emulsifier; and adding the nonionic compound emulsifier and the diluent into epoxy resin, heating and stirring, and dropwise adding distilled water to obtain the water-borne epoxy resin. According to the invention, the nonionic emulsifier is prepared from the composite acid anhydride and is compounded with the span and the Tween, so that the water-based effect of the epoxy resin emulsion is remarkably improved, and the prepared water-based epoxy resin emulsion has relatively high solid content and excellent dispersion stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of epoxy resin preparation, and in particular to a water-based epoxy resin and a preparation method thereof. Background Art

[0002] Epoxy resins are widely used in coatings, adhesives, composite materials and other fields due to their excellent mechanical properties, bonding properties and chemical resistance. However, traditional epoxy resins usually use organic solvents as carriers, and have problems such as high volatile organic compound (VOC) emissions and harm to the environment and human body. With increasingly stringent environmental protection requirements, water-based epoxy resins have gradually become a hot spot for research and application. Water-based epoxy resins contain no or very small amounts of organic solvents, and their VOC emissions are much lower than solvent-based epoxy resins. They help reduce air pollution and meet modern environmental protection requirements. They can be widely used in containers, ships, marine engineering, rail transit and other fields as anti-corrosion coatings.

[0003] However, there are certain technical difficulties in the preparation of water-based epoxy resins, especially the poor compatibility of epoxy resins with water, which makes them difficult to disperse stably, often leading to instability and performance degradation of the emulsion system. Summary of the invention

[0004] The main purpose of the present invention is to provide a water-based epoxy resin and a preparation method thereof, aiming to prepare a stable water-based epoxy resin emulsion by selecting a suitable emulsifier and process conditions, and to improve the compatibility, dispersibility and stability of the epoxy resin with water.

[0005] To achieve the above object, the preparation method of the waterborne epoxy resin proposed in the present invention comprises the following steps:

[0006] S10, mixing polyethylene glycol and polyethylene glycol monomethyl ether and removing water to obtain a mixture;

[0007] S20, mixing the mixture with a composite acid anhydride to react to obtain an intermediate product;

[0008] S30, mixing the intermediate product with an epoxy resin and a catalyst, stirring and heating, to obtain a nonionic emulsifier;

[0009] S40, mixing the nonionic emulsifier with Tween and Span to obtain a nonionic composite emulsifier;

[0010] S50, adding the nonionic composite emulsifier and diluent into the epoxy resin, heating and stirring, and dropping distilled water to obtain the water-based epoxy resin.

[0011] In one embodiment, in step S10:

[0012] The molar ratio of the polyethylene glycol to the polyethylene glycol monomethyl ether is 1:(0.5-2); and / or,

[0013] The polyethylene glycol includes one or both of PEG-200 and PEG-400; and / or,

[0014] The polyethylene glycol monomethyl ether includes one or both of mPEG-500 and mPEG-2000.

[0015] In one embodiment, in step S20:

[0016] The molar ratio of the mixture to the complex anhydride is 1:(0.15-0.25); and / or,

[0017] The composite anhydride comprises a first component and a second component; the first component comprises methyl hexahydrophthalic anhydride, and the second component comprises one or more of dodecenyl succinic anhydride, trimellitic anhydride, pyromellitic dianhydride, hexahydrophthalic anhydride and nadic anhydride; and / or,

[0018] The molar ratio of the first component to the second component is 1:(0.1-0.5).

[0019] In one embodiment, in step S30:

[0020] The mass ratio of the intermediate product, the epoxy resin and the catalyst is (11.5-12.5): (2-3): (0.016-0.045); and / or,

[0021] The viscosity of the epoxy resin is 8000-12000 mPa·s; and / or,

[0022] The catalyst includes tetrabutylammonium bromide.

[0023] In one embodiment, in step S40:

[0024] The molar ratio of the nonionic emulsifier, Tween and Span is 1: (0.15-0.25): (0.05-0.15); and / or,

[0025] The Span includes one or more of Span 20, Span 40, Span 60 and Span 80; and / or,

[0026] The Tween includes one or more of Tween 20, Tween 40, Tween 60 and Tween 80.

[0027] In one embodiment, in step S50:

[0028] The diluent includes one or both of polyethylene glycol PEG-200 and PEG-400; and / or,

[0029] The viscosity of the epoxy resin is 8000-12000 mPa·s.

[0030] In one embodiment, in step S50:

[0031] The molar ratio of the epoxy resin to the diluent is 10:(1-1.5); and / or,

[0032] The molar ratio of the epoxy resin to the nonionic composite emulsifier is 10:(1-1.5).

[0033] In one embodiment, in step S50, the heating temperature is 75-80°C.

[0034] The present invention also provides a waterborne epoxy resin, which is prepared by the waterborne epoxy resin preparation method.

[0035] In one embodiment, the average particle size of the waterborne epoxy resin is 23.9 μm-26.1 μm.

[0036] The technical solution of the present invention can make the emulsified particles of epoxy resin smaller by using a nonionic emulsifier prepared by composite acid anhydride, the stability of the emulsified system can be improved by adding Span, and the surface tension of the emulsified system can be reduced by adding Tween, so as to wet the sprayed substrate and improve the adhesion and permeability of the coating. Moreover, the nonionic emulsifier, Span and Tween are all nonionic, and after compounding, the water-based effect of the epoxy resin emulsion can be significantly improved. The prepared epoxy resin emulsion has a higher solid content and excellent dispersion stability, and is not easy to demulsify after emulsification. DETAILED DESCRIPTION

[0037] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0038] It should be noted that if "and / or" or "and / or" appears in the full text, its meaning includes three parallel solutions. Taking "A and / or B" as an example, it includes solution A, solution B, or solutions that satisfy both A and B. In addition, the technical solutions between the various embodiments can be combined with each other, but they must be based on the ability of ordinary technicians in the field to implement them. When the combination of technical solutions is contradictory or cannot be implemented, it should be deemed that such a combination of technical solutions does not exist and is not within the protection scope required by the present invention.

[0039] Traditional epoxy resins usually use organic solvents as carriers, which have problems such as high volatile organic compound (VOC) emissions and harm to the environment and human body. Although water-based epoxy resins contain no or very little organic solvents, and the emission of volatile organic compounds (VOC) is much lower than that of solvent-based epoxy resins, epoxy resins have poor compatibility with water and are difficult to disperse stably, resulting in unstable emulsion systems.

[0040] The present invention provides a method for preparing a waterborne epoxy resin, comprising the following steps:

[0041] S10, mixing polyethylene glycol and polyethylene glycol monomethyl ether and removing water to obtain a mixture;

[0042] S20, mixing the mixture with a composite acid anhydride to react to obtain an intermediate product;

[0043] S30, mixing the intermediate product with an epoxy resin and a catalyst, stirring and heating, to obtain a nonionic emulsifier;

[0044] S40, mixing the nonionic emulsifier with Tween and Span to obtain a nonionic composite emulsifier;

[0045] S50, adding the nonionic composite emulsifier and diluent into the epoxy resin, heating and stirring, and dropping distilled water to obtain the water-based epoxy resin.

[0046] The purpose of removing water after mixing is to ensure the purity of the reactants and the reaction efficiency and to avoid the adverse effects of moisture on subsequent reactions.

[0047] The water-based effect of epoxy resin emulsion can be significantly improved by preparing non-ionic emulsifier with composite acid anhydride and compounding it with Span and Tween. The prepared epoxy resin emulsion has a higher solid content and excellent dispersion stability.

[0048] In one embodiment of the present invention, in step S10:

[0049] The molar ratio of the polyethylene glycol to the polyethylene glycol monomethyl ether is 1:(0.5-2). The polyethylene glycol and the polyethylene glycol monomethyl ether promote the ring-opening esterification of the acid anhydride and provide a hydrophilic terminal group.

[0050] In one embodiment of the present invention, in step S10:

[0051] The polyethylene glycol includes one or both of PEG-200 and PEG-400. PEG-200 and PEG-400 have small molecular weight, high reactivity, low viscosity, and can also play a role in diluting high-viscosity epoxy resins (such as E44, E51).

[0052] In one embodiment of the present invention, in step S10:

[0053] The polyethylene glycol monomethyl ether includes one or both of mPEG-500 and mPEG-2000. Adding polyethylene glycol monomethyl ether can obtain a hydrophilic and lipophilic amphiphilic emulsifier, thereby enhancing the emulsification ability and emulsion stability.

[0054] In one embodiment of the present invention, in step S20:

[0055] The molar ratio of the mixture to the complex anhydride is 1:(0.15-0.25). Under this ratio, the complex anhydride and the mixture can undergo esterification reaction better and provide hydrophobic characteristic end groups.

[0056] In one embodiment of the present invention, in step S20:

[0057] The composite anhydride comprises a first component and a second component; the first component comprises methyl hexahydrophthalic anhydride, and the second component comprises one or more of dodecenyl succinic anhydride, trimellitic anhydride, pyromellitic dianhydride, hexahydrophthalic anhydride and nadic anhydride. Preferably, the second component comprises dodecenyl succinic anhydride. On the basis of the first component methyl hexahydrophthalic anhydride, the second component anhydride is introduced to react with polyethylene glycol and polyethylene glycol monomethyl ether, which can provide abundant hydrophilic end groups represented by hydroxyl groups and polyoxyethylene ether chains for the middle and end of the epoxy resin, and promote the formation of a balanced self-emulsifying system together with the long alkane chain hydrophobic end groups, changing the situation that the double epoxy end groups at both ends are not conducive to self-emulsification.

[0058] In one embodiment of the present invention, in step S20:

[0059] The molar ratio of the first component to the second component is 1:(0.1-0.5). Under this ratio, the number of hydrophilic end groups and hydrophobic end groups can be kept balanced.

[0060] In one embodiment of the present invention, in step S30:

[0061] The mass ratio of the intermediate product, the epoxy resin and the catalyst is (11.5-12.5): (2-3): (0.016-0.045). After the ring-opening esterification, the reaction process is accelerated by adding a catalyst.

[0062] In one embodiment of the present invention, in step S30:

[0063] The viscosity of the epoxy resin is 8000-12000 mPa·s. A higher viscosity helps to improve the stability of the emulsion and prevent particle sedimentation, thereby ensuring that the emulsion maintains uniformity over a long period of time.

[0064] In one embodiment of the present invention, in step S30:

[0065] The catalyst includes tetrabutylammonium bromide. When tetrabutylammonium bromide is used, the epoxy value decreases quickly and tends to stabilize quickly.

[0066] In one embodiment of the present invention, in step S40:

[0067] The molar ratio of the nonionic emulsifier, Tween and Span is 1: (0.15-0.25): (0.05-0.15). Under this ratio, the emulsion particles and system stability can be well balanced and a reasonable surface tension can be maintained. The surface tension of the coating affects the adhesion and penetration performance of the waterborne epoxy resin on the substrate, as well as the ability to inhibit corrosion.

[0068] In one embodiment of the present invention, in step S40:

[0069] The Span includes one or more of Span 20, Span 40, Span 60 and Span 80. The selected Span 20, Span 40, Span 60 and Span 80 can further improve the stability of the emulsion.

[0070] In one embodiment of the present invention, in step S40:

[0071] The Tween includes one or more of Tween 20, Tween 40, Tween 60 and Tween 80. The selected Tween 20, Tween 40, Tween 60 and Tween 80 can reduce the surface tension of the emulsion, increase the wettability and improve the leveling property.

[0072] In one embodiment of the present invention, in step S50:

[0073] The diluent includes one or both of polyethylene glycol PEG-200 and polyethylene glycol PEG-400. Polyethylene glycol PEG-200 and polyethylene glycol PEG-400 have relatively low molecular weights and high reactivity, and can also dilute viscous epoxy resins to promote the generation of smaller latex particles.

[0074] In one embodiment of the present invention, in step S50:

[0075] The molar ratio of the epoxy resin to the diluent is 10:(1-1.5). Under this ratio, the epoxy resin can be diluted without affecting the stability of the waterborne epoxy resin emulsified system.

[0076] In one embodiment of the present invention, in step S50:

[0077] The molar ratio of the epoxy resin to the nonionic composite emulsifier is 10:(1-1.5). At this ratio, a good emulsification effect can be achieved. When the nonionic composite emulsifier is added at a ratio less than this, the emulsification is incomplete.

[0078] In one embodiment of the present invention, in step S50:

[0079] The heating temperature is 75-80° C. The temperature will affect the viscosity of the epoxy resin. At this temperature, the viscosity of the epoxy resin is low and will not have an adverse effect on the emulsification effect.

[0080] The present invention also provides a waterborne epoxy resin, which is prepared by the preparation method of the waterborne epoxy resin. Since the waterborne epoxy resin adopts all the technical solutions of all the above embodiments, it has at least all the beneficial effects brought by the technical solutions of the above embodiments, which will not be repeated here. The waterborne epoxy resin has good dispersibility.

[0081] In one embodiment of the present invention, the average particle size of the waterborne epoxy resin is 23.9 μm-26.1 μm. Waterborne epoxy resin with a smaller particle size can be suitable for spraying and brushing construction.

[0082] Example 1

[0083] This embodiment provides a method for preparing a waterborne epoxy resin, comprising the following steps:

[0084] S10, 10 parts of PEG-200 and mPEG-500 (mixed in a molar ratio of 1:0.5), dehydrated under vacuum conditions, evacuated to 0.06 MPa, heated to 120°C, maintained for 25 minutes, and then filled with dry nitrogen, repeated 5 times, the temperature was maintained at 105°C, and the dehydration treatment of polyethylene glycol was completed to obtain a mixture;

[0085] S20, adding 1.8 parts of composite anhydride (the molar ratio of methyl hexahydrophthalic anhydride to dodecenyl succinic anhydride is 1:0.3) to the mixture, and performing esterification reaction in an oil bath at 110° C. for 2.5 hours to complete the anhydride ring-opening esterification to obtain an intermediate product;

[0086] S30, adding 2 parts of epoxy resin E51 with a viscosity of 8000 mPa·s and 0.03 parts of tetrabutylammonium bromide with a mass fraction of 1.5 wt% to 12 parts of the intermediate product, stirring at a rate of 270 rpm, maintaining the temperature at 115° C., and passing dry nitrogen for 1.5 h to obtain a nonionic emulsifier;

[0087] S40, mixing the nonionic emulsifier with Tween 40 and Span 20 in a molar ratio of 1:0.20:0.10 to obtain a nonionic composite emulsifier;

[0088] S50, 1 part of the nonionic composite emulsifier is mixed with 10 parts of epoxy resin E51 with a viscosity of 8000 mPa·s, and heated to 80°C. In order to reduce the viscosity of the system, 1.3 parts of polyethylene glycol PEG-200 are added, and stirred at a speed of 3000 rpm. 30 parts of distilled water at 85°C are slowly added dropwise until all the water phase is added. After cooling to room temperature, a stable dispersed water-based epoxy resin emulsion with a solid content of about 24% is obtained.

[0089] Example 2

[0090] This embodiment provides a method for preparing a waterborne epoxy resin, comprising the following steps:

[0091] S10, 10 parts of polyethylene glycol PEG-400 and polyethylene glycol monomethyl ether PEG-400 (mixed in a molar ratio of 1:1), dewatering the mixture under vacuum conditions, evacuating to 0.05 MPa, heating to 115° C., maintaining the temperature for 25 min, and then filling with dry nitrogen, repeating the process 3 times, maintaining the temperature at 102° C., and completing the dewatering of polyethylene glycol to obtain a mixture;

[0092] S20, adding 2 parts of composite anhydride (the molar ratio of methyl hexahydrophthalic anhydride, dodecenyl succinic anhydride, trimellitic anhydride and pyromellitic dianhydride is 1:0.30:0.05:0.05) to the mixture, and performing esterification reaction in an oil bath at 105° C. for 2 hours to complete the anhydride ring-opening esterification to obtain an intermediate product;

[0093] S30, adding 2 parts of epoxy resin E51 with a viscosity of 10000 mPa·s and 0.024 parts of tetrabutylammonium bromide with a mass fraction of 1.2 wt% to 10 parts of the intermediate product, stirring at a rate of 280 rpm, maintaining the temperature at 115° C., and passing dry nitrogen for 1.5 h to obtain a nonionic emulsifier;

[0094] S40, mixing the nonionic emulsifier with Tween 60 and Span 40 in a molar ratio of 1:0.25:0.14 to obtain a nonionic composite emulsifier;

[0095] S50, 1 part of the nonionic composite emulsifier is mixed with 10 parts of epoxy resin E51 with a viscosity of 10000 mPa·s, and heated to 75°C. In order to reduce the viscosity of the system, 1.2 parts of polyethylene glycol are added, and stirred at a speed of 3200 rpm. 30 parts of distilled water at 90°C are slowly added dropwise until all the water phase is added. After cooling to room temperature, a stable dispersed waterborne epoxy resin emulsion with a solid content of about 24% is obtained.

[0096] Example 3

[0097] This embodiment provides a method for preparing a waterborne epoxy resin, comprising the following steps:

[0098] S10, 10 parts of polyethylene glycol PEG-400 and polyethylene glycol monomethyl ether mPEG-2000 (mixed in a molar ratio of 1:2) are subjected to dehydration treatment under vacuum conditions, evacuated to 0.06 MPa, and heated to 120° C., maintained for 25 min, and then filled with dry nitrogen, and repeated 5 times, with the temperature maintained at 105° C., to complete the dehydration treatment of polyethylene glycol and obtain a mixture;

[0099] S20, adding 1.9 parts of composite anhydride (the molar ratio of methyl hexahydrophthalic anhydride, dodecenyl succinic anhydride, hexahydrophthalic anhydride and nadic anhydride is 1:0.46:0.02:0.02) to the mixture, and performing esterification reaction in an oil bath at 110° C. for 3 hours to complete the anhydride ring-opening esterification to obtain an intermediate product;

[0100] S30, adding 2 parts of epoxy resin E51 with a viscosity of 9000 mPa·s and 0.03 parts of tetrabutylammonium bromide with a mass fraction of 1.5 wt% to 10 parts of the intermediate product, stirring at a rate of 300 rpm, maintaining the temperature at 120° C., and passing dry nitrogen for 1 hour to obtain a nonionic emulsifier;

[0101] S40, mixing the nonionic emulsifier with Tween 40 and Span 60 in a molar ratio of 1:0.18:0.12 to obtain a nonionic composite emulsifier;

[0102] S50, 1.3 parts of the nonionic composite emulsifier and 10 parts of epoxy resin E51 with a viscosity of 9000 mPa·s were mixed and heated to 82°C. In order to reduce the viscosity of the system, 1.5 parts of polyethylene glycol were added and stirred at a speed of 3500 rpm. 30 parts of distilled water at 85°C were slowly added dropwise until all the water phase was added. After cooling to room temperature, a stable dispersed waterborne epoxy resin emulsion with a solid content of about 24% was obtained.

[0103] Example 4

[0104] This embodiment provides a method for preparing a waterborne epoxy resin, comprising the following steps:

[0105] S10, 10 parts of polyethylene glycol PEG-200 and polyethylene glycol monomethyl ether mPEG-2000 (mixed in a molar ratio of 1:1.5), dehydrated under vacuum conditions, evacuated to 0.06 MPa, heated to 120°C, maintained for 25 minutes, and then filled with dry nitrogen, repeated 5 times, the temperature was maintained at 105°C, and the dehydration treatment of polyethylene glycol was completed to obtain a mixture;

[0106] S20, adding 2.1 parts of composite anhydride (the molar ratio of methyl hexahydrophthalic anhydride to dodecenyl succinic anhydride is 1:0.5) to the mixture, and performing esterification reaction in an oil bath at 105° C. for 3 hours to complete the anhydride ring-opening esterification to obtain an intermediate product;

[0107] S30, adding 2 parts of epoxy resin E51 with a viscosity of 8500 mPa·s and 0.022 parts of tetrabutylammonium bromide with a mass fraction of 1.1 wt% to 9.5 parts of the intermediate product, stirring at a rate of 250 rpm, maintaining the temperature at 110° C., and passing dry nitrogen for 1 hour to obtain a nonionic emulsifier;

[0108] S40, mixing the nonionic emulsifier with Tween 60 and Span 20 in a molar ratio of 1:0.25:0.08 to obtain a nonionic composite emulsifier;

[0109] S50, 1.2 parts of the nonionic composite emulsifier and 10 parts of epoxy resin E51 with a viscosity of 8500 mPa·s were mixed and heated to 80°C. In order to reduce the viscosity of the system, 1.2 parts of polyethylene glycol were added and stirred at a speed of 2800 rpm. 30 parts of distilled water at 90°C were slowly added dropwise until all the water phase was added. After cooling to room temperature, a stable dispersed waterborne epoxy resin emulsion with a solid content of about 24% was obtained.

[0110] Comparative Example 1

[0111] This comparative example provides a method for preparing an emulsion, which is different from Example 1 in that, in step S10, only 10 parts of polyethylene glycol are added to obtain a stable dispersed aqueous epoxy resin emulsion with a solid content of about 24% after cooling to room temperature.

[0112] Comparative Example 2

[0113] This comparative example provides a method for preparing an emulsion, which is different from Example 1 in that, in step S20, only 1.8 parts of methylhexahydrophthalic anhydride are added to obtain a stable dispersed aqueous epoxy resin emulsion with a solid content of about 24% after cooling to room temperature.

[0114] Comparative Example 3

[0115] This comparative example provides a method for preparing an emulsion, which is different from Example 1 in that step S40 is omitted, the nonionic emulsifier is not mixed with the surfactant Tween and Span, but 1 part of the nonionic emulsifier is directly mixed with 10 parts of epoxy resin with a viscosity of 8000 mPa·s, and the subsequent operation is continued. After cooling to room temperature, a stable dispersed aqueous epoxy resin emulsion with a solid content of about 24% is obtained.

[0116] Comparative Example 4

[0117] This comparative example provides a method for preparing an emulsion, which is different from Example 1 in that in step S40, the nonionic emulsifier is only mixed with Tween at a molar ratio of 1:0.1. After cooling to room temperature, a stable dispersed aqueous epoxy resin emulsion with a solid content of about 24% is obtained.

[0118] 250 mL of each of the waterborne epoxy resin emulsion obtained in Example 1-4 and the emulsion obtained in Comparative Example 1-4 were taken and placed in a beaker, sealed with a sealing film, and left to stand at 25° C. for 7 days. The waterborne epoxy resin emulsion obtained in Example 1-4 and the emulsion obtained in Comparative Example 1-4 were analyzed using a laser particle size analyzer. The results are shown in the following table.

[0119] Table 1 Dispersibility and average particle size analysis

[0120]

[0121]

[0122] As can be seen from Table 1, when only polyethylene glycol participated in esterification (Comparative Example 1), under other conditions identical with Example 1, the composite emulsifier obtained emulsifies epoxy resin, and the emulsion particles obtained are larger, and the particles are easily unevenly sprayed when applied, affecting the coating surface quality. When only methyl hexahydrophthalic anhydride is used as anhydride to participate in esterification (Comparative Example 2), the composite emulsifier obtained emulsifies epoxy resin, and owing to not introducing hydrophobic end groups, emulsifying ability is relatively weak, so the emulsion particle size distribution obtained is uneven, and standing for 7 days has the phenomenon of stratification. When only nonionic emulsifier participates in epoxy resin emulsification (Comparative Example 3), the emulsion particles obtained are little, and owing to not introducing Span, system stability is weak, and standing for 7 days has stratification. In Comparative Example 4, when the nonionic emulsifier was mixed only with Tween to emulsify the epoxy resin (Comparative Example 4), the size of the emulsion particles did not change significantly, but since the Span was not introduced, the system stability was weak and stratification occurred after standing for 7 days.

[0123] The preparation method of the water-based epoxy resin provided by the present invention can not only effectively improve the water-based degree of the epoxy resin, but also significantly improve the stability and dispersibility of the epoxy resin emulsion. In the traditional preparation process of water-based epoxy resin, the phase separation phenomenon of the emulsion is often serious due to improper selection of emulsifiers or poor process conditions, which affects the product performance. However, the present invention significantly improves the uniformity and stability of the emulsion by introducing a composite anhydride and an emulsifier with a specific ratio, combined with a precisely controlled esterification reaction and a high-speed stirring process, and solves many problems in the prior art.

[0124] The above description is only an exemplary embodiment of the present invention, and does not limit the patent scope of the present invention. All equivalent structural changes made by using the present invention specification under the technical concept of the present invention, or directly / indirectly applied in other related technical fields are included in the patent protection scope of the present invention.

Claims

1. A method for preparing a waterborne epoxy resin, characterized in that: The following steps are involved: S10, mixing polyethylene glycol and polyethylene glycol monomethyl ether and removing water to obtain a mixture; S20, mixing the mixture with a composite acid anhydride to react to obtain an intermediate product; S30, mixing the intermediate product with an epoxy resin and a catalyst, stirring and heating, to obtain a nonionic emulsifier; S40, mixing the nonionic emulsifier with Tween and Span to obtain a nonionic composite emulsifier; S50, adding the nonionic composite emulsifier and diluent into the epoxy resin, heating and stirring, and adding distilled water dropwise to obtain the water-based epoxy resin.

2. The method for preparing a waterborne epoxy resin according to claim 1, wherein: In step S10: The molar ratio of the polyethylene glycol to the polyethylene glycol monomethyl ether is 1:(0.5-2); and / or, The polyethylene glycol includes one or both of PEG-200 and PEG-400; and / or, The polyethylene glycol monomethyl ether includes one or both of mPEG-500 and mPEG-2000.

3. The method for preparing a waterborne epoxy resin according to claim 1, wherein: In step S20: The molar ratio of the mixture to the complex anhydride is 1:(0.15-0.25); and / or, The composite anhydride comprises a first component and a second component; the first component comprises methyl hexahydrophthalic anhydride, and the second component comprises one or more of dodecenyl succinic anhydride, trimellitic anhydride, pyromellitic dianhydride, hexahydrophthalic anhydride and nadic anhydride; and / or, The molar ratio of the first component to the second component is 1:(0.1-0.5).

4. The method for preparing a waterborne epoxy resin according to claim 1, wherein: In step S30: The mass ratio of the intermediate product, the epoxy resin and the catalyst is (11.5-12.5): (2-3): (0.016-0.045); and / or, The viscosity of the epoxy resin is 8000-12000 mPa·s; and / or, The catalyst includes tetrabutylammonium bromide.

5. The method for preparing a waterborne epoxy resin according to claim 1, wherein: In step S40: The molar ratio of the nonionic emulsifier, Tween and Span is 1: (0.15-0.25): (0.05-0.15); and / or, The Span includes one or more of Span 20, Span 40, Span 60 and Span 80; and / or, The Tween includes one or more of Tween 20, Tween 40, Tween 60 and Tween 80.

6. The method for preparing a waterborne epoxy resin according to claim 1, characterized in that: In step S50: The diluent includes one or both of polyethylene glycol PEG-200 and PEG-400; and / or, The viscosity of the epoxy resin is 8000-12000 mPa·s.

7. The method for preparing a waterborne epoxy resin according to claim 1, characterized in that: In step S50: The molar ratio of the epoxy resin to the diluent is 10:(1-1.5); and / or, The molar ratio of the epoxy resin to the nonionic composite emulsifier is 10:(1-1.5).

8. The method for preparing a waterborne epoxy resin according to claim 1, wherein: In step S50, the heating temperature is 75-80°C.

9. A water-based epoxy resin, characterized in that: The waterborne epoxy resin is prepared by the preparation method of the waterborne epoxy resin according to any one of claims 1 to 8.

10. The waterborne epoxy resin according to claim 9, characterized in that The average particle size of the waterborne epoxy resin is 23.9 μm-26.1 μm.

Citation Information

Cited By

  • Method for producing water-soluble epoxy (METH)acrylate composition, emulsion, coating composition, coating film, and cured coating film

    JP2025085432A

  • Method for producing water-soluble epoxy (meth)acrylate composition, emulsion, coating composition, coating film, and cured coating film

    JP7874326B2