Method for growing large-size plate-shaped Ce: Yb: YAG single crystal

By adjusting the crucible movement speed and supplementing CeO2 into the melt during the growth process, the problems of Ce:Yb:YAG single crystal in the shoulder-release area and CeO2 volatility are solved, and high-quality growth of large-size plate-shaped single crystals is achieved.

CN118932477APending Publication Date: 2024-11-12CHINA ELECTRONICS TECH GRP NO 26 RES INST
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411004787.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

When the prior art, when growing Ce:Yb:YAG single crystal, the crucible is prone to defects such as bubbles and clouds in the shoulder area, and CeO2 is prone to volatilization at high temperatures, resulting in a decrease in the Ce4+ content.

Method used

By adjusting the movement speed of the crucible, it gradually increases from 0 to 1 to 3 mm/h, and during the movement of the crucible, CeO2 is added to the melt through the feeding mechanism to ensure the stability of the Ce4+ content.

Benefits of technology

The cloud layer and bubble defects of the crystal in the shoulder area are reduced, and the Ce4+ content is reduced due to excessive CeO2 volatility, and a high-quality finished product of large-sized plate-shaped Ce:Yb:YAG single crystal is obtained.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118932477A_ABST
    Figure CN118932477A_ABST
Patent Text Reader

Abstract

The invention discloses a method for growing a large-size plate-shaped Ce: Yb: YAG single crystal, and the method specifically comprises the following steps: step 1, uniformly mixing CeO2, Yb2O3, Y2O3 and Al2O3 according to a ratio, putting the mixture into a pressing die, and pressing the mixture into a raw material block; 2, putting the raw material blocks into a crucible with a seed crystal groove, adding seed crystals into the seed crystal groove in the crucible, and then putting the crucible into a heater of a horizontal directional crystal growth furnace; 3, heating the crystal growth furnace in a vacuum state until the raw materials are completely molten; 4, after the raw materials are molten, the moving speed of the crucible is gradually increased from 0-1 mm / h to 1-3 mm / h from the seeding point to the shouldering ending position; when the crucible begins to move, CeO2 is added into the melt through a feeding mechanism; 5, after the crucible is completely moved out of the heater, growth of the Ce: Yb: YAG crystal is completed, then cooling is conducted to the room temperature, vacuum is closed, and the large-size plate-shaped Ce: Yb: YAG single crystal is obtained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of artificial single crystal preparation, and in particular to a method for growing a large-sized plate-shaped Ce:Yb:YAG single crystal. Background Art

[0002] Ce:Yb:YAG is a YAG-based material. 3+ and Yb 3+ As a down-conversion material of co-doped ions. Ce 3 + Absorbs visible light energy and transfers it to the nearby Yb 3+ , thereby achieving the conversion of visible light to near-infrared light. The crystal is mainly used to improve the energy conversion efficiency of silicon solar cells.

[0003] In the prior art, when preparing this material, when using the horizontal directional crystallization method to grow Ce:Yb:YAG crystals, the speed is generally about 3mm / h, and the crucible is moved at a constant speed to complete the crystal seeding, shoulder release and equal width growth. However, the crystals grown at this speed are prone to defects such as bubbles and clouds in the shoulder release area, which affects the crystal quality. At the same time, CeO2 is very volatile at high temperatures, and the amount of CeO2 volatilization increases with the increase in temperature, resulting in CeO2 volatilization. 4+ The content in the crystals is reduced. Summary of the invention

[0004] In view of the above-mentioned deficiencies in the prior art, the object of the present invention is to provide a method for growing large-sized plate-shaped Ce:Yb:YAG single crystals, so as to solve the problems in the prior art that crystals are prone to defects such as bubbles and clouds when growing in the shoulder area, and CeO2 is extremely volatile.

[0005] In order to solve the above technical problems, the present invention adopts the following technical solutions:

[0006] A method for growing a large-sized plate-shaped Ce:Yb:YAG single crystal comprises the following steps:

[0007] Step 1: CeO2, Yb2O3, Y2O3 and Al2O3 are mixed evenly according to the proportion, and loaded into a pressing mold to press them into a raw material block;

[0008] Step 2: placing the raw material block into a crucible with a seed crystal groove, adding seed crystals into the seed crystal groove in the crucible, and then placing the crucible into a heater of a horizontal directional crystal growth furnace;

[0009] Step 3: The crystal growth furnace is in a vacuum state, and the temperature is raised until the raw materials are completely melted;

[0010] Step 4: After the raw materials are melted, the moving speed of the crucible gradually increases from 0-1 mm / h to 1-3 mm / h from the seeding point to the end position of the shoulder release; at the same time as the crucible starts to move, CeO2 is added to the melt through the feeding mechanism.

[0011] Step 5: After the crucible is completely removed from the heater, the growth of the Ce:Yb:YAG crystal is completed, and then the crucible is cooled to room temperature and the vacuum is turned off to obtain the large-sized plate-shaped Ce:Yb:YAG single crystal.

[0012] Preferably, the molar ratio of CeO2, Yb2O3, Y2O3 and Al2O3 is x:y:(3-xy):5; wherein, calculated as molar percentage, 0.125%≤x≤12.5%, 25%≤y≤37.375%.

[0013] Preferably, in step 3, the temperature is raised to 2100° C. at 300° C. / h, and then kept at this temperature to completely melt the raw materials.

[0014] Preferably, in step 3, the insulation time is 1 to 8 hours.

[0015] Preferably, in step 5, the temperature is lowered to room temperature at a rate of 40-45°C / h.

[0016] Preferably, in step 4, the crucible movement speed is specifically adjusted as follows: at the shoulder position, the crucible movement speed is uniformly accelerated from 0 mm / h to 3 mm / h, and at the equal width position, the crucible moves at a uniform speed of 3 mm / h until the crucible is completely moved out of the heater.

[0017] Among them, the amount of CeO2 added in step 4 needs to be confirmed in advance, and the specific steps are as follows:

[0018] S1: Weigh and prepare CeO2, Yb2O3, Y2O3 and Al2O3 in a molar ratio of x:y:(3-xy):5, mix them evenly, put them into a pressing mold and press them into raw material blocks; wherein, calculated by molar percentage, 0.125%≤x≤12.5%, 25%≤y≤37.375%.

[0019] S2: Put the raw material block obtained in S1 into a crucible with a seed crystal groove, add seed crystals into the seed crystal groove in the crucible, and then put the crucible into the heater of the horizontal directional crystal growth furnace.

[0020] S3: The crystal growth furnace is placed in a vacuum state, and the temperature is raised until the raw materials are completely melted, and the temperature is kept constant for 1h, 2h, 3h, 4h, 5h, 6h, 7h, and 8h respectively.

[0021] S4: After the raw materials are melted, the crucible moving speed is uniformly accelerated from 0 mm / h to 3 mm / h at the shoulder position, and the crucible moves at a uniform speed of 3 mm / h at the equal width position.

[0022] S5: After the crucible is completely removed from the heater, the crystals prepared at different holding times are obtained, and then the mass of the prepared crystals is subtracted from the total mass of the raw materials to obtain the mass of CeO2 that needs to be supplemented during the holding time and the crystal growth rate. For example, when the holding time is 1 hour, the crystals prepared at the holding time are obtained, and the mass of the crystals prepared at the holding time is subtracted from the total mass of the raw materials to obtain the mass of CeO2 that needs to be supplemented during the holding time of 1 hour.

[0023] Compared with the prior art, the present invention has the following beneficial effects:

[0024] 1. The present invention changes the moving speed of the crucible during the crystal growth process, especially changes the moving speed of the crucible in the three areas of crystal seeding, shoulder release, and equal-width growth, so that the moving speed of the crucible is gradually increased from 0 to 3 mm / h. In this way, the crucible is in a variable speed moving state during the crystal growth process, which can reduce the cloud layer and bubbles in the shoulder release area of ​​the crystal and prevent polycrystalline from appearing at the tail of the crystal, thereby obtaining a large-sized plate-shaped Ce:Yb:YAG single crystal.

[0025] 2. The present invention also considers solving the problem of large-scale volatilization of CeO2. The present invention uses a feeding mechanism to timely add CeO2 to the melt during crystal growth, thereby stabilizing Ce in the crystal. 4+ The content of CeO2 is very volatile, which ultimately solves the problem of Ce 4+ The problem of reduced content in crystals. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 This is the crystal image under an optical microscope before the growth method of Comparative Example 1 is improved.

[0027] Figure 2 This is the crystal image under an optical microscope after the growth method of Example 1 is improved. DETAILED DESCRIPTION

[0028] The present invention will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. All other embodiments obtained by ordinary technicians in this field based on the present invention belong to the scope of protection of the present invention.

[0029] Unless otherwise indicated in specific cases in the present invention, the numerical ranges listed herein include the upper and lower limits, and all integers and fractions within the range, and are not limited to the specific values ​​listed when defining the range.

[0030] 1. A method for growing large-size plate-shaped Ce:Yb:YAG single crystals

[0031] Step 1: CeO2, Yb2O3, Y2O3 and Al2O3 are mixed evenly according to the proportion, and loaded into a pressing mold to press them into a raw material block;

[0032] Step 2: placing the raw material block into a crucible with a seed crystal groove, adding seed crystals into the seed crystal groove in the crucible, and then placing the crucible into a heater of a horizontal directional crystal growth furnace;

[0033] Step 3: The crystal growth furnace is in a vacuum state, and the temperature is raised until the raw materials are completely melted;

[0034] Step 4: After the raw materials are melted, the moving speed of the crucible gradually increases from 0-1 mm / h to 1-3 mm / h from the seeding point to the end position of the shoulder release; at the same time as the crucible starts to move, CeO2 is added to the melt through the feeding mechanism.

[0035] Step 5: After the crucible is completely removed from the heater, the growth of the Ce:Yb:YAG crystal is completed, and then the crucible is cooled to room temperature and the vacuum is turned off to obtain the large-sized plate-shaped Ce:Yb:YAG single crystal.

[0036] When the prior art adopts the horizontal directional crystallization method to grow Ce:Yb:YAG crystals, a speed of 3mm / h is generally used to uniformly move the crucible to complete the crystal seeding, shouldering, and equal-width growth. However, crystals grown at this speed are very prone to defects such as bubbles and clouds in the shouldering area, which affects the quality of the crystal. Moreover, when faced with the problem of high-temperature volatilization of CeO2, the prior art generally increases the amount of CeO2 during the batching process to compensate for the loss caused by the high-temperature volatilization of CeO2. However, this will lead to an excessive amount of CeO2 in the raw material system, which will in turn cause new problems: composition deviation, and the inability to accurately predict the volatilization amount of CeO2 before crystal growth, resulting in Ce in the crystal. 4+ The content of ions deviates from the final expectation.

[0037] In order to solve the above technical problems, the present invention considers improving the preparation method. First, the moving speed of the crucible is adjusted. When adjusting the moving speed of the crucible, the present invention finds that if the crystal grows at a speed that ensures that no polycrystals appear at the tail of the equal-width region, more macro defects such as clouds and bubbles will appear in the seeding point and shoulder area of ​​the crystal; but if the crystal grows at a speed that ensures that no macro defects such as clouds and bubbles appear at the seeding point and shoulder area, a long distance of polycrystals will appear at the tail of the equal-width area of ​​the crystal. Both of the above situations will affect the quality and utilization rate of the crystal. Therefore, the present invention considers allowing the crucible to move at a variable speed, that is, by changing the moving speed of the crucible in the three regions of seeding, shouldering, and equal-width growth, the moving speed of the crucible in the seeding and shouldering regions is gradually increased, thereby reducing the appearance of macro defects such as clouds and bubbles in the shoulder area of ​​the crystal. However, only adjusting the crucible moving speed is not enough to solve the technical problems caused by the volatilization of CeO2. Therefore, on this basis, the present invention adds CeO2 to the melt through a feeding mechanism during the crystal growth process, thereby achieving the goal of stabilizing CeO2 in the crystal. 4+ The purpose of the content is to ensure that there will be no polycrystalline at the tail of the crystal.

[0038] In some embodiments, the present invention calculates the amount of CeO2 added in step 4 more accurately, and can accurately obtain the amount of CeO2 that needs to be added under different insulation conditions, which can fundamentally solve the technical problems caused by the volatilization of CeO2 and avoid excessive supplementation of CeO2. The amount of CeO2 added in step 4 needs to be confirmed in advance, and the specific steps are as follows:

[0039] S1: Weigh and prepare CeO2, Yb2O3, Y2O3 and Al2O3 in a molar ratio of x:y:(3-xy):5, mix them evenly, put them into a pressing mold and press them into raw material blocks; wherein, calculated by molar percentage, 0.125%≤x≤12.5%, 25%≤y≤37.375%.

[0040] S2: Put the raw material block obtained in S1 into a crucible with a seed crystal groove, add seed crystals into the seed crystal groove in the crucible, and then put the crucible into the heater of the horizontal directional crystal growth furnace.

[0041] S3: The crystal growth furnace is placed in a vacuum state, and the temperature is raised until the raw materials are completely melted, and the temperature is kept constant for 1h, 2h, 3h, 4h, 5h, 6h, 7h, and 8h respectively.

[0042] S4: After the raw materials are melted, the crucible moving speed is uniformly accelerated from 0 mm / h to 3 mm / h at the shoulder position, and the crucible moves at a uniform speed of 3 mm / h at the equal width position.

[0043] S5: After the crucible is completely removed from the heater, the crystals prepared under different holding times are obtained, and then the mass of the prepared crystals is subtracted from the total mass of the raw materials to obtain the mass of CeO2 that needs to be supplemented during the holding time and the crystal growth rate. For example, when the holding time is 1 hour, at the same time, after the raw materials are melted, the crucible movement speed is uniformly accelerated from 0mm / h to 3mm / h at the shoulder position, and the crucible moves at a uniform speed of 3mm / h at the equal width position. Under such conditions, the crystals prepared under this condition are obtained by subtracting the mass of the crystals prepared under the holding time from the total mass of the raw materials, and the mass of CeO2 that needs to be supplemented when the holding time is 1 hour is obtained.

[0044] In some embodiments, the molar ratio of CeO2, Yb2O3, Y2O3 and Al2O3 is x:y:(3-xy):5; wherein, calculated as molar percentage, 0.125%≤x≤12.5%, 25%≤y≤37.375%.

[0045] In some embodiments, in step 3, the temperature is increased to 2100° C. at 300° C. / h, and then kept at this temperature to completely melt the raw materials.

[0046] In some embodiments, in step 3, the holding time is 1 to 8 hours. If the holding time is too long, the component segregation inside the crystal will be aggravated, especially for a multi-component system, which will lead to uneven chemical composition of the crystal, and will also cause cracks to appear at the interface between the crystal and the melt, reducing the integrity and optical quality of the crystal, and some impurities will precipitate from the melt after too long holding, ultimately affecting the purity and transparency of the crystal. However, if the holding time is too short, the crystal growth will be incomplete, unable to reach the expected size and quality, and will also lead to an increase in defects such as dislocations and voids. At the same time, if the holding time is too short, the crystal will enter cooling too quickly, resulting in uneven distribution of components inside the crystal, increased internal stress, and may cause crystal rupture in severe cases. Therefore, the holding time can be 1h, 2h, 3h, 4h, 5h, 6h, 7h, 8h, etc., and all ranges and sub-ranges between the above values.

[0047] In some embodiments, in step 5, the temperature is lowered to room temperature at a rate of 40-45°C / h. The cooling rate may be 40°C / h, 41°C / h, 42°C / h, 43°C / h, 44°C / h, 45°C / h, etc., and all ranges and sub-ranges between the above values.

[0048] In some embodiments, in step 4, the crucible movement speed is specifically adjusted as follows: at the shoulder position, the crucible movement speed is uniformly accelerated from 0 mm / h to 3 mm / h, and at the equal width position, the crucible moves at a uniform speed of 3 mm / h until the crucible is completely moved out of the heater.

[0049] 2. Examples and Comparative Examples

[0050] Embodiment 1:

[0051] Use CeO2, Yb2O3, Y2O3 and Al2O3 powders with a purity of 5N as raw materials, weigh two portions of raw materials respectively, wherein each portion of raw materials contains 0.55g CeO2, 100.93g Yb2O3, 664.35g Yb2O3, 544.02g Al2O3, and the total mass of each portion of raw materials is 1309.85g. Use a three-position swing arm machine to evenly mix the weighed two portions of CeO2, Yb2O3, Y2O3 and Al2O3 for 3h, and then load them into a boat-shaped pressing mold to press the raw materials (pressure value 0.5Mpa, pressure holding 5 hours). Add one portion of the raw materials pressed into a boat shape into a molybdenum crucible with a seed crystal groove. Put a seed crystal in the seed crystal groove of the molybdenum crucible, and then put the crucible into the lateral crystal growth furnace heater, the seed crystal is located at the edge of the heater, and then the furnace is closed and the vacuum pump is turned on. After 5 hours, the furnace vacuum degree reaches 4.2x10 -3 Pa. Heating at a rate of 300℃ / h for 7h. After the heating is completed. The temperature inside the furnace is stabilized at 2100℃ and kept warm for 5h. It is found that the raw material is completely melted. Within the length of 20mm (shoulder length), the moving speed of the molybdenum crucible is gradually increased from 0mm / h to 3mm / h at a uniform speed. After that, the crucible is moved out of the heater at a uniform speed of 3mm / h in the horizontal direction for crystal growth. After 150h, the crucible is completely moved out of the heater and the crystal growth is completed. Cooling at a rate of 42℃ / h for 50h. After the actual temperature inside the furnace reaches room temperature, the vacuum is turned off to take out the crystal. The crystal weight is 1309.51g by weighing, and the mass of volatilized CeO2 is 0.34g CeO2.

[0052] Put the other pressed boat-shaped raw material into the furnace according to the above steps and evacuate. After 3.5 hours, the vacuum degree of the furnace reaches 6.8x10 -3 Pa. Heating at a rate of 300℃ / h for 7h. After the heating is completed. Let the temperature inside the furnace stabilize at 2100℃ and keep it warm for 5h. It is found that the raw material is completely melted. Weigh 0.34g CeO2 and add it to the equipment feeder. Within the range of 20mm length (shoulder length), the moving speed of the molybdenum crucible is gradually increased from 0mm / h to 3mm / h at a uniform speed. After that, the crucible is moved out of the heater at a uniform speed of 3mm / h in the horizontal direction for crystal growth. At the same time as the crucible begins to move, the raw material CeO2 in the feeder is slowly added to the melt to supplement the volatilization of CeO2. After 150h, the crucible is completely removed from the heater and the crystal growth is completed. Cool down at a rate of 42℃ / h for 50h. After the actual temperature inside the furnace reaches room temperature, turn off the vacuum and take out the crystal. The crystal is intact without cracks, and there are no defects such as cloud bubbles.

[0053] Embodiment 2:

[0054] Use CeO2, Yb2O3, Y2O3 and Al2O3 powders with a purity of 5N as raw materials, weigh two portions of raw materials respectively, wherein each portion of raw materials contains 0.55g CeO2, 100.93g Yb2O3, 664.35g Yb2O3, 544.02g Al2O3, and the total mass of each portion of raw materials is 1309.85g. Use a three-position swing arm machine to evenly mix the weighed two portions of CeO2, Yb2O3, Y2O3 and Al2O3 for 3 hours, and then load them into a boat-shaped pressing mold to press the raw materials (pressure value 0.5Mpa, pressure holding for 3 hours). Add one portion of the raw materials pressed into a boat shape into a molybdenum crucible with a seed crystal groove. Put a seed crystal in the seed crystal groove of the molybdenum crucible, and then put the crucible into the lateral crystal growth furnace heater, the seed crystal is located at the edge of the heater, and then the furnace is closed and the vacuum pump is turned on. After 6 hours, the furnace vacuum degree reaches 2.7x10 -3 Pa. Heating at a rate of 300℃ / h for 7h. After the heating is completed. The temperature inside the furnace is stabilized at 2100℃ and kept warm for 2h. It is found that the raw material is completely melted. Within the length of 20mm (shoulder length), the moving speed of the molybdenum crucible is gradually increased from 0mm / h to 3mm / h at a uniform speed. After that, the crucible is moved out of the heater at a uniform speed of 3mm / h in the horizontal direction for crystal growth. After 150h, the crucible is completely moved out of the heater and the crystal growth is completed. Cooling at a rate of 42℃ / h for 50h. After the actual temperature inside the furnace reaches room temperature, the vacuum is turned off to take out the crystal. The weight of the crystal is 1309.73g, and the mass of volatilized CeO2 is 0.12g CeO2.

[0055] Put the other pressed boat-shaped raw material into the furnace according to the above steps and evacuate. After 6 hours, the vacuum degree of the furnace reaches 3.3x10 -3 Pa. Heating at a rate of 300℃ / h for 7h. After the heating is completed. Let the temperature inside the furnace stabilize at 2100℃ and keep it warm for 2h. It is found that the raw material is completely melted. Weigh 0.12g CeO2 and add it to the equipment feeder. Within the range of 20mm length (shoulder length), the moving speed of the molybdenum crucible is gradually increased from 0mm / h to 3mm / h at a uniform speed. After that, the crucible is moved out of the heater at a uniform speed of 3mm / h in the horizontal direction for crystal growth. At the same time as the crucible begins to move, the raw material CeO2 in the feeder is slowly added to the melt to supplement the volatilization of CeO2. After 150h, the crucible is completely removed from the heater and the crystal growth is completed. Cool down at a rate of 42℃ / h for 50h. After the actual temperature inside the furnace reaches room temperature, turn off the vacuum and take out the crystal. The crystal is intact without cracks, and there are no defects such as cloud bubbles.

[0056] Comparative Example 1:

[0057] Use CeO2, Yb2O3, Y2O3 and Al2O3 powders with a purity of 5N as raw materials, and weigh 0.55g, 100.93g, 664.35g, and 544.02g respectively. Use a three-position swing arm machine to evenly mix the weighed CeO2, Yb2O3, Y2O3 and Al2O3 for 3 hours, and then put them into a boat-shaped pressing mold to press the raw materials (pressure value 0.5Mpa, pressure holding for 3 hours). Add the raw materials pressed into a boat shape into a molybdenum crucible with a seed crystal groove. Put a seed crystal in the seed crystal groove of the molybdenum crucible, and then put the crucible into the heater of the horizontal crystal growth furnace, with the seed crystal located at the edge of the heater, and then close the furnace and turn on the vacuum pump. After 4 hours, the vacuum degree of the furnace reaches 2.9x10 -3 Pa. Heating at a rate of 300℃ / h for 7h, after heating was completed. It was found that the raw material was partially melted. The temperature inside the furnace was stabilized at 2100℃ and kept warm for 3h, and it was found that the raw material was completely melted. The molybdenum crucible was moved out of the heater horizontally at a moving speed of 5mm / h for crystal growth. After 94h, the crucible was completely moved out of the heater and the crystal growth was completed. Cooling at a rate of 42℃ / h for 50h, after the actual temperature inside the furnace reached room temperature, the vacuum was turned off and the crystal was taken out. The crystal was severely cracked inside and contained a large number of defects such as clouds and bubbles.

[0058] from Figure 1 and Figure 2 It can be seen that:

[0059] (1) The crystal obtained in Example 1 is intact without cracks and has no defects such as cloud bubbles. At the same time, due to the precise addition of CeO2, the crystal does not deviate from the composition. 4+ The ion content fully meets the design requirements.

[0060] (2) The crystal obtained in Comparative Example 1 had severe cracks inside and contained a large number of defects such as clouds and bubbles as could be observed by the naked eye. In addition, since the amount of CeO2 was not supplemented, the CeO2 content in the final crystal was 4+ The ion content is low.

[0061] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the technical solution. Those skilled in the art should understand that those modifications or equivalent substitutions of the technical solution of the present invention that do not depart from the purpose and scope of the technical solution should be included in the scope of the claims of the present invention.

Claims

1. A method for growing a large-sized plate-shaped Ce:Yb:YAG single crystal, characterized in that: The specific steps include: Step 1: CeO2, Yb2O3, Y2O3 and Al2O3 are mixed evenly according to the proportion, and loaded into a pressing mold to press them into a raw material block; Step 2: placing the raw material block into a crucible with a seed crystal groove, adding seed crystals into the seed crystal groove in the crucible, and then placing the crucible into a heater of a horizontal directional crystal growth furnace; Step 3: The crystal growth furnace is in a vacuum state, and the temperature is raised until the raw materials are completely melted; Step 4: After the raw materials are melted, the moving speed of the crucible is gradually increased from 0-1 mm / h to 1-3 mm / h from the seeding point to the end position of the shoulder release; while the crucible starts to move, CeO2 is added to the melt through the feeding mechanism; Step 5: After the crucible is completely removed from the heater, the growth of the Ce:Yb:YAG crystal is completed, and then the crucible is cooled to room temperature and the vacuum is turned off to obtain the large-sized plate-shaped Ce:Yb:YAG single crystal.

2. The method according to claim 1, characterized in that: The molar ratio of CeO2, Yb2O3, Y2O3 and Al2O3 is x:y:(3-xy):5; wherein, calculated in terms of molar percentage, 0.125%≤x≤12.5%, 25%≤y≤37.375%.

3. The method according to claim 1, characterized in that: In step 3, the temperature is raised to 2100°C at 300°C / h and then maintained at this temperature to completely melt the raw materials.

4. The method according to claim 3, characterized in that: In step 3, the insulation time is 1 to 8 hours.

5. The method according to claim 1, characterized in that: In step 5, the temperature is lowered to room temperature at a rate of 40 to 45°C / h.

6. The method according to claim 1, characterized in that: In step 4, the specific adjustment method of the crucible moving speed is as follows: at the shoulder position, the crucible moving speed is uniformly accelerated from 0 mm / h to 3 mm / h, and at the equal width position, the crucible keeps moving at a uniform speed of 3 mm / h until the crucible is completely moved out of the heater.