Organic-inorganic hybrid single-crystal molecular ferroelectric and preparation and application thereof
The co-precipitation method was used to prepare organic-inorganic hybrid single-crystal molecular ferroelectrics [C8N4H28][Sb2Cl10], which solved the problem of small band gap in traditional methods, achieved a wider band gap and higher photoelectric performance, and expanded its application in optoelectronic devices.
Patent Information
- Application Number
- CN202411011809.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-12
AI Technical Summary
Traditional preparation methods result in small band gaps in organic-inorganic hybrid molecular ferroelectric materials, limiting their application potential in high-frequency electronic devices and ultraviolet light detectors. Furthermore, the high recombination rate of photogenerated carriers affects the stability and reliability of the materials.
Organic-inorganic hybrid single-crystal molecular ferroelectric [C8N4H28][Sb2Cl10] was prepared by co-precipitation method. By adjusting the ratio of Sb2O3, HCl, 1,4-diaminobutane and ethyl acetate and the reaction time, an orthorhombic crystal system with spontaneous polarization characteristics was formed, thus realizing a wide-bandgap molecular ferroelectric.
The prepared single-crystal molecular ferroelectric has a wider band gap, which improves its photoelectric properties and expands its application potential in optoelectronic devices, especially showing significant advantages in ultraviolet photodetectors.
Smart Images

Figure CN118932494A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of molecular ferroelectric technology, in particular to an organic-inorganic hybrid single crystal molecular ferroelectric and its preparation and application. Background Art
[0002] Organic-inorganic hybrid molecular ferroelectrics are emerging materials that have great potential in revolutionizing the field of optoelectronic devices, but they face important technical challenges. Traditional preparation methods usually result in a small band gap in ferroelectric materials, which becomes the main factor limiting their application efficiency and performance. A small band gap means that the material performs poorly when absorbing high-energy photons, especially energy in the ultraviolet region, limiting its application potential in high-frequency electronic devices and ultraviolet light detection devices. Due to the small band gap, the photoelectric conversion efficiency is significantly affected, and the carriers excited by photons can only be generated within a narrow energy range, thereby limiting the material's response ability in the energy peak region. For example, for ultraviolet light detection devices, the detection sensitivity and response speed of high-energy ultraviolet light are extremely sensitive to the size of the material's band gap. In addition, a small band gap may also lead to an increase in the recombination rate of photogenerated carriers, thereby affecting the material's performance in long-term stability and reliability.
[0003] Therefore, current research and development focuses on overcoming these problems and effectively regulating the electronic structure of molecular ferroelectrics through new synthesis strategies and structural design to achieve a larger band gap. These efforts aim to address the limitations of traditional preparation methods and improve the optoelectronic properties of materials to expand their potential for widespread application in optoelectronic devices. Summary of the invention
[0004] In order to solve the above problems, the purpose of the present invention is to provide an organic-inorganic hybrid single crystal molecular ferroelectric and its preparation and application. The chemical formula of the organic-inorganic hybrid single crystal molecular ferroelectric of the present invention is [C8N4H 28 ][Sb2Cl 10 ], at 193K, the crystal belongs to the orthorhombic system, the space group is Pc, and its crystal structure consists of two corner-shared SbCl6 octahedrons and independent 1,4-diaminobutane molecules. This organic molecule orderly surrounds [Sb2Cl 10 ] 2- Around , the octahedra show an obvious asymmetric structure due to the position offset or relative movement of the bridging chlorine atoms; this structural property causes the charge centers of the positive ions and anions to not overlap, thus showing the characteristics of spontaneous polarization.
[0005] The present invention adopts a coprecipitation method to prepare an organic-inorganic hybrid single crystal molecular ferroelectric, which is simple and has a low preparation cost, and can obtain [C8N4H 28 ][Sb2Cl 10Molecular ferroelectrics (wide bandgap). Their unique molecular structure and ferroelectric properties provide new possibilities for the design and development of new electronic devices, especially in ultraviolet light detection applications, bringing important innovations and progress to modern scientific and technological applications, and can be further applied to solar cells and light detectors.
[0006] The purpose of the present invention can be achieved by the following technical solutions:
[0007] The first object of the present invention is to provide a method for preparing an organic-inorganic hybrid single crystal molecular ferroelectric, comprising the following steps:
[0008] (S1) mixing Sb2O3 and HCl to obtain a SbCl3 solution;
[0009] (S2) mixing the SbCl3 solution obtained in step (S1) with 1,4-diaminobutane to obtain a mixture,
[0010] Then, the mixture is mixed with ethyl acetate and co-precipitated to obtain an organic-inorganic hybrid single crystal molecular ferroelectric;
[0011] Among them, the chemical formula of organic-inorganic hybrid single crystal molecular ferroelectric is [C8N4H 28 ][Sb2Cl 10 ].
[0012] In one embodiment of the present invention, in step (S1), the usage ratio of Sb2O3 to HCl is 1 mmol: 2-3 mL.
[0013] In one embodiment of the present invention, in step (S2), the usage ratio of Sb2O3, 1,4-diaminobutane and ethyl acetate is 1 mmol: 1-2 mmol: 4-6 mL.
[0014] In one embodiment of the present invention, in step (S2), the coprecipitation time is 4 to 8 hours.
[0015] The second object of the present invention is to provide an organic-inorganic hybrid single crystal molecular ferroelectric prepared by the above method;
[0016] The crystal data of the organic-inorganic hybrid single crystal molecular ferroelectric at 193K are:
[0017]
[0018] The third object of the present invention is to provide an application of an organic-inorganic hybrid single crystal molecular ferroelectric in the preparation of a back electrode.
[0019] The fourth object of the present invention is to provide a back electrode, wherein the back electrode is prepared from an organic-inorganic hybrid single crystal molecular ferroelectric.
[0020] A fifth object of the present invention is to provide a method for preparing a back electrode, comprising the following steps:
[0021] (A1) dissolving an organic-inorganic hybrid single crystal molecular ferroelectric and then spin coating it on a surface of a conductive substrate, and then drying and annealing the substrate to obtain a molecular ferroelectric thin film;
[0022] (A2) The molecular ferroelectric thin film prepared in step (A1) is screen-printed with silver paste to obtain a back electrode.
[0023] In one embodiment of the present invention, in step (A1), the organic-inorganic hybrid single crystal molecular ferroelectric is dissolved in a DMSO solution;
[0024] The ratio of the organic-inorganic hybrid single crystal molecular ferroelectric to the DMSO solution is 0.1 g:100 μL;
[0025] In one embodiment of the present invention, in step (A1), a coating machine is used to spin-coat the solution on the surface of the substrate, and the rotation speed of the coating machine is 3000-5000 r / min; during the drying process, the temperature is 65-80° C. and the time is 30-50 min;
[0026] During the annealing process, the temperature is 120-130°C and the time is 1-2 hours.
[0027] A fifth object of the present invention is to provide an application of a back electrode in the preparation of an optoelectronic device.
[0028] Compared with the prior art, the present invention has the following beneficial effects:
[0029] (1) The preparation method provided by the present invention is simple to operate, safe and environmentally friendly, and the prepared crystals are of good quality, uniform particles, high yield and good repeatability.
[0030] (2) Compared with the previous molecular ferroelectric materials, the organic-inorganic hybrid single crystal molecular ferroelectric of the present invention has a wider band gap, higher efficiency and wider spectral response range in optoelectronic devices. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 For [C8N4H 28 ][Sb2Cl 10 ]XRD pattern of crystals;
[0032] Figure 2 For [C8N4H 28 ][Sb2Cl10 ]Structure diagram of crystal;
[0033] Figure 3 For [C8N4H 28 ][Sb2Cl 10 ]Optical photograph of the crystal;
[0034] Figure 4 For [C8N4H 28 ][Sb2Cl 10 ] Absorption-bandgap diagram of the crystal;
[0035] Figure 5 For [C8N4H 28 ][Sb2Cl 10 ]SHG pattern of molecular ferroelectric film;
[0036] Figure 6 For [C8N4H 28 ][Sb2Cl 10 ]IT curve of photoelectric thin film materials at different polarization voltages. DETAILED DESCRIPTION
[0037] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments.
[0038] In the following examples, unless otherwise specified, all reagents used are commercially available reagents, and all detection means and methods used are conventional detection means and methods in the art.
[0039] Example 1
[0040] This embodiment provides a coprecipitation synthesis method for preparing an organic-inorganic hybrid single crystal molecular ferroelectric, which specifically includes the following steps:
[0041] (S1) Mix 5 mmol of Sb2O3 powder and 25 mL of concentrated HCl (37%) to form a stable and uniform solution in a clean beaker, i.e., SbCl3 solution;
[0042] (S2) adding 5 mmol of 1,4-diaminobutane to the SbCl3 solution obtained in step (S1), and mixing to obtain a mixture;
[0043] (S3) The mixture obtained in step (S2) was mixed with 10 mL of ethyl acetate solution and allowed to stand for 4 h; after the mixture was mixed, the supernatant was poured off and washed several times with ethyl acetate, leaving a white precipitate at the bottom, which was the organic-inorganic hybrid single crystal molecular ferroelectric: [C8N4H 28 ][Sb2Cl 10 ] The crystals (whose unit cell parameters are shown in Table 1) were placed in an oven at 60°C, dried and sealed for storage.
[0044] Table 1 [C8N4H 28 ][Sb2Cl 10 ]Unit cell parameters of molecular ferroelectrics
[0045]
[0046] The X-ray diffractometer was used to detect the [C8N4H 28 ][Sb2Cl 10 ]Single crystal powder, its XRD pattern is as follows Figure 1 As shown, it is in good agreement with the crystal structure data (Table 1), indicating that the obtained [C8N4H 28 ][Sb2Cl 10 ]The crystals are pure phase and have high crystallinity.
[0047] Using graphite monochromatized Mo Kα radiation The single crystal X-ray diffraction (XRD) was collected on the diffractometer using the ω-2θ scanning method, and the structure diagram is shown in Figure 2 As shown, according to the RT single crystal XRD data, the material has a polar orthorhombic structure of the Pc space group. The crystal structure is composed of two independent Sbl6 octahedrons sharing an angle, independent 1,4-diaminobutane molecules, and organic molecules distributed in [Sb2Cl 10 ] 2- The surroundings are in an orderly state.
[0048] The [C8N4H 28 ][Sb2Cl 10 ]Crystal morphology, such as Figure 3 As shown, the crystals are flaky and have a smooth surface.
[0049] The [C8N4H 28 ][Sb2Cl 10 ] single crystal absorption and band gap, such as Figure 4 As shown, it is shown that the single crystal molecular ferroelectric material [C8N4H 28 ][Sb2Cl 10 ] has an absorption edge at 357nm and an optical band gap of 3.47eV.
[0050] Example 2
[0051] This embodiment provides a coprecipitation synthesis method for preparing an organic-inorganic hybrid single crystal molecular ferroelectric, which specifically includes the following steps:
[0052] (S1) Mix 5 mmol of Sb2O3 powder and 25 mL of concentrated HCl (37%) to form a stable and uniform solution in a clean beaker, i.e., SbCl3 solution;
[0053] (S2) adding 5 mmol of 1,4-diaminobutane to the SbCl3 solution obtained in step (S1), and mixing to obtain a mixture;
[0054] (S3) The mixture obtained in step (S2) was mixed with 20 mL of ethyl acetate solution and allowed to stand for 6 h; after the mixture was mixed, the supernatant was poured out and washed several times with ethyl acetate, leaving a white precipitate at the bottom, which was the organic-inorganic hybrid single crystal molecular ferroelectric: [C8N4H 28 ][Sb2Cl 10 ] The crystals were placed in an oven at 60°C, dried and sealed for storage.
[0055] Example 3
[0056] This embodiment provides a coprecipitation synthesis method for preparing an organic-inorganic hybrid single crystal molecular ferroelectric, which specifically includes the following steps:
[0057] (S1) Mix 5 mmol of Sb2O3 powder and 25 mL of concentrated HCl (37%) to form a stable and uniform solution in a clean beaker, i.e., SbCl3 solution;
[0058] (S2) adding 5 mmol of 1,4-diaminobutane to the SbCl3 solution obtained in step (S1), and mixing to obtain a mixture;
[0059] (S3) The mixture obtained in step (S2) was mixed with 25 mL of ethyl acetate solution and allowed to stand for 6 h; after the mixture was mixed, the supernatant was poured out and washed several times with ethyl acetate, leaving a white precipitate at the bottom, which was the organic-inorganic hybrid single crystal molecular ferroelectric: [C8N4H 28 ][Sb2Cl 10 ] The crystals were placed in an oven at 60°C, dried and sealed for storage.
[0060] Example 4
[0061] This embodiment provides a coprecipitation synthesis method for preparing an organic-inorganic hybrid single crystal molecular ferroelectric, which specifically includes the following steps:
[0062] (S1) Mix 5 mmol Sb2O3 powder and 25 mL HCl to form a stable and uniform solution in a clean beaker, i.e., SbCl3 solution;
[0063] (S2) adding 5 mmol of 1,4-diaminobutane to the SbCl3 solution obtained in step (S1), and mixing to obtain a mixture;
[0064] (S3) The mixture obtained in step (S2) was mixed with 20 mL of ethyl acetate solution and allowed to stand for 8 h; after the mixture was mixed, the supernatant was poured off and washed several times with ethyl acetate, leaving a white precipitate at the bottom, which was the organic-inorganic hybrid single crystal molecular ferroelectric: [C8N4H 28 ][Sb2Cl 10 ] The crystals were placed in an oven at 60°C, dried and sealed for storage.
[0065] Example 5
[0066] This embodiment provides a method for preparing a molecular ferroelectric optoelectronic thin film device, which specifically includes the following steps:
[0067] (A1) 0.2 g of [C8N4H 28 ][Sb2Cl 10 ] single crystal powder was dissolved in 0.2 mL DMSO solution and stirred thoroughly to make [C8N4H 28 ][Sb2Cl 10 ] single crystal powder is completely dissolved to obtain [C8N4H 28 ][Sb2Cl 10 ] solution;
[0068] (A2) Using a gel-spinning machine at 3000 r / min, 50 μL of the stable and uniform [C8N4H 28 ][Sb2Cl 10 ] The solution was spin-coated onto a 1*1 cm ITO surface (at room temperature), and finally a film with a thickness of 3.98 μm was obtained, forming a molecular ferroelectric film;
[0069] (A3) drying the molecular ferroelectric thin film obtained in step (A2) in an oven at 60° C. for 30 min, and then annealing at 120° C. for 0.5 h to obtain a molecular ferroelectric thin film;
[0070] The SHG curve of the molecular ferroelectric film was recorded using an SHG spectrometer, such as Figure 5 As shown (in the figure, KDP refers to potassium dihydrogen phosphate crystals), [C8N4H 28 ][Sb2Cl 10 ]The signal intensity is 1.4 times higher than that of KDP, indicating that the molecular structure is non-centrosymmetric.
[0071] (A4) screen printing silver paste as a back electrode on the molecular ferroelectric film prepared in step (A3), then placing an ITO conductive substrate above the back electrode, and placing an Ag electrode below the back electrode to obtain a molecular ferroelectric ([C8N4H 28 ][Sb2Cl 10 ]) Photoelectric thin film devices.
[0072] Using Keithley 2450 as the source meter, under a xenon lamp with a power of 500W (AM 1.5G), the ITO / [C8N4H 28 ][Sb2Cl 10 ] The photoelectric response of the structure device under zero bias voltage. By applying voltage, the current will change. As the voltage increases, the photocurrent increases from 7.5nA / cm at 1V to 2 Rapidly increases to 20.3nA / cm at 5V 2 , and then quickly dropped to 5.3nA / cm at 11V 2 Under the condition of negative polarization voltage, its photocurrent is also 2.5nA / cm at -1V. 2 Increased to 19.6nA / cm at -7V 2 , and then quickly dropped to 6.1nA / cm at -11V 2 , the overall photocurrent size shows a trend of first increasing and then decreasing with the increase of polarization voltage, and the best photocurrent is obtained under the condition of -7V;
[0073] Comparative Example 1
[0074] The difference between this comparative example and Example 1 is that the HCl concentration is different.
[0075] (S1) Mix 5 mmol of Sb2O3 powder and 25 mL of dilute HCl (20%) to form a stable and uniform solution in a clean beaker, i.e., SbCl3 solution;
[0076] (S2) adding 5 mmol of 1,4-diaminobutane to the SbCl3 solution obtained in step (S1), and mixing to obtain a mixture;
[0077] (S3) The mixture obtained in step (S2) was mixed with 10 mL of ethyl acetate solution and allowed to stand for 4 h; it was found that no white precipitate was produced, the solution remained clear, and no product was generated. This was because the concentration of hydrochloric acid decreased, resulting in a decrease in the content of Cl element, which reduced the activity and reaction activity of the ions, so no product was ultimately generated.
[0078] Comparative Example 2
[0079] The difference between this comparative example and Example 1 is that different amounts of ethyl acetate are added.
[0080] (S1) Mix 5 mmol of Sb2O3 powder and 25 mL of concentrated HCl (37%) to form a stable and uniform solution in a clean beaker, i.e., SbCl3 solution;
[0081] (S2) adding 5 mmol of 1,4-diaminobutane to the SbCl3 solution obtained in step (S1), and mixing to obtain a mixture;
[0082] (S3) The mixture obtained in step (S2) was mixed with 5 mL of ethyl acetate solution and allowed to stand for 4 h; after the mixture was mixed, the supernatant was poured out and washed several times with ethyl acetate, leaving a white precipitate at the bottom, which was the organic-inorganic hybrid single crystal molecular ferroelectric: [C8N4H 28 ][Sb2Cl 10 ] crystals, placed in a 60℃ oven, dried and sealed for storage. It was found that adding a small amount of ethyl acetate would produce a small amount of white precipitate. The reason is that ethyl acetate adjusts the activity of ions in the solvent, affecting the formation and amount of precipitate. Too little ethyl acetate will result in low ion activity in the solution, resulting in less product.
[0083] Comparative Example 3
[0084] The difference between this comparative example and Example 1 is that the reaction time is different.
[0085] (S1) Mix 5 mmol of Sb2O3 powder and 25 mL of concentrated HCl (37%) to form a stable and uniform solution in a clean beaker, i.e., SbCl3 solution;
[0086] (S2) adding 5 mmol of 1,4-diaminobutane to the SbCl3 solution obtained in step (S1), and mixing to obtain a mixture;
[0087] (S3) The mixture obtained in step (S2) was mixed with 20 mL of ethyl acetate solution and allowed to stand for 2 h; after the mixture was mixed, the supernatant was discarded and washed several times with ethyl acetate, leaving a white precipitate at the bottom, which was the organic-inorganic hybrid single crystal molecular ferroelectric: [C8N4H 28 ][Sb2Cl 10 The crystals were placed in an oven at 60°C, dried and sealed for storage. The results showed that a shorter reaction time could make the crystals smaller, because a short reaction time was not conducive to complete reaction, particle growth and morphological perfection.
[0088] The above description of the embodiments is to facilitate the understanding and use of the invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the above embodiments, and improvements and modifications made by those skilled in the art based on the explanation of the present invention without departing from the scope of the present invention should be within the scope of protection of the present invention.
Claims
1. A method for preparing an organic-inorganic hybrid single crystal molecular ferroelectric, characterized in that: The following steps are involved: (S1) mixing Sb2O3 and HCl to obtain a SbCl3 solution; (S2) mixing the SbCl3 solution obtained in step (S1) with 1,4-diaminobutane to obtain a mixture, Then, the mixture is mixed with ethyl acetate and co-precipitated to obtain an organic-inorganic hybrid single crystal molecular ferroelectric; Among them, the chemical formula of organic-inorganic hybrid single crystal molecular ferroelectric is [C8N4H 28 ][Sb2Cl 10 ].
2. The method for preparing an organic-inorganic hybrid single crystal molecular ferroelectric according to claim 1, characterized in that: In step (S1), the usage ratio of Sb2O3 to HCl is 1 mmol: 2-3 mL.
3. The method for preparing an organic-inorganic hybrid single crystal molecular ferroelectric according to claim 1, characterized in that: In step (S2), the usage ratio of Sb2O3, 1,4-diaminobutane and ethyl acetate is 1 mmol: 1-2 mmol: 4-6 mL.
4. The method for preparing an organic-inorganic hybrid single crystal molecular ferroelectric according to claim 1, characterized in that: In step (S2), the coprecipitation time is 4 to 8 hours.
5. An organic-inorganic hybrid single crystal molecular ferroelectric, characterized in that: It is prepared by the method according to any one of claims 1 to 4.
6. Use of the organic-inorganic hybrid single crystal molecular ferroelectric as claimed in claim 5 in preparing a back electrode.
7. A back electrode, characterized in that: The back electrode is prepared from the organic-inorganic hybrid single crystal molecular ferroelectric according to claim 5.
8. A method for preparing a back electrode as claimed in claim 7, characterized in that: The following steps are involved: (A1) dissolving an organic-inorganic hybrid single crystal molecular ferroelectric and then spin coating it on a surface of a conductive substrate, and then drying and annealing the substrate to obtain a molecular ferroelectric thin film; (A2) The molecular ferroelectric thin film prepared in step (A1) is screen-printed with silver paste to obtain a back electrode.
9. The method for preparing a back electrode according to claim 8, characterized in that: In step (A1), the organic-inorganic hybrid single crystal molecular ferroelectric is dissolved in a DMSO solution; The ratio of the organic-inorganic hybrid single crystal molecular ferroelectric to the DMSO solution is 0.1 g:100 μL; During the drying process, the temperature is 65-80°C and the time is 30-50 minutes; During the annealing process, the temperature is 120-130°C and the time is 1-2 hours.
10. Use of the back electrode as claimed in claim 7 in preparing an optoelectronic device.