Recycling method of waste polyacrylonitrile polymerization liquid

Through dry spinning technology and multi-stage treatment, the problem of recycling and utilization of unqualified polyacrylonitrile polymer liquid in carbon fiber production is solved, the production of polyacrylonitrile chopped fibers and the recycling of organic solvents is realized, and the waste liquid treatment efficiency is improved .

CN118932519APending Publication Date: 2024-11-12INST OF COAL CHEM CHINESE ACAD OF SCI
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411020572.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The unqualified polyacrylonitrile polymer liquid produced in the carbon fiber production process is difficult to deal with, resulting in waste of raw materials and environmental pollution, and its processing complexity makes recycling difficult.

Method used

The waste polyacrylonitrile polymerization liquid is sprayed out to form a spinning stream by using dry spinning technology. The solvent is volatile and recovered through the hot air circulation system and atmosphere in the spinning corridor, and then multi-stage treatment such as drafting and molding is carried out. , water washing, hot water drafting, oiling treatment and steam drafting to form polyacrylonitrile fibers, and polyacrylonitrile chopped fibers are prepared by chopping treatment.

Benefits of technology

Effectively recycle and utilize waste polyacrylonitrile polymerization liquid to produce chopped polyacrylonitrile fibers of different strengths, and maximize the recycling of organic solvents, solving the problem of handling unqualified liquids in the production of raw silk and improving the waste liquid treatment efficiency .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118932519A_ABST
    Figure CN118932519A_ABST
Patent Text Reader

Abstract

The invention relates to a recycling method of a waste polyacrylonitrile polymerization liquid, and relates to the technical field of solid waste treatment. The recycling method of the waste polyacrylonitrile polymerization liquid comprises the following steps that the waste polyacrylonitrile polymerization liquid is sprayed out by a spinning device to form spinning trickles, and the spinning trickles enter a spinning channel; in the spinning channel, along with continuous volatilization of the solvent in the spinning trickle, the concentration of the formed sliver trickle is continuously increased until the sliver trickle is solidified, and nascent fibers are formed; sequentially carrying out drafting setting treatment, water washing treatment, hot water drafting treatment, oiling treatment, drying densification treatment and steam drafting treatment on the nascent fiber to obtain the polyacrylonitrile fiber, and carrying out chopping treatment on the polyacrylonitrile fiber to obtain the polyacrylonitrile chopped fiber. According to the invention, the treatment of the waste polyacrylonitrile polymer liquid is better solved, the polyacrylonitrile chopped fiber is produced, and meanwhile, the organic solvent in the waste polymer liquid is recycled.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of solid waste treatment, and in particular to a method for recycling waste polyacrylonitrile polymerization liquid. Background Art

[0002] With the progress of carbon fiber engineering industrialization, carbon fiber production must consider comprehensive issues such as production cost, benefit and profit, safety and environmental protection. In particular, the social responsibility of green environmental protection has increased the investment of enterprises in environmental protection and their own three wastes treatment. The production of carbon fiber is a process production, the production process is long and complicated, and the production process points are many and complex. Any inadequate control in the production process will cause irreversible solid waste generation, which not only increases production costs, but also most of these solid wastes are non-renewable solid wastes, so there must be supporting treatment methods in terms of safety and environmental protection.

[0003] In the production process of polyacrylonitrile fiber, due to the complexity of the polymerization process, especially in the test stage, it is inevitable that unqualified polyacrylonitrile polymerization liquid will be produced. These unqualified polyacrylonitrile polymerization liquids contain polyacrylonitrile and organic solvents. If they are directly treated as hazardous waste, there will be a large waste of raw materials and pollution to the environment.

[0004] Therefore, how to recycle and utilize waste polyacrylonitrile polymerization liquid has become a problem faced by carbon fiber companies. In addition, during the long-term storage process, part of the waste polyacrylonitrile polymerization liquid remains dissolved, and part of it has solidified and gelled, with poor homogenization, which brings a burden to subsequent processing. Therefore, it is necessary to deal with the waste polyacrylonitrile polymerization liquid in a timely manner. Summary of the invention

[0005] In view of this, the present invention provides a method for recycling waste polyacrylonitrile polymerization liquid, the main purpose of which is to prepare waste polyacrylonitrile liquid into polyacrylonitrile chopped fibers to achieve recycling of waste polyacrylonitrile polymerization liquid.

[0006] In order to achieve the above object, the present invention mainly provides the following technical solutions:

[0007] On the one hand, an embodiment of the present invention provides a method for recycling waste polyacrylonitrile polymerization liquid, which comprises the following steps:

[0008] The steps of preparing polyacrylonitrile fiber are as follows: waste polyacrylonitrile polymer solution is ejected from a spinning device to form a spinning fine stream, and the spinning fine stream enters a spinning tunnel; in the spinning tunnel, as the solvent in the spinning fine stream is continuously volatilized, the concentration of the formed fine stream is continuously increased until it is solidified to form a primary fiber; the primary fiber is sequentially subjected to a stretching and shaping treatment, a water washing treatment, a hot water stretching treatment, an oiling treatment, a drying and densification treatment, and a steam stretching treatment to obtain a polyacrylonitrile fiber;

[0009] Short-cutting step: the polyacrylonitrile fibers are short-cut to obtain polyacrylonitrile short-cut fibers.

[0010] Preferably, in the step of preparing polyacrylonitrile fiber: the spinning speed of the waste polyacrylonitrile polymer solution ejected from the spinning device is 1.5-5m / s; and / or the viscosity of the waste polyacrylonitrile polymer solution is 150-500Pa.s (40°C water bath falling ball viscosity); and / or the spinneret of the spinneret is located near the top of the spinning tunnel, and the spinneret is 4-10m away from the bottom of the spinning tunnel; and / or in the spinning tunnel, the drafting multiple of the filament stream is 2-10 times; the residence time of the filament stream in the spinning tunnel is 1-10s; and / or the temperature of the spinning tunnel is 150-300°C; and / or the flowing atmosphere in the spinning tunnel is selected from one or more of nitrogen, superheated water vapor, carbon dioxide, and argon; preferably, the flow rate of the flowing atmosphere is 100-500Nm 3 / h; and / or in the spinning tunnel, the volatilized solvent is taken away by the flowing atmosphere for recycling.

[0011] Preferably, in the step of preparing polyacrylonitrile fiber: the circulating use of the flowing atmosphere in the spinning tunnel and the recycling of the solvent are realized by a hot air circulation system; wherein the hot air circulation system comprises:

[0012] A flowing atmosphere input pipeline, the flowing atmosphere input pipeline is connected to the air inlet of the spinning tunnel and is used to input the flowing atmosphere into the spinning tunnel;

[0013] A flowing atmosphere output pipeline, the flowing atmosphere output pipeline and the gas outlet of the spinning tunnel are used to make the flowing atmosphere with volatile solvent flow out of the spinning tunnel;

[0014] A cooler, wherein the flowing atmosphere output pipeline is connected to the air inlet of the cooler so that the flowing atmosphere with the volatile solvent enters the cooler to condense the volatile solvent into a liquid state;

[0015] A solvent recovery device, the solvent recovery device is connected to the condensate outlet of the cooler and is used to recover the condensed solvent;

[0016] A heating pipeline, wherein the inlet end of the heating pipeline is connected to the air outlet of the cooler through a pipeline, and is used to heat the flowing atmosphere discharged from the cooler, and the air outlet of the heating pipeline is connected to the flowing atmosphere input pipeline, so as to realize the circulation of the flowing atmosphere;

[0017] Preferably, the inlet end of the heating pipeline is also connected to the air supply pipeline;

[0018] Preferably, the heating pipeline includes a pipeline and a heat exchanger arranged on the pipeline;

[0019] Preferably, the outlet end of the heating pipeline is connected to the flowing atmosphere input pipeline through a fan;

[0020] Preferably, the air outlet is located at the upper end of the side wall of the spinning tunnel. Preferably, the spinning tunnel has multiple air inlets, which are evenly distributed on the surrounding side walls of the spinning tunnel.

[0021] Preferably, in the step of preparing the polyacrylonitrile fiber: when the spun fiber is subjected to the drawing and setting treatment, the spun fiber is passed through the opening at the bottom of the spinning tunnel and then enters the setting liquid for drawing and setting; wherein the drawing multiple of the drawing and setting is 1.2-2.0 times, and the temperature of the setting liquid is 5-20°C; preferably, the drawing and setting treatment is carried out in a drawing and setting tank; wherein a wire guide structure is provided in the drawing and setting tank; wherein a plurality of wire guides are provided on the wire guide structure. The guide wire groove is formed in the guide wire groove so that the fiber bundle receives an upward supporting force in the guide wire groove, so that the bundled bundle spreads in the guide wire groove; preferably, the setting liquid is an aqueous solution of waste polyacrylonitrile solvent, preferably an aqueous solution prepared by recovering the solvent volatilized from the spinning fine flow; or the setting liquid is N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, propylene carbonate, an aqueous solution of propylene carbonate; preferably, the concentration of the setting liquid is 10-45wt%.

[0022] Preferably, in the step of preparing polyacrylonitrile fiber: the fibers after the drafting and setting treatment are sequentially passed through multiple water washing zones for water washing treatment; wherein the temperature of the latter water washing zone is 3-5°C higher than that of the former water washing zone; the temperature of the first water washing zone is 50-55°C; the water washing treatment time is 5-10min; and / or when the fibers after the drafting and setting treatment are water washed, a vibration device is provided in each water washing zone to vibrate the fibers and increase the relative movement between the fiber bundle and the water; preferably, The vibrating device is a beating stick; and / or when the fibers after the stretching and setting treatment are washed with water, deionized water is added in each washing zone by bubbling; and / or when the fibers after the stretching and setting treatment are washed with water, a partition is provided in each washing zone to increase the turbulence effect in the washing zone; and / or when the fibers after the stretching and setting treatment are washed with water, a spray device is used to spray water on the fibers leaking out of the water; and / or the organic solvent content in the washed fibers is less than or equal to 0.03wt%.

[0023] Preferably, in the step of preparing polyacrylonitrile fiber: the hot water drawing treatment is a multi-pass drawing in the temperature range of 75-95°C, and the total drawing ratio is 1-1.3; and / or the fiber after the hot water drawing treatment is first dried and then oiled to remove moisture, preferably, the fiber after the hot water drawing treatment is passed through a hot air oven or a hot roll to complete the drying treatment; and / or the temperature of the drying and densification treatment is 95-130°C, the temperature difference between adjacent temperature gradients is 0-10°C, the drying and densification time of each temperature level is 5-10s, and the drawing ratio is 0.95-1.1. The fiber after the drying and densification treatment is subjected to steam drawing treatment with saturated water vapor or superheated steam as the medium, wherein the steam pressure is 0.12-0.4MPa, the drawing ratio is 2-5 times; the residence time of the steam drawing treatment is 3-6s.

[0024] Preferably, the monofilament diameter of the polyacrylonitrile fiber is 9-20 μm and the bulk density is 1.18-1.19 g / cm 3

[0025] Preferably, in the chopped processing step: the polyacrylonitrile fibers are conveyed to a chopped device for chopped processing to obtain chopped fibers; the chopped fibers are dried and screened to obtain polyacrylonitrile-based chopped fibers of desired sizes; preferably, the chopped fibers obtained after the chopped processing are dried by a drying device under the action of a conveying device, and then the dried chopped fibers are conveyed to a screening device; preferably, the drying treatment temperature is 90-100°C, and the drying treatment time is 25-30s.

[0026] Preferably, before the short-cutting step, the polyacrylonitrile fibers from at least two spinning positions are first combined and then short-cut.

[0027] On the other hand, an embodiment of the present invention provides a polyacrylonitrile chopped fiber, wherein the polyacrylonitrile chopped fiber is prepared by using any of the above-mentioned methods for recycling waste polyacrylonitrile polymerization liquid; wherein the single fiber diameter of the chopped polyacrylonitrile fiber is 9-20 μm, and the strength is 350-670 MPa.

[0028] Compared with the prior art, the method for recycling waste polyacrylonitrile polymerization liquid of the present invention has at least the following beneficial effects:

[0029] On the one hand, the recycling method of waste polyacrylonitrile polymerization liquid provided in the embodiment of the present invention uses dry spinning to prepare waste polyacrylonitrile polymerization liquid into polyacrylonitrile fibers, and then the polyacrylonitrile fibers are chopped to prepare polyacrylonitrile chopped fibers. Through the above scheme, the embodiment of the present invention solves the problem of handling unqualified polymerization liquid in the production process of polyacrylonitrile precursor, and can prepare polyacrylonitrile chopped fibers at the same time, which better solves the problem of handling waste polymerization liquid, produces polyacrylonitrile chopped fibers of different strengths, and at the same time, the organic solvent in the waste polymerization liquid is recycled.

[0030] Furthermore, the recycling method of waste polyacrylonitrile polymerization liquid provided in the embodiment of the present invention makes the waste polyacrylonitrile polymerization liquid ejected from the spinneret to form a spinning stream and enter the spinning tunnel; in the spinning tunnel, as the solvent in the spinning stream continues to evaporate, the concentration of the filament stream is continuously increased until it solidifies to form a primary fiber; the primary fiber is sequentially subjected to a drawing and shaping treatment, a water washing treatment, a hot water drawing treatment, an oiling treatment, a drying and densification treatment, and a steam drawing treatment to obtain a polyacrylonitrile fiber. Here, the embodiment of the present invention achieves efficient recovery of the solvent and the performance of the polyacrylonitrile chopped fiber prepared from the waste polyacrylonitrile meets the required requirements by correspondingly controlling the above-mentioned process parameters.

[0031] The above description is only an overview of the technical solution of the present invention. In order to more clearly understand the technical means of the present invention and implement it according to the contents of the specification, the following is a detailed description of the preferred embodiments of the present invention in conjunction with the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 The present invention provides a flowchart of a method for recycling waste polyacrylonitrile polymerization liquid.

[0033] Figure 2 It is a schematic diagram of the structure of the guide wire groove provided in an embodiment of the present invention. DETAILED DESCRIPTION

[0034] In order to further explain the technical means and effects adopted by the present invention to achieve the predetermined invention purpose, the specific implementation methods, structures, features and effects of the present invention application are described in detail below in conjunction with the accompanying drawings and preferred embodiments. In the following description, different "one embodiment" or "embodiment" does not necessarily refer to the same embodiment. In addition, specific features, structures, or characteristics in one or more embodiments may be combined in any suitable form.

[0035] The present invention mainly solves the problem of handling unqualified polymer solution in the production process of polyacrylonitrile fiber (i.e., polyacrylonitrile fiber-based carbon fiber precursor), and can prepare polyacrylonitrile chopped fibers at the same time, thus better solving the problem of handling waste polymer solution, producing polyacrylonitrile chopped fibers of different strengths, and recycling the organic solvent in the waste polymer solution.

[0036] Due to different processes, wet spinning, dry-jet wet spinning and dry spinning have different requirements for spinning solutions, so requirements need to be put forward for the preparation of spinning solutions in the polymerization stage. Regardless of viscosity, polymer content and solvent concentration, wet spinning and dry spinning have different requirements for spinning solutions. The present invention is aimed at the early test stage of wet spinning and dry-jet wet spinning, or the occurrence of polymerization abnormalities (equipment abnormalities or public auxiliary media abnormalities, such as water, electricity, and gas outages or large fluctuations.) The spinning solution is not suitable for wet spinning and dry-jet wet spinning processes, and can only be separated by solid-liquid separation through dry spinning, converting the organic solution of polyacrylonitrile into an aqueous solution of polyacrylonitrile fibers and organic solvents, and then carrying out subsequent processing. Here, the inventor believes that: the number of spinneret holes in dry spinning is significantly more than that of wet spinning and dry-jet wet spinning. Therefore, dry spinning is more suitable for large tow products and is more conducive to the treatment of waste polymer solution in the production of polyacrylonitrile carbon fibers. Specifically, the scheme of the present invention is as follows:

[0037] The embodiment of the present invention provides a method for recycling waste polyacrylonitrile polymerization liquid, such as Figure 1 As shown, it includes the following steps:

[0038] 1) Preparation of polyacrylonitrile fiber steps:

[0039] The waste polyacrylonitrile polymer solution is quantitatively and evenly fed into the spinneret 4 (i.e., the spinneret of the spinning assembly) by a spinning metering pump. Under the action of pressure, the waste polymer solution is squeezed into a spinning stream, which is ejected from the spinneret hole and enters the spinning tunnel 1. In the spinning tunnel, the solvent in the spinning stream evaporates rapidly and is carried away by the flowing atmosphere 2. The concentration of the filaments increases continuously until they solidify. At the same time, the solidified filament stream is stretched and thinned. The obtained primary fiber is stretched by drawing, winding and stretching before entering the subsequent process.

[0040] Among them, the process of the spinning thread in the spinning channel 1 is the simultaneous evaporation of solvent and thinning of filaments. The spinning process near the spinneret 4 includes the comprehensive effects of mass transfer and heat transfer such as flash evaporation, convection and diffusion. Then pure diffusion gradually becomes the factor controlling the rate of the mass transfer and heat transfer process. The process can be divided into the following three stages according to the temperature change of the filaments.

[0041] The first stage: After the waste polyacrylonitrile polymer liquid is ejected from the spinneret hole of the spinneret device, it immediately volatilizes and flashes: when the waste polymer liquid is squeezed out from the spinneret hole, a spinning stream is formed, and the organic solvent flashes, causing the solvent to evaporate rapidly and in large quantities, and the composition and temperature of the spinning stream change dramatically. Relying on the latent heat of the waste polyacrylonitrile polymer liquid and the heat transfer of the hot air, the surface temperature of the filament drops sharply until the wet-bulb temperature reaches equilibrium. At this time, the temperature inside the filament is higher than the surface temperature of the filament, and the solvent inside the filament diffuses at a very fast speed, but the concentration of the solvent in the filament is not much different along the radial distribution of the filament. The "wet-bulb temperature" here refers to: under specific conditions, the gas temperature when the gas introduced into the spinning tunnel reaches a saturated state with the volatile organic solvent.

[0042] The second stage: the solvent diffuses outward from the inside of the spinning stream. The solvent concentration on the surface of the stream is relatively high. Heat exchange is mainly carried out by convection. The heat transfer by hot air and the heat taken away by the solvent reach a balance. The filaments maintain the wet-bulb temperature. The inside of the filaments is also at a lower temperature. The solvent diffusion rate decreases. The solvent diffusion rate inside the filaments is lower than the diffusion rate outside the filaments. The solvent content in the filaments differs radially. The solvent content outside the filaments is less than that inside. The temperature on the surface of the filaments rises, and the fiber produces a skin-core structure. The filaments maintain a circular cross-section, but shrinkage occurs in the radial direction, and the filaments become thinner.

[0043] The third stage: Convection mass transfer from the surface of the thin stream to the surrounding gas medium, the diffusion rate of the solvent inside the filament is slower, and the concentration of the solvent in the filament has a greater difference in the radial direction. The temperature of the surface of the filament has reached the temperature of the hot air. This stage is the solidification of the filament. As the solvent evaporates, the cortex of the fiber collapses, the cross-section changes to a non-circular shape, and the solvent remaining inside the fiber is removed in the subsequent process.

[0044] About dry spinning device: Figure 1As shown, a spinneret 4 is provided at the upper end of the spinning shaft 1, and the spinning shaft 1 is connected to a hot air circulation device. Specifically, the hot air circulation device comprises: a flowing atmosphere input pipeline 2, a flowing atmosphere output pipeline 3, a cooler 5, a solvent recovery device 6, and a heating pipeline. Among them, the flowing atmosphere input pipeline 2 is connected to the air inlet of the spinning shaft 1, and is used to input the flowing atmosphere into the spinning shaft 1; the flowing atmosphere output pipeline 3 is connected to the air outlet of the spinning shaft 1, and is used to make the flowing atmosphere with the volatile solvent flow out of the spinning shaft 1. The flowing atmosphere output pipeline 3 is connected to the air inlet of the cooler 5, so that the flowing atmosphere with the volatile solvent enters the cooler 5, so that the volatile solvent is condensed into a liquid state. The solvent recovery device 6 is connected to the condensate outlet of the cooler 5 for recovering the condensed solvent; the inlet end of the heating pipeline is connected to the air outlet of the cooler 5 through the pipeline for heating the flowing atmosphere discharged from the cooler 5, and the air outlet of the heating pipeline is connected to the flowing atmosphere input pipeline 2 to realize the circulation of the flowing atmosphere. Preferably, the inlet end of the heating pipeline is also connected to the air supply pipeline 7 to supply fresh air; preferably, the heating pipeline includes a pipeline and a heat exchanger 8 arranged on the pipeline; preferably, the outlet end of the heating pipeline is connected to the flowing atmosphere input pipeline 2 through a fan 9; the air outlet of the spinning tunnel 1 is located at the upper end of the side wall of the spinning tunnel 1 to form a side blowing device. Here, the spinning tunnel has multiple air inlets, which are evenly distributed on the surrounding side walls of the tunnel. Multiple air inlets are arranged around the spinning tunnel to gather air from all directions to the center, making the air flow inside the tunnel more uniform and the fiber formation more stable, thus ensuring the performance and quality of the fiber.

[0045] The spinning tunnel 1 involved in the present invention not only affects the fiber forming process, but also has an important influence on the physical properties of the fiber, the volatilization and recovery of the solvent.

[0046] (1) The length of the spinning shaft is also called the spinning process. It is generally composed of three parts: upper, middle and lower. It has a decisive influence on the amount of residual solvent inside the fiber. Theoretically, the longer the length of the spinning shaft, the longer the fiber forming time and the less residual solvent; but an overly long spinning shaft will cause problems such as increased spinning tension, inconvenient operation and spinnability.

[0047] (2) The uniformity of the air flow velocity field distribution in the spinning tunnel. In actual production, defects such as uneven side blowing wind speed and uneven wind speed along the spinning direction often occur. The present invention evenly arranges multiple air inlets around the spinning tunnel to form a ring-shaped air supply, which collects air from all directions to the center, making the air flow inside the tunnel more uniform, thereby improving the spinning speed and quality of polyacrylonitrile.

[0048] (3) Uniformity of the air flow temperature field distribution in the spinning shaft. Reasonable temperature distribution is crucial to increasing the spinning speed and stabilizing the spinning quality. In the present invention, the outer wall of the spinning shaft is heated by a companion pipe along the spinning process, and steam heating is adopted to keep the internal hot air flow of the spinning shaft at the temperature required by the process, maintain the uniformity of the air flow temperature field distribution in the spinning shaft, and achieve uniform and stable temperature in the spinning shaft, which has a great effect on the uniformity of fiber formation and structure uniformity.

[0049] The waste polyacrylonitrile polymer solution of the present invention is sprayed out through a spinneret to form a spinning fine flow, wherein the specification of the spinneret is 24-50k. The spinning fine flow is rapidly volatilized by the hot air flow in the spinning tunnel, and the volatilized solvent vapor is taken away by the flowing atmosphere. The spinning fine flow is solidified while gradually removing the solvent, and is stretched and thinned under the action of winding tension to form primary fibers.

[0050] Preferably, the spinning speed (filament collection speed) of dry spinning is generally 200-500 m / min, and the spinning speed can be increased to 700-1500 m / min when the length of the spinning tunnel 1 is increased. The spinning speed of dry spinning is high and the obtained fiber structure is denser and has better physical and mechanical properties.

[0051] In the above method, the waste polyacrylonitrile polymer solution is ejected from the spinneret device at a spinning speed of 1.5-5 m / s, the height of entering the spinning tunnel is 4-10 m, the drafting multiple in the spinning tunnel is 2-10 times, the residence time is 1-10 s, and the temperature in the spinning tunnel is 150-300° C. The filament bundle is heated in the spinning tunnel, and the solvent is quickly volatilized and initially shaped. The atmosphere in the spinning tunnel can be selected from any one or more of nitrogen, superheated water vapor, carbon dioxide, argon, etc., and the air flow is 100-500 Nm 3 .

[0052] It should be noted here that the spinning temperature (channel temperature) plays a key role in spinning and forming. Whether the temperature is set properly or not has a great impact on the fiber quality. If the temperature is too high, the polymer will degrade, affecting the fiber performance and increasing energy consumption; if the temperature is set too low, the N,N-dimethylformamide in the nascent fiber cannot evaporate quickly, resulting in paralleling, sticking and even pulp blocks. The plate change amount is an important indicator to characterize the stability of the spinning process. After the channel temperature is optimized, the plate change amount has also decreased significantly, as shown in Table 1.

[0053] Table 1

[0054] Channel temperature ℃ 130 150 200 250 270 300 Daily board replacement times excessive 12.8 6.3 5.7 2.4 3.6

[0055] Here, the present invention controls the tunnel temperature at 150-300°C based on the operation stability and energy consumption of the spinning process.

[0056] The spun fibers are subsequently treated in a subsequent treatment production line system 10; the subsequent treatment includes a drawing and shaping treatment, a water washing treatment, a hot water drawing treatment, an oiling treatment, a drying and densification treatment, and a steam drawing treatment.

[0057] The yarns are directly drawn into the setting liquid from the bottom of the spinning tunnel for drawing and setting. The setting liquid is an aqueous solution of waste polyacrylonitrile solvent, which can be N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, propylene carbonate or an organic aqueous solution of propylene carbonate, with a concentration of 10-45wt%, a temperature of 5-20°C, and a drawing multiple of 1.2-2.0 times. The solvent in the yarn bundle is further dispersed in the setting liquid, and the performance and shape of the yarn bundle are further stabilized.

[0058] In addition, the drafting and shaping process is carried out in the drafting and shaping tank; Figure 2 As shown, a wire guide structure 16 is provided in the drafting and shaping groove; wherein, a plurality of wire guide grooves 17 are provided on the wire guide structure 16, so that the fiber bundle receives an upward supporting force in the wire guide groove 17, and the bundled fiber bundle is spread in the wire guide groove 17. Here, by providing the wire guide structure 16, the width of the fiber strip is increased, the mass transfer and heat transfer effect is optimized, each fiber in the fiber strip is placed in the same drafting environment, and each fiber in the drafted fiber strip is in the same state, thereby preparing short-cut fibers with excellent performance.

[0059] The fibers after the drawing and shaping treatment are washed in multiple washing zones in sequence, wherein the temperature of the latter washing zone is slightly higher than that of the former washing zone, with a temperature difference of 3-5°C. The temperature of the first washing zone is 50-55°C, and the washing treatment time is 5-10 minutes.

[0060] Among them, during water washing, the fiber production is vibrated by a mechanical device to increase the relative movement between the fiber bundle and the water, for example, multiple beating sticks are added in the water zone. At the same time, heated deionized water is added to the water washing zone in a bubbling manner, or a partition is added in the water washing zone to increase the turbulence effect. At the same time, a spray device is added at the transmission roller where the fiber leaks out of the water washing zone; the width of the wire path is controlled so that the fiber bundle and the water in the water washing zone have a larger area. Through the above settings, the organic solvent content in the fiber after water washing is less than or equal to 0.03wt%.

[0061] The washed fibers are subjected to hot water drawing treatment, wherein the hot water drawing treatment is a multi-pass drawing at a temperature of 75-95°C and a drawing ratio of 1-1.3. Here, the washed fibers are drawn to arrange the polymer chains in an orderly manner and to improve the strength and elasticity of the fibers. Here, multi-pass drawing means that the fibers are passed through multiple drawing grooves in sequence, and the temperature of the hot water in the multiple drawing grooves increases gradually.

[0062] Preferably, the hot water drawn fibers are dried to remove any remaining moisture, typically by passing the fibers through a hot air oven or heated rolls.

[0063] Then, the fiber after hot water drawing treatment is oiled. The fiber after oiling treatment is dried and densified. The temperature of drying and densification treatment is 95-130°C, the temperature difference between adjacent temperature gradients is 0-10°C, the drying and densification time of each temperature level is 5-10s, and the drawing ratio is 0.95-1.1.

[0064] The fibers after drying and densification are subjected to steam drawing treatment using saturated water vapor or superheated steam as a medium, wherein in the step of steam drawing treatment, the steam pressure is 0.12-0.4 MPa, the drawing multiple is 2-5 times, and the residence time of the steam drawing treatment is 3-6 seconds.

[0065] After steam drawing treatment, the polyacrylonitrile fiber has the following characteristics: the diameter of the single fiber of the polyacrylonitrile fiber is 9-20 μm, and the bulk density is 1.18-1.19 g / cm 3 .

[0066] 2) Short-cutting step: the polyacrylonitrile fibers are short-cut to obtain polyacrylonitrile short-cut fibers.

[0067] In this step, the polyacrylonitrile fiber is processed by wire drawing, feeding, and short cutting (such as Figure 1 As shown, the short-cutting process is carried out in the short-cutting device 11), the drying process (such as Figure 1 As shown, the drying process is carried out in the drying device 12), and the screening process and other steps are performed to obtain short-cut fibers with different length uniformity. Figure 1 As shown, the chopped fibers are evenly distributed on the conveyor belt 13, and are heated in the drying device 12 through the conveyor belt 13 to remove moisture. The drying temperature is 90-150°C and the drying time is 10-30 seconds. Preferably, the dried chopped fibers are sent to the fiber screening device 14 for vibration screening. After passing through the fiber screening device, the chopped fibers enter the fiber collecting device 15 below for collection.

[0068] Preferably, before the short-cutting step, the polyacrylonitrile fibers from at least two spinning positions are first combined and then short-cut.

[0069] The chopped fibers provided by the present invention have uniform length and uniform dispersion, and have no strand adhesion phenomenon, and therefore can be better applied to downstream products of polyacrylonitrile chopped fibers, such as polyacrylonitrile chopped fibers reinforced with resin-based composite materials.

[0070] The present invention adopts the above technical scheme, which not only effectively treats the waste polymer solution in the production of polyacrylonitrile fibers, but also recovers the organic solvent to the maximum extent, and simultaneously obtains polyacrylonitrile chopped fibers with certain functions.

[0071] The present invention realizes stable and continuous batch production of chopped fibers within 2-20 mm. The prepared polyacrylonitrile chopped fibers have good dispersibility and uniform and stable length, and can meet the processing requirements of chopped fibers of various types and sizes.

[0072] The present invention is further described below by specific experimental examples:

[0073] Example 1

[0074] This embodiment recycles waste polyacrylonitrile polymerization liquid, mainly comprising the following steps:

[0075] 1) Waste polyacrylonitrile polymer solution (viscosity of 200 Pa.s) is ejected from a spinneret to form a spinning stream and enter a spinning tunnel; in the spinning tunnel, as the solvent in the spinning stream continues to evaporate, the concentration of the filament stream continues to increase until it solidifies to form primary fibers.

[0076] The process parameters are as follows: the spinning speed is 2m / s, the height of the spinning stream entering the spinning tunnel is 5m (i.e., the distance between the spinneret and the bottom of the spinning tunnel is 5m); the drafting multiple is 3 times; the temperature in the spinning tunnel is 150°C; the spinning stream is heated in the tunnel, and the solvent evaporates quickly before initial shaping. The flowing atmosphere in the spinning tunnel is nitrogen, and the airflow is 300Nm 3 / h. The solvent flows out of the spinning shaft along with the flowing atmosphere and is cooled and recovered in the cooler. The residence time of the filament stream in the spinning shaft is 8s. In addition, there are multiple air inlets for the flowing atmosphere, which are evenly distributed around the spinning shaft.

[0077] 2) The spun fibers are sequentially subjected to a drawing and shaping treatment, a water washing treatment, a hot water drawing treatment, an oiling treatment, a drying and densification treatment, and a steam drawing treatment to obtain polyacrylonitrile fibers.

[0078] Among them, the process parameters are controlled as follows:

[0079] In the step of drawing and setting treatment: the nascent fiber enters the setting liquid directly from the bottom of the spinning tunnel for drawing and setting treatment; wherein, the setting liquid is N,N-dimethylformamide solution with a concentration of 35wt%. The temperature of the drawing and setting treatment is 15°C, and the drawing multiple is 2.0 times. Here, the solvent in the tow is further dispersed in the setting liquid, and the performance and shape of the tow are further stabilized. The drawing and setting treatment is carried out in the drawing and setting tank; wherein, the drawing and setting tank is provided with the following Figure 2The guide wire structure 16 is shown; wherein, a plurality of guide wire grooves 17 are arranged on the guide wire structure, so that the fiber bundles receive an upward supporting force in the guide wire grooves, so that the bundled bundles are spread in the guide wire grooves.

[0080] After multi-stage water washing treatment (three-stage water washing treatment, the temperature is 55℃, 60℃, 65℃), multi-stage hot drawing treatment (hot water drawing treatment at both ends, at 85℃ and 90℃, the total drawing is 1.2 times), oiling treatment, drying and densification treatment (temperature gradient is 100℃, 105℃, 110℃, 120℃) and steam drawing treatment (drawing multiple is 3 times), high-density, high-crystallinity and high-strength polyacrylonitrile fiber is prepared. Among them, the bulk density of polyacrylonitrile fiber is 1.18g / cm 3 , crystallinity is 52.2% and strength is 490Mpa.

[0081] 3) Short cutting process steps:

[0082] First, the polyacrylonitrile fibers from at least two spinning positions are combined and then chopped. During the chopped process, the polyacrylonitrile fibers are pulled by a feed roller, and the fiber bundles are continuously processed by a fiber cutter under the rotation and traction of the cutting feed roller, and cut into target lengths to obtain chopped fibers.

[0083] The obtained chopped fibers are evenly distributed on the conveyor belt, and are heated in the drying device through the conveyor belt to remove moisture, wherein the drying temperature is 100°C and the drying time is 30 seconds. The dried chopped fibers are sent to the fiber screening device for vibration screening. After passing through the fiber screening device, the chopped fibers enter the fiber collecting device below for collection.

[0084] The collected short-cut fibers are uniform in length and dispersed evenly without any adhesion phenomenon. The single-filament diameter of the short-cut acrylonitrile fibers is 12 μm and the strength is 490 MPa.

[0085] Example 2

[0086] This embodiment recycles waste polyacrylonitrile polymerization liquid, mainly comprising the following steps:

[0087] 1) The waste polyacrylonitrile polymer solution has a viscosity of (150Pa.s) and is ejected from a spinneret to form a spinning stream and enter a spinning tunnel; in the spinning tunnel, as the solvent in the spinning stream continues to evaporate, the concentration of the filament stream continues to increase until it solidifies to form primary fibers.

[0088] The process parameters are as follows: the spinning speed is 3.5 m / s, the height of the spinning stream entering the spinning tunnel is 5 m (i.e., the distance between the spinneret and the bottom of the spinning tunnel is 5 m); the drafting multiple is 2 times; the temperature in the spinning tunnel is 200°C; the spinning stream is heated in the tunnel, and the solvent evaporates quickly before initial shaping. The flowing atmosphere in the spinning tunnel is nitrogen, and the airflow is 400 Nm 3 / h. The solvent flows out of the spinning shaft along with the flowing atmosphere and is cooled and recovered in the cooler. The residence time of the filament stream in the spinning shaft is 5s. In addition, there are multiple air inlets for the flowing atmosphere, which are evenly distributed around the spinning shaft.

[0089] 2) The spun fibers are sequentially subjected to a drawing and shaping treatment, a water washing treatment, a hot water drawing treatment, an oiling treatment, a drying and densification treatment, and a steam drawing treatment to obtain polyacrylonitrile fibers.

[0090] Among them, the process parameters are controlled as follows:

[0091] In the step of drawing and setting treatment: the nascent fiber enters the setting liquid directly from the bottom of the spinning tunnel for drawing and setting treatment; wherein the setting liquid is an aqueous solution of N,N-dimethylformamide with a concentration of 30wt%. The temperature of the drawing and setting treatment is 18°C ​​and the drawing multiple is 1.5 times. Here, the solvent in the tow is further dispersed in the setting liquid, and the performance and shape of the tow are further stabilized. The drawing and setting treatment is carried out in the drawing and setting tank; wherein the drawing and setting tank is provided with Figure 2 The guide wire structure 16 is shown; wherein, a plurality of guide wire grooves 17 are arranged on the guide wire structure, so that the fiber bundles receive an upward supporting force in the guide wire grooves, so that the bundled bundles are spread in the guide wire grooves.

[0092] After multi-stage water washing treatment (three-stage water washing treatment, the temperature is 55℃, 65℃, 70℃), multi-stage hot drawing treatment (three-stage hot water drawing treatment, the temperature is 85℃, 88℃, 95℃, the total drawing is 1.3 times), oiling treatment, drying densification treatment (temperature gradient is 100℃, 108℃, 115℃, 120℃) and steam drawing treatment (total drawing is 3.5 times), high-density, high-crystallinity and high-strength polyacrylonitrile fiber is prepared. Among them, the bulk density of polyacrylonitrile fiber is 1.19g / cm 3 , crystallinity is 54.6% and strength is 630Mpa.

[0093] 3) Short cutting process steps:

[0094] First, the polyacrylonitrile fibers from at least two spinning positions are combined and then chopped. During the chopped process, the polyacrylonitrile fibers are pulled by a feed roller, and the fiber bundles are continuously processed by a fiber cutter under the rotation and traction of the cutting feed roller, and cut into target lengths to obtain chopped fibers.

[0095] The obtained chopped fibers are evenly distributed on the conveyor belt, and are heated in the drying device through the conveyor belt to remove moisture, wherein the drying temperature is 100°C and the drying time is 30 seconds. The dried chopped fibers are sent to the fiber screening device for vibration screening. After passing through the fiber screening device, the chopped fibers enter the fiber collecting device below for collection.

[0096] The collected short-cut fibers are uniform in length and dispersed evenly without any adhesion phenomenon. The single-filament diameter of the short-cut acrylonitrile fibers is 9 μm and the strength is 630 MPa.

[0097] Example 3

[0098] This embodiment recycles waste polyacrylonitrile polymerization liquid, mainly comprising the following steps:

[0099] 1) Waste polyacrylonitrile polymer solution (viscosity of 500 Pa.s) is ejected from a spinneret to form a spinning stream and enter a spinning tunnel; in the spinning tunnel, as the solvent in the spinning stream continues to evaporate, the concentration of the filament stream continues to increase until it solidifies to form primary fibers.

[0100] The process parameters are as follows: the spinning speed is 5m / s, the height of the spinning stream entering the spinning tunnel is 5m (i.e., the distance between the spinneret and the bottom of the spinning tunnel is 5m); the drafting multiple is 2 times; the temperature in the spinning tunnel is 300℃; the spinning stream is heated in the tunnel, and the solvent evaporates quickly before initial shaping. The flowing atmosphere in the spinning tunnel is nitrogen, and the airflow is 500Nm 3 / h. The solvent flows out of the spinning shaft along with the flowing atmosphere and is cooled and recovered in the cooler. The residence time of the filament stream in the spinning shaft is 3s. In addition, there are multiple air inlets for the flowing atmosphere, which are evenly distributed around the spinning shaft.

[0101] 2) The spun fibers are sequentially subjected to a drawing and shaping treatment, a water washing treatment, a hot water drawing treatment, an oiling treatment, a drying and densification treatment, and a steam drawing treatment to obtain polyacrylonitrile fibers.

[0102] Among them, the process parameters are controlled as follows:

[0103] In the step of drawing and setting treatment: the nascent fiber enters the setting liquid directly from the bottom of the spinning tunnel for drawing and setting treatment; wherein, the setting liquid is N,N-dimethylformamide with a concentration of 40wt%. The temperature of the drawing and setting treatment is 20°C, and the drawing multiple is 2.0 times. Here, the solvent in the tow is further dispersed in the setting liquid, and the performance and shape of the tow are further stabilized. The drawing and setting treatment is carried out in the drawing and setting tank; wherein, the drawing and setting tank is provided with the following Figure 2 The guide wire structure 16 is shown; wherein, a plurality of guide wire grooves 17 are arranged on the guide wire structure, so that the fiber bundles receive an upward supporting force in the guide wire grooves, so that the bundled bundles are spread in the guide wire grooves.

[0104] After multi-stage water washing (two-stage water washing, temperature is 55 ℃ and 60 ℃), multi-stage hot drawing treatment (two-stage hot water drawing treatment, temperature is 85 ℃ and 95 ℃, total drawing is 1.2 times), oiling treatment, drying and densification treatment (the temperature gradient of drying and densification treatment is 95 ℃, 110 ℃, 115 ℃, 120 ℃) ​​and steam drawing treatment (steam drawing multiple is 3.0 times), high-density, high-crystallinity and high-strength polyacrylonitrile fiber is prepared. Among them, the bulk density of polyacrylonitrile fiber is 1.18g / cm 3 , crystallinity is 49.1% and strength is 440Mpa.

[0105] 3) Short cutting process steps:

[0106] First, the polyacrylonitrile fibers from at least two spinning positions are combined and then chopped. During the chopped process, the polyacrylonitrile fibers are pulled by a feed roller, and the fiber bundles are continuously processed by a fiber cutter under the rotation and traction of the cutting feed roller, and cut into target lengths to obtain chopped fibers.

[0107] The obtained chopped fibers are evenly distributed on the conveyor belt, and are heated in the drying device through the conveyor belt to remove moisture, wherein the drying temperature is 100°C and the drying time is 30 seconds. The dried chopped fibers are sent to the fiber screening device for vibration screening. After passing through the fiber screening device, the chopped fibers enter the fiber collecting device below for collection.

[0108] The collected short-cut fibers are uniform in length and dispersed evenly without any adhesion phenomenon. The single-filament diameter of the short-cut acrylonitrile fibers is 15 μm and the strength is 440 MPa.

[0109] Comparative Example 1

[0110] Comparative Example 1: Recycling the waste polyacrylonitrile polymerization liquid mainly includes the following steps:

[0111] 1) Waste polyacrylonitrile polymer solution (viscosity of 200 Pa.s) is ejected from a spinneret to form a spinning stream and enter a spinning tunnel; in the spinning tunnel, as the solvent in the spinning stream continues to evaporate, the concentration of the filament stream continues to increase until it solidifies to form primary fibers.

[0112] The process parameters are as follows: the spinning speed is 7m / s, the height of the spinning stream entering the spinning tunnel is 5m (i.e., the distance between the spinneret and the bottom of the spinning tunnel is 5m); the drafting multiple is 1.5 times; the temperature in the spinning tunnel is 150°C; the spinning stream is heated in the tunnel, and the solvent evaporates quickly before initial shaping. The flowing atmosphere in the spinning tunnel is nitrogen, and the airflow is 400Nm 3 / h. The solvent flows out of the spinning shaft along with the flowing atmosphere and is cooled and recovered in the cooler.

[0113] 2) The spun fibers are sequentially subjected to a drawing and shaping treatment, a water washing treatment, a hot water drawing treatment, an oiling treatment, a drying and densification treatment, and a steam drawing treatment to obtain polyacrylonitrile fibers.

[0114] Among them, the process parameters are controlled as follows:

[0115] In the step of drawing and setting treatment: the raw fiber directly enters the setting liquid from the bottom of the spinning channel for drawing and setting treatment; wherein the setting liquid is an aqueous solution of N,N-dimethylformamide with a concentration of 35wt%. The temperature of the drawing and setting treatment is 15°C, and the drawing multiple is 2.0 times. The drawing and setting treatment is carried out in the drawing and setting tank; wherein the drawing and setting tank is provided with Figure 2 The guide wire structure 16 is shown; wherein, a plurality of guide wire grooves 17 are arranged on the guide wire structure, so that the fiber bundles receive an upward supporting force in the guide wire grooves, so that the bundled bundles are spread in the guide wire grooves.

[0116] After multi-stage water washing treatment (three-stage water washing treatment, the temperature is 55℃, 60℃, 65℃), multi-stage hot drawing treatment (hot water drawing treatment at both ends, 85℃ and 90℃, the total drawing is 1.2 times), oiling treatment, drying densification treatment (temperature gradient is 100℃, 105℃, 115℃, 120℃) and steam drawing treatment (drawing multiple is 3 times), polyacrylonitrile fiber is prepared. However, the performance of the polyacrylonitrile fiber is poor, the strength is 158Mpa), and the broken wire is serious.

[0117] It should be noted here that: in Comparative Example 1, under conditions of faster spinning speed, the time before the extruded liquid flow leaves the spinneret and enters the coagulation bath is shorter, and the influence of surface tension is weaker, so the regularity of the fiber cross-sectional shape is poor, reducing the overall density of the nascent fiber.

[0118] Comparative Example 2

[0119] Comparative Example 2 recycles the waste polyacrylonitrile polymerization liquid. The difference from Example 1 is that Comparative Example 2 does not have a drafting and shaping tank. Figure 2 The guidewire structure 16 is shown.

[0120] Other steps and parameters are consistent with those in Example 1.

[0121] Comparative Example 2: The bulk density of polyacrylonitrile fiber prepared is 1.18 g / cm 3 , crystallinity is 47.6% and strength is 376Mpa.

[0122] Here, the reason why the performance of the polyacrylonitrile fiber prepared in Comparative Example 2 is inferior to that of Example 1 is that no wire guide structure is provided in the drafting and shaping groove of Comparative Example 2.

[0123] It should be noted here that: a wire guide structure is added to the stretching and shaping groove; the wire guide grooves on the wire guide structure enable the fiber bundle to receive an upward support force in the wire guide grooves, so that the bundled fiber bundle is spread and fiberized in the wire guide grooves, and each single fiber in the bundle is as fully contacted with the bath liquid in the stretching groove as possible, thereby enhancing the mass transfer and heat transfer effects of the entire fiber bundle. During the stretching process, the single fibers are in the same bath liquid environment, and the solvent in all the single fibers is guaranteed to diffuse into the water. The mass transfer and heat transfer effects of each single fiber remain consistent, thereby improving the quality of the fiber.

[0124] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Any simple modification, equivalent change and modification made to the above embodiment according to the technical essence of the present invention still falls within the scope of the technical solution of the present invention.

Claims

1. A method for recycling waste polyacrylonitrile polymerization liquid, characterized in that: It includes the following steps: The steps of preparing polyacrylonitrile fiber are as follows: waste polyacrylonitrile polymer solution is ejected from a spinning device to form a spinning fine stream, and the spinning fine stream enters a spinning tunnel; in the spinning tunnel, as the solvent in the spinning fine stream is continuously volatilized, the concentration of the formed fine stream is continuously increased until it is solidified to form a primary fiber; the primary fiber is sequentially subjected to a stretching and shaping treatment, a water washing treatment, a hot water stretching treatment, an oiling treatment, a drying and densification treatment, and a steam stretching treatment to obtain a polyacrylonitrile fiber; The short-cutting step is to short-cut the polyacrylonitrile fibers to obtain short-cut polyacrylonitrile fibers.

2. The method for recycling waste polyacrylonitrile polymerization liquid according to claim 1, characterized in that: In the step of preparing polyacrylonitrile fiber: The waste polyacrylonitrile polymer solution is ejected from the spinning device at a spinning speed of 1.5-5 m / s; and / or The viscosity of the waste polyacrylonitrile polymerization liquid is 150-500 Pa.s; and / or The spinneret of the spinneret device is located near the top of the spinning tunnel, and the distance between the spinneret and the bottom of the spinning tunnel is 4-10m; and / or In the spinning shaft, the drafting multiple of the filament stream is 2-10 times; the residence time of the filament stream in the spinning shaft is 1-10s; and / or The temperature of the spinning shaft is 150-300° C.; and / or The flowing atmosphere in the spinning tunnel is selected from one or more of nitrogen, superheated steam, carbon dioxide, and argon; preferably, the flow rate of the flowing atmosphere is 100-500Nm 3 / h; and / or In the spinning shaft, the volatilized solvent is carried away by the flowing atmosphere for recycling.

3. The method for recycling waste polyacrylonitrile polymerization liquid according to claim 1 or 2, characterized in that: In the step of preparing polyacrylonitrile fiber: The hot air circulation system is used to realize the circulation of the flowing atmosphere in the spinning tunnel and the recycling of the solvent; wherein the hot air circulation system comprises: A flowing atmosphere input pipeline, the flowing atmosphere input pipeline is connected to the air inlet of the spinning tunnel and is used to input the flowing atmosphere into the spinning tunnel; A flowing atmosphere output pipeline, the flowing atmosphere output pipeline and the gas outlet of the spinning tunnel are used to make the flowing atmosphere with volatile solvent flow out of the spinning tunnel; A cooler, wherein the flowing atmosphere output pipeline is connected to the air inlet of the cooler so that the flowing atmosphere with the volatile solvent enters the cooler to condense the volatile solvent into a liquid state; A solvent recovery device, the solvent recovery device is connected to the condensate outlet of the cooler and is used to recover the condensed solvent; A heating pipeline, wherein the inlet end of the heating pipeline is connected to the air outlet of the cooler through a pipeline, and is used to heat the flowing atmosphere discharged from the cooler, and the air outlet of the heating pipeline is connected to the flowing atmosphere input pipeline, so as to realize the circulation of the flowing atmosphere; Preferably, the inlet end of the heating pipeline is also connected to the air supply pipeline; Preferably, the heating pipeline includes a pipeline and a heat exchanger arranged on the pipeline; Preferably, the outlet end of the heating pipeline is connected to the flowing atmosphere input pipeline through a fan; Preferably, the air outlet of the spinning tunnel is located at the upper end of the side wall of the spinning tunnel; Preferably, the spinning tunnel has multiple air inlets that are evenly distributed on the surrounding side walls of the spinning tunnel.

4. The method for recycling waste polyacrylonitrile polymerization liquid according to any one of claims 1 to 3, characterized in that: In the step of preparing polyacrylonitrile fiber: When the spun fibers are subjected to a stretching and shaping treatment, the spun fibers are passed through an opening at the bottom of the spinning tunnel and then enter a shaping liquid for stretching and shaping; The drafting multiple of the draft setting is 1.2-2.0 times, and the temperature of the setting liquid is 5-20°C; Preferably, the drafting and shaping process is carried out in a drafting and shaping groove; wherein a wire guide structure is provided in the drafting and shaping groove; wherein a plurality of wire guide grooves are provided on the wire guide structure, so that the fiber bundle receives an upward supporting force in the wire guide groove, so that the bundled fiber bundle is spread in the wire guide groove; Preferably, the fixing liquid is an aqueous solution of waste polyacrylonitrile solvent, preferably an aqueous solution prepared by recovering the solvent volatilized from the spinning stream; or the fixing liquid is N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, propylene carbonate, an aqueous solution of propylene carbonate; Preferably, the concentration of the setting liquid is 10-45wt%.

5. The method for recycling waste polyacrylonitrile polymerization liquid according to any one of claims 1 to 6, characterized in that: In the step of preparing polyacrylonitrile fiber: The fibers after the drafting and setting treatment are sequentially passed through multiple washing zones for washing treatment; wherein the temperature of the latter washing zone is 3-5°C higher than that of the former washing zone; the temperature of the first washing zone is 50-55°C; the washing treatment time is 5-10 minutes; and / or When the fibers after the drawing and setting treatment are washed, a vibrating device is provided in each washing zone to vibrate the fibers and increase the relative movement between the fiber bundle and the water; preferably, the vibrating device is a beating stick; and / or When the fibers after the drawing and setting treatment are washed, deionized water is added to each washing zone by bubbling; and / or When the fibers after the drafting and setting treatment are washed, a partition is provided in each washing zone to increase the turbulence effect in the washing zone; and / or When the fibers after the drawing and setting treatment are washed with water, a spraying device is used to spray water on the fibers leaking out of the water; and / or The organic solvent content in the fiber after the water washing treatment is less than or equal to 0.03wt%.

6. The method for recycling waste polyacrylonitrile polymerization liquid according to any one of claims 1 to 5, characterized in that: In the step of preparing polyacrylonitrile fiber: The hot water drawing treatment is a multi-pass drawing at a temperature range of 75-95° C., and the total drawing multiple is 1-1.3; and / or The fibers after hot water drawing treatment are first dried and then oiled to remove moisture. Preferably, the fibers after hot water drawing treatment are dried by passing through a hot air oven or a hot roll. and / or The drying and densification treatment temperature is 95-130°C, the temperature difference between adjacent temperature gradients is 0-10°C, the drying and densification time for each temperature level is 5-10s, and the draft ratio is 0.95-1.1; and / or The fibers after drying and densification are subjected to steam drawing treatment using saturated water vapor or superheated steam as a medium, wherein the steam pressure is 0.12-0.4 MPa, the drawing multiple is 2-5 times, and the residence time of the steam drawing treatment is 3-6 seconds.

7. The method for recycling polyacrylonitrile polymerization liquid according to any one of claims 1 to 6, characterized in that: The monofilament diameter of polyacrylonitrile fiber is 9-20μm and the bulk density is 1.18-1.19g / cm 3 .

8. The method for recycling polyacrylonitrile polymerization liquid according to any one of claims 1 to 7, characterized in that: In the short-cutting step: The polyacrylonitrile fibers are conveyed to a short-cut device for short-cut processing to obtain short-cut fibers; the short-cut fibers are dried and screened to obtain polyacrylonitrile-based short-cut fibers of a desired size; Preferably, the chopped fibers obtained after the chopped treatment are dried by a drying device under the action of a conveying device, and then the dried chopped fibers are conveyed to a screening device; Preferably, the drying temperature is 90-100° C., and the drying time is 25-30 seconds.

9. The method for recycling polyacrylonitrile polymerization liquid according to any one of claims 1 to 8, characterized in that: Before the short-cutting process, the polyacrylonitrile fibers from at least two spinning positions are firstly combined and then short-cutting is performed.

10. A polyacrylonitrile chopped fiber, characterized in that: The polyacrylonitrile short-cut fibers are Prepared by the method for recycling waste polyacrylonitrile polymerization liquid according to any one of claims 1 to 9; in, The single filament diameter of the short-cut polyacrylonitrile fiber is 9-20 μm, and the strength is 350-670 MPa.

Citation Information

Cited By

  • Low-cost production process and device for polyacrylonitrile fibers

    CN119956513A