Heterocyclic aramid fiber and preparation method thereof

Through the microfluidic synthesis method, the low-temperature polyp-phenylenediamine and 5-amino-2-(4-aminophenyl)-benzimidazole were solved, and the problem of low preparation efficiency of traditional batch kettle method was realized, and heterocyclic aramid was achieved. Highly efficient and controlled synthesis of fibers and excellent mechanical properties.

CN118932529APending Publication Date: 2024-11-12HEBEI UNIV OF TECH
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411193754.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The mass transfer and heat transfer efficiency of heterocyclic aramid fibers is slow in the preparation of traditional batch kettle method, resulting in low reaction efficiency and uncontrollable reaction conditions, making it difficult to achieve efficient and controllable synthesis.

Method used

Using microfluidic synthesis method, para-phenylenediamine and 5-amino-2-(4-aminophenyl)-benzimidazole were polycondensed at low temperature in a micromixer, and heterocyclic aramid fibers were prepared by microfluidic spinning technology. , control reaction temperature and residence time, and accurately regulate the microstructure and molecular weight of the fibers.

Benefits of technology

The efficient and controllable synthesis of heterocyclic aramid fiber has been achieved, and the synthesis efficiency and mechanical properties have been improved. The viscosity and mechanical properties of the spinning liquid have been significantly improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118932529A_ABST
    Figure CN118932529A_ABST
Patent Text Reader

Abstract

The invention relates to a heterocyclic aramid fiber and a preparation method thereof. The preparation method of the heterocyclic aramid fiber comprises the following steps: dispersing p-phenylenediamine and 5-amino-2-(4-aminophenyl)-benzimidazole into a solvent I to obtain a solution A, dissolving paraphthaloyl chloride into a solvent II to obtain a solution B, injecting the solution A and the solution B into a micro-mixer to be mixed to obtain a mixed solution, and adding the mixed solution into the micro-mixer to obtain the heterocyclic aramid fiber. Carrying out low-temperature polycondensation on the mixed solution in a micro-packed bed to obtain a spinning solution, and preparing the spinning solution into the heterocyclic aramid fiber by adopting a spinning technology. The heterocyclic aramid fiber is prepared by adopting a microfluidic synthesis method, and a microfluidic technology not only can enhance the mixing efficiency and the mass transfer and heat transfer efficiency of a mixed solution, but also can accurately control the reaction time of the heterocyclic aramid fiber, so that efficient and controllable synthesis of the heterocyclic aramid fiber in the reaction process is realized; the heterocyclic aramid fiber with excellent mechanical property is prepared. The preparation method of the heterocyclic aramid fiber has the advantages of high synthesis efficiency, strong mixing heat transfer effect, controllable reaction conditions and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of heterocyclic aramid fiber preparation, and in particular relates to a heterocyclic aramid fiber and a preparation method thereof. Background Art

[0002] Aramid fibers have received extensive attention due to their excellent mechanical properties and high temperature resistance, and are considered to be key materials in the fields of bulletproof vests, aerospace, composite armor, and high-speed trains. By introducing monomers with heterocyclic rings into the traditional aramid fiber polymer molecular chain, the degree of orientation of the aramid fiber polymer chain can be improved, the defects and stress concentration points of the aramid fiber polymer chain can be reduced, and the mechanical properties of the aramid fiber can be improved. The traditional intermittent kettle method for preparing heterocyclic aramid fibers is limited by factors such as slow mass and heat transfer efficiency and uncontrollable fluids, resulting in problems such as low efficiency and uncontrollable reaction conditions. Therefore, developing a new synthesis method to achieve efficient and controllable synthesis of heterocyclic aramid fibers is a major challenge in this field.

[0003] The invention patent with application publication number CN118271596A discloses a heterocyclic aramid polymer stock solution, heterocyclic aramid fiber and a preparation method. The preparation method of the heterocyclic aramid polymer stock solution is as follows: S1, under the protection of inert gas, dissolving the diamine monomer and the third monomer into the N,N-dimethylacetamide solution of lithium chloride; S2, lowering the temperature in the system of step S1, slowly adding part of terephthaloyl chloride, stirring for reaction, neutralizing with alkaline substances, filtering to obtain the first step polymerization stock solution; S3, controlling the system temperature, adding the remaining part of terephthaloyl chloride to the first step polymerization stock solution for reaction, neutralizing with alkaline substances after the reaction to obtain the heterocyclic aramid polymer stock solution, the heterocyclic aramid polymer stock solution is prepared by the traditional intermittent kettle method, which has slow mass and heat transfer and low reaction efficiency. Summary of the invention

[0004] The first object of the present invention is to provide a method for preparing heterocyclic aramid fiber to solve the technical problems of slow mass and heat transfer and low reaction efficiency in the conventional intermittent reactor method for preparing heterocyclic aramid fiber.

[0005] A second object of the present invention is to provide a heterocyclic aramid fiber.

[0006] In order to achieve the above purpose, the technical solution adopted by the present invention is:

[0007] A method for preparing heterocyclic aramid fiber comprises the following steps: dispersing p-phenylenediamine and 5-amino-2-(4-aminophenyl)-benzimidazole in a solvent one to obtain a solution A, dissolving terephthaloyl chloride in a solvent two to obtain a solution B, injecting the solution A and the solution B into a micro mixer to mix to obtain a mixed solution, polycondensing the mixed solution at low temperature in a micro-filled bed to obtain a spinning solution, and preparing the spinning solution into heterocyclic aramid fiber by using a spinning technology.

[0008] Furthermore, the solution A and the solution B need to be preheated before being injected into the micro mixer, the preheating temperature is 0 to 5° C., and the preheating time is 10 to 30 seconds.

[0009] Furthermore, the residence time of the mixed liquid in the microchannel is 2 to 10 minutes, and the microchannel includes the micromixer and the micropacked bed.

[0010] Furthermore, the flow rate of the solution A injected into the micro mixer is 1 to 10 mL / min, and the flow rate of the solution B injected into the micro mixer is 1 to 10 mL / min.

[0011] Furthermore, the filler of the micro-packed bed is a ceramic filler or a stainless steel filler, the inner diameter of the micro-packed bed is 2-4 mmmm, and the outer diameter is 4-6 mmmm; the inner diameter of the micro-mixer is 50-200 μm.

[0012] Furthermore, the preparation method of the solution A is: dispersing 0.1-1 g of the p-phenylenediamine and 1-5 g of the 5-amino-2-(4-aminophenyl)-benzimidazole in 10-50 mL of the solvent one; the preparation method of the solution B is: dissolving 1-5 g of the terephthaloyl chloride in 10-50 mL of the solvent two.

[0013] Furthermore, the solvent one is one or more of dimethylformamide, dimethylacetamide, N-methylpyrrolidone, and dimethyl sulfoxide; the solvent two is one or more of dimethylformamide, dimethylacetamide, N-methylpyrrolidone, and dimethyl sulfoxide.

[0014] Furthermore, lithium chloride is added to the solution A, and the amount of lithium chloride added is 1 to 5 g.

[0015] Furthermore, the low-temperature polycondensation is carried out at 0 to 10° C. for 2 to 10 minutes, the viscosity of the spinning solution is 1000 to 60000 mPa·s, and the spinning technology is microfluid spinning technology.

[0016] A heterocyclic aramid fiber is prepared by adopting the above-mentioned preparation method of the heterocyclic aramid fiber.

[0017] Beneficial effects of the present invention:

[0018] The present invention adopts a microfluidic synthesis method to prepare heterocyclic aramid fibers. The microfluidic technology can not only enhance the mixing efficiency and mass transfer and heat transfer efficiency of the mixed solution, but also accurately control the reaction time of the heterocyclic aramid fibers, thereby realizing efficient and controllable synthesis of the heterocyclic aramid fiber reaction process, and preparing heterocyclic aramid fibers with excellent mechanical properties. The heterocyclic aramid fiber preparation method of the present invention has the advantages of high synthesis efficiency, strong mixing heat transfer effect, controllable reaction conditions, etc.

[0019] The aramid fibers prepared by the traditional top-down chemical stripping method have an uneven microstructure and uncontrollable molecular weight, which limits their mechanical properties. Compared with the traditional top-down chemical stripping method, the microfluidic synthesis method of the present invention adopts a bottom-up low-temperature polycondensation method. By adjusting the reaction temperature, reactant concentration and residence time, the microstructure and molecular weight of the heterocyclic aramid fibers of the present invention can be controlled, thereby accurately controlling the mechanical properties of the heterocyclic aramid fibers. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 A flow chart for preparing heterocyclic aramid fibers;

[0021] Figure 2 The actual pictures of the spinning solutions in Examples 1 to 5;

[0022] Figure 3 This is a diagram of the heterocyclic aramid fiber in Example 4. DETAILED DESCRIPTION

[0023] The present invention will be further described below in conjunction with the embodiments of the present invention and the accompanying drawings.

[0024] Figure 2 From left to right in the figure are the actual pictures of the spinning solutions of Examples 1-5.

[0025] Example 1

[0026] The method for preparing the heterocyclic aramid fiber of Example 1 comprises the following steps:

[0027] 0.432 g of p-phenylenediamine (PPD), 1.346 g of 5-amino-2-(4-aminophenyl)-benzimidazole (PABZ), and 3.5 g of lithium chloride (LiCl) were dispersed in 50 mL of dimethylacetamide to form solution A; 2.03 g of terephthaloyl chloride (TPC) was dispersed in 50 mL of dimethylacetamide to form solution B; solution A and solution B were preheated in a preheating pipe at 0°C for 10 seconds, and then solution A and solution B were injected into a micromixer using a horizontal flow pump to strengthen the mixing of solution A and solution B to form a homogeneous mixed solution, and the mixed solution was reacted in a micropacked bed at 5°C for 10 minutes to form a spinning solution, and the viscosity of the spinning solution was 2000 mPa·s; the spinning solution was prepared into heterocyclic aramid fiber using microfluidic spinning technology. The flow rate of solution A is 5mL / min, and the flow rate of solution B is 5mL / min; the inner diameter of the micro mixer is 100μm, the filler of the micro packed bed is stainless steel filler, the inner diameter of the micro packed bed is 4mm, and the outer diameter is 6mm. The residence time of the mixed liquid in the micro channel is 10min. The mixed liquid is cooled by a condensing water bath in the micro packed bed for low temperature polycondensation. The micro channel includes a preheating pipe, a micro mixer, a micro packed bed, and a delay pipe.

[0028] Example 2

[0029] The method for preparing the heterocyclic aramid fiber of Example 2 comprises the following steps:

[0030] 0.432 g of p-phenylenediamine, 1.346 g of 5-amino-2-(4-aminophenyl)-benzimidazole and 3.5 g of lithium chloride are dispersed in 40 mL of dimethylacetamide to form solution A; 2.03 g of terephthaloyl chloride is dispersed in 40 mL of dimethylacetamide to form solution B; solution A and solution B are preheated in a preheating pipe at 0°C for 10 seconds, and then solution A and solution B are injected into a micromixer by a horizontal flow pump to strengthen the mixing of solution A and solution B so as to form a homogeneous mixed solution, and the mixed solution is reacted in a micropacked bed at 5°C for 10 minutes to form a spinning solution, and the viscosity of the spinning solution is 5000 mPa·s; the spinning solution is prepared into heterocyclic aramid fiber by microfluid spinning technology. The flow rate of solution A is 5 mL / min, and the flow rate of solution B is 5 mL / min. The inner diameter of the micromixer is 100 μm, and the filler of the micropacked bed is stainless steel filler. The inner diameter of the micropacked bed is 4 mm, and the outer diameter is 6 mm. The residence time of the mixed solution in the microchannel is 10 min.

[0031] Example 3

[0032] The method for preparing the heterocyclic aramid fiber of Example 3 comprises the following steps:

[0033] 0.432 g of p-phenylenediamine, 1.346 g of 5-amino-2-(4-aminophenyl)-benzimidazole and 3.5 g of lithium chloride are dispersed in 30 mL of dimethylacetamide to form solution A; 2.03 g of terephthaloyl chloride is dispersed in 30 mL of dimethylacetamide to form solution B; solution A and solution B are preheated in a preheating pipe at 0°C for 10 seconds, and then solution A and solution B are injected into a micromixer by a horizontal flow pump to strengthen the mixing of solution A and solution B so as to form a homogeneous mixed solution, and the mixed solution is reacted in a micropacked bed at 5°C for 10 minutes to form a spinning solution, and the viscosity of the spinning solution is 30000 mPa·s; the spinning solution is prepared into heterocyclic aramid fiber by microfluid spinning technology. The flow rate of solution A is 5 mL / min, and the flow rate of solution B is 5 mL / min. The inner diameter of the micromixer is 100 μm, and the filler of the micropacked bed is stainless steel filler. The inner diameter of the micropacked bed is 4 mm, and the outer diameter is 6 mm. The residence time of the mixed solution in the microchannel is 10 min.

[0034] Example 4

[0035] The method for preparing the heterocyclic aramid fiber of Example 4 comprises the following steps:

[0036] 0.432 g of p-phenylenediamine, 1.346 g of 5-amino-2-(4-aminophenyl)-benzimidazole and 3.5 g of lithium chloride are dispersed in 20 mL of dimethylacetamide to form solution A; 2.03 g of terephthaloyl chloride is dispersed in 20 mL of dimethylacetamide to form solution B; solution A and solution B are preheated in a preheating pipe at 0°C for 10 seconds, and then solution A and solution B are injected into a micromixer by a horizontal flow pump to strengthen the mixing of solution A and solution B so as to form a homogeneous mixed solution, and the mixed solution is reacted in a micropacked bed at 5°C for 10 minutes to form a spinning solution, and the viscosity of the spinning solution is 50000 mPa·s; the spinning solution is prepared into heterocyclic aramid fiber by microfluid spinning technology. The flow rate of solution A is 5 mL / min, and the flow rate of solution B is 5 mL / min. The inner diameter of the micromixer is 100 μm, and the filler of the micropacked bed is stainless steel filler. The inner diameter of the micropacked bed is 4 mm, and the outer diameter is 6 mm. The residence time of the mixed solution in the microchannel is 10 min.

[0037] Example 5

[0038] The method for preparing the heterocyclic aramid fiber of Example 5 comprises the following steps:

[0039] 0.432 g of p-phenylenediamine, 1.346 g of 5-amino-2-(4-aminophenyl)-benzimidazole and 3.5 g of lithium chloride are dispersed in 30 mL of dimethylacetamide to form solution A; 2.03 g of terephthaloyl chloride is dispersed in 30 mL of dimethylacetamide to form solution B; solution A and solution B are preheated in a preheating pipe at 0°C for 10 seconds, and then solution A and solution B are injected into a micromixer by a horizontal flow pump to strengthen the mixing of solution A and solution B so as to form a homogeneous mixed solution, and the mixed solution is reacted in a micropacked bed at 5°C for 3 minutes to form a spinning solution, and the viscosity of the spinning solution is 10000 mPa·s; the spinning solution is prepared into heterocyclic aramid fiber by microfluid spinning technology. The flow rate of solution A is 10 mL / min, and the flow rate of solution B is 5 mL / min. The inner diameter of the micromixer is 100 μm, and the filler of the micropacked bed is stainless steel filler. The inner diameter of the micropacked bed is 4 mm, and the outer diameter is 6 mm. The residence time of the mixed solution in the microchannel is 3 min.

[0040] The heterocyclic aramid fiber prepared by the invention has a breaking strength of about 5 GPa and a breaking elongation of about 4.4%.

Claims

1. A method for preparing heterocyclic aramid fiber, characterized in that: The following steps are involved: Paraphenylenediamine and 5-amino-2-(4-aminophenyl)-benzimidazole are dispersed in solvent one to obtain solution A, terephthaloyl chloride is dissolved in solvent two to obtain solution B, solution A and solution B are injected into a micro mixer to mix to obtain a mixed solution, the mixed solution is subjected to low-temperature polycondensation in a micro-packed bed to obtain a spinning solution, and the spinning solution is prepared into heterocyclic aramid fiber by using spinning technology.

2. The method for preparing heterocyclic aramid fiber according to claim 1, characterized in that: The solution A and the solution B need to be preheated before being injected into the micro mixer. The preheating temperature is 0 to 5° C. and the preheating time is 10 to 30 seconds.

3. The method for preparing heterocyclic aramid fiber according to claim 1, characterized in that: The residence time of the mixed liquid in the microchannel is 2 to 10 minutes, and the microchannel includes the micromixer and the micropacked bed.

4. The method for preparing heterocyclic aramid fiber according to claim 1, characterized in that: The flow rate of the solution A injected into the micro mixer is 1 to 10 mL / min, and the flow rate of the solution B injected into the micro mixer is 1 to 10 mL / min.

5. The method for preparing heterocyclic aramid fiber according to claim 1, characterized in that: The filler of the micro-packed bed is a ceramic filler or a stainless steel filler, the inner diameter of the micro-packed bed is 2-4 mm, and the outer diameter is 4-6 mm; the inner diameter of the micro-mixer is 50-200 μm.

6. The method for preparing heterocyclic aramid fiber according to claim 1, characterized in that: The preparation method of the solution A is as follows: 0.1 to 1 g of the p-phenylenediamine and 1 to 5 g of the 5-amino-2-(4-aminophenyl)-benzimidazole are dispersed in 10 to 50 mL of the solvent one; the preparation method of the solution B is as follows: 1 to 5 g of the terephthaloyl chloride is dissolved in 10 to 50 mL of the solvent two.

7. The method for preparing heterocyclic aramid fiber according to claim 1, characterized in that: The first solvent is one or more of dimethylformamide, dimethylacetamide, N-methylpyrrolidone, and dimethyl sulfoxide; the second solvent is one or more of dimethylformamide, dimethylacetamide, N-methylpyrrolidone, and dimethyl sulfoxide.

8. The method for preparing heterocyclic aramid fiber according to claim 1, characterized in that: Lithium chloride is added to the solution A, and the amount of lithium chloride added is 1 to 5 g.

9. The method for preparing heterocyclic aramid fiber according to claim 1, characterized in that: The low-temperature polycondensation is carried out at 0 to 10° C. for 2 to 10 minutes, the viscosity of the spinning solution is 1000 to 60000 mPa·s, and the spinning technology is microfluid spinning technology.

10. A heterocyclic aramid fiber, characterized in that: The heterocyclic aramid fiber is prepared by the preparation method of the heterocyclic aramid fiber according to claim 1.

Citation Information

Cited By

  • Solution sample introduction polymerization method of heterocyclic aramid

    CN121495114A