MXene reinforced heterocyclic aramid fiber and preparation method thereof

The MXene nanosheets were polymerized in situ into heterocyclic aramid fibers through low-temperature reaction and microfluidic spinning technology, which solved the problem of insufficient mechanical properties of traditional fibers, and realized the preparation of high-performance MXene enhanced heterocyclic aramid fibers, significantly Improves the elongation and strength of the fibers.

CN118932532APending Publication Date: 2024-11-12HEBEI UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411193839.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The elongation and fracture strength of traditional heterocyclic aramid fibers are low, making it difficult to meet the needs of complex application scenarios. The non-covalent bond interaction and poor dispersion between MXene nanosheets and polymer molecular chains limit its mechanics. Performance improvement.

Method used

MXene nanosheets were dissolved in solvent by low temperature reaction, and p-phenylenediamine and 5-amino-2-(4-aminophenyl)-benzimidazole were added to prepare MXene reinforced heterocyclic aramid fibers by microfluidic spinning technology. , improve the viscosity of the spinning liquid and the dispersion of MXene nanosheets, and enhance the interface interaction and crystallinity of polymer molecular chains.

Benefits of technology

The elongation and fracture strength of MXene reinforced heterocyclic aramid fibers are significantly improved, and the mechanical properties are significantly better than traditional fibers, and the cost is low, and the preparation method is simple.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118932532A_ABST
    Figure CN118932532A_ABST
Patent Text Reader

Abstract

The invention relates to an MXene reinforced heterocyclic aramid fiber and a preparation method thereof. The preparation method of the MXene enhanced heterocyclic aramid fiber comprises the following steps: dissolving an MXene nanosheet in a solvent to obtain a solution I, adding p-phenylenediamine and 5-amino-2-(4-aminophenyl)-benzimidazole into the solution I, reacting at low temperature, adding paraphthaloyl chloride in a stirring state to obtain a spinning solution, and performing spinning, washing and drying to obtain the MXene enhanced heterocyclic aramid fiber. And preparing the spinning solution into the MXene reinforced heterocyclic aramid fiber by adopting a spinning technology. The elongation at break of the prepared MXene reinforced heterocyclic aramid fiber is about 5.2%, the breaking strength is about 6GPa, the elongation at break and the breaking strength of the prepared MXene reinforced heterocyclic aramid fiber are far superior to those of existing heterocyclic aramid fibers, and the mechanical property of the prepared MXene reinforced heterocyclic aramid fiber is better.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of heterocyclic aramid preparation, and specifically relates to a MXene-reinforced heterocyclic aramid fiber and a preparation method thereof. Background Art

[0002] As a high-performance organic fiber material, heteroaramid fiber has excellent comprehensive properties, such as low volume density, high mechanical properties and good thermal stability, which makes heteroaramid fiber widely used in aerospace, military, civil and other fields. However, the mechanical properties of traditional heteroaramid fibers have been difficult to meet the increasingly complex application scenarios. The key to improving the mechanical properties of heteroaramid fibers lies in how to improve the interface interaction, crystallinity and orientation between the molecular chains of heteroaramid fiber polymers. Therefore, developing a new preparation method for reinforced heteroaramid fibers is a major challenge.

[0003] As a typical two-dimensional material, MXene nanosheets have been widely used to enhance the mechanical properties of polymer fibers due to their strong π-π interactions and rich surface chemical groups, which enable MXene nanosheets to enhance the interfacial interactions between polymer molecular chains. However, the weak non-covalent interactions between polymer molecular chains and MXene nanosheets limit their effect on enhancing the mechanical properties of polymer fibers. In addition, the poor dispersibility of MXene nanosheets in polymer solutions also results in their inability to further enhance the mechanical properties of polymer fibers. Therefore, how to improve the interaction between MXene and polymer molecular chains and improve its dispersibility in polymer solutions is the key to enhancing polymer fibers.

[0004] The invention patent with application publication number CN101921395A discloses a high-performance heterocyclic aramid and its preparation and application. The preparation method of the high-performance heterocyclic aramid includes the following process steps: A. Preparation of heterocyclic polyamide solution: adding 2-(4-aminophenyl)-5-aminobenzimidazole to a reaction kettle containing a composite solvent, stirring at room temperature for 50 to 150 minutes under nitrogen protection, then lowering the temperature in the kettle to -5 to 10°C, adding terephthaloyl chloride in 3 to 6 batches, with an interval of 10 to 100 minutes between each batch, and finally obtaining a polymer solution with a polymer solid content of 2 to 10% and a dynamic viscosity of 40,000 to 300,000 centipoises; B. Degassing 2. Wet spinning: the polymer solution is transferred to a degassing kettle for degassing and filtering at normal pressure or reduced pressure, and then wet spinning is adopted. The polymer solution is sprayed into a coagulation bath through a spinneret for coagulation and forming into primary fibers. The primary fibers are then plastically stretched in a plasticizing stretching bath at a stretching ratio of 50 to 150%, and then washed, oiled, dried, heat treated and surface treated, and then wound into a tube to obtain a golden aramid fiber with a breaking strength of 25 to 34 cN / dtex, an elastic modulus of 900 to 1200 cN / dtex and an elongation at break of 2.5 to 4.0%. The high-performance heterocyclic aramid fiber prepared by this method has a low elongation at break and a low breaking strength. Summary of the invention

[0005] The first object of the present invention is to provide a MXene-reinforced heterocyclic aramid fiber to solve the technical problems of low elongation at break and low breaking strength of existing heterocyclic aramid fibers.

[0006] The second object of the present invention is to provide a method for preparing MXene-reinforced heterocyclic aramid fibers.

[0007] In order to achieve the above purpose, the technical solution adopted by the present invention is:

[0008] A method for preparing MXene-reinforced heterocyclic aramid fiber comprises the following steps: dissolving MXene nanosheets in a solvent to obtain a solution one, adding p-phenylenediamine and 5-amino-2-(4-aminophenyl)-benzimidazole to the solution one, reacting at low temperature, adding terephthaloyl chloride under stirring to obtain a spinning solution, and using a spinning technology to prepare the spinning solution into a MXene-reinforced heterocyclic aramid fiber.

[0009] Furthermore, the MXene nanosheets are Ti3SiC2, Ti3C2T x 、V4C3T x 、Ta4C3T x One or more of the following; the addition amount of the MXene nanosheet is 0.01 to 1 g.

[0010] Furthermore, the MXene nanosheets are dissolved in the solvent and stirred for 10 to 60 minutes to obtain solution one, the p-phenylenediamine and 5-amino-2-(4-aminophenyl)-benzimidazole are added to the solution one under stirring and stirred for 0.5 to 2 hours, the temperature is lowered to 0 to 10° C. and reacted for 10 to 30 minutes, and the terephthaloyl chloride is added under stirring and reacted for 0.5 to 2 hours to obtain the spinning solution.

[0011] Furthermore, the added amount of the p-phenylenediamine is 0.1 to 1 g; the added amount of the 5-amino-2-(4-aminophenyl)-benzimidazole is 1 to 5 g; and the added amount of the terephthaloyl chloride is 1 to 5 g.

[0012] Furthermore, the solvent is one or more of N,N-dimethylformamide, N,N-dimethylacetamide, N-methylpyrrolidone, and dimethyl sulfoxide; and the added amount of the solvent is 50 to 150 mL.

[0013] Furthermore, lithium chloride is added to the solvent, and the amount of lithium chloride added is 1 to 5 g.

[0014] Furthermore, the fluid viscosity of the spinning solution is 10000 to 100000 mPa·s.

[0015] Furthermore, the spinning technology is microfluidic spinning technology.

[0016] A MXene-reinforced heterocyclic aramid fiber is prepared by using the above-mentioned method for preparing the MXene-reinforced heterocyclic aramid fiber.

[0017] Beneficial effects of the present invention:

[0018] The MXene-reinforced heterocyclic aramid fiber prepared by the present invention has an elongation at break of about 5.2% and a breaking strength of about 6 GPa. The elongation at break and the breaking strength of the MXene-reinforced heterocyclic aramid fiber of the present invention are much better than the elongation at break and the breaking strength of the existing heterocyclic aramid fiber. The MXene-reinforced heterocyclic aramid fiber prepared by the present invention has better mechanical properties.

[0019] The present invention only needs to add a very small amount of MXene nanosheets to achieve the regulation of spinning solution viscosity and the enhancement of mechanical properties, and has low cost and simple preparation method.

[0020] The present invention adopts a low-temperature polycondensation reaction to in-situ polymerize MXene nanosheets into heterocyclic aramid fibers to form a spinning solution, which can not only improve the interface interaction, crystallinity and orientation between the MXene nanosheets and the polymer molecular chains of the heterocyclic aramid fibers, but also improve the dispersibility of the MXene nanosheets in the spinning solution, thereby achieving the mechanical properties of the MXene-enhanced heterocyclic aramid fibers. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 The effect of different addition amounts of MXene nanosheets on the viscosity of the spinning solution;

[0022] Figure 2 This is a physical picture of the spinning solution in Example 3;

[0023] Figure 3 This is a physical picture of the MXene reinforced heterocyclic aramid fiber in Example 3. DETAILED DESCRIPTION

[0024] The present invention will be further described below in conjunction with the embodiments of the present invention and the accompanying drawings.

[0025] Example 1

[0026] The preparation method of MXene-reinforced heterocyclic aramid fiber of Example 1 comprises the following steps: 0.01 g of Ti3C2T x The nanosheets were dispersed in a mixture of lithium chloride (LiCl) and N, N-dimethylacetamide under stirring, and solution 1 was obtained by continuous stirring for 30 minutes. Solution 1 was transferred to a reactor, and 0.532 g of p-phenylenediamine (PPD) and 2.346 g of 5-amino-2-(4-aminophenyl)-benzimidazole (PABZ) were added while stirring for 1 hour. The reaction temperature was lowered to 5 ° C and stabilized for 30 minutes. 3.03 g of terephthaloyl chloride (TPC) was added while stirring, and the spinning solution was obtained by continuous stirring for 1 hour. The fluid viscosity of the spinning solution was 19618 mPa s, and the spinning solution was prepared into MXene-enhanced heterocyclic aramid fiber using microfluid spinning technology. The elongation at break of the MXene-enhanced heterocyclic aramid fiber of Example 1 is about 3.8%, and the breaking strength is about 4.3 GPa. The mass of lithium chloride is 4.5 g, and the amount of N, N-dimethylacetamide added is 100 mL.

[0027] Example 2

[0028] The preparation method of MXene-reinforced heterocyclic aramid fiber of Example 2 comprises the following steps: 0.0523 g of Ti3C2T xThe nanosheets were dispersed in a mixture of lithium chloride and N, N-dimethylacetamide under stirring, and solution 1 was obtained by continuous stirring for 30 min. Solution 1 was transferred to a reactor, and 0.532 g of p-phenylenediamine and 2.346 g of 5-amino-2-(4-aminophenyl)-benzimidazole were added while stirring for 1 h. The reaction temperature was lowered to 5 ° C and stabilized for 30 min. 3.03 g of terephthaloyl chloride was added while stirring, and continuous stirring was performed for 1 h to obtain a spinning solution. The fluid viscosity of the spinning solution was 57399 mPa s, and the spinning solution was prepared into MXene-enhanced heterocyclic aramid fiber using microfluid spinning technology. The elongation at break of the MXene-enhanced heterocyclic aramid fiber of Example 2 is about 4.1%, and the breaking strength is about 4.8 GPa. The mass of lithium chloride is 4.5 g, and the amount of N, N-dimethylacetamide added is 100 mL.

[0029] Example 3

[0030] The preparation method of MXene-reinforced heterocyclic aramid fiber of Example 3 comprises the following steps: 0.0785 g of Ti3C2T x The nanosheets were dispersed in a mixture of lithium chloride and N, N-dimethylacetamide under stirring, and solution 1 was obtained by continuous stirring for 30 min. Solution 1 was transferred to a reactor, and 0.532 g of p-phenylenediamine and 2.346 g of 5-amino-2-(4-aminophenyl)-benzimidazole were added while stirring for 1 h. The reaction temperature was lowered to 5 ° C and stabilized for 30 min. 3.03 g of terephthaloyl chloride was added while stirring, and continuous stirring was performed for 1 h to obtain a spinning solution. The fluid viscosity of the spinning solution was 64018 mPa s, and the spinning solution was prepared into MXene-enhanced heterocyclic aramid fiber using microfluid spinning technology. The elongation at break of the MXene-enhanced heterocyclic aramid fiber of Example 3 is about 5.2%, and the breaking strength is about 6 GPa. The mass of lithium chloride is 4.5 g, and the amount of N, N-dimethylacetamide added is 100 mL.

[0031] Example 4

[0032] The preparation method of MXene-reinforced heterocyclic aramid fiber of Example 4 comprises the following steps: 0.1047 g of Ti3C2T xThe nanosheets were dispersed in a mixture of lithium chloride and N, N-dimethylacetamide under stirring, and solution 1 was obtained by continuous stirring for 30 minutes. Solution 1 was transferred to a reactor, and 0.532 g of p-phenylenediamine and 2.346 g of 5-amino-2-(4-aminophenyl)-benzimidazole were added while stirring for 1 hour. The reaction temperature was lowered to 5 ° C and stabilized for 30 minutes. 3.03 g of terephthaloyl chloride was added while stirring, and the spinning solution was obtained by continuous stirring for 1 hour. The fluid viscosity of the spinning solution was 49584 mPa s, and the spinning solution was prepared into MXene-enhanced heterocyclic aramid fiber using microfluid spinning technology. The elongation at break of the MXene-enhanced heterocyclic aramid fiber of Example 4 is about 4.6%, and the breaking strength is about 5.3 GPa. The mass of lithium chloride is 4.5 g, and the amount of N, N-dimethylacetamide added is 100 mL.

[0033] Example 5

[0034] The preparation method of MXene-reinforced heterocyclic aramid fiber of Example 5 comprises the following steps: 0.0785 g of V4C3T x The nanosheets were dispersed in a mixture of lithium chloride and N, N-dimethylacetamide under stirring, and solution 1 was obtained by continuous stirring for 30 minutes. Solution 1 was transferred to a reactor, and 0.532 g of p-phenylenediamine and 2.346 g of 5-amino-2-(4-aminophenyl)-benzimidazole were added while stirring for 1 hour. The reaction temperature was lowered to 5 ° C and stabilized for 30 minutes. 3.03 g of terephthaloyl chloride was added while stirring, and the spinning solution was obtained by continuous stirring for 1 hour. The fluid viscosity of the spinning solution was 64018 mPa s, and the spinning solution was prepared into MXene-enhanced heterocyclic aramid fiber using microfluid spinning technology. The elongation at break of the MXene-enhanced heterocyclic aramid fiber of Example 5 is about 5.2%, and the breaking strength is about 6 GPa. The mass of lithium chloride is 4.5 g, and the amount of N, N-dimethylacetamide added is 100 mL.

Claims

1. A method for preparing MXene-reinforced heterocyclic aramid fibers, It is characterized in that The method comprises the following steps: dissolving MXene nanosheets in a solvent to obtain a solution one, adding p-phenylenediamine and 5-amino-2-(4-aminophenyl)-benzimidazole to the solution one, reacting at low temperature, adding terephthaloyl chloride under stirring to obtain a spinning solution, and using a spinning technology to prepare the spinning solution into MXene-reinforced heterocyclic aramid fibers.

2. The method for preparing the MXene-reinforced heterocyclic aramid fiber according to claim 1, It is characterized in that The MXene nanosheets are Ti 3 SiC 2 、Ti 3 C 2 T x 、V 4 C 3 T x 、 4 C 3 T x One or more of the following; the addition amount of the MXene nanosheet is 0.01 to 1 g.

3. The method for preparing MXene-reinforced heterocyclic aramid fiber according to claim 1, It is characterized in that The MXene nanosheets are dissolved in the solvent and stirred for 10 to 60 minutes to obtain solution one, and the p-phenylenediamine and 5-amino-2-(4-aminophenyl)-benzimidazole are added to the solution one under stirring and stirred for 0.5 to 2 hours, the temperature is lowered to 0 to 10° C. and reacted for 10 to 30 minutes, and the terephthaloyl chloride is added under stirring and reacted for 0.5 to 2 hours to obtain the spinning solution.

4. The method for preparing MXene-reinforced heterocyclic aramid fiber according to claim 1, It is characterized in that The added amount of the p-phenylenediamine is 0.1 to 1 g; the added amount of the 5-amino-2-(4-aminophenyl)-benzimidazole is 1 to 5 g; and the added amount of the terephthaloyl chloride is 1 to 5 g.

5. The method for preparing MXene-reinforced heterocyclic aramid fiber according to claim 1, It is characterized in that The solvent is one or more of N,N-dimethylformamide, N,N-dimethylacetamide, N-methylpyrrolidone, and dimethyl sulfoxide; The amount of the solvent added is 50 to 150 mL.

6. The method for preparing MXene-reinforced heterocyclic aramid fiber according to claim 1, It is characterized in that Lithium chloride is added to the solvent, and the added amount of the lithium chloride is 1 to 5 g.

7. The method for preparing MXene-reinforced heterocyclic aramid fiber according to claim 1, It is characterized in that The fluid viscosity of the spinning solution is 10000-100000 mPa·s.

8. The method for preparing MXene-reinforced heterocyclic aramid fiber according to claim 1, It is characterized in that The spinning technology is microfluid spinning technology.

9. A MXene-reinforced heterocyclic aramid fiber, It is characterized in that The MXene-reinforced heterocyclic aramid fiber is prepared by the preparation method of claim 1.