Antistatic DTY stretch yarn and preparation method thereof
By introducing macromolecular antistatic agents into DTY wires, the conductive paths are formed using compounds such as allyl chloride, N,N-dimethylethanolamine and 1-vinyl imidazole, which solves the electrostatic problem of DTY wires and improves the antistatic properties and mechanical properties avoid the migration and consumption of traditional antistatic agents.
Patent Information
- Application Number
- CN202411271760.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-11
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
DTY wire materials are prone to static electricity when rubbing, leading to problems such as broken heads and adhesion of flying flowers. In addition, traditional antistatic agents have a long migration time and are easily consumed, so they cannot maintain antistatic properties for a long time.
Polyamide fiber, polyolefin fiber and polypropylene fiber are used as matrix, and allyl chloride is introduced and N,N-dimethylethanolamine is reacted to form a quaternary ammonium intermediate, followed by reaction of 1-vinyl imidazole with chloro-n-butane. Carbon-carbon double bond ionic liquid is formed, copolymerized by maleic anhydride, and finally esterified with the polymer to form a macromolecular antistatic agent, forming a conductive path to improve antistatic properties.
It significantly improves the antistatic properties of DTY elastic wire, solves the problems of migration and consumption of small molecule antistatic agents, and is better compatible with the matrix, maintaining excellent mechanical properties and antistatic effects.
Smart Images

Figure BDA0005038920490000021 
Figure BDA0005038920490000022 
Figure BDA0005038920490000031
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of DTY materials, and in particular to an antistatic DTY elastic yarn and a preparation method thereof. Background Art
[0002] DTY yarn is also called stretched textured yarn. It is the finished yarn that is continuously or simultaneously stretched on a texturing machine and deformed by a twister. Usually, the raw material of DTY yarn is nylon or polyester and other artificial fibers. DTY yarn is an ideal material for various knitting or weaving processes.
[0003] At present, due to the high insulation resistance of artificial fiber materials such as nylon and polyester, the DTY silk materials prepared from these fiber materials are prone to generate static electricity during friction. This part of static electricity is very easy to leak, causing problems such as broken ends and flying flower adhesion during the silk processing process, greatly reducing the yield rate. Moreover, people will have physical problems if they are in a static environment for a long time. The concentrated discharge of static electricity can also cause dangers such as combustion and explosion. Therefore, antistatic materials are usually added to the raw materials of the silk thread, or antistatic oil is added to the silk thread during the processing of the silk thread, so as to improve the antistatic performance of the silk thread. The antistatic principle of traditional antistatic agents is: due to the low relative molecular mass of traditional antistatic agents, surface treatment or addition to silk thread raw materials will cause the antistatic agents to continuously migrate out from the inside during the use of the silk thread, and absorb moisture in the air through the hydrophilic groups at the ends of the antistatic agents to channel static electricity, thereby reducing the surface resistance. Therefore, a certain migration time is required to play an antistatic role, and with the wiping or washing process during use, the antistatic agent on the surface gradually disappears, and the internal antistatic agent molecules continue to migrate until they are completely consumed, so small molecule antistatic agents are more restricted. Summary of the invention
[0004] In order to solve the above technical problems, the present invention provides an antistatic DTY elastic yarn and a preparation method thereof.
[0005] The purpose of the present invention can be achieved through the following technical solutions:
[0006] An antistatic DTY elastic yarn comprises the following raw materials in parts by weight: 55-65 parts of polyamide fiber, 30-50 parts of polyolefin fiber, 60-80 parts of polypropylene fiber, 10-15 parts of elastomer, 1-1.5 parts of antioxidant, 1-2 parts of antistatic agent, 1-2 parts of dispersant, and 1-2 parts of matting agent;
[0007] The antistatic agent is prepared by the following steps:
[0008] Step S1, adding allyl chloride to acetone, heating to 35-40°C, adding N,N-dimethylethanolamine, stirring at a uniform speed and reacting for 24 hours, washing with acetone three times after the reaction, and vacuum drying at 45°C for 12 hours to obtain intermediate 1, wherein the dosage ratio of allyl chloride, N,N-dimethylethanolamine and acetone is controlled to be 0.1-0.2 mol: 0.1-0.2 mol: 50 mL;
[0009] In step S1, allyl chloride and N,N-dimethylethanolamine undergo quaternization reaction to prepare intermediate 1, which is a quaternary ammonium salt that can form a conductive path, play the role of an antistatic agent, and improve the antistatic performance of the substrate. The reaction process is as follows:
[0010]
[0011] Step S2, adding 1-vinylimidazole to n-butyl chloride, heating to 70° C., stirring at a uniform speed and reacting for 32 hours, washing with ethyl acetate three times after the reaction, and then rotary distilling at 80° C. for 10 hours to obtain intermediate 2, wherein the molar ratio of 1-vinylimidazole to n-butyl chloride in step S2 is controlled to be 1:1;
[0012] In step S2, 1-vinylimidazole and n-butyl chloride react to prepare intermediate 2, which is an ionic liquid containing a carbon-carbon double bond. The reaction process is as follows:
[0013]
[0014] Step S3, adding intermediate 2 and maleic anhydride into deionized water, introducing nitrogen to expel air, stirring at a uniform speed and heating to 65°C, adjusting pH to 6.5, continuing to heat to 85°C, slowly dropping a 15% by mass aqueous solution of ammonium persulfate, keeping the temperature for reaction for 6-8h, and obtaining a polymer, wherein the molar ratio of intermediate 2 to maleic anhydride is controlled to be 1-1.2:1, and the amount of ammonium persulfate used is 1-1.5% of the total weight of intermediate 2 and maleic anhydride;
[0015] In step S3, under the condition of ammonium persulfate as an initiator, the carbon-carbon double bond on the intermediate 2 and maleic anhydride are copolymerized to prepare a polymer. The reaction process is as follows:
[0016]
[0017] Step S4, adding the polymer and intermediate 1 to N, N-dimethylformamide, adding p-toluenesulfonic acid hydrate, heating to 65-80°C, stirring at a uniform speed and reacting for 54 hours to obtain an antistatic agent, controlling the amount ratio of the polymer, intermediate 1 and N, N-dimethylformamide to be 10-12g: 0.3-0.5g: 80-100mL, and the amount of p-toluenesulfonic acid hydrate to be 5-8% of the weight of the polymer.
[0018] In step S4, p-toluenesulfonic acid hydrate is used as a catalyst, and the carboxyl group on the polymer undergoes an esterification reaction with the hydroxyl group on the intermediate 1, and then the intermediate 1 is grafted onto the side chain of the polymer to prepare a macromolecular polymer antistatic agent. The antistatic agent has a polymer long chain as the main chain, and quaternary ammonium salts and ionic liquids are grafted onto the side chains respectively, so that the quaternary ammonium salt cations and the ionic liquids cooperate to form a conductive path, thereby improving the antistatic performance of the matrix, and the antistatic agent exists in the form of a polymer macromolecular structure, which can solve the disadvantages of small molecule antistatic agents. In addition, the antistatic agent prepared by the present invention has a polyolefin as the main chain, and can be better compatible with the matrix polypropylene and polyolefin when melt extruded.
[0019] Furthermore, the elastomer is a mixture of ethylene-vinyl acetate copolymer and isobutylene-4-methylstyrene copolymer in a weight ratio of 1:1.
[0020] Furthermore, the antioxidant is antioxidant 168 or antioxidant 1010, the dispersant is polyvinyl alcohol, and the matting agent is nano titanium dioxide.
[0021] A method for preparing an antistatic DTY elastic yarn comprises the following steps:
[0022] The first step is to mix the raw materials evenly to obtain a mixed material, and then send it into a twin-screw extruder to perform melt treatment at 240°C, 210°C, 250°C and 220°C, and then send it into a spinning box and extrude it from the fine holes of the spinneret, and obtain thick filaments after cooling;
[0023] In the second step, the obtained thick wire is oiled by an oiling roller and then wound on a bobbin, and then passed through a 50°C hot roller and wound on a wire drum to obtain an antistatic DTY elastic wire.
[0024] Beneficial effects of the present invention:
[0025] The present invention prepares an antistatic DTY elastic yarn, which uses polyamide fiber, polyolefin fiber and polypropylene fiber as a matrix, introduces an elastomer to impart excellent mechanical properties, and adds a synthetic antistatic agent to impart excellent antistatic properties to the elastic yarn. In the preparation process, the antistatic agent first undergoes a quaternization reaction with allyl chloride and N,N-dimethylethanolamine to prepare an intermediate 1, which is a quaternary ammonium salt that can form a conductive path and exert the effect of an antistatic agent. Then, 1-vinylimidazole and n-butyl chloride are reacted to prepare an intermediate 2, which is an ionic liquid containing a carbon-carbon double bond. The carbon-carbon double bond on the intermediate 2 is subsequently reacted with malachite. The method comprises the following steps: copolymerizing anhydride with an acid anhydride to prepare a polymer, and finally the carboxyl group on the polymer undergoes an esterification reaction with the hydroxyl group on the intermediate 1, and then grafting the intermediate 1 onto the side chain of the polymer to prepare a macromolecular polymer antistatic agent. The antistatic agent has a polymer long chain as the main chain, and quaternary ammonium salt and ionic liquid are grafted onto the side chain respectively, so that the quaternary ammonium salt cation and the ionic liquid cooperate to form a conductive path, thereby improving the antistatic performance of the matrix, and exists in the form of a polymer macromolecular structure, which can solve the disadvantages of small molecule antistatic agents. In addition, the antistatic agent prepared by the present invention has a polyolefin as the main chain, and can be better compatible with the matrix polypropylene and polyolefin when melt extruded. DETAILED DESCRIPTION
[0026] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0027] Embodiment 1: An antistatic DTY elastic yarn comprises the following raw materials in parts by weight: 55 parts of polyamide fiber, 30 parts of polyolefin fiber, 60 parts of polypropylene fiber, 10 parts of elastomer, 1 part of antioxidant, 1 part of antistatic agent, 1 part of dispersant, and 1 part of matting agent;
[0028] Antistatic DTY elastic yarn is made by the following method:
[0029] The first step is to mix the raw materials evenly to obtain a mixed material, and then send it into a twin-screw extruder to perform melt treatment at 240°C, 210°C, 250°C and 220°C, and then send it into a spinning box and extrude it from the fine holes of the spinneret, and obtain thick filaments after cooling;
[0030] In the second step, the obtained thick wire is oiled by an oiling roller and then wound on a bobbin, and then passed through a 50°C hot roller and wound on a wire drum to obtain an antistatic DTY elastic wire.
[0031] The antistatic agent is prepared by the following steps:
[0032] Step S1, adding allyl chloride to acetone, heating to 35°C, adding N,N-dimethylethanolamine, stirring at a uniform speed and reacting for 24 hours, washing with acetone three times after the reaction, and vacuum drying at 45°C for 12 hours to obtain intermediate 1, wherein the dosage ratio of allyl chloride, N,N-dimethylethanolamine and acetone is controlled to be 0.1 mol:0.1 mol:50 mL;
[0033] Step S2, adding 1-vinylimidazole to n-butyl chloride, heating to 70° C., stirring at a uniform speed and reacting for 32 hours, washing with ethyl acetate three times after the reaction, and then rotary distilling at 80° C. for 10 hours to obtain intermediate 2, wherein the molar ratio of 1-vinylimidazole to n-butyl chloride in step S2 is controlled to be 1:1;
[0034] Step S3, adding intermediate 2 and maleic anhydride into deionized water, introducing nitrogen to expel air, stirring at a uniform speed and heating to 65°C, adjusting pH to 6.5, continuing to heat to 85°C, slowly dropping a 15% by mass aqueous solution of ammonium persulfate, keeping the temperature for reaction for 6-8h, to obtain a polymer, wherein the molar ratio of intermediate 2 to maleic anhydride is controlled to be 1:1, and the amount of ammonium persulfate used is 1% of the total weight of intermediate 2 and maleic anhydride;
[0035] Step S4, adding the polymer and intermediate 1 to N, N-dimethylformamide, adding p-toluenesulfonic acid hydrate, heating to 65°C, stirring at a uniform speed and reacting for 54 hours to obtain an antistatic agent, controlling the amount ratio of the polymer, intermediate 1 and N, N-dimethylformamide to be 10g:0.3g:80mL, and the amount of p-toluenesulfonic acid hydrate to be 5% of the weight of the polymer.
[0036] The elastomer is prepared by mixing ethylene-vinyl acetate copolymer and isobutylene-4-methylstyrene copolymer in a weight ratio of 1:1.
[0037] The antioxidant is antioxidant 168, the dispersant is polyvinyl alcohol, and the matting agent is nano titanium dioxide.
[0038] Embodiment 2: An antistatic DTY elastic yarn comprises the following raw materials in parts by weight: 60 parts of polyamide fiber, 40 parts of polyolefin fiber, 70 parts of polypropylene fiber, 12 parts of elastomer, 1.2 parts of antioxidant, 1.5 parts of antistatic agent, 1.5 parts of dispersant, and 1.5 parts of matting agent;
[0039] Antistatic DTY elastic yarn is made by the following method:
[0040] The first step is to mix the raw materials evenly to obtain a mixed material, and then send it into a twin-screw extruder to perform melt treatment at 240°C, 210°C, 250°C and 220°C, and then send it into a spinning box and extrude it from the fine holes of the spinneret, and obtain thick filaments after cooling;
[0041] In the second step, the obtained thick wire is oiled by an oiling roller and then wound on a bobbin, and then passed through a 50°C hot roller and wound on a wire drum to obtain an antistatic DTY elastic wire.
[0042] The antistatic agent is prepared by the following steps:
[0043] Step S1, adding allyl chloride to acetone, heating to 38°C, adding N,N-dimethylethanolamine, stirring at a uniform speed and reacting for 24 hours, washing with acetone three times after the reaction, and vacuum drying at 45°C for 12 hours to obtain intermediate 1, wherein the dosage ratio of allyl chloride, N,N-dimethylethanolamine and acetone is controlled to be 0.15 mol:0.15 mol:50 mL;
[0044] Step S2, adding 1-vinylimidazole to n-butyl chloride, heating to 70° C., stirring at a uniform speed and reacting for 32 hours, washing with ethyl acetate three times after the reaction, and then rotary distilling at 80° C. for 10 hours to obtain intermediate 2, wherein the molar ratio of 1-vinylimidazole to n-butyl chloride in step S2 is controlled to be 1:1;
[0045] Step S3, adding intermediate 2 and maleic anhydride into deionized water, introducing nitrogen to expel air, stirring at a uniform speed and heating to 65°C, adjusting pH to 6.5, continuing to heat to 85°C, slowly dropping a 15% by mass aqueous solution of ammonium persulfate, keeping the temperature for reaction for 7 hours, and obtaining a polymer, wherein the molar ratio of intermediate 2 to maleic anhydride is controlled to be 1.1:1, and the amount of ammonium persulfate used is 1.2% of the total weight of intermediate 2 and maleic anhydride;
[0046] Step S4, adding the polymer and intermediate 1 to N, N-dimethylformamide, adding p-toluenesulfonic acid hydrate, heating to 65-80°C, stirring at a uniform speed and reacting for 54 hours to obtain an antistatic agent, controlling the amount ratio of the polymer, intermediate 1 and N, N-dimethylformamide to be 12g:0.4g:90mL, and the amount of p-toluenesulfonic acid hydrate to be 6% of the weight of the polymer.
[0047] The elastomer is prepared by mixing ethylene-vinyl acetate copolymer and isobutylene-4-methylstyrene copolymer in a weight ratio of 1:1.
[0048] The antioxidant is antioxidant 1010, the dispersant is polyvinyl alcohol, and the matting agent is nano titanium dioxide.
[0049] Example 3: An antistatic DTY elastic yarn comprises the following raw materials in parts by weight: 65 parts of polyamide fiber, 50 parts of polyolefin fiber, 80 parts of polypropylene fiber, 15 parts of elastomer, 1.5 parts of antioxidant, 2 parts of antistatic agent, 2 parts of dispersant, and 2 parts of matting agent;
[0050] Antistatic DTY elastic yarn is made by the following method:
[0051] The first step is to mix the raw materials evenly to obtain a mixed material, and then send it into a twin-screw extruder to perform melt treatment at 240°C, 210°C, 250°C and 220°C, and then send it into a spinning box and extrude it from the fine holes of the spinneret, and obtain thick filaments after cooling;
[0052] In the second step, the obtained thick wire is oiled by an oiling roller and then wound on a bobbin, and then passed through a 50°C hot roller and wound on a wire drum to obtain an antistatic DTY elastic wire.
[0053] The antistatic agent is prepared by the following steps:
[0054] Step S1, adding allyl chloride to acetone, heating to 40°C, adding N,N-dimethylethanolamine, stirring at a uniform speed and reacting for 24 hours, washing with acetone three times after the reaction, and vacuum drying at 45°C for 12 hours to obtain intermediate 1, wherein the dosage ratio of allyl chloride, N,N-dimethylethanolamine and acetone is controlled to be 0.2 mol:0.2 mol:50 mL;
[0055] Step S2, adding 1-vinylimidazole to n-butyl chloride, heating to 70° C., stirring at a uniform speed and reacting for 32 hours, washing with ethyl acetate three times after the reaction, and then rotary distilling at 80° C. for 10 hours to obtain intermediate 2, wherein the molar ratio of 1-vinylimidazole to n-butyl chloride in step S2 is controlled to be 1:1;
[0056] Step S3, adding intermediate 2 and maleic anhydride into deionized water, introducing nitrogen to expel air, stirring at a uniform speed and heating to 65°C, adjusting pH to 6.5, continuing to heat to 85°C, slowly dropping a 15% by mass aqueous solution of ammonium persulfate, keeping the temperature for reaction for 6-8h, and obtaining a polymer, wherein the molar ratio of intermediate 2 to maleic anhydride is controlled to be 1.2:1, and the amount of ammonium persulfate used is 1.5% of the total weight of intermediate 2 and maleic anhydride;
[0057] Step S4, adding the polymer and intermediate 1 to N, N-dimethylformamide, adding p-toluenesulfonic acid hydrate, heating to 80°C, stirring at a uniform speed and reacting for 54 hours to obtain an antistatic agent, controlling the amount ratio of the polymer, intermediate 1 and N, N-dimethylformamide to be 12g:0.5g:100mL, and the amount of p-toluenesulfonic acid hydrate to be 8% of the weight of the polymer.
[0058] The elastomer is prepared by mixing ethylene-vinyl acetate copolymer and isobutylene-4-methylstyrene copolymer in a weight ratio of 1:1.
[0059] The antioxidant is antioxidant 168, the dispersant is polyvinyl alcohol, and the matting agent is nano titanium dioxide.
[0060] Comparative Example 1: Compared with Example 1, this comparative example uses the intermediate 1 prepared in step S1 as an antistatic agent, and the rest is the same as Example 1.
[0061] Comparative Example 2: Compared with Example 1i, this comparative example uses the intermediate 2 prepared in step S2 as an antistatic agent, and the rest is the same as Example 2.
[0062] The properties of the DTY elastic yarns prepared in Examples 1 to 3 and Comparative Examples 1 to 2 were tested, and the results are shown in Table 1 below:
[0063] Crimping shrinkage performance test: The crimping shrinkage rate and crimping stability rate of high elastic DTY are tested according to the test method in GB6506-86 "Test method for crimping performance of synthetic fiber textured yarn".
[0064] Antistatic performance: The DTY elastic yarn prepared in Example 1-Example 3 and Comparative Example 1-Comparative Example 2 was first rinsed with deionized water for 300 times, each rinsing time was 5 minutes, and then dried in an oven at a temperature of 50°C for 0.5h and dried for use. Then it was measured according to FZ / T50035-2016 "Test Method for Resistance of Synthetic Fiber Filaments". Take a 100mm long fiber, stick conductive glue on both ends of the fiber, and use EST121 digital ultra-high resistance micro-current meter to test the resistance value of the fiber with a spacing of 100mm. The test voltage is (100±5)V, and the average value is taken after 5 measurements to calculate the surface resistance of the fiber.
[0065] Table 1
[0066]
[0067] It can be seen from Table 1 above that the DTY elastic yarns prepared in Examples 1 to 3 of the present invention have better curl shrinkage and curl stability, and still maintain excellent antistatic properties after 300 rinses.
[0068] The above contents are merely examples and explanations of the concept of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the concept of the invention or exceed the scope defined by the claims, they should all fall within the protection scope of the present invention.
Claims
1. An antistatic DTY elastic yarn, It is characterized in that The invention comprises the following raw materials in parts by weight: 55-65 parts of polyamide fiber, 30-50 parts of polyolefin fiber, 60-80 parts of polypropylene fiber, 10-15 parts of elastomer, 1-2 parts of antistatic agent, 1-1.5 parts of antioxidant, 1-2 parts of dispersant, and 1-2 parts of matting agent; The antistatic agent is prepared by the following steps: Step S1, adding allyl chloride to acetone, heating to 35-40°C, adding N,N-dimethylethanolamine, stirring at a uniform speed and reacting for 24 hours, washing with acetone three times after the reaction, and vacuum drying at 45°C for 12 hours to obtain intermediate 1; Step S2, adding 1-vinylimidazole to n-butyl chloride, heating to 70° C., stirring at a constant speed and reacting for 32 hours, washing with ethyl acetate three times after the reaction, and then rotary distilling at 80° C. for 10 hours to obtain intermediate 2; Step S3, adding intermediate 2 and maleic anhydride into deionized water, introducing nitrogen to expel air, stirring at a uniform speed and heating to 65° C., adjusting pH to 6.5, continuing to heat to 85° C., slowly dropping a 15% by mass aqueous solution of ammonium persulfate, and keeping the temperature for reaction for 6-8 hours to obtain a polymer; Step S4, adding the polymer and intermediate 1 into N,N-dimethylformamide, adding p-toluenesulfonic acid hydrate, raising the temperature to 65-80° C., stirring at a constant speed and reacting for 54 hours to obtain an antistatic agent.
2. The antistatic DTY elastic yarn according to claim 1, It is characterized in that The elastomer is prepared by mixing ethylene-vinyl acetate copolymer and isobutylene-4-methylstyrene copolymer in a weight ratio of 1:
1.
3. The antistatic DTY elastic yarn according to claim 1, It is characterized in that The antioxidant is antioxidant 168 or antioxidant 1010, the dispersant is polyvinyl alcohol, and the matting agent is nano titanium dioxide.
4. The antistatic DTY elastic yarn according to claim 1, It is characterized in that In step S1, the dosage ratio of allyl chloride, N,N-dimethylethanolamine and acetone is controlled to be 0.1-0.2 mol: 0.1-0.2 mol: 50 mL.
5. The antistatic DTY elastic yarn according to claim 1, It is characterized in that In step S2, the molar ratio of 1-vinylimidazole to n-butyl chloride is controlled to be 1:
1.
6. The antistatic DTY elastic yarn according to claim 1, It is characterized in that In step S3, the molar ratio of the intermediate 2 to maleic anhydride is controlled to be 1-1.2:1, and the amount of ammonium persulfate used is 1-1.5% of the total weight of the intermediate 2 and maleic anhydride.
7. The antistatic DTY elastic yarn according to claim 1, It is characterized in that In step S4, the dosage ratio of the polymer, intermediate 1 and N,N-dimethylformamide is controlled to be 10-12 g: 0.3-0.5 g: 80-100 mL, and the dosage of p-toluenesulfonic acid hydrate is 5-8% of the weight of the polymer.
8. The method for preparing an antistatic DTY elastic yarn according to claim 1, It is characterized in that The steps include: The first step is to mix the raw materials evenly to obtain a mixed material, and then send it into a twin-screw extruder to perform melt treatment at 240°C, 210°C, 250°C and 220°C, and then send it into a spinning box and extrude it from the fine holes of the spinneret, and obtain thick filaments after cooling; In the second step, the obtained thick wire is oiled by an oiling roller and then wound on a bobbin, and then passed through a 50°C hot roller and wound on a wire drum to obtain an antistatic DTY elastic wire.
Citation Information
Patent Citations
Polypropylene fiber and production process thereof
CN113026137A
Antistatic DTY and preparation process thereof
CN113529202A
Cited By
Antistatic polyester fiber and preparation method thereof
CN120666462A