Preparation method of active chitosan quaternary ammonium salt modified cellulose fabric based on dispersion system

By using a dispersion system on textiles, the grafting of chitosan quaternary ammonium salt and nitrogen-containing heterocyclic monomers is solved, the problem of insufficient covalent bonding method is improved, the antibacterial performance and dyeing effect of cellulose fabrics are achieved, and the Efficient staining and long-lasting antibacterial properties.

CN118932713AActive Publication Date: 2024-11-12QINGDAO UNIV +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410957937.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-11-12
Estimated Expiration
2044-07-17

AI Technical Summary

Technical Problem

The lack of effective covalent bonding methods in the prior art limits the application of HTCC in textiles.

Method used

Using a dispersion system-based method, through homogeneous reaction and homogeneous dispersion, the grafting of chitosan quaternary ammonium salt and nitrogen-containing heterocyclic monomer is achieved, the active site is improved, and the chitosan quaternary ammonium salt and cellulose fabric are promoted. The covalent grafting of the cellulose fabric imparts a long-lasting antibacterial function, and reduces the amount of neutral salt during the dyeing process, thereby increasing the dyeing depth.

Benefits of technology

Effective covalent grafting of chitosan quaternary ammonium salt and cellulose fabrics is achieved, which significantly improves antibacterial performance, reduces the amount of dyeing neutral salts, increases the dyeing depth, and maintains a high-efficiency antibacterial rate after multiple washes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118932713A_ABST
    Figure CN118932713A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of active chitosan quaternary ammonium salt modified cellulose fabric based on a dispersion system, and belongs to the field of textile chemistry. Effective grafting of the chitosan quaternary ammonium salt and the nitrogen-containing heterocyclic ring monomer is realized by utilizing a dispersion system, and active sites on the chitosan quaternary ammonium salt are improved, so that the covalent grafting effect of the active chitosan quaternary ammonium salt and the cellulose fabric is improved, the cellulose fabric is endowed with a lasting antibacterial function, the dyeing performance of the cellulose fabric in natural dye and reactive dye is improved, and the antibacterial property of the cellulose fabric is improved. Moreover, when the cellulose fabric prepared by the method is dyed by using an active dye, the dosage of neutral salt can be reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a preparation method of active chitosan quaternary ammonium salt modified cellulose fabric based on a dispersion system, and belongs to the field of textile chemistry. Background Art

[0002] Cellulose fiber is a fiber with cellulose polysaccharide as the main component. According to different sources and processing methods, it can be divided into cotton, linen, lyocell, bamboo fiber, etc., which occupies a large share of my country's textile raw materials. Cellulose fiber textiles have the advantages of good moisture absorption and permeability, comfortable wearing, soft touch, etc., and are deeply loved by consumers. Chitosan is a natural cationic polysaccharide derived from chitin, which is abundant in nature. Its structure is similar to that of cellulose and has good biocompatibility and biodegradability.

[0003] Chitosan is used for the functional finishing of textiles, which can not only give textiles certain antibacterial properties, but also improve the dyeing quality of textiles, effectively increase the added value of textiles, and meet people's demand for high-quality textiles. Chitosan is difficult to dissolve in water and organic solvents due to its large molecular weight and easy to form strong hydrogen bonds within and between molecules, which greatly limits the application of chitosan. Quaternization of chitosan can effectively improve the solubility of chitosan and expand the application range of chitosan. N-(2-hydroxy-3-trimethyl)propyl ammonium chloride chitosan (HTCC) is a commonly used soluble chitosan quaternary ammonium salt. HTCC exhibits similar biological properties to chitosan, such as biodegradability, biocompatibility and antibacterial properties. In addition to these common properties, HTCC also exhibits better water solubility, wettability, mucosal adsorption and good positive charge, and can be used as an ideal functional modification material for cellulose textiles. However, there is currently a lack of effective covalent bonding methods for the functional finishing of HTCC for textiles, which limits the application of HTCC in textiles. Summary of the invention

[0004] [Technical issues]

[0005] In the prior art, there is a lack of effective covalent bonding methods for using HTCC for functional finishing of textiles, which limits the application of HTCC on textiles.

[0006] [Technical solution]

[0007] In order to solve the above problems, the present invention aims to provide a preparation method of chitosan quaternary ammonium salt modified cellulose fabric based on a dispersion system, which utilizes the dispersion system to achieve effective grafting of chitosan quaternary ammonium salt and nitrogen-containing heterocyclic monomers, thereby increasing the active sites on the chitosan quaternary ammonium salt, thereby improving the covalent grafting effect of the active chitosan quaternary ammonium salt and the cellulose fabric, and giving the cellulose fabric a lasting antibacterial function. At the same time, when the cellulose fabric prepared by the method is dyed with a reactive dye, the amount of neutral salt used can be reduced, thereby increasing the dyeing depth.

[0008] The first object of the present invention is to provide a method for preparing an active chitosan quaternary ammonium salt modified cellulose fabric based on a dispersion system, comprising the following steps:

[0009] S1. Synthesis of chitosan quaternary ammonium salt: dissolving chitosan and glycidyltrimethylammonium chloride in an ionic liquid to prepare chitosan quaternary ammonium salt by homogeneous reaction;

[0010] S2, preparation of active chitosan quaternary ammonium salt solution: homogeneously dispersing the nitrogen-containing heterocyclic monomer and the dispersant, mixing with the chitosan quaternary ammonium salt prepared in step S1 after dispersion, and then adding an acid binding agent, reacting to obtain an active chitosan quaternary ammonium salt solution;

[0011] S3. Preparation of active chitosan quaternary ammonium salt modified cellulose fabric: the active chitosan quaternary ammonium salt solution prepared in step S2, cellulose fabric and sodium carbonate are mixed in deionized water, shaken, and active chitosan quaternary ammonium salt modified cellulose fabric is prepared by nucleophilic reaction.

[0012] In one embodiment of the present invention, in step S1, the ionic liquid is 1-allyl-3-methylimidazolium chloride [AMIm]Cl ionic liquid.

[0013] In one embodiment of the present invention, in step S1, the molecular weight of the chitosan quaternary ammonium salt is 3000-5000.

[0014] In one embodiment of the present invention, in step S1, the reaction temperature is 70-90°C, more preferably 80°C.

[0015] In one embodiment of the present invention, in step S1, the reaction time is 7-9 hours, more preferably 8 hours.

[0016] In one embodiment of the present invention, in step S1, the mass ratio of chitosan, ionic liquid and glycidyltrimethylammonium chloride is 1:(40-60):(2-3), and more preferably 1:50:2.3.

[0017] In one embodiment of the present invention, in step S2, the dispersant is one or a combination of octadecyltrimethylammonium chloride and N-dodecyl-2-pyrrolidone.

[0018] In one embodiment of the present invention, in step S2, the nitrogen-containing heterocyclic monomer is one or more of cyanuric chloride, 2,4-dichloro-1,3,5-triazine, 3,4,6-trichloropyridazine, 2-amino-4,6-dichloro-1,3,5-triazine, and phosphazene.

[0019] In one embodiment of the present invention, in step S2, the temperature of homogenous dispersion is 0-5°C, more preferably 0°C.

[0020] In one embodiment of the present invention, in step S2, the homogenization dispersion time is 5-10 minutes, more preferably 10 minutes.

[0021] In one embodiment of the present invention, in step S2, the rotation speed of homogenous dispersion is 1000-5000 rpm, more preferably 3000 rpm.

[0022] In one embodiment of the present invention, in step S2, the mass ratio of chitosan quaternary ammonium salt, nitrogen-containing heterocyclic monomer and dispersant is 4:(7.5-17.35):(2-3), and more preferably 4:9:2.7.

[0023] In one embodiment of the present invention, in step S2, the acid binding agent is a 0.1-0.2 g / mL sodium carbonate solution, more preferably a 0.106 g / mL sodium carbonate solution.

[0024] In one embodiment of the present invention, in step S2, the volume mass ratio of the added amount of the acid binding agent to the chitosan quaternary ammonium salt is (20-25):1, mL / g, and more preferably 25:1, mL / g.

[0025] In one embodiment of the present invention, in step S2, the reaction temperature is 0-5°C, more preferably 0°C.

[0026] In one embodiment of the present invention, in step S2, the reaction time is 1-3 hours, more preferably 3 hours.

[0027] In one embodiment of the present invention, in step S3, the cellulose fabric is one of cotton fabric, viscose fabric and lyocell fabric.

[0028] In one embodiment of the present invention, in step S3, the bath ratio of the nucleophilic reaction is 1:(20-30), and more preferably 1:25.

[0029] In one embodiment of the present invention, in step S3, the temperature of the nucleophilic reaction is 30-50°C, more preferably 50°C.

[0030] In one embodiment of the present invention, in step S3, the time of the nucleophilic reaction is 2-4 hours, more preferably 4 hours.

[0031] In one embodiment of the present invention, in step S3, the volume mass ratio of the active chitosan quaternary ammonium salt solution to the cellulose fabric is (4-6):1, mL / g, and more preferably 5:1, mL / g.

[0032] In one embodiment of the present invention, in step S3, the mass ratio of sodium carbonate to cellulose fabric is 1:(3-5), more preferably 1:4.

[0033] The second object of the present invention is to provide an active chitosan quaternary ammonium salt modified cellulose fabric prepared by the above method.

[0034] The third object of the present invention is to provide the application of the above-mentioned active chitosan quaternary ammonium salt modified cellulose fabric in the field of functional textiles and textile dyeing.

[0035] [Beneficial Effects]

[0036] (1) The present invention can achieve effective covalent grafting of chitosan quaternary ammonium salt and cellulose fabric through a dispersed system.

[0037] (2) The chitosan quaternary ammonium salt modified cellulose fabric prepared by the present invention can effectively reduce the amount of neutral salt used in dyeing cellulose fabric with reactive dyes, while improving the dyeing depth.

[0038] (3) The active chitosan modified cotton prepared by the present invention has significantly improved antibacterial properties against Escherichia coli and Staphylococcus aureus compared to raw cotton. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] Figure 1 Images of raw cotton and activated chitosan-modified cotton;

[0040] Figure 2 SEM images of raw cotton and active chitosan-modified cotton;

[0041] Figure 3 Example 1-7 Active chitosan-modified cellulose fabric treated E. coli and S. aureus agar plate images. DETAILED DESCRIPTION

[0042] The present invention is further described below in conjunction with specific examples. The examples are only used to explain the present invention and are not used to limit the scope of the present invention.

[0043] The performance tests involved in the present invention are as follows:

[0044] ① Grafting rate test: Based on the mass change of cotton after drying before and after modification, the grafting rate calculation formula is calculated by the following equation;

[0045]

[0046] Where: m 1 —Mass of fabric sample before grafting; m 2 —Quality of fabric samples after grafting.

[0047] ② Natural / reactive dyeing test: Fold the dyed fabric twice to ensure that the color of the fabric test site is uniform and opaque. Use a Datacolor spectrophotometer (D65 light source, 10° field of view) with a large aperture (30mm) to measure the K / S value of cellulose fabric. Randomly change the measurement position of each sample for multiple measurements and calculate the average value.

[0048] ③ Antibacterial performance test: The antibacterial effect of the modified cotton was evaluated using the improved AATCC-100 method. The inoculated Staphylococcus aureus and Escherichia coli were transferred to a constant temperature shaker at 37°C and 130r for 18-24h, and the bacterial solution was diluted to 3×10 with 0.03mol / L phosphate (PBS) buffer. 5 -4×10 5 CFU / mL. Take 0.15g of grafted cellulose fabric sample, sterilize it by UV irradiation for 30min, add it to a conical flask, add 100uL of diluted bacterial solution and culture it at 24℃ and 150r with shaking for 18-24h. Dilute the shaken bacterial solution by ten-fold dilution method, take 100uL of bacterial solution for each dilution gradient and spread it on the agar plate, spread two plates in parallel for each dilution gradient, and count the colonies on the plate after culturing at 37℃ for 24h. The sample without grafted cellulose fabric is used as the control group. The antibacterial rate calculation formula is calculated by the following equation;

[0049]

[0050] Where: E anti —Antibacterial rate of grafted cellulose fabric; Nc—the number of colonies in the control group; Ne—the number of colonies in the grafted cellulose fabric.

[0051] ④ Washing resistance test: refer to GB / T20944.3-2008, weigh 1g of modified cellulose fabric, the following procedure is equivalent to 5 washes: water temperature 40℃, bath ratio 1:50, detergent concentration 0.2%, 10 steel balls, wash for 45min. Take out the sample after washing, wash it twice in 40℃ and 50mL water, 1min each time. Repeat this procedure until the specified number of washes and then dry. Test the antibacterial performance of antibacterial cellulose fabric after washing.

[0052] Example 1

[0053] A method for effectively grafting cellulose fabric with chitosan quaternary ammonium salt based on a dispersed system:

[0054] S1. Synthesis of chitosan quaternary ammonium salt (HTCC)

[0055] 0.2g chitosan (CS) and 10g 1-allyl-3-methylimidazolium chloride [AMIm]Cl ionic liquid were added to a three-necked flask and heated in an oil bath at 80°C with stirring until the chitosan was completely dissolved. Then 0.46g glycidyl trimethylammonium chloride was added to the flask and stirred at 80°C for 8h. Then, a mixed solution of ethanol / acetone was added to the flask to precipitate HTCC. After the mixed solution was filtered to obtain the HTCC filter cake, it was washed 3 times with a mixed solution of ethanol / acetone to remove the residual [AMIm]Cl ionic liquid and glycidyl trimethylammonium chloride. Finally, the HTCC was dried in an oven at 70°C for 12h.

[0056] S2. Preparation of active chitosan quaternary ammonium salt solution

[0057] Place 0.4g HTCC in a flask, add 20mL deionized water and stir at 0℃ until completely dissolved. Take 10mL deionized water in a beaker and cool it to 0℃, then add 0.9g cyanuric chloride and 0.27g octadecyltrimethylammonium chloride, homogenize and disperse at 3000rpm for 10min, and add to the flask after dispersion. Take 1.06g sodium carbonate and dissolve it in 10mL deionized water, drip it into the flask at a rate of 10mL / h through a syringe pump, and react at 0℃ for 3h to obtain an active chitosan quaternary ammonium salt solution.

[0058] S3. Preparation of Cellulose Fabric Modified by Active Chitosan Quaternary Ammonium Salt

[0059] Weigh 2g cotton cloth, add 0.25g sodium carbonate, 40mL deionized water, and 10mL active chitosan quaternary ammonium salt solution into a conical flask, and the bath ratio of the reaction is 1:25. Place the conical flask in an oscillating water bath at 50℃ for 4h, take out the active chitosan quaternary ammonium salt modified cellulose fabric, wash it with water, and place it in an oven to dry.

[0060] Example 2

[0061] The 0.27 g of octadecyltrimethylammonium chloride in step S2 of Example 1 was adjusted to 0.135 g of octadecyltrimethylammonium chloride and 0.135 g of N-dodecyl-2-pyrrolidone, and the other conditions were the same as in Example 1.

[0062] Example 3

[0063] The 0.27 g of octadecyltrimethylammonium chloride in step S2 of Example 1 was adjusted to 0.27 g of N-dodecyl-2-pyrrolidone, and the other conditions were the same as those of Example 1.

[0064] Embodiment 4:

[0065] The 0.9 g of cyanuric chloride in step S2 of Example 1 was adjusted to 0.75 g of 2,4-dichloro-1,3,5-triazine, and the other conditions were the same as those of Example 1.

[0066] Example 5

[0067] The 0.9 g of cyanuric chloride in step S2 of Example 1 was adjusted to 0.9 g of 3,4,6-trichloropyridazine, and the other conditions were the same as those in Example 1.

[0068] Example 6

[0069] The cotton fabric in step S3 of Example 1 was changed to viscose fabric, and the other conditions were the same as those of Example 1.

[0070] Example 7

[0071] The cotton fabric in step S3 of Example 1 was changed to lyocell fabric, and the other conditions were the same as those of Example 1.

[0072] The grafting rate of the active chitosan quaternary ammonium salt modified cellulose fabric prepared in Examples 1-7 was tested. The grafting rate is shown in Table 1. The grafting rate of the active chitosan quaternary ammonium salt modified cellulose fabric can reach up to 3.69%.

[0073] Table 1 Grafting rate of modified cellulose fabric

[0074] Example 1 2 3 4 5 6 7 Grafting rate / % 3.69 3.55 3.28 2.98 2.88 3.04 3.47

[0075] The active chitosan quaternary ammonium salt modified cellulose fabrics prepared in Examples 1-7 were dyed with the natural dye sophora beige, and the K / S values ​​are shown in Table 2. The K / S of the active chitosan quaternary ammonium salt modified cellulose fabrics with the natural dye sophora beige can reach up to 9.47.

[0076] Table 2 K / S values ​​of modified cellulose fabrics dyed with natural dyes

[0077] Example 1 2 3 4 5 6 7 K / S value 9.47 8.91 8.55 8.07 7.89 8.88 9.15

[0078] The reactive chitosan quaternary ammonium salt modified cellulose fabrics prepared in Examples 1-7 were dyed with reactive dyes for low salt, and the K / S values ​​were shown in Table 3. The K / S of the reactive chitosan quaternary ammonium salt modified cellulose fabrics for low salt dyeing with reactive dyes can be as high as 19.86.

[0079] Table 3 K / S values ​​of reactive dyes with low salt dyeing of modified cellulose fabrics

[0080] Comparative Example 1 2 3 4 5 6 7 K / S value 19.86 18.11 17.72 16.65 16.33 18.69 18.91

[0081] The active chitosan quaternary ammonium salt modified cellulose fabrics prepared in Examples 1-7 were subjected to 5, 10, 15, 20, 25, and 30 washing cycles of soap washing (5 soap washings per cycle), and then the antibacterial performance test was performed. The relationship between the antibacterial rate against Escherichia coli and Staphylococcus aureus and the number of washing cycles is shown in Tables 4 and 5. The antibacterial rate of the active chitosan quaternary ammonium salt modified cellulose fabric against Escherichia coli and Staphylococcus aureus remained above 99% after 30 washing cycles.

[0082] Table 4 Relationship between the antibacterial rate of modified cellulose fabrics against Escherichia coli and the number of washing cycles

[0083]

[0084] Table 5 Relationship between the antibacterial rate of modified cellulose fabrics against Staphylococcus aureus and the number of washing cycles

[0085]

[0086]

[0087] Comparative Example 1

[0088] The 1-allyl-3-methylimidazolium chloride [AMIm]Cl ionic liquid in step S1 of Example 2 was adjusted to isopropanol, and the other conditions were consistent with those of Example 2.

[0089] Comparative Example 2

[0090] The step of adding a dispersant for homogeneous dispersion in step S2 of Example 2 is removed, and the other conditions are consistent with Example 2.

[0091] Comparative Example 3

[0092] The 0.135 g of octadecyltrimethylammonium chloride and 0.135 g of N-dodecyl-2-pyrrolidone in step S2 of Example 2 were adjusted to 0.37 g of sodium dodecyl sulfate, and the other conditions were the same as those in Example 2.

[0093] It can be seen from the following Tables 6-10 that after the dispersant in Example 2 was replaced with the conventional dispersant sodium dodecyl sulfate, the grafting rate, K / S value and antibacterial effect of the modified cellulose fabric were significantly reduced.

[0094] Comparative Example 4

[0095] The homogenization dispersion time in step S2 of Example 2 was adjusted from 10 min to 5 min, and the other conditions were consistent with Example 2.

[0096] Comparative Example 5

[0097] The acid binding agent sodium carbonate in step S2 of Example 2 is adjusted to sodium hydroxide, and the other conditions are consistent with Example 2.

[0098] Comparative Example 6

[0099] The reaction time of 3 h in step S2 of Example 2 was adjusted to 1 h, and the other conditions were consistent with those of Example 2.

[0100] Comparative Example 7

[0101] The bath ratio of the cellulose fabric to the modified solution in step S3 of Example 2 was adjusted from 1:25 to 1:50, and the other conditions were the same as those in Example 2.

[0102] Comparative Example 8

[0103] The reaction temperature in step S3 of Example 2 was adjusted from 50°C to 40°C, and the other conditions were the same as those of Example 2.

[0104] Comparative Example 9

[0105] The reaction temperature in step S3 of Example 2 was adjusted from 4h to 3h, and the other conditions were the same as those in Example 2.

[0106] The grafting rate of the active chitosan quaternary ammonium salt modified cellulose fabrics prepared in Comparative Examples 1-9 was tested, and the grafting rate was shown in Table 6. Compared with the examples, the grafting rate was only 1% to 2%.

[0107] Table 6 Grafting rate of modified cellulose fabric

[0108] Comparative Example 1 2 3 4 5 6 7 8 9 Grafting rate / % 1.85 1.39 1.45 1.81 1.52 1.49 1.75 1.59 1.68

[0109] The active chitosan quaternary ammonium salt modified cellulose fabrics prepared in Comparative Examples 1-9 were dyed with the natural dye Sophora japonica yellow. The K / S values ​​are shown in Table 7, which are lower than those in Example 7. The highest K / S of the active chitosan quaternary ammonium salt modified cellulose fabrics with the natural dye Sophora japonica yellow is only 6.43.

[0110] Table 7 K / S values ​​of natural dyes on modified cellulose fabrics

[0111] Comparative Example 1 2 3 4 5 6 7 8 9 K / S value 6.43 3.54 3.88 5.99 4.12 3.87 5.35 4.98 4.57

[0112] The active chitosan quaternary ammonium salt modified cellulose fabrics prepared in Comparative Examples 1-9 were dyed with reactive dyes for low salt. The K / S values ​​are shown in Table 8, which are lower than those in Example 8. The highest K / S value of the active chitosan quaternary ammonium salt modified cellulose fabrics for low salt dyeing with reactive dyes is only 13.45.

[0113] Table 8 K / S value of reactive dyes dyeing modified cellulose fabrics with low salt

[0114] Comparative Example 1 2 3 4 5 6 7 8 9 K / S value 13.45 7.37 7.98 12.68 8.19 8.74 11.92 9.75 10.77

[0115] The active chitosan quaternary ammonium salt modified cellulose fabric prepared in Comparative Examples 1-9 was subjected to soaping for 5, 10, 15, 20, 25, and 30 washing cycles (5 soaping cycles per cycle), and then the antibacterial performance test was performed. The relationship between the antibacterial rate of Escherichia coli and Staphylococcus aureus and the number of washing cycles was shown in Table 9 and Table 10. Compared with the embodiment, the antibacterial rate of the active chitosan quaternary ammonium salt modified cellulose fabric to Escherichia coli and Staphylococcus aureus decreased significantly, with the highest being only 94.5% and 90.5%. After 30 washing cycles, the antibacterial rate was reduced to 89.5% and 75.8%.

[0116] Table 9 Relationship between the antibacterial rate of modified cellulose fabrics against Escherichia coli and the number of washing cycles

[0117]

[0118] Table 10 Relationship between the antibacterial rate of modified cellulose fabrics against Staphylococcus aureus and the number of washing cycles

[0119]

[0120]

[0121] The embodiments provided above are not intended to limit the scope of the present invention, and the steps described are not intended to limit the execution order thereof. Those skilled in the art may make obvious improvements to the present invention in combination with existing common knowledge, which also fall within the scope of protection defined by the claims of the present invention.

Claims

1. A method for preparing active chitosan quaternary ammonium salt modified cellulose fabric based on a dispersion system, characterized in that: The following steps are involved: S1. Synthesis of chitosan quaternary ammonium salt: dissolving chitosan and glycidyltrimethylammonium chloride in an ionic liquid to prepare chitosan quaternary ammonium salt by homogeneous reaction; S2, preparation of active chitosan quaternary ammonium salt solution: homogeneously dispersing the nitrogen-containing heterocyclic monomer and the dispersant in water, mixing with the chitosan quaternary ammonium salt prepared in step S1 after dispersion, and then adding an acid binding agent, reacting to obtain an active chitosan quaternary ammonium salt solution; S3. Preparation of active chitosan quaternary ammonium salt modified cellulose fabric: the active chitosan quaternary ammonium salt solution prepared in step S2, cellulose fabric and sodium carbonate are mixed in deionized water, shaken, and active chitosan quaternary ammonium salt modified cellulose fabric is prepared by nucleophilic reaction.

2. The method according to claim 1, characterized in that In step S1, the ionic liquid is 1-allyl-3-methylimidazolium chloride [AMIm]Cl ionic liquid, and the molecular weight of the chitosan quaternary ammonium salt is 3000-5000.

3. The method according to claim 1, characterized in that In step S1, the reaction temperature is 70-90°C, the reaction time is 7-9h, and the mass ratio of chitosan, ionic liquid and glycidyltrimethylammonium chloride is 1:(40-60):(2-3).

4. The method according to claim 1, characterized in that In step S2, the dispersant is one or a combination of octadecyltrimethylammonium chloride and N-dodecyl-2-pyrrolidone.

5. The method according to claim 1, characterized in that: In step S2, the nitrogen-containing heterocyclic monomer is one or more of cyanuric chloride, 2,4-dichloro-1,3,5-triazine, 3,4,6-trichloropyridazine, and 2-amino-4,6-dichloro-1,3,5-triazine.

6. The method according to claim 1, characterized in that In step S2, the temperature of the homogeneous dispersion is 0-5°C, the time of the homogeneous dispersion is 5-10min, the speed of the homogeneous dispersion is 1000-5000rpm, the mass ratio of chitosan quaternary ammonium salt, nitrogen-containing heterocyclic monomer and dispersant is 4:(7.5-17.35):(2-3); the acid binding agent is 0.1-0.2g / mL of sodium carbonate solution, the volume mass ratio of the added amount of the acid binding agent to the chitosan quaternary ammonium salt is (20-25):1, mL / g, the reaction temperature is 0-5°C, and the reaction time is 1-3h.

7. The method according to claim 1, characterized in that In step S3, the cellulose fabric is one of cotton fabric, viscose fabric and lyocell fabric.

8. The method according to claim 1, characterized in that In step S3, the bath ratio of the nucleophilic reaction is 1:(20-30), the reaction temperature is 30-50°C, the reaction time is 2-4h, the volume mass ratio of the active chitosan quaternary ammonium salt solution to the cellulose fabric is (4-6):1, mL / g, and the mass ratio of sodium carbonate to the cellulose fabric is 1:(3-5).

9. The active chitosan quaternary ammonium salt modified cellulose fabric prepared according to the method described in any one of claims 1 to 8.

10. Use of the active chitosan quaternary ammonium salt modified cellulose fabric according to claim 9 in the field of functional textiles and textile dyeing.

Citation Information

Patent Citations

  • Reactive chitosan quaternary ammonium salt, and preparation method and application thereof

    CN106188340A

  • Preparation method of reaction type chitosan-based fabric antibacterial agent

    CN111041829A

  • Preparation method of guanidyl chitosan quaternary ammonium salt antibacterial agent

    CN111057164A

  • Ionic cross-linking of ionic cotton with small molecular weight anionic or cationic molecules

    US20050241073A1

  • Chitosan as an intumescing, thermoformable flame retardant

    US20210095102A1