Modified carbon fiber material as well as preparation method and application thereof
By adding antioxidant coatings and pyrolytic carbon coatings to carbon fiber materials, the oxidation problem of traditional thermal insulation materials is solved, extending service life and reducing maintenance costs, and achieving more efficient production.
Patent Information
- Application Number
- CN202411222552.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-02
- Publication Date
- 2024-11-12
AI Technical Summary
The thermal insulation materials in traditional continuous high-temperature carbonization furnaces cause structural damage due to oxidation, which affects service life and increases maintenance costs.
Modified carbon fiber materials composed of carbon fiber layer, antioxidant coating and pyrolytic carbon coating are used to reduce oxygen content and porosity through replacement treatment and pyrolytic carbon treatment, and improve oxidation resistance.
It significantly improves the antioxidant performance of modified carbon fiber materials, extends service life, reduces maintenance costs, and improves production efficiency.
Smart Images

Figure CN118932714A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a modified carbon fiber material and a preparation method and application thereof. Background Art
[0002] When the continuous high-temperature carbonization furnace is working, there will be trace oxygen in the furnace. The trace oxygen mainly comes from two aspects. On the one hand, because the insulation material is a porous material, some air will remain inside; on the other hand, a small amount of air will be mixed into the furnace when the continuous high-temperature carbonization furnace is working. If the oxygen in these two parts of air is not handled properly, it will seriously affect the service life of the carbon fiber insulation material.
[0003] At present, the thermal insulation material in the traditional continuous high-temperature carbonization furnace is mainly carbon fiber thermal insulation material with graphite sheets bonded to its surface. The bonded graphite sheets can effectively isolate the thermal insulation material from contact with oxygen molecules, and the graphite sheets can act as a reflective screen to improve the thermal insulation performance. However, after 1-2 years, due to the continuous presence of oxygen molecules in the continuous carbonization furnace, the thermal insulation material is oxidized, the internal structure is damaged, and the graphite sheets are peeled off. If the peeled graphite sheets touch the graphite heater, the heater will ignite and then cause a short circuit, which seriously affects the use efficiency of the carbonization furnace and increases the maintenance cost. Summary of the invention
[0004] In order to solve the defect of poor oxidation resistance of thermal insulation materials in the prior art, the present invention provides a modified carbon fiber material and a preparation method and application thereof. The modified carbon fiber material has excellent oxidation resistance.
[0005] The present invention solves the above technical problems through the following technical solutions.
[0006] The invention provides a modified carbon fiber material, which comprises a carbon fiber layer, an anti-oxidation coating and a pyrolytic carbon coating in order from the inside to the outside; the oxygen content of the modified carbon fiber material is less than 100 ppm; and the porosity of the modified carbon fiber material is 0-10%.
[0007] In the present invention, the oxygen content of the modified carbon fiber material is preferably less than 70 ppm, for example, 65 ppm or 67 ppm.
[0008] In the present invention, the porosity of the modified carbon fiber material is preferably 0-5%, for example 4.3%.
[0009] In the present invention, the density of the modified carbon fiber material is preferably 0.13-0.18 g / cm 3 , for example 0.166 g / cm 3 or 0.168 g / cm 3 .
[0010] In the present invention, the carbon content of the modified carbon fiber material is preferably greater than 99%, for example, 99.4%, 99.5% or 99.6%. The carbon content refers to the mass content of carbon in the modified carbon fiber material.
[0011] In the present invention, preferably, the compression strength of the modified carbon fiber material in the thickness direction is ≥0.43 MPa, more preferably ≥0.45 MPa.
[0012] In the present invention, preferably, the bending strength of the modified carbon fiber material is ≥1.15 MPa, more preferably ≥1.46 MPa.
[0013] In the present invention, preferably, the thickness of the pyrolytic carbon coating is 10-100 μm, for example, 17.7 μm or 29.5 μm.
[0014] In the present invention, preferably, the oxidation loss of the modified carbon fiber material is less than 20%, more preferably less than 18%, for example, 12.3% or 17.5%. The test method of oxidation loss is, for example, placing the modified carbon fiber material in a muffle furnace and passing air, keeping the temperature at 620°C for 24 hours, and measuring the mass of the modified carbon fiber material before and after high temperature treatment. The calculation formula of oxidation loss is: oxidation loss = (mass of modified carbon fiber material before high temperature treatment - mass of modified carbon fiber material after high temperature treatment) / mass of modified carbon fiber material before high temperature treatment * 100%.
[0015] The present invention also provides a method for preparing a modified carbon fiber material, which comprises the following steps:
[0016] The modified carbon fiber material is obtained by subjecting the carbon fiber substrate to an anti-oxidation treatment and a pyrolysis carbon treatment in sequence; the oxygen content of the carbon fiber substrate is less than 100 ppm.
[0017] The present invention adopts a carbon fiber substrate with an internal oxygen content of less than 100 ppm, and then sequentially undergoes an anti-oxidation treatment and a pyrolysis carbon treatment to improve the density of the surface layer of the modified carbon fiber material, thereby improving the air isolation and anti-oxidation effects.
[0018] The oxygen content in the present invention means the content of oxygen remaining inside the modified carbon fiber material, and the test method thereof can be as follows: in a temperature range of -40 to 120°C and a humidity range of 0-100%RH, the modified carbon fiber material is placed in the closed device, and vacuum is evacuated and inert gas is introduced to displace the oxygen inside the modified carbon fiber material, so that the gas in the closed device is discharged from the gas outlet, and when the vacuum degree is 0.06MPa, the oxygen concentration at the gas outlet is measured, and the oxygen concentration is defined as the oxygen content in the modified carbon fiber material. The inert gas can be nitrogen, and the flow rate when introduced can be 1-10L / min.
[0019] In the present invention, preferably, the method for preparing the carbon fiber substrate comprises: subjecting the carbon fiber precursor to a replacement treatment.
[0020] The substitution treatment means that the oxygen inside the material can be discharged through the treatment.
[0021] The replacement treatment step includes, for example: placing the carbon fiber precursor in a replacement device, and simultaneously evacuating the replacement device and introducing an inert gas.
[0022] The vacuum pressure is preferably 0.01-0.1 MPa, for example 0.05 MPa.
[0023] Wherein, the inert gas is preferably nitrogen and / or argon.
[0024] The purity of the nitrogen is, for example, 99.99%.
[0025] The purity of the argon gas is, for example, 99.99%.
[0026] The temperature of the replacement treatment is room temperature, which is 20-40°C.
[0027] The present invention does not impose any particular limitation on the time of the replacement treatment, as long as the oxygen content in the replaced gas is less than 100 ppm after the replacement treatment, wherein the oxygen content in the replaced gas is the oxygen content of the carbon fiber substrate.
[0028] In the present invention, the oxygen content of the carbon fiber substrate is preferably less than 70 ppm, for example, 65 ppm or 67 ppm.
[0029] In the present invention, the method for preparing the carbon fiber precursor may include the following steps:
[0030] The mixture is sequentially subjected to curing treatment and graphitization treatment to obtain a carbon fiber precursor; the mixture comprises phenolic resin and carbon fiber.
[0031] The carbon fiber is, for example, carbon fiber soft felt, and the carbon fiber soft felt is, for example, one or more of asphalt-based carbon fiber soft felt, PAN (polyacrylonitrile)-based carbon fiber soft felt and viscose-based carbon fiber soft felt.
[0032] Wherein, the preparation method of the mixture is preferably: impregnating the carbon fiber in the phenolic resin.
[0033] The device used for the curing process may be conventional in the art, such as a hot press.
[0034] The pressure of the curing treatment is preferably 4-15 MPa, for example, 10 MPa.
[0035] The curing temperature is preferably 130-220°C, for example 200°C.
[0036] The curing time can be determined according to actual production requirements, and the curing time is preferably 2-15 hours, for example, 10 hours.
[0037] The temperature of the graphitization treatment is preferably 2200-2400°C, for example 2300°C.
[0038] The graphitization treatment time is preferably 50-150 hours, for example 100 hours.
[0039] Among them, in the preparation process of the carbon fiber precursor, further graphitization treatment is carried out after the curing treatment. On the one hand, it can make the volatile gas in the material evaporate out of the material and reduce the impurity content in the material. On the other hand, it can make the lattice of the carbon fiber precursor more complete, which is beneficial to improve the bonding strength between the carbon fiber precursor and the materials used in the subsequent antioxidant treatment and pyrolytic carbon treatment, and further improve the antioxidant capacity of the modified carbon fiber material.
[0040] Among them, those skilled in the art generally understand that the graphitization treatment generally also includes a mechanical processing step for adjusting the size of the carbon fiber precursor.
[0041] In the present invention, the anti-oxidation treatment means that the material can be isolated from the external oxygen environment through the treatment, thereby improving the anti-oxidation performance.
[0042] In the present invention, the step of the anti-oxidation treatment is, for example, to coat an antioxidant on the surface of the carbon fiber substrate and then perform a heat treatment.
[0043] Wherein, the antioxidant preferably comprises a resin, and the resin is preferably one or more of a vinyl resin, an epoxy resin and a phenolic resin.
[0044] The mass percentage of the resin to the antioxidant is preferably 10%-50%, for example 25%.
[0045] Wherein, the antioxidant preferably also includes carbon black, a surfactant and a solvent.
[0046] The solvent is, for example, ethanol.
[0047] The mass percentage of the carbon black to the antioxidant is preferably 5%-15%, for example 10%.
[0048] Wherein, the average particle size of the carbon black is preferably 60-200 mesh.
[0049] The mass percentage of the surfactant to the antioxidant is preferably 0.1%-0.5%, for example 0.2%.
[0050] Wherein, the type of the surfactant is preferably alcohol compound and / or alcohol ether compound.
[0051] Wherein, the alcohol compound is preferably polyethylene glycol and / or polypropylene glycol.
[0052] The alcohol ether compound is preferably a glycol ether compound, such as propylene glycol ether and / or diethylene glycol ether. The alcohol ether compound means a compound having both an ether bond and a hydroxyl group, and the glycol ether compound means an alcohol ether compound containing two hydroxyl groups in the molecular formula.
[0053] In certain specific embodiments of the present invention, the propylene glycol ether is propylene glycol propyl ether.
[0054] Wherein, the heat treatment preferably includes a first heat treatment and a second heat treatment in sequence, the temperature of the first heat treatment is 100-300°C, and the temperature of the second heat treatment is 2000-2400°C.
[0055] The temperature of the first heat treatment is, for example, 200°C.
[0056] Wherein, the temperature of the second heat treatment is preferably 2200-2400°C.
[0057] Wherein, the time of the first heat treatment is preferably 5-8 hours.
[0058] The second heat treatment time is preferably 50-150 hours, for example 70 hours or 100 hours.
[0059] Wherein, the number of times of the anti-oxidation treatment is preferably twice.
[0060] The temperature and time of the first heat treatment in the two anti-oxidation treatments may be the same or different.
[0061] The temperature and time of the second heat treatment in the two anti-oxidation treatments may be the same or different.
[0062] In certain specific embodiments of the present invention, the step of anti-oxidation treatment comprises:
[0063] S1: coating an antioxidant on the surface of the carbon fiber substrate, performing a first heat treatment and a second heat treatment in sequence, and then cooling to room temperature to obtain a product;
[0064] S2: coating the surface of the product with an antioxidant, performing a first heat treatment and a second heat treatment in sequence, and then cooling the product to room temperature.
[0065] In the present invention, pyrolytic carbon treatment means that the pores on the surface and inside of the material can be sealed by heating.
[0066] In the present invention, preferably, the raw material for the pyrolysis carbon treatment also includes a carbon source gas.
[0067] The carbon source gas refers to an organic gas containing carbon, and the carbon source gas is preferably one or more of methane, ethane and propylene.
[0068] In the present invention, the temperature of the pyrolytic carbon treatment is preferably 1000-1800°C, for example 1200°C.
[0069] In the present invention, the pyrolytic carbon treatment time is preferably 20-30 hours, for example 24 hours.
[0070] In the present invention, the pressure of the pyrolytic carbon treatment is preferably below 10 kPa, for example, 8 kPa.
[0071] In the present invention, preferably, the pyrolytic carbon treatment is performed using, for example, a chemical vapor deposition furnace (CVD furnace).
[0072] The present invention also provides a modified carbon fiber material prepared by the preparation method of the modified carbon fiber material.
[0073] The present invention also provides an application of the carbon fiber material in thermal insulation materials.
[0074] On the basis of being in accordance with the common sense in the art, the above-mentioned preferred conditions can be arbitrarily combined to obtain the preferred embodiments of the present invention.
[0075] The reagents and raw materials used in the present invention are commercially available.
[0076] The positive and progressive effects of the present invention are:
[0077] The modified carbon fiber material of the present invention has low oxygen content and low porosity of the modified carbon fiber material, and its oxidation loss is low, indicating that it has excellent anti-oxidation performance, can overcome the problem of peeling of the anti-oxidation coating and the pyrolytic carbon coating, and the damage of the internal structure, can improve the service life of the modified carbon fiber material, and can also improve the production efficiency of the modified carbon fiber material and reduce the maintenance cost. At the same time, the modified carbon fiber material of the present invention also has excellent compressive strength and bending strength. BRIEF DESCRIPTION OF THE DRAWINGS
[0078] Figure 1 This is a scanning electron microscope image of the carbon fiber layer of the modified carbon fiber material of Example 1.
[0079] Figure 2 This is a scanning electron microscope image of the anti-oxidation coating of the modified carbon fiber material of Example 1.
[0080] Figure 3 This is a scanning electron microscope image of the pyrolytic carbon coating of the modified carbon fiber material of Example 1.
[0081] Figure 4 This is a schematic diagram of the structure of the modified carbon fiber material prepared in Example 1.
[0082] The reference numerals are as follows:
[0083] 1-carbon fiber layer; 2-anti-oxidation coating; 3-pyrolytic carbon coating. DETAILED DESCRIPTION
[0084] The present invention is further described below by way of examples, but the present invention is not limited to the scope of the examples. The experimental methods in the following examples without specifying specific conditions are carried out according to conventional methods and conditions, or selected according to the product specifications.
[0085] The raw materials used in the following examples are: asphalt-based carbon fiber soft felt purchased from Tianjin Yufeng Carbon Co., Ltd., model number is YFC-137, its carbon content is ≥99.5wt%, width is 600mm, length is 11.5m, initial thickness is 15mm, surface density is 800g / m 2 Phenolic resin was purchased from Jinan Shengquan Group Co., Ltd., model PF9701-1, and the type was aminophenol-formaldehyde resin; carbon black was purchased from Qingdao Risheng Graphite Co., Ltd., and its average particle size was 60-200 mesh; propylene glycol propyl ether was purchased from Guangdong Wengjiang Chemical Reagent Co., Ltd., model 1569-01-3.
[0086] Example 1
[0087] The modified carbon fiber material is prepared by the following steps:
[0088] S1: The asphalt-based carbon fiber soft felt impregnated in phenolic resin is successively subjected to curing treatment, graphitization treatment and mechanical processing to obtain a carbon fiber precursor; the curing treatment is carried out in a hot press, the curing treatment temperature is 200°C, the curing treatment pressure is 10MPa, and the curing treatment time is 10h; the graphitization treatment temperature is 2300°C, and the graphitization treatment time is 100h.
[0089] S2: The above-mentioned carbon fiber precursor is placed in a replacement device for replacement treatment, and the replacement device is evacuated and nitrogen with a purity of 99.99% is introduced at room temperature to obtain a carbon fiber substrate; wherein, the vacuum pressure is 0.05MPa, and after the replacement treatment, the oxygen content in the replaced gas is 65ppm, which is the oxygen content of the carbon fiber substrate.
[0090] S3: subjecting the carbon fiber substrate to an anti-oxidation treatment and a pyrolysis carbon treatment in sequence to obtain a modified carbon fiber material;
[0091] Among them, the number of antioxidant treatments is 2 times, and the specific steps are: after the antioxidant is coated on the surface of the carbon fiber substrate, a first heat treatment at a temperature of 200°C and a time of 8 hours and a second heat treatment at a temperature of 2000°C and a time of 70 hours are sequentially performed, and the product is cooled to room temperature after the second heat treatment; after the antioxidant is coated on the surface of the product, a first heat treatment at a temperature of 200°C and a time of 8 hours and a second heat treatment at a temperature of 2000°C and a time of 70 hours are sequentially performed, and the product is cooled to room temperature after the second heat treatment; the antioxidant is composed of 25% by mass of vinyl resin, 10% by mass of carbon black, 0.2% by mass of propylene glycol propyl ether and the balance of ethanol.
[0092] Among them, the steps of pyrolytic carbon treatment are: pyrolysis treatment of the mixture of the material after antioxidant treatment and methane in a CVD furnace; the temperature of the pyrolytic carbon treatment is 1200°C, the time of the pyrolytic carbon treatment is 24h, and the pressure of the pyrolytic carbon treatment is 8kPa.
[0093] The prepared modified carbon fiber material includes a carbon fiber layer 1, an anti-oxidation coating 2 and a pyrolytic carbon coating 3 from the inside to the outside, and the specific structure is as follows: Figure 4 As shown; the scanning electron microscope image of the carbon fiber layer is as follows Figure 1 The scanning electron microscopy image of the anti-oxidation coating is shown in Figure 2 The SEM images of the pyrolytic carbon coating are shown in Figure 3 shown.
[0094] Example 2
[0095] The oxygen content of the carbon fiber substrate in step S2 is 67 ppm, the temperature of the pyrolysis carbon treatment in step S3 is 1000° C., and the remaining steps are the same as in Example 1.
[0096] Comparative Example 1
[0097] Without performing the replacement treatment of step S2, the carbon fiber precursor obtained in step S1 is directly used as a carbon fiber substrate with an oxygen content of 640 ppm, and then treated according to step S3 of Example 1.
[0098] Comparative Example 2
[0099] The oxygen content of the carbon fiber substrate in step S2 is 84 ppm, no pyrolysis carbon treatment is performed in step S3, and the remaining steps are the same as in Example 1.
[0100] Effect Example 1
[0101] The modified carbon fiber materials prepared in Examples 1 and 2 and Comparative Examples 1 and 2 were tested as follows:
[0102] 1. Carbon content test: Determine according to standard GBT 31292-2014.
[0103] 2. Compression strength: measured in accordance with standard GB / T1431-2019.
[0104] 3. Bending strength: measured in accordance with standard JB / T 8133.7-2013.
[0105] 4. Thickness test of pyrolytic carbon coating: The cross section is taken to characterize each layer structure by electron microscopy. The model of scanning electron microscope is Thermo Fisher ApreoC. The thickness of pyrolytic carbon coating is obtained according to the cross-section scanning electron microscope image.
[0106] 5. Test of oxygen content in modified carbon fiber materials: The test equipment is a closed device and an oxygen detector. The model of the oxygen detector is MOT500-O2-M. The specific test steps are: in the temperature range of -40 to 120 ° C and the humidity range of 0-100% RH, place the modified carbon fiber material in the closed device, and simultaneously evacuate and introduce high-purity nitrogen at a flow rate of 1-10L / min to replace the oxygen inside the modified carbon fiber material, and evacuate the device so that the air in the closed device is discharged from the gas outlet. When the vacuum degree is 0.06MPa, measure the oxygen concentration at the gas outlet, and define the oxygen concentration as the oxygen content in the modified carbon fiber material.
[0107] 6. Oxidation reduction test: Place the modified carbon fiber material with a mass of m1 in a muffle furnace, and introduce nitrogen into the muffle furnace. After the temperature of the muffle furnace rises to 620°C, stop passing nitrogen and start introducing compressed air. After the muffle furnace is kept at a constant temperature of 620°C for 24 hours, it starts to cool down and stop passing compressed air and start introducing nitrogen. After the muffle furnace cools down to 25°C, take out the modified carbon fiber material with a mass of m2. Oxidation reduction = (m1-m2) / m1*100%. Oxidation reduction can reflect the antioxidant performance of the material. The lower the oxidation reduction, the better the antioxidant performance of the material.
[0108] 7. Porosity test: The porosity of the modified carbon fiber material is tested by mercury injection method.
[0109] 8. Density test: Determine according to standard GBT24528-2009.
[0110] The test results of the above tests are listed in Table 1 below:
[0111] Table 1
[0112]
[0113] It can be seen from the above table that the oxygen content of the modified carbon fiber materials of Example 1 and Example 2 is less than 100 ppm, the porosity of the modified carbon fiber materials is less than 10%, and the oxidation loss of the modified carbon fiber materials is less than 18%, indicating that they have excellent antioxidant properties.
[0114] Comparative Example 1 does not undergo replacement treatment, and Comparative Example 2 does not undergo pyrolytic carbon treatment, resulting in oxidation reductions of the modified carbon fiber materials of Comparative Example 1 and Comparative Example 2 exceeding 18%, and having poor antioxidant properties.
Claims
1. A modified carbon fiber material, characterized in that: It comprises a carbon fiber layer, an anti-oxidation coating and a pyrolytic carbon coating in order from the inside to the outside; the oxygen content of the modified carbon fiber material is less than 100 ppm; and the porosity of the modified carbon fiber material is 0-10%.
2. The modified carbon fiber material according to claim 1, characterized in that: The oxygen content of the modified carbon fiber material is less than 70 ppm, for example, 65 ppm or 67 ppm; And / or, the porosity of the modified carbon fiber material is 0-5%, for example, 4.3%; And / or, the density of the modified carbon fiber material is 0.13-0.18 g / cm 3 , for example 0.166 g / cm 3 or 0.168 g / cm 3 ; And / or, the carbon content of the modified carbon fiber material is greater than 99%, for example, 99.4%, 99.5% or 99.6%; And / or, the compression strength of the modified carbon fiber material in the thickness direction is ≥0.43 MPa, preferably ≥0.45 MPa; And / or, the bending strength of the modified carbon fiber material is ≥1.15 MPa, preferably ≥1.46 MPa; And / or, the thickness of the pyrolytic carbon coating is 10-100 μm, for example, 17.7 μm or 29.5 μm; And / or, the oxidation reduction of the modified carbon fiber material is less than 20%, preferably less than 18%, for example, 12.3% or 17.5%.
3. A method for preparing a modified carbon fiber material, characterized in that: It includes the following steps: The modified carbon fiber material is obtained by subjecting the carbon fiber substrate to an anti-oxidation treatment and a pyrolysis carbon treatment in sequence; the oxygen content of the carbon fiber substrate is less than 100 ppm.
4. The method for preparing the modified carbon fiber material according to claim 3, characterized in that: The oxygen content of the carbon fiber substrate is less than 70 ppm, for example, 65 ppm or 67 ppm; And / or, the method for preparing the carbon fiber substrate comprises: subjecting the carbon fiber precursor to a replacement treatment; wherein the replacement treatment step comprises, for example: placing the carbon fiber precursor in a replacement device, and simultaneously evacuating the replacement device and introducing an inert gas; The vacuum pressure is preferably 0.01-0.1 MPa, for example 0.05 MPa; Wherein, the inert gas is preferably nitrogen and / or argon; wherein, the purity of the nitrogen is, for example, 99.99%; wherein, the purity of the argon is, for example, 99.99%; The temperature of the replacement treatment is, for example, room temperature.
5. The method for preparing the modified carbon fiber material according to claim 4, characterized in that: The method for preparing the carbon fiber precursor comprises the following steps: subjecting the mixture to curing treatment and graphitization treatment in sequence to obtain the carbon fiber precursor; the mixture comprises phenolic resin and carbon fiber; Wherein, the carbon fiber is, for example, carbon fiber soft felt, and the carbon fiber soft felt is, for example, one or more of asphalt-based carbon fiber soft felt, PAN-based carbon fiber soft felt and viscose-based carbon fiber soft felt; Wherein, the preparation method of the mixture is preferably: impregnating the carbon fiber in the phenolic resin; Wherein, the pressure of the curing treatment is preferably 4-15 MPa, for example, 10 MPa; Wherein, the curing temperature is preferably 130-220°C, for example, 200°C; Wherein, the temperature of the graphitization treatment is preferably 2200-2400°C, for example, 2300°C; The graphitization treatment time is preferably 50-150 hours, for example 100 hours.
6. The method for preparing the modified carbon fiber material according to claim 3, characterized in that: The number of times of the antioxidant treatment is twice; And / or, the step of the anti-oxidation treatment is: coating an antioxidant on the surface of the carbon fiber substrate and then performing a heat treatment; Wherein, the antioxidant preferably comprises a resin; the resin is preferably one or more of a vinyl resin, an epoxy resin and a phenolic resin; wherein, the antioxidant preferably also comprises carbon black, a surfactant and a solvent; Wherein, the heat treatment preferably includes a first heat treatment and a second heat treatment in sequence, the temperature of the first heat treatment is 100-300°C, and the temperature of the second heat treatment is 2000-2400°C; wherein, the temperature of the first heat treatment is, for example, 200°C; wherein, the temperature of the second heat treatment is preferably 2200-2400°C; wherein, the time of the first heat treatment is preferably 5-8h; wherein, the time of the second heat treatment is preferably 50-150h, for example, 70h or 100h.
7. The method for preparing the modified carbon fiber material according to claim 6, characterized in that: The mass percentage of the resin to the antioxidant is 10%-50%, for example, 25%; And / or, the solvent is ethanol; And / or, the mass percentage of the carbon black to the antioxidant is 5%-15%, for example, 10%; And / or, the average particle size of the carbon black is 60-200 mesh; And / or, the mass percentage of the surfactant to the antioxidant is preferably 0.1%-0.5%, for example 0.2%; And / or, the type of surfactant is an alcohol compound and / or an alcohol ether compound; wherein the alcohol compound is preferably polyethylene glycol and / or polypropylene glycol; wherein the alcohol ether compound is preferably a glycol ether compound, for example, propylene glycol ether and / or diethylene glycol ether; wherein the propylene glycol ether is, for example, propylene glycol propyl ether.
8. The method for preparing the modified carbon fiber material according to claim 3, characterized in that: The raw material for the pyrolysis carbon treatment also includes a carbon source gas; wherein the carbon source gas is preferably one or more of methane, ethane and propylene; And / or, the temperature of the pyrolytic carbon treatment is 1000-1800° C., for example, 1200° C.; And / or, the pyrolytic carbon treatment time is 20-30 hours, for example, 24 hours; And / or, the pressure of the pyrolytic carbon treatment is below 10 kPa, for example, 8 kPa; And / or, the pyrolytic carbon treatment adopts a chemical vapor deposition furnace.
9. A modified carbon fiber material obtained by the method for preparing a modified carbon fiber material as described in any one of claims 3 to 8.