Polyester-viscose fabric one-bath dyeing process
By adding dye, Yuanming powder and sodium sulfonate organic components in dispersions and other components in the one-bath dyeing process of polyester-tight fabrics, combined with temperature control, the problems of large water use and insufficient color fastness in traditional processes are solved, and the problem of Efficient and uniform dyeing effect meets the market's demand for dyeing polyester fabrics.
Patent Information
- Application Number
- CN202411051675.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-01
- Publication Date
- 2024-11-12
AI Technical Summary
The traditional polyester-tight fabric one-bath dyeing process uses a lot of water and is cost-effective, and the dyed fabrics are insufficient in color fastness, making it difficult to meet market demand.
A one-bath dyeing process for polyester fabrics, including pretreatment, one-bath dyeing, dehydration and shaping, and vaporization. Use a one-bath dyeing working liquid to add dye, Yuanming powder, and sodium sulfonate salt to organically penetrate the dispersion and permeability. The agent and stabilizer improve the dyeing effect by controlling the temperature and soaking time.
On the basis of simplifying the process and saving water, the wet friction color fastness and soap washing color fastness of dyed fabrics are improved to ensure uniform color and meet the market's requirements for friction color fastness and soap washing color fastness.
Smart Images

Figure CN118932754A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of fabric dyeing, and more specifically, to a one-bath dyeing process for polyester-viscose fabrics. Background Art
[0002] Polyester-viscose fabric is a blend of polyester fiber and viscose fiber. It not only has the characteristics of polyester's wear resistance, wrinkle resistance, easy washing and quick drying, but also has the advantages of viscose's softness, hygroscopicity and breathability. It has been widely used in clothing, furniture and other fields. The traditional one-bath dyeing process of polyester-viscose fabric includes pre-treatment, disperse dyeing, reactive dyeing, dehydration and shaping, steaming, finished product inspection and warehousing. Among them, the two processes of disperse dyeing and reactive dyeing are long in use, large in water consumption and high in production cost.
[0003] In order to simplify the process, save dyeing time and reduce water consumption, some manufacturers adopt the dyeing process as follows: take disperse dyes with a weight of 0.5-1% of the PLA / PHBV blended silk component in the interwoven fabric and active dyes with a weight of 0.5-1% of the viscose component in the interwoven fabric, add environmentally friendly carriers to prepare dyeing solution, wherein the concentration of the environmentally friendly carrier in the dyeing solution is 0.4-0.6g / L, put the pre-treated interwoven fabric into the dyeing solution with a bath ratio of 1:20-30 for dyeing: heat it to 60-65℃, add anhydrous sodium sulfate to make its concentration in the dyeing solution 40-60g / L, continue to heat it to 80-85℃, dye it for 10 minutes, then add anhydrous sodium carbonate to fix the color, the concentration of anhydrous sodium carbonate in the dyeing solution is 0.5-1g / L, continue to keep warm and dye for 20-30 minutes, cool it to 50℃-60℃ and take out the interwoven fabric. The dyed fabric obtained by the method has a color fastness to rubbing of 3-4 and a color fastness to soaping of 3-4, and the color fastness needs to be further improved. Summary of the invention
[0004] In order to improve the color fastness of dyed fabrics, the present application provides a one-bath dyeing process for polyester-viscose fabrics, which adopts the following technical scheme: A one-bath dyeing process for polyester-viscose fabrics, comprising the following steps: pre-treatment, one-bath dyeing, dehydration and shaping, and steaming; The one-bath dyeing method is as follows: the pre-treated polyester-viscose fabric and the one-bath dyeing working solution are mixed at a bath ratio of 1:(10-20), and then the temperature is raised to 120-140°C at a speed of 1-3°C / min, and the heat preservation dyeing treatment is performed for 20-40 minutes, and then the temperature is lowered to 50-70°C at a speed of 2-5°C / min, and the liquid is drained, and water is added for washing at a bath ratio of 1:(10-20), and the liquid is drained, and the cleaning working solution is added for washing at a bath ratio of 1:(10-20), and the liquid is drained, and water is added for washing at a bath ratio of 1:(10-20), and the liquid is drained, and the liquid is added for washing at a bath ratio of 1:(10-20), and the liquid is drained; The one-bath dyeing working solution uses water as a solvent, and the solute of the one-bath dyeing working solution includes the following components: 3-7 g / L dye, 13-17 g / L glauber powder, 2-4 g / L sulfonic acid sodium salt organic dispersant, 1-3 g / L penetrant, 1-3 g / L stabilizer, and 0.3-1 g / L chelating dispersant.
[0005] By adopting the above technical scheme, the raw materials of the one-bath dyeing working solution are matched with each other, and the temperature is 120-140°C, the pre-treated polyester-viscose fabric is dyed to obtain the dyed fabric. On the basis of simplifying the process, saving dyeing time, and reducing water consumption, the wet friction color fastness of the dyed fabric is 4-5, and the color fastness to soap washing is 5. The dyed fabric has no scattered defects or local defects and has uniform color. The dyed fabric has the advantages of good color fastness to friction, good color fastness to soap washing, and uniform color, meeting market demand.
[0006] Dyes are added to the raw materials of the one-bath dyeing working solution to achieve the purpose of dyeing. The addition of penetrants can improve the penetration ability of dyes and improve the dyeing rate. The addition of stabilizers can improve the stability of dyes, reduce the side reactions of dyes, and ensure the smooth progress of the dyeing process. The addition of chelating dispersants can complex metal ions in water and generate stable soluble complexes to reduce the combination of metal ions and dyes. The addition of sodium sulfate and sodium sulfonate organic can be used in the dispersion, and the synergistic effect between the two is used to enhance the color fastness to friction, the color fastness to soaping, and the uniform color, so that the dyed fabrics show better comprehensive performance.
[0007] Optionally, the sodium sulfonate organic salt can be prepared in a dispersion by the following method: T1. Add itaconic anhydride to toluene and mix, then drop diethylenetriamine within 20-40 minutes, continue stirring for 3-5 hours, and perform distillation under reduced pressure to obtain a monomer; T2. Add diaminobutane to water at a temperature of 80-100° C., then add the monomer obtained in step T1, stir for 3-5 hours, then add diethylene glycol monoallyl ether and sodium styrene sulfonate, mix, then add an inorganic initiator, stir for 3-5 hours, and dry to obtain an organic dispersion of sodium sulfonate.
[0008] Optionally, the weight ratio of itaconic anhydride, diethylenetriamine, butanediamine, diethylene glycol monoallyl ether, and sodium styrene sulfonate is (13-17):(9-11):(1-3):(2-4):(2-4).
[0009] By adopting the above technical scheme, the anhydride group in itaconic anhydride and the secondary amine group in diethylenetriamine are firstly reacted to obtain a monomer containing a carboxyl group, a primary amine group and a carbon-carbon double bond. Then, with dibutylene diamine as the core, the amine group in dibutylene diamine and the carboxyl group in the monomer are reacted, and then the monomer undergoes a self-condensation reaction to form a dendritic polycondensate with more branches. Afterwards, by means of a polymerization reaction, diethylene glycol monoallyl ether and sodium styrene sulfonate are grafted on the surface of the dendritic polycondensate to obtain a sodium sulfonate organic dispersion.
[0010] In the preparation method of the sodium sulfonate organic dispersion of the present application, itaconic anhydride, diethylenetriamine, butanediamine, diethylene glycol monoallyl ether, and sodium styrene sulfonate are reacted in steps, which is convenient for the preparation of the sodium sulfonate organic dispersion. In addition, the sodium sulfonate organic dispersion contains more amide groups, hydroxyl groups, carboxyl groups, ether groups, and sodium sulfonate groups, which makes it easier for dyes to dye polyester-viscosity fabrics, enhances the affinity between polyester-viscosity fabrics and dyes, improves the uniformity of color dispersion, makes the sodium sulfonate organic dispersion show better use effects, and also improves color fastness and color uniformity.
[0011] Optionally, the weight ratio of diethylene glycol monoallyl ether and inorganic initiator is (2-4):(0.1-0.5).
[0012] By adopting the above technical solution, the addition amount of the inorganic initiator is optimized, which makes it easier to control the rate of the polymerization reaction, ensure the polymerization reaction proceeds in a balanced manner, and ensure the stability of the sodium sulfonate organic phase in the dispersion.
[0013] Further, the inorganic initiator is one or more of ammonium persulfate, sodium persulfate, and potassium persulfate. In multiple embodiments, the inorganic initiator is ammonium persulfate, and the inorganic initiator can also be set to sodium persulfate or potassium persulfate as needed, but it is not limited to the listed options, and other options not listed within the selection range are also applicable.
[0014] Further, the weight ratio of toluene and itaconic anhydride is (70-130):(13-17). In one embodiment, the weight ratio of toluene and itaconic anhydride is 20:3, in another embodiment, the weight ratio of toluene and itaconic anhydride is 100:13, in another embodiment, the weight ratio of toluene and itaconic anhydride is 100:17, and the weight ratio can also be set to 70:13, 70:17, 130:13, 130:17 as needed, but it is not limited to the listed values, and other values not listed in the numerical range are also applicable.
[0015] Further, the weight ratio of water to diethylenediamine is (70-130):(1-3). In one embodiment, the weight ratio of water to diethylenediamine is 50:1, in another embodiment, the weight ratio of water to diethylenediamine is 100:3, in another embodiment, the weight ratio of water to diethylenediamine is 100:1, and the weight ratio can also be set to 70:1, 70:3, 130:1, 130:3 as needed, but it is not limited to the listed values, and other values not listed in the numerical range are also applicable.
[0016] Optionally, the penetrant is one or more of penetrant OE35, polyoxyethylene ether, and sorbitan fatty acid ester.
[0017] By adopting the above technical solution, the penetrant is optimized and the selection of the penetrant is facilitated. In multiple embodiments, the penetrant is the penetrant OE35, and the penetrant can also be set as polyoxyethylene ether or sorbitan fatty acid ester as needed, but it is not limited to the listed options, and other options not listed within the selection range are also applicable.
[0018] Further, the dye is dye Yagxin CP, and dye Yagxin CP is one or more of dye Yagxin CP black, dye Yagxin CP red, dye Yagxin CP blue, dye Yagxin CP green, dye Yagxin CP yellow, dye Yagxin CP orange, dye Yagxin CP cyan, dye Yagxin CP brown, and dye Yagxin CP purple.
[0019] Further, the polyester content in the polyester-viscose fabric is 60-70wt%, and the viscose content is 30-40wt%. In multiple embodiments, the polyester content in the polyester-viscose fabric is 60wt%, and the viscose content is 40wt%. The polyester content can also be set to 63wt%, 65wt%, 68wt%, 70wt% as needed. In this case, the corresponding viscose content is 37wt%, 35wt%, 32wt%, 30wt%, but it is not limited to the listed options, and other options not listed within the selection range are also applicable.
[0020] Optionally, the cleaning working solution uses water as a solvent, and the solute of the cleaning working solution includes the following components: 1-5 g / L of cleaning agent.
[0021] By adopting the above technical solution, the cleaning working solution contains a cleaning agent, which can effectively remove floating colors and unreacted dyes, reduce the influence of floating colors on color fastness and color brightness, and improve the overall quality of dyed fabrics.
[0022] In multiple embodiments, the solute of the cleaning working solution includes the following components: 3g / L of cleaning agent. The content of the cleaning agent can also be set to 1g / L, 2g / L, 4g / L, 5g / L as needed, but is not limited to the listed values. Other unlisted values within the numerical range are also applicable.
[0023] Further, in step S2, the cleaning temperature is 70-90°C and the time is 10-30 minutes. In multiple embodiments, the cleaning temperature is 80°C and the time is 20 minutes. The temperature can also be set to 70°C, 75°C, 85°C, 90°C as needed, and the time can also be set to 10 minutes, 15 minutes, 25 minutes, 30 minutes as needed, but it is not limited to the listed values, and other values not listed in the numerical range are also applicable.
[0024] Optionally, the pre-treatment is specifically as follows: immersing the polyester-viscose fabric in the pre-treatment working solution with a bath ratio of 1:(10-20), then heating to 90-100°C at a rate of 1-3°C / min, keeping warm for 20-40 minutes, then cooling to 50-70°C at a rate of 2-5°C / min, draining the liquid, adding water for washing, with a bath ratio of 1:(10-20), and draining the liquid.
[0025] Optionally, the pre-treatment working solution uses water as a solvent, and the solute of the pre-treatment working solution includes the following components: 2-5 g / L of a desizing agent, 1-3 g / L of an oil removing agent, and 0.3-1 g / L of a chelating dispersant.
[0026] By adopting the above technical scheme, polyester-viscose fabrics are pre-treated, so that slurry and oil stains on the surface of the polyester-viscose fabrics can be effectively removed, and the softness and water absorption of the polyester-viscose fabrics can be restored, which is beneficial to the subsequent one-bath dyeing process.
[0027] In multiple embodiments, the bath ratio of the polyester-viscose fabric immersed in the pretreatment working solution in the pretreatment is 1:15, the heating rate is 2°C / min, the temperature is raised to 95°C, the heat treatment is carried out for 30 minutes, the cooling rate is 3°C / min, and the temperature is lowered to 60°C. The bath ratio can also be set to 1:10, 1:13, 1:18, 1:20 as needed, and the heating rate can also be set to 1°C / min, 1.5°C / min, 2.5°C / min, 3°C / min as needed. The temperature can also be raised to 9 0℃, 93℃, 98℃, 100℃. The insulation time can also be set to 20min, 25min, 35min, 40min as needed. The cooling rate can also be set to 2℃ / min, 2.5℃ / min, 3.5℃ / min, 4℃ / min, 4.5℃ / min, 5℃ / min as needed. The temperature can also be cooled to 50℃, 55℃, 65℃, 70℃ as needed, but it is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0028] In multiple embodiments, the bath ratio of water added for washing in the pretreatment is 1:15. The bath ratio can also be set to 1:10, 1:13, 1:18, 1:20 as needed, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0029] In multiple embodiments, the solute of the pretreatment working solution includes the following components: 3 g / L desizing agent, 2 g / L deoiling agent, and 0.5 g / L chelating dispersant. The solute content of the pretreatment working solution can also be set to 2 g / L desizing agent, 3 g / L deoiling agent, and 0.3 g / L chelating dispersant as needed. The solute content of the pretreatment working solution can also be set to 5 g / L desizing agent, 1 g / L deoiling agent, and 1 g / L chelating dispersant as needed, but it is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0030] Optionally, the dehydration and shaping is specifically: drying and shaping the polyester-viscose fabric after the one-bath dyeing treatment at a temperature of 105-120° C. and a vehicle speed of 20-40 m / min.
[0031] By adopting the technical scheme, the polyester-viscose fabric after one-bath dyeing is subjected to shaping treatment, excess water in the polyester-viscose fabric is removed, and the polyester-viscose fabric can be made to drape and be flat.
[0032] In multiple embodiments, the temperature in the dehydration and shaping treatment is 110°C and the vehicle speed is 30m / min. The temperature can also be set to 105°C, 115°C, or 120°C as needed. The vehicle speed can also be set to 20m / min, 25m / min, 35m / min, or 40m / min as needed. However, the above values are not limited to the above values, and other values not listed within the range are also applicable.
[0033] Optionally, the steaming specifically comprises: steaming the polyester-viscose fabric after the dehydration and setting treatment for 20-40 minutes in a saturated water vapor atmosphere at a temperature of 120-130° C.
[0034] By adopting the above technical scheme, the polyester-viscose fabric after dehydration and setting treatment is subjected to steaming treatment, which can not only improve the feel of the polyester-viscose fabric, but also increase the interaction between the polyester-viscose fabric and the dye, thereby improving the dyeing durability and color fastness.
[0035] In multiple embodiments, the saturated water vapor temperature in the steam treatment is 125°C and the steam treatment time is 30 minutes. The saturated water vapor temperature can also be set to 120°C, 123°C, 128°C, or 130°C as needed. The steam treatment time can also be set to 20 minutes, 25 minutes, 35 minutes, or 40 minutes as needed. However, the above values are not limited to the above values, and other values not listed within the above range are also applicable.
[0036] In summary, this application has at least the following beneficial effects: 1. The one-bath dyeing process for polyester-viscose fabrics of the present application comprises the following steps: pretreatment, one-bath dyeing, dehydration and shaping, and steaming; in the one-bath dyeing process, the raw materials of the one-bath dyeing working solution are coordinated with each other, and the dyeing is carried out at a temperature of 120-140°C. On the basis of simplifying the process, saving dyeing time, and reducing water consumption, the color fastness is improved, the color fastness to wet friction is 4-5, and the color fastness to soap washing is 5. At the same time, the dyed fabric has no scattered defects or local defects and has uniform color. The dyed fabric has the advantages of good color fastness to friction, good color fastness to soap washing, and uniform color, which meets market demand.
[0037] 2. Add sodium sulfonate and organic sodium sulfonate dispersion to the raw materials of the one-bath dyeing working solution. The organic sodium sulfonate dispersion contains more amide groups, hydroxyl groups, carboxyl groups, ether groups and sodium sulfonate groups. The synergistic effect between the two is utilized to enhance the color fastness to rubbing, color fastness to soaping and color uniformity, so that the dyed fabrics show better comprehensive performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] Figure 1 It is a schematic diagram of the one-bath dyeing process of Example 1 of the present application. DETAILED DESCRIPTION
[0039] In order to make the present application easier to understand, the present application will be further described in detail below in conjunction with the examples, which are merely illustrative and are not intended to limit the scope of application of the present application. The raw materials or components used in the present application can be obtained through commercial routes or conventional methods unless otherwise specified.
[0040] Preparation Example Preparation Example 1 A sodium sulfonate organic dispersion is prepared by the following method: T1. Add 15 g of itaconic anhydride to 100 g of toluene and stir for 2 min. Then add 10 g of diethylenetriamine dropwise for 30 min. Continue stirring for 4 h and remove toluene by distillation under reduced pressure to obtain a monomer.
[0041] T2. In water at a temperature of 90°C, add 2 g of diaminodiamine to 100 g of water and stir for 2 min. Then add the monomer obtained in step T1 and stir for 4 h. Then add 3 g of diethylene glycol monoallyl ether and 3 g of sodium styrene sulfonate and stir for 2 min. Then add 0.3 g of ammonium persulfate and stir for 4 h. Dry to obtain an organic dispersion of sodium sulfonate.
[0042] Preparation Example 2 A sodium sulfonate organic dispersion is prepared by the following method: T1. Add 13 g of itaconic anhydride to 100 g of toluene and stir for 2 min. Then add 11 g of diethylenetriamine dropwise for 40 min. Continue stirring for 3 h. Remove toluene by distillation under reduced pressure to obtain a monomer.
[0043] T2. Add 3 g of diaminobutane to 100 g of water at 90°C and stir for 2 min. Then add the monomer obtained in step T1 and stir for 5 h. Then add 2 g of diethylene glycol monoallyl ether and 4 g of sodium styrene sulfonate and stir for 2 min. Then add 0.1 g of ammonium persulfate and stir for 3 h. Dry to obtain an organic dispersion of sodium sulfonate.
[0044] Preparation Example 3 A sodium sulfonate organic dispersion is prepared by the following method: T1. Add 17 g of itaconic anhydride to 100 g of toluene and stir for 2 min. Then add 9 g of diethylenetriamine dropwise for 20 min. Continue stirring for 5 h and remove toluene by distillation under reduced pressure to obtain a monomer.
[0045] T2. In water at a temperature of 90°C, add 1g of diaminobutane to 100g of water and stir for 2min. Then add the monomer obtained in step T1 and stir for 3h. Then add 4g of diethylene glycol monoallyl ether and 2g of sodium styrene sulfonate and stir for 2min. Then add 0.5g of ammonium persulfate and stir for 5h. Dry to obtain an organic dispersion of sodium sulfonate. Example
[0046] Example 1 The one-bath dyeing process for polyester-viscose fabrics comprises the following steps: pre-treatment, one-bath dyeing, dehydration and shaping, steaming, finished product inspection and storage.
[0047] Specifically: S1, pre-treatment: At a temperature of 40°C, immerse the polyester-viscose fabric in the pre-treatment working solution, the amount of pre-treatment working solution added is 4 tons, and the bath ratio is 1:15. Then, heat it to 95°C at a rate of 2°C / min, and keep it warm for 30 minutes. Then cool it to 60°C at a rate of 3°C / min, and drain the liquid. Add water, the amount of water added is 4 tons, the bath ratio is 1:15, wash it with water for 5 minutes, and drain it.
[0048] The pre-treatment working solution uses water as solvent, and the solute of the pre-treatment working solution includes the following components: 3 g / L desizing agent, 2 g / L degreasing agent, and 0.5 g / L chelating dispersant.
[0049] The desizing agent is refined desizing agent M1011, and is selected from Hangzhou Meigao Huayi Chemical Co., Ltd.; the deoiling agent is refined deoiling agent TY1-20, and is selected from Dongguan Taiyang New Material Technology Co., Ltd.; the chelating dispersant is chelating dispersant M1075, and is selected from Hangzhou Meigao Huayi Chemical Co., Ltd.
[0050] The polyester-viscose fabric is a fabric blended from polyester fiber and viscose fiber, wherein the polyester content in the polyester-viscose fabric is 60wt% and the viscose content is 40wt%.
[0051] S2, one-bath dyeing: refer to Figure 1 , at a temperature of 40°C, mix the pre-treated polyester-viscose fabric and the one-bath dyeing working solution in the dyeing vat, the addition amount of the one-bath dyeing working solution is 4 tons, and the bath ratio is 1:15. Then heat it to 130°C at a rate of 2°C / min, keep it warm and dye it for 30 minutes. Then cool it to 60°C at a rate of 3°C / min, and drain it. Add water, the addition amount of water is 4 tons, the bath ratio is 1:15, wash it with water for 5 minutes, and drain it. Add the cleaning working solution, the addition amount of the cleaning working solution is 4 tons, and the bath ratio is 1:15. Then heat it to 80°C at a rate of 2°C / min, keep it warm and wash it for 20 minutes, and drain it. Add water, the addition amount of water is 4 tons, the bath ratio is 1:15, wash it with water for 5 minutes, and drain it.
[0052] Among them, the one-bath dyeing working solution uses water as solvent, and the solute of the one-bath dyeing working solution includes the following components: dye 5g / L, glauber powder 15g / L, sodium sulfonate organic dispersant 3g / L, penetrant 2g / L, stabilizer 2g / L, chelating dispersant 0.5g / L.
[0053] The dye is the dye Yagenxin CP black, and the dye Yagenxin CP black is selected from Shanghai Yayun Textile Chemical Co., Ltd.; the penetrant is the penetrant OE35, and is selected from Nantong Yongle Chemical Co., Ltd.; the stabilizer is the stabilizer CBA, and is selected from Shanghai Yayun Textile Chemical Co., Ltd.; the chelating dispersant is the chelating dispersant M1075, and is selected from Hangzhou Meigao Huayi Chemical Co., Ltd.; the sodium sulfonate organic can be prepared in the dispersion by the method of Preparation Example 1.
[0054] The cleaning working solution uses water as solvent, and the solute of the cleaning working solution includes the following components: 3g / L of cleaning agent. The cleaning agent is cleaning agent TCW, and is selected from Shanghai Yayun Textile Chemical Co., Ltd.
[0055] S3, dehydration and shaping: drying and shaping the polyester-viscose fabric after one-bath dyeing at a temperature of 110°C and a speed of 30m / min.
[0056] S4. Steaming: steaming the polyester-viscose fabric after dehydration and setting for 30 minutes in a saturated steam atmosphere at a temperature of 125° C. to obtain a dyed fabric.
[0057] S5. Finished product inspection.
[0058] S6. Storage.
[0059] Example 2 A one-bath dyeing process for polyester-viscose fabrics, which differs from Example 1 in that, in step S2, the one-bath dyeing working solution has a different ratio, and the solute of the one-bath dyeing working solution includes the following components: 3 g / L dye, 17 g / L glauber salt, 2 g / L sulfonic acid sodium salt organic dispersant, 3 g / L penetrant, 3 g / L stabilizer, and 0.3 g / L chelating dispersant.
[0060] Example 3 A one-bath dyeing process for polyester-viscose fabrics, which differs from Example 1 in that, in step S2, the one-bath dyeing working solution has a different ratio, and the solute of the one-bath dyeing working solution includes the following components: 7 g / L dye, 13 g / L glauber salt, 4 g / L sulfonic acid sodium salt organic dispersant, 1 g / L penetrant, 1 g / L stabilizer, and 1 g / L chelating dispersant.
[0061] Example 4 A one-bath dyeing process for polyester-viscose fabrics is different from Example 1 in that, in step S2, the raw materials of the one-bath dyeing working solution have different sources of sodium sulfonate organic dispersions, and the sodium sulfonate organic dispersion is prepared by the method of Preparation Example 2.
[0062] Example 5 A one-bath dyeing process for polyester-viscose fabrics is different from Example 1 in that, in step S2, the raw materials of the one-bath dyeing working solution have different sources of sodium sulfonate organic dispersions, and the sodium sulfonate organic dispersion is prepared by the method of Preparation Example 3.
[0063] Comparative Example Comparative Example 1 A one-bath dyeing process for polyester-viscose fabrics is different from Example 1 in that, in step S2, an equal amount of sodium sulfonate organic dispersant is used in the raw materials of the one-bath dyeing working solution.
[0064] Comparative Example 2 A one-bath dyeing process for polyester-viscose fabrics is different from Example 1 in that, in step S2, an equal amount of sodium sulfonate organic dispersion is used to replace sodium sulfate in the raw materials of the one-bath dyeing working solution.
[0065] Comparative Example 3 A one-bath dyeing process for polyester-viscose fabrics is different from Example 1 in that, in step S2, in the raw materials of the one-bath dyeing working solution, the sodium sulfonate salt organic can be used in the dispersion preparation method to replace diethylene glycol monoallyl ether and sodium styrene sulfonate with an equal amount of monomers.
[0066] Comparative Example 4 A one-bath dyeing process for polyester-viscose fabrics is different from Example 1 in that, in step S2, in the raw materials of the one-bath dyeing working solution, sodium sulfonate salt is organicallyl ether in the dispersion preparation method, and an equal amount of diethylene glycol monoallyl ether is used to replace sodium styrene sulfonate.
[0067] Comparative Example 5 A one-bath dyeing process for polyester-viscose fabrics is different from Example 1 in that, in step S2, in the raw materials of the one-bath dyeing working solution, the sodium sulfonate salt organic dispersion is replaced by an equal amount of sodium styrene sulfonate in the dispersion preparation method.
[0068] Comparative Example 6 A one-bath dyeing process for polyester-viscose fabrics is different from Example 1 in that, in step S2, an equal amount of sodium dodecyl sulfonate is used to replace the organic dispersible sodium sulfonate in the raw materials of the one-bath dyeing working solution.
[0069] Performance Testing (1) A discussion group of 30 professionals was formed to evaluate and score the color uniformity of the dyed fabrics obtained in Examples 1-5 and Comparative Examples 1-6. Color uniformity is divided into five levels: Level 1 is a large number of scattered defects, with a score of 1-1.9 points; Level 2 is a small number of scattered defects, with a score of 2-2.9 points; Level 3 is a large number of local defects, with a score of 3-3.9 points; Level 4 is a small number of local defects, with a score of 4-4.9 points; Level 5 is uniform color, with a score of 5 points. The color uniformity scoring results of the dyed fabrics are shown in Table 1.
[0070] (2) The dyed fabrics obtained in Examples 1-5 and Comparative Examples 1-6 were respectively taken, and the color fastness to wet rubbing and the color fastness to discoloration with soap washing of the dyed fabrics were tested according to GB / T3920-2008 and GB / T3921-2008. The test results are shown in Table 1. The greater the color fastness to wet rubbing, the better the color fastness to rubbing of the dyed fabric, and the better the color fastness to discoloration with soap washing, the better the color fastness to soap washing of the dyed fabric.
[0071] (3) According to GB / T3923.1-2013, the breaking strength of the polyester-viscose fabrics of Examples 1-5 and Comparative Examples 1-6 before and after dyeing was tested, and the breaking strength loss rate was calculated. The test results are shown in Table 1.
[0072] Breaking strength loss rate / (%)=(breaking strength of polyester-viscose fabric before dyeing-breaking strength of polyester-viscose fabric after dyeing) / breaking strength of polyester-viscose fabric before dyeing×100%.
[0073] Table 1 Test results As can be seen from Table 1, the one-bath dyeing process for polyester-viscose fabrics of the present application, in which the dyed fabric obtained after dyeing the polyester-viscose fabric, has a color fastness to wet rubbing of level 4-5, a color fastness to discoloration after soaping of level 5, and a color uniformity of 5.0 points, so that the dyed fabric exhibits high color fastness to rubbing and color fastness to soaping, and has no scattered defects or local defects, and has uniform color, so that the dyed fabric exhibits the advantages of good color fastness to rubbing, good color fastness to soaping, and uniform color, meeting market demand.
[0074] Comparative Examples 1-2 are compared, and 18g / L of sodium sulfate is added to the raw materials of the one-bath dyeing working solution of Comparative Example 1; 18g / L of sodium sulfonate salt is added to the raw materials of the one-bath dyeing working solution of Comparative Example 2. It can be seen that adding sodium sulfate in the raw materials is conducive to improving the color fastness to rubbing and the color fastness to soaping, but adding sodium sulfonate salt organic in the dispersion in the raw materials is conducive to improving the color uniformity, and adding sodium sulfate or sodium sulfonate salt organic in the dispersion has basically no effect on the breaking strength loss rate. Combined with Example 1, 15g / L of sodium sulfate and 3g / L of sodium sulfonate salt organic in the dispersion are added to the raw materials of the one-bath dyeing working solution of Example 1. It can be seen that sodium sulfate and sodium sulfonate salt organic in the dispersion are added simultaneously in the raw materials of the one-bath dyeing working solution, and the synergistic effect between them can be further improved. The color fastness to rubbing, the color fastness to soaping and the color uniformity can be further improved, so that the dyed fabric shows a better comprehensive performance.
[0075] Compare Example 1 with Comparative Examples 3-4. The sodium sulfonate salt in the raw material of the one-bath dyeing working liquid of Comparative Example 3 is organically available in a dispersion, which is obtained by processing itaconic anhydride, diethylenetriamine, and diethylenediamine; the sodium sulfonate salt in the raw material of the one-bath dyeing working liquid of Comparative Example 4 is organically available in a dispersion, which is obtained by processing itaconic anhydride, diethylenetriamine, diethylenediamine, and diethylene glycol monoallyl ether; the sodium sulfonate salt in the raw material of the one-bath dyeing working liquid of Comparative Example 5 is organically available in a dispersion, which is obtained by processing itaconic anhydride, diethylenetriamine, diethylenediamine, and sodium styrene sulfonate; the sodium sulfonate salt in the raw material of the one-bath dyeing working liquid of Example 1 is organically available in a dispersion, which is obtained by processing itaconic anhydride, diethylenetriamine, diethylenediamine, diethylene glycol monoallyl ether, and sodium styrene sulfonate. It can be seen from this that on the basis of the condensation reaction of itaconic anhydride, diethylenetriamine and dibutylene diamine to form a dendritic polycondensate, diethylene glycol monoallyl ether and sodium styrene sulfonate are further grafted by polymerization reaction, so that the sodium sulfonate organic salt contains more branched chains, amide groups, hydroxyl groups, carboxyl groups, ether groups and sodium sulfonate groups in the dispersion, making it easier for the dye to dye polyester-viscose fabrics, enhancing the affinity between polyester-viscose fabrics and dyes, improving the uniformity of color dispersion, making the sodium sulfonate organic salt show better use effect in the dispersion, and improving the color fastness and color uniformity of the dyed fabrics.
[0076] It should be noted that the embodiments described above are only used to explain the present application and do not constitute any limitation to the present application. The present application is described with reference to typical embodiments, but it should be understood that the words used therein are descriptive and explanatory words, rather than restrictive words. The present application may be modified as specified within the scope of the claims of the present application, and the present invention may be revised without departing from the scope and spirit of the present application. Although the present application described therein relates to specific methods, materials and embodiments, it does not mean that the present application is limited to the specific examples disclosed therein. On the contrary, the present application can be extended to all other methods and applications with the same functions.
Claims
1. A one-bath dyeing process for polyester-viscose fabrics, characterized in that: The process includes the following steps: pre-treatment, one-bath dyeing, dehydration and setting, and steaming; The one-bath dyeing method is as follows: the pre-treated polyester-viscose fabric and the one-bath dyeing working solution are mixed at a bath ratio of 1:(10-20), and then the temperature is raised to 120-140°C at a speed of 1-3°C / min, and the heat preservation dyeing treatment is performed for 20-40 minutes, and then the temperature is lowered to 50-70°C at a speed of 2-5°C / min, and the liquid is drained, and water is added for washing at a bath ratio of 1:(10-20), and the liquid is drained, and the cleaning working solution is added for washing at a bath ratio of 1:(10-20), and the liquid is drained, and water is added for washing at a bath ratio of 1:(10-20), and the liquid is drained, and the liquid is added for washing at a bath ratio of 1:(10-20), and the liquid is drained; The one-bath dyeing working solution uses water as a solvent, and the solute of the one-bath dyeing working solution includes the following components: 3-7 g / L dye, 13-17 g / L glauber powder, 2-4 g / L sulfonic acid sodium salt organic dispersant, 1-3 g / L penetrant, 1-3 g / L stabilizer, and 0.3-1 g / L chelating dispersant.
2. A one-bath dyeing process for polyester-viscose fabric according to claim 1, characterized in that: The sodium sulfonate organic salt can be prepared in a dispersion by the following method: T1. Add itaconic anhydride to toluene and mix, then drop diethylenetriamine within 20-40 min, continue stirring for 3-5 h, and perform vacuum distillation to obtain a monomer; T2. Add diaminobutane to water at a temperature of 80-100° C., then add the monomer obtained in step T1, stir for 3-5 hours, then add diethylene glycol monoallyl ether and sodium styrene sulfonate, mix, then add an inorganic initiator, stir for 3-5 hours, and dry to obtain an organic dispersion of sodium sulfonate.
3. A one-bath dyeing process for polyester-viscose fabric according to claim 2, characterized in that: The weight ratio of itaconic anhydride, diethylenetriamine, butanediamine, diethylene glycol monoallyl ether and sodium styrene sulfonate is (13-17):(9-11):(1-3):(2-4):(2-4).
4. A one-bath dyeing process for polyester-viscose fabric according to claim 2, characterized in that: The weight ratio of diethylene glycol monoallyl ether and inorganic initiator is (2-4):(0.1-0.5).
5. A one-bath dyeing process for polyester-viscose fabric according to claim 1, characterized in that: The penetrant is one or more of penetrant OE35, polyoxyethylene ether, and sorbitan fatty acid ester.
6. A one-bath dyeing process for polyester-viscose fabric according to claim 1, characterized in that: The cleaning working solution uses water as solvent, and the solute of the cleaning working solution includes the following components: 1-5 g / L of cleaning agent.
7. A one-bath dyeing process for polyester-viscose fabric according to claim 1, characterized in that: The specific pretreatment is as follows: immerse the polyester-viscose fabric in the pretreatment working solution with a bath ratio of 1:(10-20), then heat it to 90-100°C at a rate of 1-3°C / min, keep it warm for 20-40min, then cool it to 50-70°C at a rate of 2-5°C / min, drain the liquid, add water for washing, with a bath ratio of 1:(10-20), and drain the liquid.
8. A one-bath dyeing process for polyester-viscose fabric according to claim 7, characterized in that: The pre-treatment working solution uses water as a solvent, and the solute of the pre-treatment working solution includes the following components: 2-5 g / L of desizing agent, 1-3 g / L of degreasing agent, and 0.3-1 g / L of chelating dispersant.
9. A one-bath dyeing process for polyester-viscose fabric according to claim 1, characterized in that: The dehydration and shaping process is as follows: drying and shaping the polyester-viscose fabric after one-bath dyeing at a temperature of 105-120° C. and a vehicle speed of 20-40 m / min.
10. A one-bath dyeing process for polyester-viscose fabric according to claim 1, characterized in that: The steaming method specifically includes steaming the polyester-viscose fabric after dehydration and setting for 20-40 minutes in a saturated steam atmosphere at a temperature of 120-130°C.