Early-strength high-toughness structure in-situ recycled asphalt pavement and construction method thereof
By adding water and high-viscosity modified emulsified asphalt to the asphalt recycling material, an early-strength high-strength cold regeneration structure layer is formed, and combined with hot mixing and heat-stirring high-strength ultra-thin asphalt wear layer, the asphalt is solved The high production cost of recycling pavement and the slow formation of early strength have been achieved, which has achieved the early opening and efficient utilization of asphalt pavement.
Patent Information
- Application Number
- CN202411177556.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-11-12
AI Technical Summary
In the prior art, the production cost of recycled pavement of asphalt recycling materials is high, and the early strength formation speed is slow, so it is impossible to achieve the early opening of asphalt pavement.
The construction method of in-situ regenerated asphalt pavement of early strength and high toughness structure is adopted. After milling, water and high viscosity modified emulsified asphalt are added to the asphalt recycling material, and early strength organic deemulsifier is added to form cold mixing and cold paving. The strong and high-tough asphalt regeneration mixture forms an early-strength high-tough cold regeneration structural layer after curing at room temperature, and combines hot mixing and heat to lay the high-tough ultra-thin asphalt wear layer to achieve rapid formation of early strength.
It reduces production costs, shortens construction cycles, improves the utilization rate of asphalt recycling materials, realizes the early opening of asphalt pavement, and improves the stability and crack resistance of pavement.
Smart Images

Figure BDA0005011133260000141 
Figure BDA0005011133260000151
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of road engineering construction, and in particular to an early-strength and high-toughness structure in-situ regenerated asphalt pavement and a construction method thereof. Background Art
[0002] In the field of traditional road engineering, the recycling of asphalt waste is an important challenge that needs to be solved urgently. With the acceleration of industrialization and the advancement of urbanization, the demand for road construction and maintenance is increasing, and the amount of asphalt waste (i.e. recycled asphalt) is also increasing. If the above-mentioned recycled asphalt is not properly handled and effectively utilized, it will not only cause a huge waste of resources, but also may cause serious pollution to the environment.
[0003] In order to alleviate the above-mentioned problems of resource waste and environmental pollution, the traditional process usually mixes asphalt recycling materials with new asphalt, new aggregates and other raw materials to obtain hot mix hot paving asphalt recycled mixture. Although the performance of hot mix hot paving asphalt recycled mixture is good, in the preparation process of hot mix hot paving asphalt recycled mixture, the old asphalt mixture needs to be heated to fully blend with new aggregates and new asphalt, which not only consumes a lot of energy, but also easily causes environmental pollution.
[0004] In order to overcome the defects of hot-mixed hot-laid asphalt recycled mixture, the prior art has a solution of mixing asphalt recycling materials with raw materials such as emulsified asphalt and aggregate to obtain cold-mixed cold-laid asphalt recycled mixture. However, due to the selection of materials, the early strength of the obtained cold-mixed cold-laid asphalt recycled mixture is low, and the early strength formation speed is slow, which makes it impossible to open the recycled asphalt pavement as soon as possible. In addition, the regenerated layer obtained after paving the cold-mixed cold-laid asphalt recycled mixture obtained by the conventional scheme can only be used as the base and lower layer of high-grade roads (such as expressways or first and second-class highways), or as the middle surface layer of low-grade roads, and cannot be used as the surface layer of low-grade roads. In general, a 3-5 cm thick hot-mixed hot-laid asphalt wear layer is required on the top of the asphalt pavement paved with the cold-mixed cold-laid asphalt recycled mixture to meet the use requirements of low-grade roads. The above method not only increases production costs due to the addition of a thicker wearing layer, but also increases construction time and maintenance time due to the slow strength formation time of the regenerated layer. It is impossible to form early strength as soon as possible, making it difficult to open the asphalt pavement as soon as possible. Summary of the invention
[0005] The purpose of the present invention is to propose a construction method for an early-strength and high-toughness structure in-situ regenerated asphalt pavement. The construction method is simple and easy to operate. It only needs to lay an early-strength and high-toughness cold regenerated structure layer to meet the use requirements of low-grade roads. On the premise of reducing production costs and improving the utilization rate of asphalt recycled materials, it is beneficial to accelerate the formation of early strength, realize the early opening of the in-situ regenerated asphalt pavement, and overcome the shortcomings of the prior art.
[0006] Another object of the present invention is to propose an early-strength and high-toughness in-situ regenerated asphalt pavement, which, under the premise of reducing production costs, is conducive to solving the technical problems in the prior art of high production cost of asphalt pavements obtained using recycled asphalt materials, slow early strength formation speed, and inability to realize early opening of in-situ regenerated asphalt pavements.
[0007] To achieve this object, the present invention adopts the following technical solutions:
[0008] A construction method for in-situ regeneration of an early-strength and high-toughness structured asphalt pavement comprises the following steps:
[0009] A. Milling the asphalt pavement to be regenerated to obtain asphalt recycled material, and adding water to the asphalt recycled material to obtain a first mixture;
[0010] Adding high-viscosity modified emulsified asphalt to the first mixed aggregate and mixing evenly to obtain a second mixed aggregate; wherein the high-viscosity modified emulsified asphalt has a PG grade of ≥PG82, an elastic recovery of ≥98% at 25°C, a composite shear modulus G* of ≥10KPa at 60°C, a dynamic viscosity of ≥30,000 Pa·s at 60°C, an evaporation residue G* / sinδ of ≥2.2kPa, and a critical temperature of ≥82°C;
[0011] Spraying an early-strength organic demulsifier into the second mixed aggregate, and mixing evenly to obtain a cold-mixed, cold-laid, early-strength, high-toughness asphalt recycled mixture;
[0012] B. Lay the cold-mixed and cold-laid early-strength and high-toughness asphalt recycled mixture on the top of the asphalt pavement after milling in step A. After reaching the preset elevation, roll it and maintain it at room temperature for 2 to 48 hours to form an early-strength and high-toughness cold-recycled structural layer with a thickness of 2 to 20 cm, and obtain an early-strength and high-toughness in-situ structural recycled asphalt pavement.
[0013] Furthermore, in step A, the molecular weight of the early strength organic demulsifier is 1000 to 10000.
[0014] Furthermore, in step A, the early-strength organic demulsifier includes at least one of a polyacrylamide copolymer, an acrylic acid copolymer and an acrylamide copolymer.
[0015] Further, in step A, the solid content of the high-viscosity modified emulsified asphalt is 62-65% by mass percentage;
[0016] The high-viscosity modified emulsified asphalt includes an SBS modifier, and the amount of the SBS modifier added is ≥ 3% by mass percentage;
[0017] The high-viscosity modified emulsified asphalt includes any one of star-shaped SBS high-viscosity modified emulsified asphalt and linear SBS high-viscosity modified emulsified asphalt.
[0018] Furthermore, in step A, calculated by weight, the cold-mixed, cold-laid, early-strength and high-toughness asphalt recycled mixture includes 92 to 105 parts of recycled asphalt, 1 to 6 parts of water, 1 to 6 parts of high-viscosity modified emulsified asphalt and 0.2 to 1 part of early-strength organic demulsifier.
[0019] Furthermore, in step B, the thickness of the early-strength and high-toughness cold-regenerated structural layer is 2 to 20 cm;
[0020] The 15°C splitting test strength of the early-strength and high-toughness cold-regenerated structural layer is ≥0.6MPa.
[0021] Furthermore, the method further comprises step C, and step C is after step B;
[0022] B. Paving the cold-mixed and cold-laid early-strength and high-toughness asphalt recycled mixture on the top of the asphalt pavement after milling in step A, rolling and curing at room temperature for 2 to 48 hours to form an early-strength and high-toughness cold recycled structural layer with a thickness of 2 to 20 cm;
[0023] C. Lay the hot-mixed and hot-laid high-toughness ultra-thin asphalt mixture on the top of the early-strength and high-toughness cold-regenerated structural layer. After reaching the preset elevation, it is rolled and cured at 185-190°C to form a high-toughness ultra-thin asphalt wear layer with a thickness of 0.8-2.0 cm, and obtain an early-strength and high-toughness in-situ structural recycled asphalt pavement.
[0024] Furthermore, in step C, the water permeability coefficient of the hot-mixed and hot-laid high-toughness ultra-thin asphalt mixture is ≤120ml / min, the dynamic stability is ≥5000 times, under the test conditions of 15°C and 1000με, the four-point bending fatigue life is ≥200,000 times, the Kentburgh scattering loss is ≤8%, the immersion Marshall residual stability ratio is ≥85%, the freeze-thaw splitting tensile strength ratio is ≥85%, and the low-temperature bending test failure strain at -10°C is ≥3800με.
[0025] Furthermore, calculated by weight, the hot-mixed, hot-laid, high-toughness, ultra-thin asphalt mixture includes 6.5 to 7.5 parts of high-viscosity, high-elasticity modified asphalt and 92.5 to 93.5 parts of mineral material;
[0026] The high-viscosity and high-elasticity modified asphalt has a softening point of ≥90°C, elastic recovery of ≥95%, a composite shear modulus G* of ≥10KPa at 60°C, and a dynamic viscosity of ≥400,000 Pa·s at 60°C;
[0027] Calculated by weight, the mineral material includes 40 to 55 parts of coarse aggregate of 2 to 20 mm, 15 to 25 parts of coarse aggregate of 3 to 5 mm, 25 to 35 parts of fine aggregate of 0 to 3 mm and 1 to 4 parts of limestone powder.
[0028] An early-strength and high-toughness in-situ regenerated asphalt pavement is prepared using the above-mentioned method for preparing an early-strength and high-toughness in-situ regenerated asphalt pavement.
[0029] The technical solution provided by the present invention may include the following beneficial effects:
[0030] 1. After the cold-mixed and cold-laid early-strength and high-toughness asphalt recycled mixture is cured at room temperature for 2 to 48 hours, an early-strength and high-toughness cold recycled structural layer can be obtained. The early strength of the early-strength and high-toughness cold recycled structural layer is formed quickly and has high early strength. There is no need to lay a high-toughness ultra-thin asphalt wear layer on the top to obtain an early-strength and high-toughness in-situ asphalt pavement, which is beneficial to accelerate the formation of early strength and realize the early opening of the asphalt pavement under the premise of reducing production costs.
[0031] 2. Early strength organic demulsifier can react with the water in high viscosity modified emulsified asphalt, causing the high viscosity modified emulsified asphalt to demulsify quickly at room temperature, adhere to the surface of the asphalt recycled material to form an asphalt film to wrap and bond the asphalt recycled material, so that the asphalt recycled mixture is bonded to form a whole, ensuring that the asphalt recycled mixture can form early strength after curing for 2 to 48 hours at room temperature, which is conducive to the early opening of the asphalt pavement. At the same time, since no cement is used, the asphalt recycled mixture will not become brittle during long-term use, and the low-temperature crack resistance will decrease, resulting in cracks in the asphalt pavement and a decrease in road performance. DETAILED DESCRIPTION
[0032] The present technical solution provides a construction method for an early-strength and high-toughness in-situ regenerated asphalt pavement, comprising the following steps:
[0033] A. Milling the asphalt pavement to be regenerated to obtain asphalt recycled material, and adding water to the asphalt recycled material to obtain a first mixture;
[0034] Adding high-viscosity modified emulsified asphalt to the first mixed aggregate and mixing evenly to obtain a second mixed aggregate; wherein the high-viscosity modified emulsified asphalt has a PG grade of ≥PG82, an elastic recovery of ≥98% at 25°C, a composite shear modulus G* of ≥10KPa at 60°C, a dynamic viscosity of ≥30,000 Pa·s at 60°C, an evaporation residue G* / sinδ of ≥2.2kPa, and a critical temperature of ≥82°C;
[0035] Spraying an early-strength organic demulsifier into the second mixed aggregate, and mixing evenly to obtain a cold-mixed, cold-laid, early-strength, high-toughness asphalt recycled mixture;
[0036] B. Lay the cold-mixed and cold-laid early-strength and high-toughness asphalt recycled mixture on the top of the asphalt pavement after milling in step A. After reaching the preset elevation, roll it and maintain it at room temperature for 2 to 48 hours to form an early-strength and high-toughness cold recycled structural layer, and obtain an early-strength and high-toughness in-situ structural recycled asphalt pavement.
[0037] In order to solve the technical problems in the prior art of high production cost of asphalt pavement obtained by using recycled asphalt materials, slow early strength formation speed, and inability to open the asphalt pavement as soon as possible, the present technical scheme proposes a construction method for an early-strength and high-toughness in-situ regenerated asphalt pavement. The prepared early-strength and high-toughness in-situ structure regenerated asphalt pavement includes a milled asphalt pavement (hereinafter referred to as "base layer"), an early-strength and high-toughness cold regenerated structural layer, and a high-toughness ultra-thin asphalt wear layer distributed in sequence from bottom to top.
[0038] Specifically, the early-strength and high-toughness cold-recycled structure layer can be obtained after the cold-mixed and cold-laid early-strength and high-toughness asphalt recycled mixture is cured at room temperature for 2 to 48 hours. The early-strength and high-toughness cold-recycled structure layer has a fast early strength formation rate and high early strength. It is not necessary to lay a high-toughness ultra-thin asphalt wear layer on top to obtain an early-strength and high-toughness in-situ asphalt pavement, which is conducive to accelerating the formation of early strength and realizing the early opening of the asphalt pavement under the premise of reducing production costs. At the same time, compared with the traditional repair scheme, the early-strength and high-toughness in-situ structure recycled asphalt pavement formed by this technical scheme is not only conducive to shortening the construction period, simplifying the construction process, and improving construction efficiency, but also conducive to achieving 100% recycling of asphalt recovery and improving its utilization efficiency.
[0039] It should be noted that, after the asphalt recycled material is milled, its surface voids are larger than those of conventional new aggregates, and its hygroscopicity is lower, which seriously affects the demulsification effect of the high-viscosity modified emulsified asphalt. Therefore, in the preparation process of the cold-mixed cold-laid early-strength high-toughness asphalt recycled mixture, the technical solution first adds water to the asphalt recycled material to obtain the first mixture, and uses water to wet the asphalt recycled material.
[0040] Secondly, since cement has strong hydrophilicity, it can absorb water in high-viscosity modified emulsified asphalt and react with the water in the high-viscosity modified emulsified asphalt to accelerate the demulsification process of the high-viscosity modified emulsified asphalt. Therefore, in the prior art, cement is usually added to the asphalt regeneration mixture to promote the accelerated formation of its early strength. However, since the hydration reaction of cement in high-viscosity modified emulsified asphalt takes time, and high-viscosity modified emulsified asphalt will inhibit the hydration reaction of cement to a certain extent, even if cement is added to the asphalt regeneration mixture, it will take 3 to 7 days to form early strength, which is not conducive to the early opening of the asphalt pavement. In addition, cement is also likely to cause a significant decrease in the fatigue performance and low-temperature cracking resistance of the asphalt cold regeneration mixture. Therefore, this technical solution cannot adopt the above principle. Therefore, in order to achieve rapid formation of early strength, the technical solution specifically selects early-strength organic demulsifiers to be added to the asphalt regeneration mixture formula. The early-strength organic demulsifier can react with the water in the high-viscosity modified emulsified asphalt, prompting the high-viscosity modified emulsified asphalt to quickly demulsify at room temperature, adhere to the surface of the asphalt recycled material to form an asphalt film to wrap and bond the asphalt recycled material, so that the asphalt recycled mixture is bonded to form a whole, ensuring that the asphalt recycled mixture can form early strength after curing for 2 to 48 hours at room temperature, which is conducive to the early opening of the asphalt pavement. At the same time, since cement is not used, it is avoided that the asphalt recycled mixture will become brittle during long-term use, and the low-temperature crack resistance will decrease, resulting in cracks in the asphalt pavement and a decrease in road performance.
[0041] Finally, since the asphalt recycling material is an aged asphalt mixture that has been used many times, the oil content in the asphalt recycling material is reduced, while the colloid and asphaltene content is increased, which reduces the viscosity of the asphalt recycling material, and the low-temperature crack resistance and toughness are both deteriorated. When ordinary modified emulsified asphalt is used, it is easy to have insufficient adhesion to the asphalt recycling material, so this scheme specifically uses high-viscosity modified emulsified asphalt to ensure the performance of the asphalt recycling mixture. This scheme uses PG grade ≥ PG82, 25℃ elastic recovery ≥ 98%, 60℃ composite shear modulus G* ≥ 10KPa, 60℃ dynamic viscosity ≥ 30,000 Pa·s, evaporation residue G* / sinδ ≥ 2.2kPa, and critical temperature ≥ 82℃ as raw materials, which is conducive to improving the adhesion of high-viscosity modified emulsified asphalt to the asphalt recycling material, thereby giving the asphalt recycling mixture high temperature stability, high crack resistance and high toughness and other properties, and increasing the stability of the road surface.
[0042] This technical solution, through the mutual coordination of asphalt recycled materials, water, high-viscosity modified emulsified asphalt and early-strength organic demulsifier, endows the cold-mixed and cold-laid early-strength and high-toughness asphalt recycled mixture with properties such as high-temperature stability, high crack resistance and high toughness. The early-strength and high-toughness cold recycled structural layer formed by curing the cold-mixed and cold-laid early-strength and high-toughness asphalt recycled mixture directly on the surface of the base layer can meet the use requirements of low-grade roads. This overcomes the technical defect in the prior art that the cold-mixed and cold-laid asphalt recycled mixture can only be used as the base layer and lower layer of high-grade highways, or as the middle surface layer of low-grade pavements, but cannot be used as the surface layer of low-grade roads. This increases its road performance and is conducive to the early opening of asphalt pavements.
[0043] It should be noted that low-grade roads refer to third- and fourth-class highways, urban secondary roads, branch roads, rural roads, or roads that meet the speed limit of 60km / h. In addition, according to the use requirements, the thickness of the early-strength and high-toughness cold-regenerated structural layer can be selected within the range of 2 to 20cm, so the maintenance time is also determined according to the thickness of the regenerated layer, which is 2 to 48h. In addition, the preset elevation refers to the setting of a preset total height for the early-strength and high-toughness in-situ structural regenerated asphalt pavement, so that after laying the early-strength and high-toughness cold-regenerated structural layer, the in-situ structural regenerated asphalt pavement obtained reaches the above height.
[0044] Further, in step A, the molecular weight of the early strength organic demulsifier is 1000-10000.
[0045] When the molecular weight of the early-strength organic demulsifier is lower than 1000, the degree of polymerization of the early-strength organic demulsifier is low, and its addition amount needs to be increased to achieve the specified demulsification effect, but too high an addition amount will further affect the porosity and strength of the asphalt recycled mixture; when the molecular weight of the early-strength organic demulsifier is higher than 10000, the degree of polymerization of the early-strength organic demulsifier is high, and its addition amount needs to be reduced to achieve the specified demulsification effect, but too low an addition amount makes it difficult to evenly disperse it in the interior of the asphalt recycled mixture during the mixing process, thereby affecting the strength of the asphalt recycled mixture.
[0046] Further, in step A, the early strength organic demulsifier includes at least one of a polyacrylamide copolymer, an acrylic acid copolymer and an acrylamide copolymer.
[0047] Since the copolymer acrylic acid contains a hydrophilic group carboxyl, and the acrylamide copolymer and the polyacrylamide copolymer both contain a hydrophilic group amide, it is beneficial to give the early-strength organic demulsifier good hydrophilicity, and react with the water in the high-viscosity modified emulsified asphalt, promote the water consumption in the high-viscosity modified emulsified asphalt, destroy the stable emulsified structure in the high-viscosity modified emulsified asphalt, and further promote the high-viscosity modified emulsified asphalt to quickly demulsify and form strength, so as to increase the speed of early strength formation. In addition, in the later curing process, the early-strength organic demulsifier can better form a continuous and stable membrane structure with the asphalt recycled material, further enhancing the continuity and stability of the asphalt recycled mixture structure at the microscopic scale, thereby ensuring the early strength of the asphalt recycled mixture.
[0048] Further, in step A, the solid content of the high-viscosity modified emulsified asphalt is 62-65% by mass percentage;
[0049] The high-viscosity modified emulsified asphalt includes an SBS modifier, and the amount of the SBS modifier added is ≥ 3% by mass percentage;
[0050] The high-viscosity modified emulsified asphalt includes any one of star-shaped SBS high-viscosity modified emulsified asphalt and linear SBS high-viscosity modified emulsified asphalt.
[0051] According to the mass percentage, the solid content of high-viscosity modified emulsified asphalt is 62-65%, which further improves the viscoelastic properties of high-viscosity modified emulsified asphalt, thereby further improving the early strength of the asphalt mixture and further improving its road performance. If the solid content of the modified asphalt is not within this range, the emulsification performance, stability, viscosity and high temperature performance of the high-viscosity modified emulsified asphalt will be affected, thereby affecting the road performance of the asphalt pavement formed by the asphalt mixture, such as anti-rutting and anti-cracking.
[0052] Furthermore, when the addition amount of SBS modifier is ≥3%, it can effectively improve the high temperature performance and toughness of asphalt recycled mixture, and give the asphalt recycled mixture better road performance such as anti-rutting, anti-cracking, anti-fatigue and anti-water damage. In addition, when the addition amount of SBS modifier is ≥3%, it is conducive to providing sufficient viscosity for high-viscosity modified emulsified asphalt, making it more encapsulating and bonding to asphalt recycled materials, further improving the performance of asphalt recycled mixture.
[0053] Furthermore, the high-viscosity modified emulsified asphalt includes any one of the star-shaped SBS high-viscosity modified emulsified asphalt or the linear SBS high-viscosity modified emulsified asphalt. The star-shaped SBS high-viscosity modified emulsified asphalt or the linear SBS high-viscosity modified emulsified asphalt can not only adhere to the surface of the asphalt recycled material at room temperature to form an asphalt film to wrap and bond the asphalt recycled material, so that the asphalt recycled mixture is bonded to form a whole, ensuring that the asphalt recycled mixture has good early strength, but also has excellent viscoelastic properties, further improving the early strength of the asphalt recycled mixture, thereby improving its road performance.
[0054] Further explanation, step A, calculated by weight, the cold-mixed, cold-laid, early-strength and high-toughness asphalt recycled mixture includes 92 to 105 parts of recycled asphalt, 1 to 6 parts of water, 1 to 6 parts of high-viscosity modified emulsified asphalt and 0.2 to 1 part of early-strength organic demulsifier.
[0055] In this technical solution, by optimizing the addition amount of each raw material in the asphalt recycled mixture, the addition amount of asphalt recycled materials in the asphalt recycled mixture exceeds 85% while ensuring the relevant performance of the asphalt recycled mixture, which is conducive to further reducing production costs.
[0056] Further, in step B, the thickness of the early-strength and high-toughness cold-regenerated structural layer is 2 to 20 cm;
[0057] The 15°C splitting test strength of the early-strength and high-toughness cold-regenerated structural layer is ≥0.6MPa.
[0058] In the prior art, the thickness of the middle surface layer is generally 4 to 18 cm. The technical solution optimizes the thickness of the early-strength and high-toughness cold recycled structural layer, which is beneficial to ensuring the early strength formation speed of the asphalt recycled mixture and the compaction during rolling, thereby being more conducive to ensuring the performance of the early-strength and high-toughness cold recycled structural layer.
[0059] In addition, the technical solution optimizes the 15°C splitting test strength of the early-strength and high-toughness cold regenerated structural layer, which is beneficial to ensure that the performance of the early-strength and high-toughness cold regenerated structural layer meets the relevant standards before laying the high-toughness ultra-thin asphalt wear layer, thereby ensuring the performance of the resulting asphalt pavement.
[0060] Further description, step C is also included, and step C is located after step B;
[0061] B. Paving the cold-mixed and cold-laid early-strength and high-toughness asphalt recycled mixture on the top of the asphalt pavement after milling in step A, rolling and curing at room temperature for 2 to 48 hours to form an early-strength and high-toughness cold recycled structural layer;
[0062] C. Lay the hot-mixed and hot-laid high-toughness ultra-thin asphalt mixture on the top of the early-strength and high-toughness cold-regenerated structural layer. After reaching the preset elevation, it is rolled and cured at 185-190°C to form a high-toughness ultra-thin asphalt wear layer with a thickness of 0.8-2.0 cm, and obtain an early-strength and high-toughness in-situ structural recycled asphalt pavement.
[0063] The high-toughness ultra-thin asphalt wear layer is an asphalt pavement surface layer technology that combines asphalt mixture with a high-viscosity modified emulsified asphalt adhesive layer. It can efficiently and reliably solve diseases such as medium and light cracks, loose pavement and anti-skid failure, and restore the road surface structural depth and anti-skid ability. In order to enable the asphalt pavement to meet the use requirements of higher-demand asphalt pavements, this technical solution sets a high-toughness ultra-thin asphalt wear layer on the top of the early-strength high-toughness cold-regenerated structural layer. Since the early strength of the early-strength high-toughness cold-regenerated structural layer is formed quickly and has a high early strength, the high-toughness ultra-thin asphalt wear layer only needs to be laid 0.8 to 2.0 cm before it can be put into use. Compared with the existing technology of re-laying a 3 to 5 cm thick hot-mixed hot-laid asphalt wear layer, its laying thickness is greatly reduced, which is conducive to reducing production costs. At the same time, since the thickness of the high-toughness ultra-thin asphalt wear layer is extremely thin, the high-toughness ultra-thin asphalt wear layer can be completed in a relatively short time, the construction speed is extremely fast, and the interference with traffic is reduced, which is also conducive to the early opening of the asphalt pavement. In addition, since the high-toughness and ultra-thin asphalt wear layer is paved with hot-mixed and hot-laid high-toughness and ultra-thin asphalt mixture, and when the temperature of the hot-mixed and hot-laid high-toughness and ultra-thin asphalt mixture drops below 50°C, it can be opened to traffic, which is conducive to accelerating the opening of in-situ regenerated asphalt pavement.
[0064] In addition, the technical solution can meet the use requirements of low-grade roads through the early-strength and high-toughness cold recycled structural layer, or can meet the use requirements of high-grade roads by laying a high-toughness ultra-thin asphalt wear layer on the top of the early-strength and high-toughness cold recycled structural layer. The specific solution to be used can be adjusted according to actual conditions, which increases the flexibility of the solution.
[0065] It should be noted that when it is necessary to add a high-toughness ultra-thin asphalt wear layer, the asphalt pavement to be regenerated can be milled to a corresponding depth according to actual needs, so that after laying the early-strength high-toughness cold-regenerated structural layer and the high-toughness ultra-thin asphalt wear layer, the preset elevation can still be reached.
[0066] It should be noted that the temperature during the laying of the hot-mixed and hot-laid high-toughness ultra-thin asphalt mixture in this technical solution is 185-200°C.
[0067] It is further specified that in step C, the water permeability coefficient of the hot-mixed and hot-laid high-toughness ultra-thin asphalt mixture is ≤120ml / min, the dynamic stability is ≥5000 times, under the test conditions of 15°C and 1000με, the four-point bending fatigue life is ≥200,000 times, the Kentburgh scattering loss is ≤8%, the immersion Marshall residual stability ratio is ≥85%, the freeze-thaw splitting tensile strength ratio is ≥85%, and the low-temperature bending test failure strain at -10°C is ≥3800με.
[0068] This technical solution optimizes the performance of hot-mixed and hot-laid high-toughness and ultra-thin asphalt mixture, which is beneficial to ensure the road performance of the high-toughness and ultra-thin asphalt wear layer obtained by paving the hot-mixed and hot-laid high-toughness and ultra-thin asphalt mixture, so that even if the laying thickness of the high-toughness and ultra-thin asphalt wear layer is only 0.8 to 2.0 cm, it can meet the actual road use requirements of high-grade highways.
[0069] Further explanation: calculated by weight, the hot-mixed and hot-laid high-toughness ultra-thin asphalt mixture includes 6.5-7.5 parts of high-viscosity and high-elasticity modified asphalt and 92.5-93.5 parts of mineral material;
[0070] The high-viscosity and high-elasticity modified asphalt has a softening point of ≥90°C, elastic recovery of ≥95%, a composite shear modulus G* of ≥10KPa at 60°C, and a dynamic viscosity of ≥400,000 Pa·s at 60°C;
[0071] Calculated by weight, the mineral material includes 40 to 55 parts of coarse aggregate of 2 to 20 mm, 15 to 25 parts of coarse aggregate of 3 to 5 mm, 25 to 35 parts of fine aggregate of 0 to 3 mm and 1 to 4 parts of limestone powder.
[0072] The 2-20mm coarse aggregate acts as a skeleton, providing the main bearing capacity and stability; the 3-5mm coarse aggregate further fills the gaps between the skeletons, improving the density and strength; the 0-3mm fine aggregate mainly fills the smaller gaps, further improving the density and helping to improve the ease of construction; the limestone powder is used as a filler to increase the adhesion between the high-viscosity and high-elasticity modified asphalt and the aggregate, improving the overall performance of the mixture. This technical solution is conducive to ensuring the performance of high-toughness ultra-thin asphalt mixture by optimizing the raw materials and their addition amounts in the mineral material.
[0073] Furthermore, the technical solution adopts high-performance high-viscosity and high-elastic modified asphalt to add to the high-toughness ultra-thin asphalt mixture formula, which is beneficial to give the high-toughness ultra-thin asphalt mixture excellent high-temperature stability, elastic recovery ability and shear resistance, making it suitable for occasions with higher requirements for road performance.
[0074] An early-strength and high-toughness in-situ regenerated asphalt pavement is prepared using the above-mentioned method for preparing an early-strength and high-toughness in-situ regenerated asphalt pavement.
[0075] The scheme proposes an early-strength and high-toughness in-situ structure regenerated asphalt pavement prepared by a preparation method of an early-strength and high-toughness in-situ structure regenerated asphalt pavement, which is conducive to solving the technical problems in the prior art of high production cost of asphalt pavements obtained using recycled asphalt materials, slow early strength formation speed, and inability to realize early opening of asphalt pavements.
[0076] The technical solution of the present invention is further illustrated below through specific implementation methods.
[0077] Example 1
[0078] In this embodiment, the cold-mixed cold-laid early-strength high-toughness asphalt recycled mixture includes 95 parts of asphalt recycling material, 2 parts of water, 4 parts of star-shaped SBS high-viscosity modified emulsified asphalt, and 0.5 parts of polyacrylamide copolymer with a molecular weight of 2400; wherein the star-shaped SBS high-viscosity modified emulsified asphalt has a 60°C dynamic viscosity of 40,000 Pa·s, a 25°C elastic recovery of 98%, a 60°C composite shear modulus G* of 12KPa, an evaporation residue G* / sinδ of 2.5kPa, a critical temperature of 82°C, a solid content of the star-shaped SBS high-viscosity modified emulsified asphalt of 62.7%, and an addition amount of the modifier of 5%;
[0079] In this embodiment, a construction method for in-situ regeneration of an early-strength and high-toughness structure asphalt pavement comprises the following steps:
[0080] A. Milling the asphalt pavement to be regenerated to obtain recycled asphalt material, and adding water to the recycled asphalt material during the milling process to obtain a first mixture;
[0081] Adding the star-shaped SBS high-viscosity modified emulsified asphalt into the first mixed aggregate and mixing them evenly to obtain a second mixed aggregate;
[0082] Spraying a polyacrylamide copolymer with a molecular weight of 2400 into the second mixed aggregate, and mixing evenly to obtain a cold-mixed, cold-laid, early-strength, high-toughness asphalt recycled mixture;
[0083] B. Lay the cold-mixed and cold-laid early-strength and high-toughness asphalt recycled mixture on the top of the asphalt pavement after milling in step A. After reaching the preset elevation, roll it and maintain it at room temperature for 3 hours to form an early-strength and high-toughness cold-recycled structural layer with a thickness of 7 cm and a 15°C splitting test strength of 0.6 MPa, and obtain an early-strength and high-toughness in-situ structural recycled asphalt pavement.
[0084] Example 2
[0085] In this embodiment, the cold-mixed cold-laid early-strength high-toughness asphalt recycled mixture includes 100 parts of asphalt recycling material, 3 parts of water, 6 parts of linear SBS high-viscosity modified emulsified asphalt, and 0.4 parts of an acrylic copolymer with a molecular weight of 4500; wherein the linear SBS high-viscosity modified emulsified asphalt has a 60°C dynamic viscosity of 35,000 Pa·s, a 25°C elastic recovery of 98%, a 60°C composite shear modulus G* of 10KPa, an evaporation residue G* / sinδ of 2.2kPa, a critical temperature of 82°C, a solid content of the linear SBS high-viscosity modified emulsified asphalt of 62.4%, and an amount of the modifier added of 3%;
[0086] Calculated by weight, the hot-mixed, hot-laid, high-toughness, ultra-thin asphalt mixture includes 7 parts of high-viscosity, high-elasticity modified asphalt and 93 parts of mineral materials; among them, the high-viscosity, high-elasticity modified asphalt has a softening point of 95°C, an elastic recovery of 95%, a composite shear modulus G* of 10KPa at 60°C, and a dynamic viscosity of 450,000 Pa·s at 60°C; calculated by weight, the mineral materials include 50 parts of 2-20mm diabase crushed stone, 20 parts of 3-5mm diabase crushed stone, and 0-3mm limestone machine 25 parts of made sand and 4 parts of limestone powder; the water permeability coefficient of the hot-mixed and hot-laid high-toughness ultra-thin asphalt mixture is 43ml / min, the dynamic stability is 9127 times, under the test conditions of 15℃ and 1000με, the four-point bending fatigue life is 681.203 million times, the Kentucky Fort flying loss is 2.4%, the immersion Marshall residual stability ratio is 92.3%, the freeze-thaw splitting tensile strength ratio is 91.2%, and the low-temperature bending test failure strain at -10℃ is 4200με.
[0087] In this embodiment, a construction method for in-situ regeneration of an early-strength and high-toughness structure asphalt pavement comprises the following steps:
[0088] A. Milling the asphalt pavement to be regenerated to obtain recycled asphalt material, and adding water to the recycled asphalt material during the milling process to obtain a first mixture;
[0089] Adding the star-shaped SBS high-viscosity modified emulsified asphalt into the first mixed aggregate and mixing them evenly to obtain a second mixed aggregate;
[0090] Spraying an acrylic copolymer with a molecular weight of 4500 into the second mixed aggregate, and mixing evenly to obtain a cold-mixed, cold-laid, early-strength, high-toughness asphalt recycled mixture;
[0091] B. The cold-mixed and cold-laid early-strength and high-toughness asphalt recycled mixture is laid on the top of the asphalt pavement after milling in step A. After reaching the preset elevation, it is rolled and cured at room temperature for 2 hours to form an early-strength and high-toughness cold recycled structural layer with a thickness of 5 cm and a 15°C splitting test strength of 0.6 MPa;
[0092] C. Lay the hot-mixed and hot-laid high-toughness ultra-thin asphalt mixture on the top of the early-strength and high-toughness cold-regenerated structural layer. After reaching the preset elevation, it is rolled and cured at 185°C to form a high-toughness ultra-thin asphalt wear layer with a thickness of 1.5 cm, and obtain an early-strength and high-toughness in-situ structural recycled asphalt pavement.
[0093] Example 3
[0094] In this embodiment, the cold-mixed cold-laid early-strength high-toughness asphalt recycled mixture includes 105 parts of asphalt recycling material, 2.5 parts of water, 6 parts of star-shaped SBS high-viscosity modified emulsified asphalt, and 0.3 parts of acrylamide copolymer with a molecular weight of 7200; wherein the star-shaped SBS high-viscosity modified emulsified asphalt has a 60°C dynamic viscosity of 30,000 Pa·s, a 25°C elastic recovery of 98%, a 60°C composite shear modulus G* of 10KPa, an evaporation residue G* / sinδ of 2.2kPa, a critical temperature of 82°C, a solid content of the star-shaped SBS high-viscosity modified emulsified asphalt of 64.2%, and an addition amount of the modifier of 8%;
[0095] Calculated by weight, the hot-mixed, hot-laid, high-toughness, ultra-thin asphalt mixture includes 7.5 parts of high-viscosity, high-elasticity modified asphalt and 92.5 parts of mineral materials; among them, the high-viscosity, high-elasticity modified asphalt has a softening point of 90°C, an elastic recovery of 95%, a composite shear modulus G* of 10KPa at 60°C, and a dynamic viscosity of 400,000 Pa·s at 60°C; calculated by weight, the mineral materials include 55 parts of 2-20mm diabase crushed stone, 15 parts of 3-5mm diabase crushed stone, and 0-3mm stone crushed stone. 35 parts of limestone machine-made sand and 4 parts of limestone mineral powder; the water permeability coefficient of hot-mixed and hot-laid high-toughness ultra-thin asphalt mixture is 47ml / min, the dynamic stability is 9349 times, under the test conditions of 15℃ and 1000με, the four-point bending fatigue life is 670523 times, the Kentucky Fort flying loss is 2.5%, the immersion Marshall residual stability ratio is 91.1%, the freeze-thaw splitting tensile strength ratio is 90.8%, and the low-temperature bending test failure strain at -10℃ is 4300με.
[0096] In this embodiment, a construction method for in-situ regeneration of an early-strength and high-toughness structure asphalt pavement comprises the following steps:
[0097] A. Milling the asphalt pavement to be regenerated to obtain recycled asphalt material, and adding water to the recycled asphalt material during the milling process to obtain a first mixture;
[0098] Adding the star-shaped SBS high-viscosity modified emulsified asphalt into the first mixed aggregate and mixing them evenly to obtain a second mixed aggregate;
[0099] Spraying acrylamide copolymer with a molecular weight of 7200 into the second mixed aggregate, and mixing evenly to obtain a cold-mixed and cold-laid early-strength and high-toughness asphalt recycled mixture;
[0100] B. Pave the cold-mixed and cold-laid early-strength and high-toughness asphalt recycled mixture on the top of the asphalt pavement after milling in step A, roll it and cure it at room temperature for 6 hours to form an early-strength and high-toughness cold recycled structural layer with a thickness of 10 cm and a 15°C splitting test strength of 0.6 MPa;
[0101] C. Lay the hot-mixed and hot-laid high-toughness ultra-thin asphalt mixture on the top of the early-strength and high-toughness cold-regenerated structural layer. After reaching the preset elevation, it is rolled and cured at 190°C to form a high-toughness ultra-thin asphalt wear layer with a thickness of 0.8 cm, and obtain an early-strength and high-toughness in-situ structural recycled asphalt pavement.
[0102] Comparative Example 1
[0103] Comparative Example 1 has the same preparation method and raw materials as Example 1, except that the cold-mixed cold-laid early-strength high-toughness asphalt regeneration mixture in Comparative Example 1 adopts a conventional cold-mixed cold-laid asphalt regeneration mixture. That is, calculated by weight, the cold-mixed cold-laid asphalt regeneration mixture includes 91.5 parts of asphalt recycling material, 2.6 parts of water, 4.5 parts of ordinary modified emulsified asphalt and 1.4 parts of PO42.5 cement.
[0104] The asphalt pavements prepared by the implementation methods of Examples 1-3 and Comparative Example 1 were tested for relevant properties according to the standards specified in the "Test Procedures for Asphalt and Asphalt Mixtures in Highway Engineering" (JTG E20-2011), and the results are shown in Table 1 below:
[0105] Table 1 Related performance test results of in-situ regenerated asphalt pavement
[0106]
[0107]
[0108] From the performance test results in Table 1, it can be seen that the asphalt pavement obtained by this technical solution meets the standards for the opening of asphalt pavements specified in the "Test Procedures for Asphalt and Asphalt Mixtures in Highway Engineering" (JTG E20-2011). On the premise of reducing production costs and improving the utilization rate of recycled asphalt materials, it is beneficial to accelerate the formation of early strength and realize the early opening of the asphalt pavement, so as to overcome the shortcomings of the existing technology.
[0109] In Comparative Example 1, due to the use of conventional cold-mixed and cold-laid asphalt recycled mixture, it cannot quickly form early strength, and the recycled layer obtained after paving the conventional cold-mixed and cold-laid asphalt recycled mixture can only be used as the base layer and lower layer of high-grade roads, and cannot be used as the surface layer of low-grade roads. The obtained in-situ regenerated asphalt pavement does not meet the asphalt pavement opening standards specified in the "Test Procedures for Asphalt and Asphalt Mixtures for Highway Engineering" (JTG E20-2011), and cannot meet the use requirements.
[0110] The technical principle of the present invention is described above in conjunction with specific embodiments. These descriptions are only for explaining the principle of the present invention and cannot be interpreted as limiting the scope of protection of the present invention in any way. Based on the explanations herein, those skilled in the art can associate other specific implementations of the present invention without paying creative labor, and these methods will fall within the scope of protection of the present invention.
Claims
1. A construction method for in-situ regeneration of asphalt pavement with early strength and high toughness structure, It is characterized in that The following steps are involved: A. Milling the asphalt pavement to be regenerated to obtain asphalt recycled material, and adding water to the asphalt recycled material to obtain a first mixture; Adding high-viscosity modified emulsified asphalt to the first mixed aggregate and mixing evenly to obtain a second mixed aggregate; wherein the high-viscosity modified emulsified asphalt has a PG grade of ≥PG82, an elastic recovery of ≥98% at 25°C, a composite shear modulus G* of ≥10KPa at 60°C, a dynamic viscosity of ≥30,000 Pa·s at 60°C, an evaporation residue G* / sinδ of ≥2.2kPa, and a critical temperature of ≥82°C; Spraying an early-strength organic demulsifier into the second mixed aggregate, and mixing evenly to obtain a cold-mixed, cold-laid, early-strength, high-toughness asphalt recycled mixture; B. Lay the cold-mixed and cold-laid early-strength and high-toughness asphalt recycled mixture on the top of the asphalt pavement after milling in step A. After reaching the preset elevation, roll it and maintain it at room temperature for 2 to 48 hours to form an early-strength and high-toughness cold-recycled structural layer with a thickness of 2 to 20 cm, and obtain an early-strength and high-toughness in-situ structural recycled asphalt pavement.
2. The construction method of an early-strength and high-toughness structure in-situ regenerated asphalt pavement according to claim 1, It is characterized in that In step A, the molecular weight of the early strength organic demulsifier is 1000-10000.
3. The construction method of an early-strength and high-toughness structure in-situ regenerated asphalt pavement according to claim 1, It is characterized in that In step A, the early-strength organic demulsifier includes at least one of a polyacrylamide copolymer, an acrylic acid copolymer and an acrylamide copolymer.
4. The construction method of an early-strength and high-toughness structure in-situ regenerated asphalt pavement according to claim 1, It is characterized in that In step A, the solid content of the high-viscosity modified emulsified asphalt is 62-65% by mass percentage; The high-viscosity modified emulsified asphalt includes an SBS modifier, and the amount of the SBS modifier added is ≥ 3% by mass percentage; The high-viscosity modified emulsified asphalt includes any one of star-shaped SBS high-viscosity modified emulsified asphalt and linear SBS high-viscosity modified emulsified asphalt.
5. The construction method of an early-strength and high-toughness structure in-situ regenerated asphalt pavement according to claim 1, It is characterized in that Step A, calculated by weight, the cold-mixed, cold-laid, early-strength, high-toughness asphalt recycled mixture includes 92 to 105 parts of recycled asphalt, 1 to 6 parts of water, 1 to 6 parts of high-viscosity modified emulsified asphalt, and 0.2 to 1 part of early-strength organic demulsifier.
6. The construction method of an early-strength and high-toughness structure in-situ regenerated asphalt pavement according to claim 1, It is characterized in that In step B, the thickness of the early-strength and high-toughness cold-regenerated structural layer is 2 to 20 cm; The 15°C splitting test strength of the early-strength and high-toughness cold-regenerated structural layer is ≥0.6MPa.
7. The construction method of an early-strength and high-toughness structure in-situ regenerated asphalt pavement according to claim 1, It is characterized in that The method further comprises step C, wherein step C is after step B; B. Paving the cold-mixed and cold-laid early-strength and high-toughness asphalt recycled mixture on the top of the asphalt pavement after milling in step A, rolling and curing at room temperature for 2 to 48 hours to form an early-strength and high-toughness cold recycled structural layer with a thickness of 2 to 20 cm; C. Lay the hot-mixed and hot-laid high-toughness ultra-thin asphalt mixture on the top of the early-strength and high-toughness cold-regenerated structural layer. After reaching the preset elevation, it is rolled and cured at 185-190°C to form a high-toughness ultra-thin asphalt wear layer with a thickness of 0.8-2.0 cm, and obtain an early-strength and high-toughness in-situ structural recycled asphalt pavement.
8. The construction method of the in-situ regeneration asphalt pavement with early strength and high toughness structure according to claim 7, It is characterized in that In step C, the water permeability coefficient of the hot-mixed and hot-laid high-toughness ultra-thin asphalt mixture is ≤120ml / min, the dynamic stability is ≥5000 times, under the test conditions of 15°C and 1000με, the four-point bending fatigue life is ≥200,000 times, the Kentburgh scattering loss is ≤8%, the immersion Marshall residual stability ratio is ≥85%, the freeze-thaw splitting tensile strength ratio is ≥85%, and the low-temperature bending test failure strain at -10°C is ≥3800με.
9. The construction method of the in-situ regeneration asphalt pavement with early strength and high toughness structure according to claim 7, It is characterized in that Calculated by weight, the hot-mixed, hot-laid, high-toughness, ultra-thin asphalt mixture includes 6.5 to 7.5 parts of high-viscosity, high-elasticity modified asphalt and 92.5 to 93.5 parts of mineral material; The high-viscosity and high-elasticity modified asphalt has a softening point of ≥90°C, elastic recovery of ≥95%, a composite shear modulus G* of ≥10KPa at 60°C, and a dynamic viscosity of ≥400,000 Pa·s at 60°C; Calculated by weight, the mineral material includes 40 to 55 parts of coarse aggregate of 2 to 20 mm, 15 to 25 parts of coarse aggregate of 3 to 5 mm, 25 to 35 parts of fine aggregate of 0 to 3 mm and 1 to 4 parts of limestone powder.
10. An early-strength and high-toughness in-situ regenerated asphalt pavement. It is characterized in that The asphalt pavement is prepared by the method for preparing the early-strength and high-toughness in-situ structure regenerated asphalt pavement as described in any one of claims 1 to 9.
Citation Information
Patent Citations
Cold-mixed and cold-paved asphalt mixture, preparation method thereof and asphalt pavement
CN111718166A
Early-strength anti-loosening emulsified asphalt cold-recycled mixture and preparation method thereof
CN112694287A
Emulsifier type cold-mixed and cold-laid asphalt mixture and preparation method thereof
CN116789393A
Road asphalt pavement surface layer polymorphic asphalt in-situ cold recycling construction method
CN117306339A
Method for producing bitumen compositions
US20080060551A1
Cited By
Multi-dimensional active curing method for paving cold-mixed emulsified asphalt thin layer
CN121205054A