Method for rapidly stripping inner electrode of MLCC
By placing the MLCC in a salt solution and stripping the inner electrode with a DC power supply, the difficulties in observing and evaluating the MLCC internal electrode in the prior art are solved, and the rapid, safe and accurate stripping and detection of the internal electrode is achieved, which is suitable for a variety of purposes Specifications and models MLCC.
Patent Information
- Application Number
- CN202411015238.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-12
AI Technical Summary
It is difficult for the prior art to effectively observe and evaluate the actual situation of MLCC internal electrodes, especially to obtain a complete internal electrode structure and calculate its coverage. The traditional method has limited applicability to different specifications and models, and there are operational difficulties and safety risks.
The MLCC is placed in a salt solution, and the voltage is adjusted by DC power supply to separate the inner electrode from the dielectric layer. The inner electrode is peeled off by gas expansion effect, and the complete structure is obtained by sandpaper grinding and microscopy observation.
It realizes fast, safe and reliable peeling of the inner electrodes of MLCC, and can observe the holes and coverage of the inner electrodes. It is suitable for MLCC of different specifications and models, simplifies the operation process and improves the accuracy and safety of detection.
Smart Images

Figure HDA0004965504740000011 
Figure HDA0004965504740000012 
Figure HDA0004965504740000013
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of electronic material detection and relates to a method for quickly stripping an inner electrode of an MLCC. Background Art
[0002] Multilayer ceramic capacitors (MLCCs), as a key electronic component, have important applications in consumer electronics, communications, industry, automotive, aerospace, and other fields. MLCCs, with their small size, high specific capacitance, and high precision, align with the trend toward miniaturization and lightweighting in consumer electronics, and account for over 90% of the ceramic capacitor market.
[0003] MLCCs are constructed by stacking ceramic dielectric diaphragms with printed electrodes (internal electrodes) alternately, calcining at high temperatures, and then sealing them with metal layers (terminal electrodes) at both ends. In other words, MLCCs consist of three components: ceramic dielectric layers, internal electrodes, and terminal electrodes. In recent years, MLCCs have developed towards miniaturization, higher capacity, and higher reliability. The MLCC capacitance calculation formula shows that capacitance is positively correlated with the area facing the internal electrodes. For MLCCs of the same specifications and size, the larger the area facing the internal electrodes, the higher the capacitance. Furthermore, the quality of the internal electrodes significantly impacts MLCC reliability. Therefore, testing and evaluating MLCC internal electrodes is crucial. Currently, there are two common methods for inspecting the internal electrodes of MLCCs: one is to grind and polish the ends or sides of the MLCC and then observe the continuity and morphology of the internal electrodes under a microscope. This method can only observe a portion of the internal electrode, and because the internal electrode is usually a mesh structure, the observed continuity of the internal electrode varies with the grinding depth. The other method is to grind and polish the top / bottom of the MLCC to observe the planar state of the internal electrode. However, because the internal electrode layer is relatively thin (about a few microns), the operation is difficult, time-consuming, and it is difficult to obtain the overall structure. Both of the above methods have limitations, making it difficult to observe the actual situation of the internal electrode and to calculate the actual coverage of the internal electrode. CN 103397374A discloses a method for stripping the nickel electrodes inside ceramic capacitors. This patent can only be used for ceramic capacitors with nickel internal electrodes. Its principle is to use the reduction reaction of NiO. It cannot be used for ceramic capacitors with internal electrodes such as Ag / Pd or Cu, and the alkaline solution used is also dangerous. TW 202220271 A discloses a method for recycling battery electrodes. This method is suitable for batteries with polymer electrode materials and cannot be applied to MLCCs.
[0004] Based on the above background, in order to observe the actual situation of the internal electrodes of MLCC, the present invention proposes a method for quickly stripping the internal electrodes of MLCC. Summary of the Invention
[0005] In order to overcome the defects of the existing technology, the present invention provides a method for quickly stripping the internal electrodes of MLCC, which can be used to strip the internal electrodes of MLCCs of different specifications and models to obtain a complete internal electrode structure.
[0006] In order to achieve the above object, the present invention adopts the following technical solution: a method for quickly stripping the inner electrode of MLCC, comprising the following steps:
[0007] Place the MLCC with all four sides of the inner electrodes exposed in a saline solution;
[0008] Using two ejector pin electrodes, the salt solution and the MLCC inner electrode are connected to the positive and negative electrodes of a DC power supply respectively;
[0009] Turn on the DC power supply and adjust the voltage until the MLCC inner electrode is separated from the dielectric layer; specifically, the MLCC inner electrode layer in the salt solution undergoes 2H + +2e - →H2 chemical reaction, the generated gas peels off the MLCC internal electrode from the porcelain dielectric layer.
[0010] Furthermore, the four-side exposed internal electrodes are obtained by polishing the two end faces and two side faces of the MLCC with 800-3000 grit sandpaper until the multiple layers of internal electrodes are visually exposed.
[0011] Furthermore, the liquid level of the salt solution is 1 / 3 to 2 / 3 of the height of the MLCC.
[0012] Furthermore, the salt solution is one of Na2SO4, NaHSO4, and KHSO4.
[0013] Furthermore, the concentration of the salt solution is 1% wt to 10% wt.
[0014] Furthermore, the ejector pin electrode is connected to one layer of the inner electrodes of the MLCC.
[0015] Furthermore, the voltage range of the DC power supply is 1V to 5V, and the voltage holding time of the DC power supply is 1 minute to 30 minutes.
[0016] Furthermore, the stripped MLCC inner electrodes were observed and inspected.
[0017] Furthermore, as the size of MLCC increases, increasing the DC voltage prolongs the voltage holding time.
[0018] Compared with the existing technology, the present invention has the following technical advantages: the method for quickly stripping the MLCC internal electrode provided by the present invention can obtain a complete internal electrode structure, can effectively observe the internal electrode holes, and thus accurately calculate the internal electrode coverage; the quick stripping MLCC internal electrode device designed by the present invention is safe, reliable, simple, easy to operate, and has wide applicability, and can be widely used in various types of MLCCs; the method developed by the present invention is unique and innovative, solves the problem of difficulty in stripping the internal electrode, and provides effective technical guidance for improving the capacity and reliability of MLCC. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] The following drawings depict only certain embodiments of the present invention and therefore should not be considered limiting of the scope.
[0020] Figure 1 It is a schematic diagram of the present invention;
[0021] Figure 2 This is a physical picture of the complete MLCC inner electrode peeled off by the present invention;
[0022] Figure 3 This is an electron microscope image of the inner electrode and ceramic surface of Example 1;
[0023] Figure 4 This is an electron microscope image of the inner electrode and ceramic surface of Example 2;
[0024] Figure 5 This is an electron microscope image of the inner electrode and ceramic surface of Example 3;
[0025] Figure 6 This is an electron microscope image of the inner electrode and ceramic surface of Example 4;
[0026] Figure 7 This is an electron microscope image of the inner electrode and ceramic surface of Example 5;
[0027] In the accompanying drawings, 1-DC power supply; 2-MLCC sample; 21-MLCC inner electrode; 3-salt solution; 4-thimble electrode; 5-culture dish. DETAILED DESCRIPTION
[0028] The present invention is described in further detail below.
[0029] A method for quickly stripping an inner electrode of an MLCC comprises the following steps:
[0030] Step 1: Grind the two end faces and two side faces of MLCC sample 2 on 800-3000 mesh sandpaper, using sandpaper with mesh numbers from low to high, and observe under a microscope until all the internal electrodes on the four surfaces are exposed. After cleaning with alcohol, dry at 60-100°C to obtain the prepared MLCC sample 2; wherein the size specification of MLCC sample 2 is not greater than 6878 (EIA standard specification).
[0031] Step 2: Prepare a salt solution 3 with a concentration of 1% wt to 10% wt in a culture dish 5; as an optional embodiment, the salt solution can be one of Na2SO4, NaHSO4, and KHSO4.
[0032] Step 3: Place the MLCC sample 2 obtained in step 1 vertically in the salt solution of step 2; wherein the liquid level of the salt solution is between 1 / 3 and 2 / 3 of the MLCC sample 2.
[0033] Step 4: Prepare two connecting wires, one of which has a pin electrode 4 at its end and is connected to one layer of the MLCC inner electrode sample 21, and the other end is connected to the negative electrode of the DC power supply 1; the other connecting wire connects the salt solution to the positive electrode of the DC power supply 1; for details, refer to Figure 1 Schematic diagram.
[0034] Step 5: Turn on the DC power supply and slowly adjust the voltage of the power supply from low to high; the voltage range is 1V to 5V, and the voltage holding time is 1 minute to 30 minutes.
[0035] The present invention is described in detail below in conjunction with the embodiments and drawings to facilitate a more comprehensive understanding of the present invention by those skilled in the art, but the present invention is not limited to the scope of all embodiments. All other embodiments obtained without creative work are within the scope of protection of the present invention.
[0036] Example 1
[0037] In this embodiment, the MLCC sample size is 0603 (EIA standard specification), and the 1% wt NaHSO4 salt solution is prepared as follows:
[0038] Step 1: Grind the two end faces and two side faces of the 0603 specification MLCC with 800-3000 mesh sandpaper in sequence until all four in-plane electrodes are exposed under a microscope. After cleaning with alcohol, dry at 60°C.
[0039] Step 2, preparing a 1% wt NaHSO4 salt solution in a container;
[0040] Step 3, vertically placing the MLCC sample obtained in step 1 in the salt solution of step 2; wherein the liquid level of the salt solution is within the range of 1 / 3 to 2 / 3 of the MLCC sample;
[0041] Step 4, such as Figure 1 As shown, a connecting wire with a pin electrode at the end is connected to one of the inner electrodes of the MLCC sample, and the other end is connected to the negative electrode of the DC power supply; another connecting wire connects the salt solution to the positive electrode of the DC power supply;
[0042] Step 5. Turn on the DC power supply and slowly adjust the voltage of the DC power supply from low to high to 1V, and maintain the voltage for 1 minute.
[0043] Example 2
[0044] In this embodiment, the MLCC sample size is 1210 (EIA standard specification), and the 2% wt Na2SO4 salt solution is prepared as follows:
[0045] Step 1: Grind the two end faces and two side faces of the 1210 specification MLCC with 800-3000 mesh sandpaper in sequence until all four in-plane electrodes are exposed under a microscope. After cleaning with alcohol, dry at 70°C.
[0046] Step 2, preparing a 2% wt Na2SO4 salt solution in a container;
[0047] Step 3, vertically placing the MLCC sample obtained in step 1 in the salt solution of step 2; wherein the liquid level of the salt solution is between 1 / 3 and 2 / 3 of the MLCC sample;
[0048] Step 4, such as Figure 1 As shown, a connecting wire with a pin electrode at the end is connected to one layer of the inner electrode of the MLCC, and the other end is connected to the negative electrode of the DC power supply 1; another connecting wire connects the salt solution 3 to the positive electrode of the DC power supply;
[0049] Step 5: Turn on DC power supply 1, slowly adjust the voltage of the DC power supply from low to high to 1V, and maintain the voltage for 10 minutes.
[0050] Example 3
[0051] In this embodiment, the MLCC sample size specification is 2220 (EIA standard specification), and the 3% wt NaHSO4 salt solution is prepared as follows:
[0052] Step 1: Grind the two end faces and two side faces of the 2220 specification MLCC on 800-3000 mesh sandpaper in sequence until all four in-plane electrodes are exposed under a microscope. After cleaning with alcohol, dry at 100°C.
[0053] Step 2, preparing a 3% wt NaHSO4 salt solution in a container;
[0054] Step 3, vertically placing the MLCC sample obtained in step 1 in the salt solution of step 2; wherein the liquid level of the salt solution is between 1 / 3 and 2 / 3 of the MLCC sample;
[0055] Step 4, such as Figure 1 As shown, a connecting wire with a pin electrode at the end is connected to one of the inner electrodes of the MLCC sample, and the other end is connected to the negative electrode of the DC power supply; another connecting wire connects the salt solution to the positive electrode of the DC power supply;
[0056] Step 5. Turn on the DC power supply and slowly adjust the voltage of the DC power supply from low to high to 2V, and maintain the voltage for 10 minutes.
[0057] Example 4
[0058] In this embodiment, the MLCC sample size is 3035 (EIA standard specification), and the 5% wt NaHSO4 salt solution is prepared as follows:
[0059] Step 1: Grind the two end faces and two side faces of the 3035 specification MLCC on 800-3000 mesh sandpaper in sequence until all four in-plane electrodes are exposed under a microscope. After cleaning with alcohol, dry at 80°C.
[0060] Step 2, preparing a 5% wt NaHSO4 salt solution in a container;
[0061] Step 3, vertically placing the MLCC sample obtained in step 1 in the salt solution of step 2; wherein the liquid level of the salt solution is between 1 / 3 and 2 / 3 of the MLCC sample;
[0062] Step 4, such as Figure 1 As shown, a connecting wire with a pin electrode at the end is connected to one of the inner electrodes of the MLCC sample, and the other end is connected to the negative electrode of the DC power supply; another connecting wire connects the salt solution to the positive electrode of the DC power supply;
[0063] Step 5. Turn on the DC power supply and slowly adjust the voltage of the DC power supply from low to high to 3V, and maintain the voltage for 20 minutes.
[0064] Example 5
[0065] In this embodiment, the MLCC sample size specification is 6878 (EIA standard specification), and the 10% wt KHSO4 salt solution is prepared as follows:
[0066] Step 1: Grind the two end faces and two side faces of the 6878 specification MLCC on 800-3000 mesh sandpaper in sequence until all four in-plane electrodes are exposed under a microscope. After cleaning with alcohol, dry at 100°C.
[0067] Step 2, preparing a 10% wt concentration of KHSO4 salt solution in a container;
[0068] Step 3, vertically placing the MLCC sample obtained in step 1 in the salt solution of step 2; wherein the liquid level of the salt solution is between 1 / 3 and 2 / 3 of the MLCC sample;
[0069] Step 4, such as Figure 1 As shown, a connecting wire with a pin electrode at the end is connected to one of the inner electrodes of the MLCC sample, and the other end is connected to the negative electrode of the DC power supply; another connecting wire connects the salt solution to the positive electrode of the DC power supply;
[0070] Step 5. Turn on the DC power supply and slowly adjust the voltage of the DC power supply from low to high to 5V, and maintain the voltage for 60 minutes.
[0071] Figure 1 This is a schematic diagram of the inner electrode stripping process of the present invention. The MLCC inner electrode is connected to the negative electrode of the DC power supply using a pin electrode, and the salt solution is connected to the positive electrode of the DC power supply. + When the DC power supply is turned on, the negative electrode will generate 2H + +2e - →H2 chemical reaction, that is, a small amount of H2 is produced at the MLCC internal electrode. By adjusting the voltage, the rate of gas production can be adjusted. After a certain period of time, due to the expansion effect of the gas, the MLCC internal electrode is peeled off from the ceramic interface, such as Figure 2 shown.
[0072] Figure 3 This is an electron microscope image of the inner electrode and ceramic surface of Example 1. The MLCC used in this example is of 0603 specification and the salt solution is 1% wt NaHSO4. Since the MLCC in this example is of smaller specification, the inner electrode of the MLCC can be peeled off from the ceramic dielectric layer by applying a voltage of 1V and maintaining the voltage for 1 minute. Figure 3 It can be observed that the inner electrode has a mesh structure with many internal holes, and there is no inner electrode attached to the porcelain dielectric layer. The above shows that the inner electrode of the MLCC obtained in this embodiment is completely peeled off from the porcelain dielectric.
[0073] Figure 4This is an electron microscope image of the inner electrode and ceramic surface of Example 2. The MLCC specification used in this example is 1210, and the salt solution is 2% wt Na2SO4. In this example, for the 1210 specification MLCC, the salt solution concentration is increased to 2% wt, and the voltage is still applied at 1V and maintained for 1 minute, and the MLCC inner electrode can be peeled off from the ceramic dielectric layer. Figure 4 The inner electrode surface with a mesh structure and the clean ceramic dielectric surface without other impurities can be observed, which shows that the inner electrode of the MLCC obtained in this embodiment is completely peeled off from the ceramic dielectric.
[0074] Figure 5 This is an electron microscope image of the internal electrode and ceramic surface of Example 3. This example, targeting a 2220 MLCC, used a 3% wt NaHSO4 salt solution. By applying a voltage of 2V and holding the pressure for 10 minutes, the MLCC internal electrode was peeled from the ceramic dielectric layer. Because the MLCC in this example is larger than those in Examples 1 and 2, the salt solution concentration, applied voltage, and holding time were increased. This resulted in a mesh-like internal electrode surface and a clean, impurity-free ceramic dielectric layer. This demonstrates that the MLCC internal electrode obtained in this example was completely peeled from the ceramic dielectric.
[0075] Figure 6 This is an electron micrograph of the internal electrode and ceramic surface of Example 4. This example used a 5% wt NaHSO4 salt solution, a DC voltage of 3V, and a hold time of 10 minutes to peel the internal electrode of a 2220 MLCC from the ceramic dielectric layer. Compared to Example 3, the MLCC size in this example was further increased, requiring a corresponding increase in the salt solution concentration, DC voltage, and hold time. This resulted in a mesh-like internal electrode surface and a clean, impurity-free ceramic dielectric layer. This demonstrates that the internal electrode of the MLCC obtained in this example was completely peeled from the ceramic dielectric.
[0076] Figure 7 This is an electron micrograph of the internal electrode and ceramic surface of Example 5. This example used a 10% wt KHSO4 salt solution, a DC voltage of 5V, and a dwell time of 60 minutes to peel the internal electrode of a 2220 MLCC from the ceramic dielectric layer. Compared to Examples 1-4, this example has the largest MLCC size, so the salt solution concentration, DC voltage, and dwell time were increased accordingly. The internal electrode surface exhibits a reticulated porous structure, while the ceramic dielectric surface is clean and free of other impurities. This demonstrates that the internal electrode of the MLCC obtained in this example was completely peeled from the ceramic dielectric.
[0077] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the above embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the above embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for quickly stripping the inner electrode of MLCC, characterized in that: The following steps are involved: Place the MLCC with all four sides of the inner electrodes exposed in a saline solution; The salt solution and the inner electrode of the MLCC are connected to the positive electrode and the negative electrode of the DC power supply respectively by using two ejector electrodes; Turn on the DC power supply and adjust the voltage until the MLCC inner electrode is separated from the dielectric layer; specifically, the MLCC inner electrode layer in the salt solution undergoes 2H + +2e - →H2 chemical reaction, the generated gas peels off the MLCC internal electrode from the porcelain dielectric layer.
2. A method for rapidly stripping an inner electrode of an MLCC according to claim 1, characterized in that: The four-side exposed internal electrodes are obtained by grinding the two end faces and two side faces of the MLCC with 800-3000 grit sandpaper until the multi-layer internal electrodes are exposed visually.
3. A method for rapidly stripping an inner electrode of an MLCC according to claim 1, characterized in that: The liquid level of the salt solution is 1 / 3 to 2 / 3 of the height of the MLCC.
4. A method for rapidly stripping an inner electrode of an MLCC according to claim 1, characterized in that: The salt solution is one of Na2SO4, NaHSO4, and KHSO4.
5. A method for rapidly stripping an inner electrode of an MLCC according to claim 4, characterized in that: The concentration of the salt solution is 1%wt to 10%wt.
6. A method for rapidly stripping an inner electrode of an MLCC according to claim 1, characterized in that: The ejector pin electrode connects one of the electrodes inside the MLCC.
7. A method for rapidly stripping an inner electrode of an MLCC according to claim 1, characterized in that: The voltage range of the DC power supply is 1V to 5V, and the voltage holding time of the DC power supply is 1 minute to 30 minutes.
8. A method for rapidly stripping an inner electrode of an MLCC according to claim 1, characterized in that: The stripped MLCC internal electrodes were observed and inspected.
9. A method for rapidly stripping an inner electrode of an MLCC according to claim 1, characterized in that: As the size of MLCC increases, increasing the DC voltage will extend the holding time.