Optical filter and preparation method and application thereof

By using a combination of stress balance film layer and optical film layer in optical filters, the problem of film stress affecting optical performance is solved, deep cut-off low reflection effect and stability are achieved, and it is suitable for optical modules and patterned applications.

CN118938371APending Publication Date: 2024-11-12SUZHOU WUFANG PHOTOELECTRIC MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411010504.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The energy loss and film stress problems of existing optical filters in optical materials lead to poor detection sensitivity, reduced signal-to-noise ratio, reduced image resolution, and difficult to achieve deep cutoff and low reflection effects. At the same time, film stress affects the yield rate of the components and stability.

Method used

The stress balance film layer and the optical film layer are adopted. The optical film layer presents tensile or compressive stress, and the stress balance film layer presents opposite stress. By alternately depositing Cr and Cr2O3 film layers, combining SiO2 film layers, the film stress is balanced and warping is reduced. , achieve deep cut-off low reflection effect.

Benefits of technology

Effectively reduce the warpage of the filter, improve optical parameters, ensure performance stability, achieve OD < 4 depth cutoff and reflectivity below 2.0% in the 420-750nm band, suitable for optical modules and graphics applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118938371A_ABST
    Figure CN118938371A_ABST
Patent Text Reader

Abstract

The invention discloses an optical filter which sequentially comprises a stress balance film layer, an optical film layer and a base material, the stress balance film layer and the optical film layer are located on the same side of the base material, and the optical film layer is located between the stress balance film layer and the base material. And the stress balance film layer is used for balancing the influence of the stress of the optical film layer on the optical filter. According to the optical filter, the optical film layer and the stress balance film layer with opposite stress results are arranged, so that the stress balance film layer balances the influence of the stress of the optical film layer on the optical filter, and the optical parameters and the effect of the optical filter are effectively improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of optical filters, and in particular to a black chrome deep cutoff low reflection filter with glass as a substrate, a preparation method of the optical filter and its application in the field of optical modules, as well as a patterning method of the filter and the obtained patterned filter. Background Art

[0002] Optical modules are an indispensable and important part of modern technology and are widely used in machine vision, security monitoring, mobile devices and other fields. In order to meet the needs of different scenarios, through reasonable layout, the specific optical performance of the module is determined to bring more convenience and innovation to people's life and work.

[0003] As an important optical element in the optical module, the cut-off filter selectively reflects and absorbs light in a specific wavelength range through multi-layer coating technology, thereby achieving a filtering effect on a specific wavelength. However, due to the characteristics of the optical material itself, light is accompanied by energy loss during propagation, which will lead to problems such as poor detection sensitivity of optical components, reduced signal-to-noise ratio, and reduced image resolution. Low-reflection film can effectively reduce the optical loss of light during propagation and some harmful effects caused by reflected light beams at the interface. At the same time, black chrome materials can completely absorb the spectrum and appear black.

[0004] Therefore, for optical elements that require deep cutoff and low reflection in the visible light band, this can be achieved by preparing black chrome deep cutoff low reflection filters.

[0005] At the same time, the wet etching process in photolithography uses chromium etching solution (high-purity cerium ammonium nitrate solution), which can accurately etch black chrome film without reacting with the photoresist on the surface of the black chrome film. Black chrome has high thermal stability and good adhesion to many commonly used materials. Black chrome can be used to produce products such as patternable photomasks and apertures.

[0006] However, almost all films have large stress, and the existence of film stress directly affects the yield, stability and reliability of optical components. Within a certain range, stress acts on the substrate, causing the substrate to deform, thereby distorting the optical information transmitted through the component. Therefore, it is of great significance to control the total stress of the filter to ensure the performance of the components. The basic formula for film stress is:

[0007]

[0008] Where r is the film curvature, d s is the substrate thickness, d f is the film thickness, E s is the Young's constant of the substrate, ν sis the Poisson coefficient of the substrate. f When is positive, the stress is tensile stress. Otherwise, the stress is compressive stress.

[0009] Thin film stress is generally divided into tensile stress and compressive stress, which is mainly composed of thermal stress and internal stress. Thermal stress is caused by the difference in thermal expansion coefficient between the film and the substrate. Under the condition of high temperature deposition of the film layer, the different thermal expansion coefficients between the film and the substrate cause the sample after coating to expand or contract. The thermal stress of the thin film material σ f The formula is:

[0010]

[0011] Among them, α s is the thermal expansion coefficient of the substrate, α f is the thermal expansion coefficient of the film, ΔT is the difference between the deposition temperature and the measurement temperature, E f is the film Young's constant, ν f is the Poisson coefficient of the film.

[0012] Internal stress is very complex, not only related to the characteristics of the film material itself, but also affected by the process parameters during the coating process. The deposition rate, film thickness, substrate temperature and other process parameters during the coating process determine the microstructure and defects of the film, which in turn affects the magnitude of stress in the film and even changes the nature of the stress.

[0013] Prior art, such as the Chinese invention patent with application number 202410285018.4, discloses a method for preparing a black film, a black film, and an electronic product, which uses magnetron sputtering to prepare a multi-layer silicon nitrogen hydrogen layer and a multi-layer silicon dioxide layer on the glass surface to obtain a black film, and its average transmittance in the 400-700nm band is less than 1%. The cutoff depth of the black film prepared by this method for visible light is only OD2, and it cannot be patterned.

[0014] For example, the Chinese invention patent with application number 201911296593.X discloses a graphable wide-band absorption device and its preparation method, which uses vacuum evaporation to deposit a metal absorption layer Cr, a dielectric-metal film stack Cr2O3-Cr and a protective layer SiO2 on a substrate silicon wafer in sequence, and then the composite film layer is subjected to photoresist spin coating, exposure, and development in sequence, and then the mask pattern is transferred to the photoresist to achieve graphing. Its film system design focuses on the absorption of a wide-band spectrum, with an average absorption rate of 99.6% in the visible light band of 380-780nm. The protective layer SiO2 plays a protective role to protect the absorption layer Cr and the dielectric-metal film stack Cr2O3-Cr from being affected by the external environment. However, the cutoff depth of the absorption device is less than OD3 and cannot reach OD4, and the problem of film layer stress affecting the deformation of the device is not explained.

[0015] The disclosure of the above background technology content is only used to assist in understanding the inventive concept and technical solution of the present invention. It does not necessarily belong to the prior art of this patent application. In the absence of clear evidence that the above content has been disclosed before the filing date of this patent application, the above background technology should not be used to evaluate the novelty and creativity of the present application. Summary of the invention

[0016] In view of this, the present invention discloses an improved optical filter, which can reduce the warping of the optical filter.

[0017] A filter comprises a stress-balancing film layer, an optical film layer and a substrate in sequence, wherein the stress-balancing film layer and the optical film layer are located on the same side of the substrate and the optical film layer is located between the stress-balancing film layer and the substrate, and the stress-balancing film layer is used to balance the influence of the stress of the optical film layer on the filter.

[0018] According to some preferred implementation aspects of the present invention, the stress presented by the optical film layer is one of tensile stress or compressive stress; the stress presented by the stress balancing film layer is the other of the tensile stress or compressive stress. That is, the stress presented by the optical film layer is opposite to the stress presented by the stress balancing film layer. Specifically, when the stress presented by the optical film layer is tensile stress, the stress presented by the stress balancing film layer is compressive stress; when the stress presented by the optical film layer is compressive stress, the stress presented by the stress balancing film layer is tensile stress, so as to achieve the stress balancing effect of the stress balancing film layer.

[0019] Preferably, the optical film layer exhibits tensile stress; and the stress-balancing film layer exhibits compressive stress.

[0020] According to some preferred implementation aspects of the present invention, the compressive stress of the stress-balancing film layer is used to reduce deformation problems, such as warping, caused by the tensile stress of the optical film layer on the optical filter.

[0021] According to some preferred implementation aspects of the present invention, the maximum warping value of the optical filter is less than 0.5 mm, and has a deep cutoff of OD < 4 and a reflectivity lower than 2.0% in the 420-750 nm band.

[0022] According to some preferred implementation aspects of the present invention, preferably, under the premise of a certain thickness of the optical film layer, the smaller the thickness of the substrate, the greater the thickness of the stress balance film layer, so as to better balance the stress. At the same time, under the premise of a certain thickness of the substrate, the greater the thickness of the optical film layer, the greater the thickness of the stress balance film layer.

[0023] According to some preferred implementation aspects of the present invention, the optical film layer is a visible light cutoff and low-reflection optical film layer, specifically a deep cutoff low-reflection optical film layer, more preferably a black chrome (blCr) film, which is formed by alternating deposition of a Cr film and a Cr2O3 film, and the layer closest to the glass substrate is a Cr2O3 film layer, which achieves low reflection, and the black chrome deposited on the glass substrate presents tensile stress. The deep cutoff low-reflection optical film layer achieves a deep cutoff effect by the absorption of metal Cr, and the cutoff can reach OD4. The Cr2O3 film layer has good adhesion to the substrate, has a good film-forming effect, and is not easy to fall off.

[0024] Preferably, the optical thin film Cr and Cr2O3 are deposited by vacuum evaporation or magnetron sputtering, wherein vacuum evaporation with higher deposition rate and lower cost is more preferred.

[0025] According to some preferred embodiments of the present invention, the total number of layers in the optical film layer is 6-9 layers, which are formed by alternating deposition of Cr and Cr2O3, and the layer closest to the glass substrate is a Cr2O3 film layer, the total thickness of the film layer is 0.3-0.5um, and the film thickness ratio of Cr and Cr2O3 is 0.8-1.2.

[0026] According to some preferred implementation aspects of the present invention, the stress balancing film layer is a SiO2 film layer with a thickness of 300-700 nm. The SiO2 film exhibits compressive stress, effectively balancing the tensile stress of the black chrome film, reducing the warping of the filter, ensuring the stability of the filter performance, and making the maximum warping value of the filter less than 0.5 mm.

[0027] According to some preferred embodiments of the present invention, the ratio of the thickness of the optical film layer to the thickness of the stress-balancing film layer is 0.8-1.5.

[0028] According to some preferred embodiments of the present invention, the substrate is glass with a thickness of 0.05-0.35 mm, preferably white glass.

[0029] According to some preferred embodiments of the present invention, the maximum transmittance of the optical film layer spectrum in the wavelength range of 420-750nm when the incident angle is 0° is less than 0.025%, preferably less than 0.015%, and more preferably less than 0.01%.

[0030] According to some preferred embodiments of the present invention, the reflectivity of the optical film layer spectrum in the wavelength range of 420-750nm when the incident angle is 5° (here is the back reflectivity, light is incident from the non-coated surface) is less than 3.0% on average, preferably less than 2.5%, and more preferably less than 2.0%.

[0031] According to some preferred implementation aspects of the present invention, the optical filter has a deep cutoff of OD < 4 in the 420-750 nm band.

[0032] The present invention also provides a method for preparing the filter as described above, comprising the following steps:

[0033] An optical film layer is first deposited on the surface of a substrate, and then a stress-balancing film layer is continuously plated on the surface of the optical film layer away from the substrate to obtain the optical filter; the stress presented by the optical film layer is opposite to the stress presented by the stress-balancing film layer.

[0034] Specifically, in some embodiments of the present invention, the method for preparing the filter as described above comprises the following steps:

[0035] 1. Membrane system design

[0036] According to the requirements of deep cutoff (ultra-low transmittance) and reflectivity, the filter is simulated and the thickness of each layer of film is optimized to design a deep cutoff low-reflection filter of the required band. Specifically, the filter can be simulated by the film system design software Essential Macleod or TFCalc to optimize the structure and film thickness of the dielectric-metal film stack.

[0037] 2. Glass pretreatment

[0038] Clean and pre-treat the glass substrate to ensure the cleanliness of the glass surface and prevent surface dirt from affecting the uniformity of the film and its optical properties.

[0039] First, the glass was placed in a stripping agent for ultrasonic cleaning for 3 minutes, rinsed with deionized water to remove the stripping agent, rinsed with a detergent for 3 minutes after rinsing, rinsed with deionized water to remove the detergent, and finally the cleaned glass was placed in a centrifuge for drying.

[0040] 3. Preparation of optical film layer and stress balance layer

[0041] Cr and Cr2O3 film layers are alternately deposited on the surface of a glass substrate, and the layer closest to the glass substrate is the Cr2O3 film layer, so as to prepare a deep cutoff and low-reflection optical film layer.

[0042] The vacuum evaporation method is used for coating. According to the thickness of each layer of the film system design, the thickness of each layer is 9×10 -4 Visible light cutoff and low reflection optical film layers and balanced stress layers are deposited in sequence under vacuum conditions of 1.5 Pa gas pressure. The film thicknesses are monitored by a quartz crystal oscillator to obtain a deep cutoff low reflection filter of the required wavelength band.

[0043] SiO2 is continuously plated on the surface of the deep cut-off low reflection optical film layer to achieve the effect of balancing stress, reduce or eliminate the warping of the filter, and prepare a black chrome deep cut-off low reflection filter.

[0044] The present invention also provides an application of the above-mentioned filter in an imaging module or a photolithography patterned mask plate, specifically, as a light-clearing aperture applied to a sensor module, an optical lens module, etc., and can also be used for a photolithography patterned mask plate, etc. The optical film layer is composed of Cr and Cr2O3. After Cr and Cr2O3 are etched by a chromium etching solution, they are very soluble in water, so a patterned black chrome film layer can be prepared.

[0045] The present invention also provides a method for patterning the filter as described above and the prepared patterned filter, which can be used in an optical module.

[0046] According to some preferred implementation aspects of the present invention, the method for patterning the filter specifically comprises the following steps:

[0047] Spin-coating photoresist on the filter;

[0048] exposure;

[0049] Then develop it;

[0050] Removing the stress balancing layer and the optical film layer at corresponding positions;

[0051] The remaining photoresist is removed to obtain a patterned filter.

[0052] The deep cutoff low-reflection film layer has the characteristics of ultra-low transmittance and low reflectivity. When light is irradiated from the air medium to the surface of the film layer, light of some bands is almost not transmitted, and the incident light is efficiently cut off; when light is incident from the glass interface (non-coated surface) to the surface of the film layer, light of some bands is absorbed and interfered, reducing or eliminating the optical loss of light during propagation and some harmful effects caused by reflected light at the interface; black chrome material is used to prepare the optical film layer, and chrome etching solution can be used to corrode the black chrome film layer, and a graphic deep cutoff low-reflection filter is prepared through a photolithography process. However, the black chrome film layer prepared by vacuum evaporation is deposited on the surface of the white glass substrate, causing deformation of the substrate. Excessive stress will cause surface damage of the film and degradation of performance. The present invention uses thin film materials with different stress properties to balance the influence of the stress of the black chrome film layer on the substrate and ensure the performance of the filter.

[0053] Specifically, the present invention deposits a deep cutoff low-reflection optical film layer on the surface of a white glass substrate by vacuum evaporation technology, and then deposits a balanced stress film layer after the optical film layer to reduce the warping of the filter and ensure its flatness. The optical film layer and the balanced stress film layer are both located on the same surface of the glass.

[0054] The principle of the present invention is as follows: Due to the high absorption characteristics of black chrome in the sunlight band and the deep cutoff requirement in the visible light band, the structure of the dielectric-metal film stack is composed of dielectric film Cr2O3 and metal film Cr. The comprehensive stress of the black chrome film layer is tensile stress, and the filter is seriously warped and the flatness is damaged, which affects the product quality. The thermal expansion coefficient of the black chrome film layer is smaller than the thermal expansion coefficient of the glass. It can be calculated from Formula 2 that the thermal stress of the black chrome film layer is compressive stress, which is inconsistent with the stress properties finally presented by the black film layer. This is because the film stress is the result of the interaction between thermal stress and internal stress. The surface density of the black chrome film prepared by vacuum evaporation on the white glass substrate is poor, and the internal stress is tensile stress, which has a dominant influence.

[0055] The comprehensive stress of the SiO2 film is presented as compressive stress. SiO2 is used as a balancing stress layer to effectively balance the tensile stress of the black chrome film, reduce the warping of the filter, and ensure its flatness. The thermal expansion coefficient of the SiO2 film is smaller than that of the black chrome. It can be calculated from Formula 2 that the thermal stress of the SiO2 film layer is compressive stress. At the same time, the SiO2 film prepared by vacuum evaporation has good surface density, and the internal stress also presents compressive stress, which can effectively balance the tensile stress of the black chrome film layer. That is, the present application plates a suitable thickness of SiO2 on the surface of the deep cutoff low-reflection optical film layer to reduce or eliminate the warping of the filter and ensure the flatness of the filter.

[0056] Compared with traditional filters, the beneficial effect of the present invention is that the filter of the present invention, by setting an optical film layer and a stress balancing film layer with opposite stress results, makes the stress balancing film layer balance the influence of the stress of the optical film layer on the filter, thereby effectively improving the optical parameters and effects of the filter. BRIEF DESCRIPTION OF THE DRAWINGS

[0057] In order to more clearly illustrate the embodiments of the present invention and the technical solutions in the prior art, the drawings required for use in the description of the technical solutions in the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0058] Figure 1 This is a flow chart of the preparation of a black chrome deep cut-off low reflection filter in a preferred embodiment of the present invention;

[0059] Figure 2 It is a schematic diagram of the structure of a black chrome deep cut-off low reflection filter in a preferred embodiment of the present invention;

[0060] Figure 3 This is a schematic diagram of the measurement path of the reflection spectrum of the black chrome deep cutoff low reflection filter in the preferred embodiment of the present invention;

[0061] Figure 4 The transmission spectrum of the deep cut-off low reflection filter in the wavelength range of 420-750nm prepared in the preferred embodiment 1 of the present invention when the incident angle is 0°;

[0062] Figure 5 The back reflection spectrum of the deep cut-off low reflection filter in the wavelength range of 420-750nm prepared in the preferred embodiment 1 of the present invention at an incident angle of 5°;

[0063] Figure 6 Schematic diagram of the preparation process of the patternable black chrome deep cut-off low reflection filter in the preferred embodiment 4 of the present invention;

[0064] Figure 7 It is a schematic diagram of the process of patterning a black chrome deep cut-off low reflection filter that can be patterned in the preferred embodiment 4 of the present invention;

[0065] Figure 8 This is an appearance diagram of the graphable black chrome deep cutoff low reflection filter in the preferred embodiment 4 of the present invention. DETAILED DESCRIPTION

[0066] To make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific implementation methods described herein are only used to explain the present invention and are not limited to the protection scope of the present invention.

[0067] The preparation flow chart of the filter prepared in the following examples is as follows Figure 1 As shown in the structure diagram Figure 2 As shown, the reflectance spectrum measurement path is as follows Figure 3 shown.

[0068] Example 1

[0069] The method for preparing the black chrome deep cut-off low reflection filter in this embodiment specifically comprises the following steps:

[0070] 1. Membrane system design

[0071] Essential Macleod software was used for membrane system design.

[0072] 2. Glass pretreatment

[0073] A square white glass with a thickness of 0.3 mm, a length and width of 150×150 mm and a brand of D263T was selected as the substrate.

[0074] The glass is pre-treated by washing: the glass is placed in a stripping agent for ultrasonic cleaning for 3 minutes, the stripping agent is rinsed with deionized water, and then washed with a cleaning agent for 3 minutes, the cleaning agent is rinsed with deionized water, and finally the cleaned glass is placed in a centrifuge for drying.

[0075] 3. Preparation of optical film layer and balanced stress layer

[0076] Put the cleaned and pre-treated glass into the OTFC-1500 coating equipment and wait until it is pumped to 9×10 -4 Under the vacuum condition of 1.5 Pa gas pressure, the visible light cut-off and low-reflection optical film layers and the balanced stress layer are deposited in sequence to obtain a filter with deep cut-off and low-reflection in the visible light band. The schematic diagram of its structure is shown in FIG. Figure 2 shown.

[0077] The visible light cutoff and low-reflection optical film layer prepared in this embodiment corresponds to a 7-layer Cr2O3 / Cr / Cr2O3 / Cr / Cr2O3 / Cr / Cr2O3 thin film structure, and the total thickness of the film layer is about 400nm.

[0078] The balanced stress layer deposited on the surface of the optical film layer is made of SiO2 and has a thickness of about 400 nm.

[0079] 4. Testing

[0080] The warpage of the prepared filter sample was measured using a step profiler. The calculation result according to Formula 1 showed that the filter exhibited comprehensive tensile stress, and the warpage height was as shown in the measurement result of Example 1 in Table 2.

[0081] The prepared filter sample was subjected to spectral testing. The transmittance performance of the filter sample in the 420-750nm band was measured with a UV-2600 instrument at an incident angle of 0°. The transmittance spectrum is shown in FIG. Figure 4 shown.

[0082] The reflectance performance of the filter sample in the 420-750nm band was measured using an Olympus instrument with an incident angle of 5°. The reflectance spectrum is shown in Figure 5 The measured spectrum results are shown in Table 1, the measurement results of Example 1.

[0083] Comparative Example 1

[0084] The difference between the optical filter of this comparative example and Example 1 is that there is no balanced stress layer SiO2 on the optical filter of this comparative example. The remaining steps and parameters are basically the same as those of Example 1.

[0085] The coated filter was taken as a sample, and the warpage of the film surface was measured using a step meter. The calculation results according to Formula 1 showed that the black chrome film plated on the surface of the glass substrate showed comprehensive tensile stress, and the warpage height was as shown in the measurement results of Comparative Example 1 in Table 2.

[0086] The optical properties (transmittance and reflection properties) of the filter in the 420-750 nm band were measured using a UV-2600 instrument and an Olympus microscope. The spectral measurement results are shown in the measurement results of Comparative Example 1 in Table 1.

[0087] Comparative Example 2

[0088] The black chrome deep cut-off filter prepared in this comparative example is different from that in Example 1 in that the optical film layer in this comparative example corresponds to an 11-layer thin film structure. The specific steps for preparing the filter are:

[0089] 1. Membrane system design

[0090] Essential Macleod software was used for membrane system design.

[0091] 2. Glass pretreatment

[0092] A square white glass with a thickness of 0.3 mm, a length and width of 150×150 mm and a brand of D263T was selected as the substrate.

[0093] The glass is pre-treated by washing: the glass is placed in a stripping agent for ultrasonic cleaning for 3 minutes, the stripping agent is rinsed with deionized water, and then washed with a cleaning agent for 3 minutes, the cleaning agent is rinsed with deionized water, and finally the cleaned glass is placed in a centrifuge for drying.

[0094] 3. Preparation of optical film layer and balanced stress layer

[0095] Put the cleaned and pre-treated glass into the OTFC-1500 coating equipment and wait until it is pumped to 9×10 -4 Under the vacuum condition of Pa pressure, Cr / Cr2O3 optical film layer and stress balance layer SiO2 are deposited in sequence to obtain a filter with deep cutoff in the visible light band. The schematic diagram of its structure is shown in Figure 2 shown.

[0096] The prepared deep cutoff optical film layer corresponds to a thin film structure of 11 layers of Cr2O3 / Cr / Cr2O3...Cr / Cr2O3, and the total thickness of the film layer is about 460nm.

[0097] The balanced stress layer deposited on the surface of the optical film layer is made of SiO2 and has a thickness of about 400nm.

[0098] 4. Testing

[0099] The optical performance of the filter in the 420-750nm band was measured using a UV-2600 instrument and an Olympus instrument. The spectrum measurement results are shown in the measurement results of Comparative Example 2 in Table 1.

[0100] Comparative Example 3

[0101] This comparative example prepares a low-reflection filter. Compared with Example 1, the difference is that the optical film layer of this comparative example corresponds to a 4-layer thin film structure. The specific steps of preparing the filter are:

[0102] 1. Membrane system design

[0103] Use Essential software for membrane system design.

[0104] 2. Glass pretreatment

[0105] A square white glass with a thickness of 0.3 mm, a length and width of 150×150 mm and a brand of D263T was selected as the substrate.

[0106] The glass is pre-treated by washing: the glass is placed in a stripping agent for ultrasonic cleaning for 3 minutes, the stripping agent is rinsed with deionized water, and then washed with a cleaning agent for 3 minutes, the cleaning agent is rinsed with deionized water, and finally the cleaned glass is placed in a centrifuge for drying.

[0107] 3. Preparation of optical film layer and balanced stress layer

[0108] Put the cleaned and pre-treated glass into the OTFC-1500 coating equipment and wait until it is pumped to 9×10 -4 Under the vacuum condition of Pa pressure, Cr / Cr2O3 optical film layer and stress balance layer SiO2 are deposited in sequence to obtain a low-reflection filter in the visible light band.

[0109] The prepared optical film layer corresponds to a 4-layer Cr2O3 / Cr / Cr2O3 / Cr thin film structure, and the total thickness of the film layer is about 150nm.

[0110] The balanced stress layer deposited on the surface of the optical film layer is made of SiO2 and has a thickness of about 100 nm.

[0111] 4. Testing

[0112] The optical performance of the filter in the 420-750nm band was measured using a UV-2600 instrument and an Olympus instrument. The spectrum measurement results are shown in the measurement results of Comparative Example 3 in Table 1.

[0113] Example 2

[0114] The steps and parameters of this embodiment are basically the same as those of embodiment 1, except that in this embodiment, a square white glass with a thickness of 0.1 mm, a length and width of 150×150 mm, and a grade of D263T is selected as the substrate. A SiO2 film layer with a thickness of 600 nm is deposited to balance the stress of the optical film layer.

[0115] The filters without SiO2 film layer and the filters with SiO2 film layer were used as samples, and the warpage of the film surface was measured using a step meter. The calculation results based on Formula 1 showed that both filters showed tensile stress, and the warpage height was as shown in the measurement results of Example 2 in Table 2.

[0116] The optical performance of the filter in the 420-750 nm band was measured using a UV-2600 instrument and an Olympus instrument. The spectrum measurement results are shown in Table 1 for the measurement results of Example 2.

[0117] Example 3

[0118] The steps and parameters of this embodiment are basically the same as those of embodiment 1, except that in this embodiment, a square white glass with a thickness of 0.05 mm, a length and width of 150×150 mm, and a grade of AS87 is selected as the substrate. A SiO2 film layer with a thickness of 700 nm is deposited to balance the stress of the optical film layer.

[0119] The filters without SiO2 film layer and the filters with 700nm thick SiO2 film layer were used as samples, and the warping of the film surface was measured using a step meter. The calculation results based on Formula 1 showed that both filters showed tensile stress, and the warping height was as shown in the measurement results of Example 3 in Table 2.

[0120] The optical performance of the filter in the 420-750 nm band was measured using a UV-2600 instrument and an Olympus instrument. The spectral measurement results are shown in Table 1 for the measurement results of Example 3.

[0121] Example 4

[0122] In this embodiment, the filter prepared in embodiment 1 is patterned to provide a patternable black chrome deep cutoff low reflection filter. The preparation process is as follows: Figure 6 shown.

[0123] Spin-coat the photoresist on the prepared filter at a pre-rotation speed of 500 rmps for 10 s and a main rotation speed of 4000 rmps for 40 s;

[0124] The exposure wavelength is 365nm and the exposure energy is 120mJ;

[0125] Then develop in TMAH (tetramethylammonium hydroxide) for 80 s;

[0126] Finally, the balanced stress layer SiO2 at the corresponding position is removed by etching with hydrofluoric acid slow-release solution for 120 seconds, and the black chrome film layer at the corresponding position is corroded in chromium etching solution for 90 seconds;

[0127] The remaining photoresist is removed to obtain a patterned black chrome deep cut-off low reflection filter. The schematic diagram of the patterning process of photolithography to prepare the pattern filter is shown in Figure 7 shown.

[0128] Figure 8 Product picture of the prepared graphic black chrome deep cut-off low reflection filter, which has been applied to optical modules.

[0129] Tests and Results

[0130] 1) The optical filters prepared in the embodiments and comparative examples were optically tested using a UV-2600 instrument and an Olympus microscope, and the test method was based on GB / T2680-2021. Table 1 below shows the optical test results.

[0131] Table 1 Optical test results

[0132] Spectral data 420-750nmRave 420-750nmTmax Example 1 1.25% 0.001% Comparative Example 1 1.24% 0.0008% Comparative Example 2 18.9% 0.002% Comparative Example 3 0.6% 6% Example 2 1.23% 0.001% Example 3 0.76% 0.0007%

[0133] The results in Table 1 show that the reflectivity and transmittance of the final product spectrum of the optical filter prepared in the embodiment in the 420-750nm band are relatively ideal, and the effects of deep cutoff and low reflection can be achieved at the same time.

[0134] Comparing the spectral data of Example 1 and Comparative Example 1, the maximum transmittance of the filter coated with the balanced stress layer SiO2 in the 420-750nm band is 0.0002% higher than that of the filter without the balanced stress layer SiO2, and the average value of the reflection spectrum is 0.01% lower. The results show that the balanced stress layer SiO2 has almost no effect on the transmittance and reflection spectra of the filter in the 420-750nm band; since the optical film on the filter in Comparative Example 2 has an 11-layer film structure, the maximum transmittance of the filter in the 420-750nm band is 0.002%, which has the effect of deep cutoff but no low reflection; since the optical film on the filter in Comparative Example 3 has only a 4-layer film structure, and the total thickness of the film layer is 150nm, the average reflectance of the filter in the 420-750nm band is 0.6%, which has the effect of low reflection but no deep cutoff.

[0135] 2) Use a step profiler to measure the warpage of the film surface. The test method is based on GB / T25257-2010. Table 2 below shows the warpage height test results.

[0136] Table 2 Warpage height test results

[0137] Optical Filters Example 1 Comparative Example 1 Example 2 Example 3 Substrate thickness 0.3mm 0.3mm 0.1mm 0.05mm <![CDATA[Thickness of SiO2 film layer]]> 400nm 0nm 600nm 700nm <![CDATA[Warpage height before SiO2 coating]]> / 1.06 2.54 2.83 <![CDATA[Warpage height after SiO2 coating]]> 0.38 / 0.42 0.49

[0138] The results in Table 2 show that in Comparative Example 1, the sample warping height is 1.06 mm without SiO2 film coating, and the sample warping height is 0.38 mm with SiO2 film coating in Example 1, indicating that the SiO2 film coating can effectively improve the sample warping. By comparing substrates of different thicknesses, the experimental results show that the smaller the substrate thickness, the greater the warping height of the filter, and the thicker the required balanced stress SiO2 film. This is consistent with the rule of Formula 1, that is, under the premise of fixed film stress, the smaller the substrate thickness, the greater the curvature, and the corresponding increase in the SiO2 film thickness is required.

[0139] On the one hand, a large amount of data research shows that most metal films exist in the form of tensile stress, and most dielectric films are tensile stress, but compressive stress also exists. Based on this, the present application combines film layers with different stress properties to improve the severe deformation problem of the substrate and reduce its warping. On the other hand, the black chrome coating is mainly composed of metallic chromium and chromium trioxide, and has good selective absorption of sunlight. The black chrome film layer can be prepared by evaporation using alternating deposition of Cr2O3 / Cr, but the stress of the Cr2O3 / Cr optical film layer causes severe deformation of the substrate. Therefore, the present application uses SiO2 as a stress balance film layer to improve the effect of the Cr2O3 / Cr film layer stress on the deformation of the filter.

[0140] The present invention discloses a black chrome deep cutoff low reflection filter and its preparation method and application, which sequentially comprises a balanced stress film layer, a visible light cutoff and low reflection optical film layer, and a substrate, wherein the substrate is white glass, the balanced stress film layer and the visible light cutoff and low reflection optical film layer are located on the same surface of the white glass, and the material of the balanced stress film layer is SiO2. The surface of the deep cutoff low reflection optical film layer is plated with SiO2 of appropriate thickness to reduce or eliminate the warping of the filter and ensure its flatness; the filter of the present invention has the optical characteristics of deep cutoff and low reflection in the visible light band of 420-750nm; the black chrome optical film layer can be removed by chrome etching solution to obtain a graphic deep cutoff low reflection filter; the filter can be used to prepare an optical module with specific optical performance requirements, and has a wide range of applications in the fields of machine vision, security monitoring and mobile devices. The filter of the present invention, by setting an optical film layer and a stress balance film layer with opposite stress results, allows the stress balance film layer to balance the influence of the stress of the optical film layer on the filter, effectively improving the optical parameters and effects of the filter. The filter provided by the present invention has a higher cut-off performance and has an optical performance of low reflectivity on the back side. In addition, the filter has the characteristic of being able to be patterned, and various patterns can be prepared according to actual needs, so that the deep cut-off low-reflection filter has a wider application prospect.

[0141] The above embodiments are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with the technology to understand the content of the present invention and implement it accordingly, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.

Claims

1. A filter, characterized in that: The invention comprises a stress-balancing film layer, an optical film layer and a substrate in sequence. The stress-balancing film layer and the optical film layer are located on the same side of the substrate and the optical film layer is located between the stress-balancing film layer and the substrate. The stress-balancing film layer is used to balance the influence of the stress of the optical film layer on the filter.

2. The optical filter according to claim 1, characterized in that: The stress presented by the optical film layer is one of tensile stress and compressive stress; the stress presented by the stress-balancing film layer is the other of the tensile stress and compressive stress.

3. The optical filter according to claim 1, characterized in that: The optical film layer exhibits tensile stress; and the stress-balancing film layer exhibits compressive stress.

4. The optical filter according to claim 1, characterized in that The compressive stress of the stress-balancing film layer is used to reduce the warping of the filter caused by the tensile stress of the optical film layer.

5. The optical filter according to claim 1 or 3, characterized in that: The maximum warping value of the filter is less than 0.5 mm.

6. The optical filter according to claim 1, characterized in that: The optical film layer is formed by alternately depositing a Cr film and a Cr2O3 film.

7. The optical filter according to claim 6, characterized in that: The total number of layers in the optical film layer is 6-9 layers, which are formed by alternate deposition of Cr and Cr2O3. The total thickness of the film layer is 0.3-0.5um, and the film thickness ratio of Cr to Cr2O3 is 0.8-1.

2.

8. The optical filter according to claim 1, characterized in that: The stress balance film layer is a SiO2 film layer with a thickness of 300-700nm.

9. The optical filter according to claim 1, characterized in that: The ratio of the thickness of the optical film layer to the thickness of the stress balance film layer is 0.8-1.

5.

10. The optical filter according to claim 1, characterized in that: The substrate is glass with a thickness of 0.05-0.35 mm.

11. The optical filter according to claim 1, characterized in that: When the incident angle of the optical film layer spectrum is 0°, the maximum transmittance in the wavelength range of 420-750nm is less than 0.025%.

12. The optical filter according to claim 1, characterized in that: When the incident angle of the optical film layer is 5°, the reflectivity of the optical film layer in the wavelength range of 420-750nm is less than 3.0% on average.

13. The optical filter according to claim 1, characterized in that: The filter has a deep cutoff of OD < 4 in the 420-750nm band.

14. A method for preparing a filter according to any one of claims 1 to 13, characterized in that: The steps include: An optical film layer is first deposited on the surface of a substrate, and then a stress-balancing film layer is continuously plated on the surface of the optical film layer away from the substrate to obtain the optical filter.

15. Use of the filter according to any one of claims 1 to 13 in an imaging module or a mask.

16. A method for patterning a filter, characterized in that: The steps include: A photoresist is coated on the filter as claimed in any one of claims 1 to 13; after exposure, it is developed; the corresponding stress-balancing film layer and the optical film layer are removed, and the remaining photoresist is removed to obtain a patterned filter.

17. A patterned filter obtained by the patterning method according to claim 16.