Photoresist removing liquid for Lift-off process and photoresist removing method
By introducing sulfonate anionic surfactant, polar organic solvent and heterocyclic protector into the degluing solution, the problem of poor photoresist peeling effect in the Lift-off process is solved, and efficient removal of interdigital light is achieved Resist, which reduces metal corrosion and production costs, is suitable for a variety of metals and substrate materials.
Patent Information
- Application Number
- CN202411022486.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-11-12
AI Technical Summary
When processing photoresist in the interfinger zone, the deglue removal liquid combination has poor effect on the photoresist peeling effect. Conventional methods such as raising the temperature or pressurized flushing will cause residual glue and metal fragments, increasing production costs. and metal corrosion risks.
Adopt the degluent solution containing sulfonate anionic surfactant, polar organic solvent and heterocyclic adsorption metal protector to optimize the composition of the degluent solution to improve the swelling and peeling capacity of the photoresist, reduce metal corrosion, and is applicable in a variety of metal materials.
It significantly improves the removal efficiency and quality of photoresist, reduces the amount of metal corrosion, and is suitable for a variety of workpieces, especially Cr, Ti, Ag and other materials, and does not corrode SiO2 and SiN substrates, reducing metals during the flushing process. Risk of debris scratches.
Smart Images

Figure CN118938614A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of photoresist stripping agents, and in particular to a photoresist stripping solution and a photoresist stripping method for a Lift-Off process. Background Art
[0002] The lift-off process is to use a photolithography process to obtain a patterned photoresist structure or metal mask on a substrate, use a coating process to coat the mask with a target metal layer, and then use a stripping solution to dissolve the photoresist or mechanically remove the metal hard mask to obtain a target graphic metal layer consistent with the pattern.
[0003] There are the following differences between the lift-off process and the wet etching process for photoresist stripping: the surface of the photoresist in the lift-off process is covered with a target metal layer, and only the photoresist on the side in the thickness direction is exposed to the workpiece surface; the surface of the photoresist in the wet etching process that is away from the substrate and the side in the thickness direction are both exposed to the workpiece surface. In order to fully protect the target graphic structure, the stripping solution usually contains a metal corrosion inhibitor, which will also inhibit the corrosion of the target metal layer on the surface of the photoresist layer. Therefore, the photoresist exposed on the surface of the workpiece is in direct contact with the stripping solution, and the size of the photoresist area exposed on the surface of the workpiece directly determines the speed at which the stripping solution swells and dissolves the photoresist.
[0004] Some specific workpieces include interdigital areas and empty areas. The interdigital areas have a periodic pattern similar to a finger or comb. The pattern is densely distributed in a predetermined area. The photoresist line width is about 0.4μm, and the target pattern line width between adjacent photoresist lines is about 0.2μm. Conventional lift-off process degumming uses a combination of nitrogen methyl pyrrolidone and metal protective agent, and in order to be compatible with a variety of metals, metal corrosion inhibitors usually use adsorption-type corrosion inhibitors. Whether it is physical adsorption or chemical adsorption, it can be stably adsorbed on the surface of the metal, that is, adsorbed on the surface and side of the target pattern away from the substrate and the surface and side of the metal layer on the photoresist surface away from the photoresist. The corrosion inhibitor adsorption structure is not conducive to the rapid penetration of the degumming liquid penetrating components into the space between the substrate and the photoresist.
[0005] Conventional degumming liquid combination has poor degumming effect on the interdigital area, and the photoresist in the interdigital area is almost completely swollen and retained in the groove body composed of the target pattern metal wiring. The improved solution adopts increasing the immersion temperature of the degumming liquid, pressurized washing or removing the metal layer on the surface of the photoresist. Increasing the temperature is limited by the flash point of the components and the uneven temperature distribution in the groove; pressurized washing will increase the probability of residual glue fragments and metal fragments, and the washing process will aggravate the problem of metal fragments scratching the target metal wiring; removing the metal layer on the surface of the photoresist will inevitably lengthen the process route and increase production costs. Summary of the invention
[0006] The purpose of the present invention is to overcome the defects existing in the prior art and provide a degumming solution for Lift-Off process, introduce a sulfonate anion surfactant into the degumming solution, and use a metal-protective polar organic solvent B and a heterocyclic adsorption-type metal protective agent in combination to improve the stripping effect of the photoresist in the interdigital area of the Lift-off workpiece.
[0007] In order to achieve the above technical effects, the technical solution of the present invention is: a degumming solution for lift-off process, the main components of which include, by mass percentage: 50% to 80% of polar organic solvent A, 15% to 40% of metal protective polar organic solvent B, 3% to 15% of sulfonate anionic surfactant and 0.1% to 10% of adsorption type metal protective agent.
[0008] A preferred technical solution is that the metal-protecting polar organic solvent B is one selected from dimethyl sulfoxide and alcohol metal-protecting solvents, or a combination of two or more thereof.
[0009] A preferred technical solution is that the polar organic solvent is one or a combination of two or more selected from azacycloalkanones.
[0010] The preferred technical solution is that the anionic surfactant is selected from one or a combination of two or more aromatic sulfonates;
[0011] Furthermore, the anionic surfactant is one or a combination of two or more selected from benzene sulfonates having a C10-C18 long-chain alkyl group.
[0012] The preferred technical solution is that the main components of the adsorption-type metal protective agent are azole protective agents and sugar alcohol protective agents;
[0013] The mass percentage of the azole protective agent in the degumming solution is 0.05% to 2.5%; the mass percentage of the sugar alcohol protective agent is 1% to 7%;
[0014] Furthermore, the mass percentage of the azole protective agent in the degumming solution is 0.1% to 1.5%; the mass percentage of the sugar alcohol protective agent is 1% to 5%.
[0015] A preferred technical solution is that the alcohol metal protection solvent is one selected from ethylene glycol, isopropanol, propylene glycol, glycerol, or a combination of two or more thereof.
[0016] A preferred technical solution is that the azole protective agent is selected from one or a combination of two or more of thiadiazole and benzotriazole derivatives, and / or the sugar alcohol protective agent is selected from one or a combination of two or more of sorbitol, mannitol, erythritol, maltitol, lactitol, and xylitol.
[0017] A preferred technical solution is that the azole protective agent is one or a combination of two or more selected from 2,5-bis(octyl disulfide) thiadiazole, 2,5-bis(tert-nonyl disulfide) thiadiazole, and 2,5-bis(tert-dodecyl disulfide) thiadiazole; and / or the sugar alcohol protective agent is sorbitol and / or xylitol.
[0018] The second object of the present invention is to provide a lift-off process degumming method, which adopts the lift-off process to remove the photoresist of the workpiece to be degummed with a degumming liquid.
[0019] The preferred technical solution is to immerse the workpiece to be debonded in the debonding solution for the lift-off process at 50-85°C;
[0020] Furthermore, the workpiece to be debonded is immersed in the debonding solution for the lift-off process at a temperature of 65 to 85°C.
[0021] Furthermore, the photoresist includes photoresist in the interdigital region of the workpiece to be stripped.
[0022] The advantages and beneficial effects of the present invention are:
[0023] The Lift-Off process uses a degumming liquid, based on a combination of a polar solvent and a metal protective agent, to add a sulfonate anionic surfactant to enhance the degumming liquid's ability to swell and strip the photoresist, thereby accelerating the photoresist stripping processing efficiency of the workpiece.
[0024] The metal protection effect is optimized on the basis of introducing sulfonate anionic surfactant, so that the combined degumming liquid, which is mainly composed of polar solvent, anionic surfactant and metal protective agent, has no obvious corrosion to the metal materials of Cr, Ti and Ag, which are commonly used target patterns of workpieces to be degummed. The corrosion amount of Al and Cu in the degumming process meets the production requirements and is generally applicable to various workpieces with exposed metal layers.
[0025] The degumming liquid system has no corrosion to SiO2 and SiN, and is suitable for lift-off workpieces with SiO2 and SiN as substrates. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 It is the main view of the interdigitated area of the workpiece;
[0027] Figure 2 It is a partial schematic diagram of the cross section of the photoresist line in the interdigital area (comparison before and after stripping);
[0028] Figure 3 This is the SEM photo of the photoresist stripping result with the photoresist completely removed;
[0029] Figure 4This is a SEM photo of the stripping result with a small amount of residual photoresist. The curved photoresist swells but does not separate from the workpiece;
[0030] Figure 5 This is a SEM photo of the stripping result with a large amount of residual photoresist. The curved photoresist swells but does not separate from the workpiece. DETAILED DESCRIPTION
[0031] The specific implementation of the present invention is further described below in conjunction with the accompanying drawings and embodiments. The following embodiments are only used to more clearly illustrate the technical solution of the present invention, and cannot be used to limit the protection scope of the present invention.
[0032] Polar organic solvent A and polar organic solvent B
[0033] Polar organic solvent A is different from polar organic solvent B. Polar organic solvent A mainly functions to swell the photoresist, while polar organic solvent B functions to enhance metal protection performance.
[0034] The polar organic solvent A can be selected from one or a combination of two or more of imidazolidinone, pyrrolidone and imidazolinone, preferably azacycloalkanone, and the selection range includes N-methylpyrrolidone and N-ethylpyrrolidone.
[0035] The metal protected by the polar organic solvent B is the accessory metal in the lift-off process workpiece, including but not limited to conventional Al, Cr, Ti, Al, Ag, Cu, and the polar organic solvent B has a protective effect on any one or more of the above known metal types. The polar organic solvent B can be selected from dimethyl sulfoxide and alcohol organic solvents, and the alcohol organic solvents also include alcoholamine organic solvents. Further, the alcohol organic solvent is ethylene glycol.
[0036] Sulfonate anionic surfactant
[0037] The sulfonate anionic surfactant may be a long-chain alkyl sulfonate or an alkylbenzene sulfonate, usually a sodium salt. Specifically, it may be a sodium salt of dodecyl sulfonic acid, tridecyl sulfonic acid, tetradecyl sulfonic acid, pentadecyl sulfonic acid, hexadecyl sulfonic acid, nonylbenzene sulfonic acid, decylbenzene sulfonic acid, hydroxynonylbenzene sulfonic acid, dodecylbenzene sulfonic acid, tridecylbenzene sulfonic acid, tetradecylbenzene sulfonic acid, pentadecylbenzene sulfonic acid, hexadecylbenzene sulfonic acid, heptadecanylbenzene sulfonic acid, or octadecylbenzene sulfonic acid.
[0038] Compared with sulfonates, benzenesulfonates are beneficial to promoting the stripping of swollen photoresist from the corresponding grooves, reducing the operation probability or flushing pressure of using a stripping solution to rinse the photoresist, thereby reducing the probability of metal fragments scratching the target metal wiring due to flushing.
[0039] Adsorption type metal protective agent
[0040] Adsorption-type metal protective agents are a type of chemical adsorption-type protective agents, mainly including heterocyclic compounds containing nitrogen and oxygen elements such as mercaptobenzothiazole, benzotriazole, thiadiazole, tetrazole, and sugar alcohols.
[0041] Specific selections of heterocyclic compounds include, but are not limited to, 3-amino-1,2,4-triazole, 1,2,4-triazole, 4-amino-1,2,4-triazole, 5-aminotetrazole, benzimidazole, 2-mercapto-1-methylimidazole, 2-mercaptobenzoxazole, mercapto-benzothiazole, benzotriazole, methylbenzotriazole, 1-hydroxybenzotriazole, 1-phenyl-5-mercaptotetrazole, 2-amino-5-mercapto-1,3,4-thiadiazole, 2-methyl-5-(pentyldisulfide)-1,3,4-thiadiazole, 2-mercapto-5-methyl-1,3,4-thiadiazole, 2,5-bis(octyldisulfide)thiadiazole, 2,5-bis(tert-nonyldisulfide)thiadiazole, and 2,5-bis(tert-dodecyldisulfide)thiadiazole.
[0042] Sugar alcohol metal protectors refer to monosaccharides that are converted into corresponding polyols through catalytic hydrogenation and sodium borohydride reduction. The polar hydroxyl groups in the molecules are tightly adsorbed on the metal surface by charge action.
[0043] Both the corrosion inhibitor heterocyclic compounds and sugar alcohols form protective films on the metal surface. The metal protective film formed by the thiadiazole with a long-chain alkyl group and the sugar alcohol metal protective agent is more dense and orderly, and has excellent corrosion protection effects on various metals of the debonding workpiece. The thiadiazole is preferably 2,5-bis(octyl disulfide)thiadiazole with a straight-chain alkyl group.
[0044] Furthermore, the degumming liquid system is an organic system, and no water is added except the inevitable water in the raw material components.
[0045] Example
[0046] The components used in the embodiment are configured as follows:
[0047] Polar organic solvent A
[0048] A1——N-methylpyrrolidone
[0049] Polar organic solvent B
[0050] B1——Dimethyl sulfoxide
[0051] B2——ethylene glycol
[0052] Anionic surfactant C
[0053] C1——Sodium dodecylbenzene sulfonate
[0054] C2——Sodium dodecyl sulfate
[0055] C3——Sodium 4-octylbenzenesulfonate
[0056] Heterocyclic adsorption type metal protective agent D
[0057] D1——1,2,3-benzotriazole
[0058] D2——2,5-bis(octyl dithio)thiadiazole
[0059] D3——2,5-bis(tert-nonyldithio)thiadiazole
[0060] D4——Maltitol
[0061] D5——Xylitol
[0062] 1. Effect of component content on degumming effect and metal corrosion rate
[0063] 1. The component contents of Examples 1-3 and Comparative Examples 1-4 are configured according to the following table:
[0064]
[0065]
[0066] Comparative Example 5
[0067] Comparative Example 5 is based on Example 1, except that dodecylbenzenesulfonic acid is used instead of sodium dodecylbenzenesulfonate.
[0068] 2. Evaluation of degumming performance
[0069] 2a Configuration of debonding workpiece
[0070] The top view of the interdigital area structure of the debonding workpiece is as follows: Figure 1 As shown, the shaded parts represent the removed photoresist lines, and the blank areas between adjacent shaded parts represent the target pattern metal lines.
[0071] The cross section of the workpiece interdigital area before and after degumming treatment is shown in Figure 2. Figure 2 As shown, the shaded parts represent the metal layer, the target pattern metal wire is covered on the substrate and located between adjacent photoresist lines; the photoresist line and the target pattern metal wire are both slender strips; the cross-section of the target pattern metal wire in the finger area is a right trapezoid, the top edge of the right trapezoid is 0.2 to 0.4 μm, and the bottom edge is 0.3 to 0.4 μm; the thickness of the metal wire is about 0.4 μm; the cross-section of the photoresist wire is an inverted trapezoid, and the width of the photoresist wire is slightly larger than the width of the metal wire.
[0072] The photoresist is a naphthoquinone diazide type ultraviolet photoresist.
[0073] 2b The degumming process includes the following steps:
[0074] S1: Prepare the workpiece to be debonded and the debonding liquid, heat the debonding liquid to 80°C, introduce the workpiece into the debonding liquid, keep it warm for 30 minutes and then take it out. In this process, keep the debonding liquid overflow circulation;
[0075] S2: Pressurized flushing with degumming liquid, the flushing pressure is limited to the tolerance pressure of the workpiece;
[0076] S2: isopropyl alcohol rinse;
[0077] S3: deionized water rinse;
[0078] S4: Drying the workpiece.
[0079] Evaluation of 2c interdigital area degumming results:
[0080] The target observation area is set in the SEM photo of the workpiece. The degumming area refers to the area where the photoresist line is completely separated from its line groove. The degumming rate is calculated as the percentage of the degumming area of the interdigital area after immersion in the degumming solution to the total area of the photoresist line in the target observation area:
[0081] ——Degumming rate 100%
[0082] ○——Degumming rate is greater than or equal to 95% and less than 100%;
[0083] ◎——Degumming rate is greater than or equal to 80% and less than 95%;
[0084] ●——Degumming rate is greater than or equal to 65% and less than 80%;
[0085] ◆——Degumming rate is greater than or equal to 50% and less than 65%;
[0086] ▲——Degumming rate is less than 50%;
[0087] When the debonding rate reaches 100%, there is no need to perform pressurized washing with the debonding liquid, which reduces the probability of damage to other parts of the workpiece by the metal layer stacked with the photoresist during the washing process. Generally, when the debonding rate of the workpiece is greater than or equal to 80%, the photoresist can be removed by pressurized washing.
[0088] 4. Metal corrosion test and corrosion rate calculation
[0089] Evaporation on the substrate surface The target metals Ti, Ag, Al, and Cu were immersed in the degumming solution at 80°C for 3 hours, the thickness of the target metal layer remaining on the surface of the substrate was measured, and the corrosion rate of the metal was calculated.
[0090] The evaluation of the degumming results and the corrosion rates of Examples 1-3 and Comparative Examples 1-4 are shown in the following table:
[0091]
[0092] The residue in the interdigital area of the sample of Example 1 before rinsing is less than that of the sample of Example 2, and the rinsing pressure of the degumming solution is also correspondingly smaller; the photoresist stripping effect of the sample of Example 3 before rinsing is the best, but the corrosion rate of the metal is generally greater than that of Examples 1 and 2.
[0093] Comparative Example 1 uses a combination of NMP and a metal protective agent, and Comparative Example 2 uses a combination of NMP, ethylene glycol and a metal protective agent. The photoresist degumming rates before and after rinsing are both less than 50%. Comparative Example 3 uses a combination of NMP, a sulfonate anion surfactant and a metal protective agent, indicating that the sulfonate anion surfactant has a significant effect on the swelling of the photoresist and its detachment from the workpiece; the addition of ethylene glycol to the degumming solution promotes the reduction of the metal corrosion rate.
[0094] In Comparative Example 4, the contents of NMP and ethylene glycol in the degumming solution are similar, the photoresist is insufficiently swollen, and the photoresist degumming rate of the interdigital area before and after rinsing with the degumming solution is generally worse than that of Example 1, indicating that the ratio of the two organic solvents in the degumming solution must be appropriate.
[0095] Comparative Example 5 The addition of dodecylbenzenesulfonic acid increases the acidity of the degumming solution; dodecylbenzenesulfonic acid is beneficial to promoting the swelling of the photoresist and its detachment from the workpiece, but will increase the metal corrosion rate.
[0096] 2. Effect of polar organic solvent B on metal corrosion rate
[0097] The component contents of Examples 4-7 are configured according to the following table, and the degumming test and metal corrosion test are the same as those of Example 1:
[0098]
[0099] The evaluation of the degumming results and the corrosion rates of Examples 4-7 are shown in the following table:
[0100]
[0101] In Example 4, the polar organic solvent B is dimethyl sulfoxide. The degumming solution in Example 4 has a better swelling effect and degumming rate on the photoresist, indicating that the combined organic system of NMP and dimethyl sulfoxide has an excellent swelling and stripping effect on the photoresist, but the metal corrosion rate is relatively high.
[0102] It can be seen from the above table that with the increase of ethylene glycol content and the decrease of dimethyl sulfoxide content in polar organic solvent B, the metal corrosion rate shows a decreasing trend, indicating that except for the necessary metal protective agent, the swelling and stripping effect of ethylene glycol on photoresist is weaker than that of dimethyl sulfoxide, but it has the effects of swelling and stripping of photoresist and reducing metal corrosion rate, so it is more suitable for the stripping solution system that comes into contact with multiple metals in the Lift-OFF process.
[0103] 3. Effect of anionic surfactant carbon chain on metal corrosion rate
[0104] The component contents of Examples 8-11 are configured according to the following table, and the degumming test and metal corrosion test are the same as those of Example 1:
[0105]
[0106] The evaluation of the degumming results and the corrosion rates of Examples 8-11 are shown in the following table:
[0107]
[0108] Examples 8-10 all use a high-pressure rinse with a degumming solution to completely remove the photoresist, and the pressure of the high-pressure rinse with the degumming solution increases in the order of Examples 10, 9, and 8;
[0109] *: The sample of Example 11 was not able to completely remove the photoresist after being immersed in the degumming solution for 30 minutes and then rinsed under high pressure. The photoresist was completely removed by extending the immersion time in the degumming solution to 50 hours and then rinsing under high pressure.
[0110] The results in the above table show that the type of anionic surfactant has a greater impact on the stripping rate of the interdigital area and a smaller impact on the corrosion rate; the preferred C10-C18 long-chain alkyl benzene sulfonate is more conducive to improving the stripping rate; if the carbon number of the long-chain alkyl is too small, the attraction and aggregation ability between the surfactant molecules will be weakened, resulting in a weakened penetration ability of the stripping solution and a slower swelling and stripping rate of the photoresist.
[0111] 4. Effect of heterocyclic adsorption metal protective agent D on metal corrosion rate
[0112] The component contents of Examples 12-16 are configured according to the following table, and the degumming test and metal corrosion test are the same as those of Example 1:
[0113]
[0114]
[0115] The evaluation of the degumming results and the corrosion rates of Examples 4-7 are shown in the following table:
[0116]
[0117] Compared with Example 13, the degumming solutions of Examples 12 and 14 have lower metal corrosion rates. The metal corrosion rates of Examples 12-15 are all maintained within a predetermined smaller range, among which the metal corrosion rates of Examples 12-14 are smaller, indicating that the degumming solution samples are highly compatible with workpieces with various metal surfaces.
[0118] The metal protective agent of Example 16 has the same amount of thiadiazole and sugar alcohol, and the metal corrosion rate is slightly higher than that of Example 14, among which the corrosion rates of silver, aluminum and copper are all greater than 0.4. This indicates that the ratio of thiadiazoles used as metal protective agents to sugar alcohol metal protective agents must be appropriate.
[0119] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the technical principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A degumming solution for lift-off process, characterized in that: The main components, calculated by mass percentage, include: 50% to 80% of polar organic solvent A, 15% to 40% of metal protection type polar organic solvent B, 3% to 15% of sulfonate anionic surfactant and 0.1% to 10% of adsorption type metal protection agent.
2. The degumming solution for lift-off process according to claim 1, characterized in that: The metal-protecting polar organic solvent B is one selected from dimethyl sulfoxide and alcohol metal-protecting solvents, or a combination of two or more thereof.
3. The degumming solution for lift-off process according to claim 1, characterized in that: The polar organic solvent is one or a combination of two or more selected from azacycloalkanones.
4. The degumming solution for lift-off process according to claim 1, characterized in that: The anionic surfactant is selected from one or a combination of two or more aromatic sulfonates; Furthermore, the anionic surfactant is one or a combination of two or more selected from benzene sulfonates having a C10-C18 long-chain alkyl group.
5. The degumming solution for lift-off process according to claim 1, characterized in that: The main components of the heterocyclic adsorption type metal protective agent are azole protective agents and sugar alcohol protective agents; The mass percentage of azole protective agent in the degumming solution is 0.05% to 2.5%; the mass percentage of sugar alcohol protective agent is 1% to 7%; Furthermore, the mass percentage of the azole protective agent in the degumming solution is 0.1% to 1.5%; the mass percentage of the sugar alcohol protective agent is 1% to 5%.
6. The degumming solution for lift-off process according to claim 1, characterized in that: The alcohol metal protection solvent is one selected from ethylene glycol, isopropanol, propylene glycol, glycerol or a combination of two or more thereof.
7. The degumming solution for lift-off process according to claim 1, characterized in that: The azole protective agent is selected from one or a combination of two or more of thiadiazole and benzotriazole derivatives, and / or the sugar alcohol protective agent is selected from one or a combination of two or more of sorbitol, mannitol, erythritol, maltitol, lactitol and xylitol.
8. The degumming solution for lift-off process according to claim 7, characterized in that: The azole protective agent is one or a combination of two or more selected from 2,5-bis(octyl disulfide) thiadiazole, 2,5-bis(tert-nonyl disulfide) thiadiazole, and 2,5-bis(tert-dodecyl disulfide) thiadiazole; and / or the sugar alcohol protective agent is sorbitol and / or xylitol.
9. A lift-off process degumming method, characterized in that: The lift-off process described in any one of claims 1 to 8 is used to remove the photoresist of the workpiece to be removed using a degumming solution.
10. The lift-off process degumming method according to claim 9, characterized in that: The following steps are involved: S1: Soaking the workpiece to be debonded in the debonding solution for the lift-off process at 50-85° C.; Further, S1: immersing the workpiece to be debonded in the debonding solution for the lift-off process at 65-85° C.; Furthermore, it also includes: S2: using the lift-off process to pressurize and rinse the soaked workpiece to be debonded with a debonding liquid.
Citation Information
Cited By
Copper-molybdenum-based photoresist stripping liquid and wet photoresist removing method
CN121432822A