Hybrid capacitor composite positive electrode material and preparation method thereof

Through the composite material of nano-microstructure lithium cobalt oxide particles and nitrogen-doped activated carbon, combined with the characteristics of lithium cobalt oxide and nitrogen-doped activated carbon, the problem of low energy density of the positive electrode material of hybrid capacitors is solved, and high energy density and high power are achieved The hybrid capacitor with density meets the application needs of high energy density and high power density.

CN118942919APending Publication Date: 2024-11-12GUIZHOU MEILING POWER SUPPLY CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411234926.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-04
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The cathode material of existing hybrid capacitors has low energy density and cannot meet the application needs of high power density working scenarios.

Method used

Using composite materials with nano-microstructure lithium cobalt oxide particles and nitrogen-doped activated carbon, a composite positive electrode material with ultrafast ion/electronic energy storage effect is prepared through ball milling technology, combining the embedded pseudocapacitance characteristics of lithium cobalt oxide and nitrogen doping. The adsorption and desorption capacitance characteristics of hybrid activated carbon improve the rate performance of energy storage devices.

Benefits of technology

The energy density and power density of hybrid capacitors are significantly improved, with energy density ≥100Wh/kg and power density ≥80kW/kg, meeting the application needs of high energy density and high power density.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118942919A_ABST
    Figure CN118942919A_ABST
Patent Text Reader

Abstract

The invention discloses a hybrid capacitor composite positive electrode material in the field of electrochemical energy storage batteries, a composite material is prepared by optimizing and mixing nano-microstructure lithium cobalt oxide (the secondary particle size is 50 nm) and high-capacity nitrogen-doped activated carbon with the gram specific capacity larger than 35 mAh / g according to the mass ratio of (80-95): (5-20), and by means of the high specific capacity of the lithium cobalt oxide and the high-rate characteristic of the nitrogen-doped activated carbon, the composite material can be used for preparing the hybrid capacitor composite positive electrode material with the high specific capacity of the lithium cobalt oxide and the high-rate characteristic of the nitrogen-doped activated carbon. Compared with a traditional hybrid capacitor, the hybrid capacitor composite positive electrode material with the ultrafast ion / electron synergistic energy storage effect is greatly improved in energy density and power density, the energy density of the prepared composite positive electrode material is larger than or equal to 100 Wh / kg, the power density of the composite positive electrode material is larger than or equal to 80 kW / kg, the practical application capacity of the hybrid capacitor is improved, and the hybrid capacitor composite positive electrode material is suitable for being used in the field of hybrid capacitors. And the application requirements of high-energy-density and high-power-density working scenes can be met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of electrochemical energy storage, and in particular relates to a hybrid capacitor composite positive electrode material and a preparation method thereof. Background Art

[0002] As a new type of electrochemical energy storage device that combines the high energy density of lithium-ion batteries and the high power density of supercapacitors, hybrid capacitors are widely used in aerospace, energy storage, industry, medicine, electric / hybrid vehicles, rail transportation and other fields. Hybrid capacitors are usually composed of carbon materials with high specific surface area (such as activated carbon, graphene, etc.) as positive electrode materials, carbon materials with lithium ion intercalation (such as graphite, soft carbon, hard carbon, etc.) as negative electrode materials and organic electrolytes. They can store and convert energy through the adsorption and desorption of charges and the deintercalation of lithium ions. Compared with supercapacitors, the energy density of hybrid capacitors can be increased by more than 2 times. Compared with lithium-ion batteries, they can be charged and discharged quickly, and have better high and low temperature performance, cycle performance and safety performance.

[0003] When hybrid capacitors use activated carbon as the positive electrode material, the prepared hybrid capacitors have good power performance, which can reach 20kW / kg, but the energy density is relatively low, usually <50Wh / kg, which cannot meet the application requirements of some working scenarios that require both high energy density and high power density, such as frequency modulation (coordinated regulation of thermal energy storage) and peak shaving and valley filling in the energy storage field, rail transit sources, etc. Summary of the invention

[0004] The present invention aims to provide a hybrid capacitor composite positive electrode material based on the ultrafast ion / electron synergistic energy storage effect to solve the problem that the hybrid capacitor prepared by the positive electrode material in the prior art has low energy density and cannot meet the application requirements of high power density working scenarios.

[0005] The first aspect of the present invention provides a hybrid capacitor composite positive electrode material, comprising nano-microstructured lithium cobalt oxide particles and nitrogen-doped activated carbon in a mass ratio of 80 to 95:5 to 20, wherein the nano-microstructured lithium cobalt oxide particles are micron-sized lithium cobalt oxide particles with a particle size of 2 to 5 μm formed by a combination of nano-scale lithium cobalt oxide particles, and the gram-specific capacity of the nitrogen-doped activated carbon is greater than 35 mAh / g.

[0006] The second aspect of the present invention provides a method for preparing the hybrid capacitor composite positive electrode material, comprising the following steps:

[0007] S1. Preparation of nitrogen-doped activated carbon

[0008] The quinoa is crushed and carbonized, and then Ca(OH)2 or K2CO3 is added, ground and mixed, and then a nitrogen source is added, ground and mixed to obtain a mixture, which is then carbonized to obtain a product, and the product is acid-washed to neutrality, washed and dried to obtain nitrogen-doped activated carbon;

[0009] S2. Preparation of nanostructured lithium cobalt oxide particles

[0010] Dissolve the cobalt source in deionized water to prepare a concentration of 0.1-0.5 mol / L Co 2+ aqueous solution, the prepared Co 2 + The aqueous solution is treated and then spray-dried to obtain a precursor, and the precursor is calcined at 400°C to 600°C under oxygen protection to obtain cobalt tetroxide; the cobalt tetroxide and lithium carbonate are ground and mixed, and then calcined at 600°C to 1000°C under oxygen protection, and nano-microstructured lithium cobalt oxide particles are obtained after grinding;

[0011] S3. Preparation of hybrid capacitor composite positive electrode materials

[0012] The nitrogen-doped activated carbon prepared by S1 and the nano-microstructured lithium cobalt oxide particles prepared by S2 were mixed in a mass ratio, placed in a high-energy ball mill in an agate jar, and ball-milled at a speed of 300-600 r / min for 2-8 h to obtain a composite positive electrode material based on ultrafast ion / electron synergistic energy storage effect.

[0013] Furthermore, the nitrogen source includes one or more of pyridine, urea, melamine, acrylamide, polyacrylamide, and polyvinylpyrrolidone.

[0014] Furthermore, the cobalt source is selected from one or more of cobalt nitrate hexahydrate, cobalt acetate tetrahydrate, cobalt carbonate, cobalt chloride hexahydrate, and cobalt sulfate heptahydrate.

[0015] Furthermore, the molar ratio of cobalt element to lithium element in S2 is 1:1.02-1.06.

[0016] Further, the product in S1 was acid washed with 0.1 mol / L hydrochloric acid.

[0017] Furthermore, the spray inlet temperature is 160°C to 180°C, the feed rate is 400 to 600 mL / h, and the precursor is spray dried.

[0018] Furthermore, the preparation steps of the nitrogen-doped activated carbon are specifically as follows:

[0019] S1-1, wash quinoa with deionized water and dry it at 100°C to 120°C, grind it and sieve the powder through a 100-mesh standard sieve, heat it to 400°C to 600°C under nitrogen protection and carbonize it for 3 to 6 hours at a heating rate of 5°C / min, and grind it to obtain quinoa carbon powder;

[0020] S1-2, grinding and mixing quinoa carbon powder and Ca(OH)2 or K2CO3 at a mass ratio of 1:1 to 3 to obtain a mixture A; grinding and mixing a nitrogen source and the mixture A at a mass ratio of 1:1 to 3 to obtain a mixture B;

[0021] S1-3. Heat the mixture B to 700°C-900°C under nitrogen protection and carbonize for 2-4h at a heating rate of 5°C / min and a nitrogen flow rate of 0.4-0.6L / min to obtain a product; the product is acid-washed until the solution is neutral, then rinsed with deionized water and dried at 100°C to obtain nitrogen-doped activated carbon.

[0022] Furthermore, the calcination time of the precursor in S2 is 2 to 4 hours, and the calcination time of the mixture of cobalt tetroxide and lithium carbonate is 6 to 12 hours.

[0023] Furthermore, the heating rate during calcination in S2 is 5°C / min, and the oxygen flow rate is 0.4-0.6 L / min.

[0024] The working principle of the present invention is:

[0025] Lithium cobalt oxide has a layered crystal structure. + and Co 2+ Atoms occupy octahedral coordination, Li + It can move in the lattice and has high stability during the charge and discharge process. The layered crystal structure of lithium cobalt oxide can be divided into a surface layer and a bulk layer. + In the surface layer, highly reversible deintercalation can be performed, and its behavior is similar to that of a capacitor, i.e., an intercalation-type pseudocapacitor; in the bulk layer, it is a typical diffusion behavior, i.e., a battery-type behavior. Therefore, as long as the particle size of the layered transition metal oxide material is reduced, Li + Reversible deintercalation is performed in the surface layer as much as possible to increase its embedded pseudocapacitive behavior, thereby improving the power performance of the positive electrode material. Therefore, this patent prepares a lithium cobalt oxide material with a nano-microstructure, and at the same time, composites it with nitrogen-doped activated carbon with a high specific surface area, and greatly improves the rate performance of the energy storage device by combining the embedded pseudocapacitive characteristics of nano-scale lithium cobalt oxide materials, the adsorption and desorption capacitance characteristics of nitrogen-doped activated carbon, and the ionic / electronic synergistic coupling of the battery characteristics of micron-scale lithium cobalt oxide materials.

[0026] The beneficial technical effects of the present invention are:

[0027] 1. The present invention prepares a composite material by optimizing the mixing of nanostructured lithium cobalt oxide (secondary particle size 50nm) and large-capacity nitrogen-doped activated carbon with a gram-specific capacity of >35mAh / g at a mass ratio of 80-95:5-20, and utilizes the high specific capacity of lithium cobalt oxide and the high rate characteristics of nitrogen-doped activated carbon to construct a hybrid capacitor composite positive electrode material with an ultrafast ion / electron synergistic energy storage effect. Compared with traditional hybrid capacitors, the energy density and power density are greatly improved. The hybrid capacitor assembled using the composite positive electrode material prepared by the present invention has an energy density of ≥100Wh / kg and a power density of ≥80kW / kg, which effectively improves the practical application capability of the hybrid capacitor and can meet the application requirements of high energy density and high power density working scenarios, such as frequency modulation (coordinated regulation of thermal storage) and peak shaving and valley filling in the field of energy storage, rail transit sources, etc.

[0028] 2. Using quinoa as the carbon source, nitrogen-doped activated carbon was prepared by Ca(OH)2 or K2CO3 activation method. The synthesized nitrogen-doped activated carbon has rich micro-mesoporous structure and rich specific surface area, which can provide a high specific capacity of 36mAh / g. Ultrasonic-assisted spray drying technology was used to synthesize nano-microsphere lithium cobalt oxide particles with a main particle size of 2-5μm assembled from 50nm secondary particles. The capacitance performance of nano-scale particles and the battery performance of micron-scale particles were used to provide high specific capacity and fast charge and discharge performance, and the specific capacity can reach 150mAh / g.

[0029] 3. The hybrid capacitor assembled with the positive electrode material with ultrafast ion / electron synergistic energy storage effect prepared by this patent has a 1C discharge capacity of about 1.3Ah, a 100C discharge capacity of more than 80% of the 1C discharge capacity, and a 1000C pulse power density of up to 2800W. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 This is a SEM photo of the composite material prepared in Example 1 of the present invention;

[0031] Figure 2 The 0.2C charge-discharge curve of the nanostructured lithium cobalt oxide and nitrogen-doped activated carbon material prepared in Example 1 of the present invention;

[0032] Figure 3 0.2C charge-discharge curves of the composite materials prepared in Examples 1 to 5 of the present invention;

[0033] Figure 4 1C discharge curves of Examples 1 to 4 of the present invention and Comparative Examples 1 to 3;

[0034] Figure 5 100C discharge curves of Application Examples 1 to 4 and Comparative Examples 1 to 3 of the present invention;

[0035] Figure 6 1000C pulse discharge curves of Application Examples 1 to 4 and Comparative Examples 1 to 3 of the present invention. DETAILED DESCRIPTION

[0036] The following is further described in detail through specific implementation methods:

[0037] Example 1: Preparation of hybrid capacitor composite positive electrode material

[0038] (1) Preparation of nitrogen-doped activated carbon:

[0039] The quinoa washed with deionized water was dried at 120°C for 8 hours, and the quinoa powder after passing through a 100-mesh standard sieve was placed in a porcelain crucible, and carbonized at 600°C for 4 hours under nitrogen protection with a heating rate of 5°C / min to obtain quinoa carbon powder;

[0040] The ground quinoa carbon powder and Ca(OH)2 were ground and mixed at a mass ratio of 1:1.5 to obtain a mixture A, and urea and the mixture A were ground and mixed at a mass ratio of 1:2 to obtain a mixture B;

[0041] Mixture B was placed in a porcelain crucible and heated to 900°C for carbonization for 2h under nitrogen protection, with a heating rate of 5°C / min and a nitrogen flow rate of 0.5L / min to obtain a product; the product was pickled with 0.1mol / L hydrochloric acid until the solution was neutral, and then rinsed with deionized water for 5 times; the rinsed product was dried at 100°C for 10h to obtain nitrogen-doped activated carbon, whose SEM photo is shown as follows Figure 1 As shown;

[0042] (2) Preparation of nanostructured lithium cobalt oxide particles:

[0043] Dissolve cobalt nitrate hexahydrate in deionized water to prepare a 0.5 mol / L concentration of Co 2+ aqueous solution, the prepared Co 2+ The aqueous solution was placed on an ultrasonic cleaning machine with an ultrasonic frequency of 50 kHz and an ultrasonic power of 60, and connected to a spray dryer for spray drying; the spray drying parameters were: spray inlet temperature of 180° C., feed rate of 500 mL / h, and precursor C was obtained after the spray drying was completed;

[0044] Precursor C was placed in a porcelain crucible, heated to 400°C and calcined for 2 h under oxygen protection, with a heating rate of 5°C / min and an oxygen flow rate of 0.4 L / min to obtain cobalt tetroxide;

[0045] Cobalt trioxide and lithium carbonate were fully ground and mixed in a mortar to obtain a mixture D. The molar ratio of lithium element to cobalt element was 1.05:1. Mixture D was placed in a porcelain crucible and heated to 600°C for 8 hours under oxygen protection, with a heating rate of 5°C / min and an oxygen flow rate of 0.4L / min to obtain nano-microstructured lithium cobalt oxide particles, the SEM photo of which is shown in the figure. Figure 2 As shown;

[0046] (3) Preparation of cathode materials based on ultrafast ion / electron synergistic energy storage effect:

[0047] The prepared nanostructured lithium cobalt oxide particles and nitrogen-doped activated carbon were placed in a high-energy ball mill with an agate jar at a mass ratio of 95:5, and ball-milled at a speed of 400 r / min for 4 h to obtain a nanostructured lithium cobalt oxide particle / nitrogen-doped activated carbon composite material, the SEM photo of which is shown in FIG. Figure 1 shown.

[0048] Example 2: Preparation of hybrid capacitor composite positive electrode material

[0049] (1) Preparation of nitrogen-doped activated carbon:

[0050] The quinoa washed with deionized water was dried at 100°C for 10 h, the quinoa powder passed through a 100-mesh standard sieve was placed in a porcelain crucible, and carbonized at 500°C for 6 h under nitrogen protection with a heating rate of 5°C / min to obtain quinoa carbon powder.

[0051] The ground quinoa carbon powder and K2CO3 are ground and mixed at a mass ratio of 1:2 to obtain a mixture A, and pyridine is ground and mixed with the mixture A at a mass ratio of 1:2 to obtain a mixture B;

[0052] Mixture B was placed in a porcelain crucible, heated to 800°C for carbonization for 3 h under nitrogen protection, with a heating rate of 5°C / min and a nitrogen flow rate of 0.5 L / min to obtain a product, which was pickled with 0.1 mol / L hydrochloric acid until the solution was neutral, and then rinsed with deionized water for 5, and the rinsed product was dried at 100°C for 10 h to obtain nitrogen-doped activated carbon;

[0053] (2) Preparation of nanostructured lithium cobalt oxide particles:

[0054] Dissolve cobalt chloride hexahydrate in deionized water to prepare a 0.4 mol / L concentration of Co 2+ aqueous solution, the prepared Co 2+ The aqueous solution was placed in an ultrasonic cleaning machine with an ultrasonic frequency of 50 kHz and an ultrasonic power of 70%, and connected to a spray dryer for spray drying. The spray drying parameters were: spray inlet temperature of 180°C and feed rate of 400 mL / h. After spray drying, precursor C was obtained;

[0055] Precursor C was placed in a porcelain crucible, heated to 500°C and calcined for 2 h under oxygen protection, with a heating rate of 5°C / min and an oxygen flow rate of 0.5 L / min to obtain cobalt tetroxide;

[0056] Cobalt trioxide and lithium carbonate were fully ground and mixed in a mortar to obtain a mixture D, wherein the molar ratio of lithium element to cobalt element was 1.03:1. The mixture D was placed in a porcelain crucible, heated to 800°C and calcined for 6 hours under oxygen protection, with a heating rate of 5°C / min and an oxygen flow rate of 0.5 L / min, to obtain nano-microstructured lithium cobalt oxide particles;

[0057] (3) Preparation of cathode materials based on ultrafast ion / electron synergistic energy storage effect:

[0058] The prepared nano-microstructured lithium cobalt oxide particles and nitrogen-doped activated carbon were placed in a high-energy ball mill with an agate jar at a mass ratio of 90:10, and ball-milled at a speed of 500 r / min for 3 h to obtain a nano-microstructured lithium cobalt oxide particle / nitrogen-doped activated carbon composite material.

[0059] Example 3: Preparation of hybrid capacitor composite positive electrode material

[0060] (1) Preparation of nitrogen-doped activated carbon:

[0061] The quinoa washed with deionized water was dried at 120°C for 8 hours, and the quinoa powder after passing through a 100-mesh standard sieve was placed in a porcelain crucible, and carbonized at 400°C for 6 hours under nitrogen protection with a heating rate of 5°C / min to obtain quinoa carbon powder;

[0062] The ground quinoa carbon powder and K2CO3 were ground and mixed at a mass ratio of 1:2.5 to obtain a mixture A, and polyvinyl pyrrolidone and the mixture A were ground and mixed at a mass ratio of 1:2.5 to obtain a mixture B;

[0063] Mixture B was placed in a porcelain crucible, heated to 900°C for carbonization for 2h under nitrogen protection, with a heating rate of 5°C / min and a nitrogen flow rate of 0.4L / min to obtain a product, which was pickled with 0.1mol / L hydrochloric acid until the solution was neutral, and then rinsed with deionized water for 5 times, and the rinsed product was dried at 100°C for 10h to obtain nitrogen-doped activated carbon;

[0064] (2) Preparation of nanostructured lithium cobalt oxide particles:

[0065] Dissolve cobalt acetate tetrahydrate in deionized water to prepare a 0.3 mol / L concentration of Co 2+ aqueous solution, the prepared Co 2+The aqueous solution was placed on an ultrasonic cleaning machine with an ultrasonic frequency of 50 kHz and an ultrasonic power of 80%, and connected to a spray dryer for spray drying. The spray drying parameters were: a spray inlet temperature of 160° C. and a feed rate of 500 mL / h. After the spray drying was completed, a precursor C was obtained.

[0066] Precursor C was placed in a porcelain crucible, heated to 400°C and calcined for 4 hours under oxygen protection, with a heating rate of 5°C / min and an oxygen flow rate of 0.6L / min to obtain cobalt tetroxide;

[0067] Cobalt trioxide and lithium carbonate were fully ground and mixed in a mortar to obtain a mixture D, wherein the molar ratio of lithium element to cobalt element was 1.04:1. The mixture D was placed in a porcelain crucible, heated to 600°C and calcined for 8 hours under oxygen protection, with a heating rate of 5°C / min and an oxygen flow rate of 0.6 L / min, to obtain nano-microstructured lithium cobalt oxide particles;

[0068] (3) Preparation of cathode materials based on ultrafast ion / electron synergistic energy storage effect:

[0069] The prepared nano-microstructured lithium cobalt oxide particles and nitrogen-doped activated carbon were placed in a high-energy ball mill with an agate jar at a mass ratio of 85:15, and ball-milled at a speed of 600 r / min for 2 h to obtain a nano-microstructured lithium cobalt oxide particle / nitrogen-doped activated carbon composite material.

[0070] Example 4: Preparation of hybrid capacitor composite positive electrode material

[0071] (1) Preparation of nitrogen-doped activated carbon:

[0072] The quinoa washed with deionized water was dried at 100°C for 10 hours, and the quinoa powder after passing through a 100-mesh standard sieve was placed in a porcelain crucible, and carbonized at 500°C for 4 hours under nitrogen protection with a heating rate of 5°C / min to obtain quinoa carbon powder;

[0073] Grind and mix the ground quinoa carbon powder and Ca(OH)2 at a mass ratio of 1:3 to obtain a mixture A, and grind and mix melamine and the mixture A at a mass ratio of 1:3 to obtain a mixture B;

[0074] Mixture B was placed in a porcelain crucible, heated to 800°C for carbonization for 4 hours under nitrogen protection, with a heating rate of 5°C / min and a nitrogen flow rate of 0.5L / min to obtain a product, which was pickled with 0.1mol / L hydrochloric acid until the solution was neutral, and then rinsed with deionized water for 5 times, and the rinsed product was dried at 100°C for 10 hours to obtain nitrogen-doped activated carbon;

[0075] (2) Preparation of nanostructured lithium cobalt oxide particles:

[0076] Dissolve cobalt carbonate in deionized water to prepare a 0.5 mol / L concentration of Co 2+ aqueous solution, the prepared Co 2+ The aqueous solution was placed in an ultrasonic cleaning machine with an ultrasonic frequency of 50 kHz and an ultrasonic power of 75%, and connected to a spray dryer for spray drying. The spray drying parameters were: spray inlet temperature of 180°C and feed rate of 500 mL / h. After the spray drying was completed, precursor C was obtained;

[0077] Precursor C was placed in a porcelain crucible, heated to 600°C and calcined for 4 hours under oxygen protection, with a heating rate of 5°C / min and an oxygen flow rate of 0.5L / min to obtain cobalt tetroxide;

[0078] Cobalt trioxide and lithium carbonate were fully ground and mixed in a mortar to obtain a mixture D. The molar ratio of lithium element to cobalt element was 1.05:1. The mixture D was placed in a porcelain crucible, heated to 800°C and calcined for 6 hours under oxygen protection, with a heating rate of 5°C / min and an oxygen flow rate of 0.5L / min to obtain nano-microstructured lithium cobalt oxide particles.

[0079] (3) Preparation of cathode materials based on ultrafast ion / electron synergistic energy storage effect:

[0080] The prepared nano-microstructured lithium cobalt oxide particles and nitrogen-doped activated carbon were placed in a high-energy ball mill with an agate jar at a mass ratio of 80:20, and ball-milled at a speed of 400 r / min for 6 h to obtain a nano-microstructured lithium cobalt oxide particle / nitrogen-doped activated carbon composite material.

[0081] Example 5: Preparation of hybrid capacitor composite positive electrode material

[0082] The difference from Example 4 is that the nanostructured lithium cobalt oxide particles and nitrogen-doped activated carbon prepared in Example 4 are placed in a high-energy ball mill with an agate jar at a mass ratio of 50:50, and ball milled at a speed of 400 r / min for 6 h to obtain a nanostructured lithium cobalt oxide particle / nitrogen-doped activated carbon composite material.

[0083] Application Example 1: Preparation of a battery cell using the composite positive electrode material of Example 1

[0084] The nanostructured lithium cobalt oxide particles / nitrogen-doped activated carbon composite material prepared in Example 1 is used as the positive electrode active material, and the positive electrode sheet is prepared according to the ratio of active material: conductive agent: binder = 95:3:2. The hard carbon material is used as the negative electrode active material, and the negative electrode sheet is prepared according to the ratio of active material: conductive agent: binder = 96:2:2, wherein the conductive agent and the binder are carbon nanotubes (CNTs) and polyvinylidene fluoride (PVDF), respectively. The positive electrode sheet and the negative electrode sheet are cut into a certain size by a mold, and then stacked by a semi-automatic stacking machine to prepare a battery cell; after the battery cell is welded with pole ears, packaged, injected, and aged, it is formed, and the capacity and rate performance can be tested after the formation.

[0085] Application Example 2: Preparation of a battery cell using the composite positive electrode material of Example 2

[0086] The nanostructured lithium cobalt oxide particles / nitrogen-doped activated carbon composite material prepared in Example 2 is used as the positive electrode active material, and the positive electrode sheet is prepared according to the ratio of active material: conductive agent: binder = 95:3:2. The hard carbon material is used as the negative electrode active material, and the negative electrode sheet is prepared according to the ratio of active material: conductive agent: binder = 96:2:2, wherein the conductive agent and the binder are carbon nanotubes (CNTs) and polyvinylidene fluoride (PVDF), respectively. The positive electrode sheet and the negative electrode sheet are cut into a certain size by a mold, and then stacked by a semi-automatic stacking machine to prepare a battery cell; after the battery cell is welded with pole ears, encapsulated, injected, and aged, it is formed, and the capacity and rate performance can be tested after the formation.

[0087] Application Example 3: Preparation of a battery cell using the composite positive electrode material of Example 3

[0088] The nanostructured lithium cobalt oxide particles / nitrogen-doped activated carbon composite material prepared in Example 3 is used as the positive electrode active material, and the positive electrode sheet is prepared according to the ratio of active material: conductive agent: binder = 95:3:2. The hard carbon material is used as the negative electrode active material, and the negative electrode sheet is prepared according to the ratio of active material: conductive agent: binder = 96:2:2, wherein the conductive agent and the binder are carbon nanotubes (CNTs) and polyvinylidene fluoride (PVDF), respectively. The positive electrode sheet and the negative electrode sheet are cut into a certain size by a mold, and then stacked by a semi-automatic stacking machine to prepare a battery cell; after the battery cell is welded with pole ears, packaged, injected, and aged, it is formed, and the capacity and rate performance can be tested after the formation.

[0089] Application Example 4: Preparation of a battery cell using the composite positive electrode material of Example 4

[0090] The nanostructured lithium cobalt oxide particles / nitrogen-doped activated carbon composite material prepared in Example 4 is used as the positive electrode active material, and the positive electrode sheet is prepared according to the ratio of active material: conductive agent: binder = 95:3:2. The hard carbon material is used as the negative electrode active material, and the negative electrode sheet is prepared according to the ratio of active material: conductive agent: binder = 96:2:2, wherein the conductive agent and the binder are carbon nanotubes (CNTs) and polyvinylidene fluoride (PVDF), respectively. The positive electrode sheet and the negative electrode sheet are cut into a certain size by a mold, and then stacked by a semi-automatic stacking machine to prepare a battery cell; after the battery cell is welded with pole ears, packaged, injected, and aged, it is formed, and the capacity and rate performance can be tested after the formation.

[0091] Comparative Example 1: Preparation of lithium cobalt oxide / activated carbon composite materials and battery cells

[0092] Commercial lithium cobalt oxide (particle size 7-12μm) and commercial activated carbon (particle size 5-10μm) were placed in a high-energy ball mill with an agate jar at a mass ratio of 95:5, and ball-milled at a speed of 600r / min for 2h to obtain a lithium cobalt oxide / activated carbon composite material. The obtained lithium cobalt oxide / activated carbon composite material was used as the positive electrode active material, and the positive electrode sheet was prepared according to the ratio of active material: conductive agent: binder = 95:3:2. The hard carbon material was used as the negative electrode active material, and the negative electrode sheet was prepared according to the ratio of active material: conductive agent: binder = 96:2:2, wherein the conductive agent and binder were carbon nanotubes (CNTs) and polyvinylidene fluoride (PVDF) respectively. The positive and negative electrode sheets were cut into a certain size through a mold, and then stacked by a semi-automatic stacking machine to prepare a battery cell; after welding the pole ears, encapsulating, injecting liquid, and aging, the battery cell was formed, and the capacity and rate performance test could be carried out after the formation.

[0093] Comparative Example 2: Preparation of a battery cell using the composite positive electrode material of Example 5

[0094] The nanostructured lithium cobalt oxide particles / nitrogen-doped activated carbon composite material prepared in Example 5 is used as the positive electrode active material, and the positive electrode sheet is prepared according to the ratio of active material: conductive agent: binder = 95:3:2. The hard carbon material is used as the negative electrode active material, and the negative electrode sheet is prepared according to the ratio of active material: conductive agent: binder = 96:2:2, wherein the conductive agent and the binder are carbon nanotubes (CNTs) and polyvinylidene fluoride (PVDF), respectively. The positive electrode sheet and the negative electrode sheet are cut into a certain size through a mold, and then stacked by a semi-automatic stacking machine to prepare a battery cell; after the battery cell is welded with pole ears, packaged, injected, and aged, it is formed, and the capacity and rate performance can be tested after the formation.

[0095] Comparative Example 3: Preparation of a battery cell using the lithium cobalt oxide material of Example 5

[0096] The nanostructured lithium cobalt oxide granular material prepared in Example 5 is used as the positive electrode active material, and the positive electrode sheet is prepared according to the ratio of active material: conductive agent: binder = 95:3:2. The hard carbon material is used as the negative electrode active material, and the negative electrode sheet is prepared according to the ratio of active material: conductive agent: binder = 96:2:2, wherein the conductive agent and the binder are carbon nanotubes (CNTs) and polyvinylidene fluoride (PVDF), respectively. The positive electrode sheet and the negative electrode sheet are cut into a certain size by a mold, and then stacked by a semi-automatic stacking machine to prepare a battery cell; after the battery cell is welded with the pole ear, encapsulated, injected, and aged, it is formed, and the capacity and rate performance can be tested after the formation.

[0097] The SEM image of the nanostructured lithium cobalt oxide particles / nitrogen-doped activated carbon composite material prepared in Example 1 is as follows: Figure 1 As shown, it can be seen that the nano-structured lithium cobalt oxide particles and the nitrogen-doped activated carbon are evenly mixed. By utilizing the embedded pseudocapacitance characteristics of nano-scale lithium cobalt oxide materials, the adsorption and desorption capacitance characteristics of nitrogen-doped activated carbon, and the ionic / electronic synergistic coupling of the battery characteristics of micron-scale lithium cobalt oxide materials, the rate performance of the energy storage device can be greatly improved.

[0098] Test Example 1 Preparation of Nanostructured LiCoO2 Particles and Nitrogen-doped Activated Carbon Materials 0.2C Charge-Discharge Curves Figure 2 As shown, the discharge specific capacities are 36 mAh / g and 150 mAh / g respectively.

[0099] The 0.2C charge-discharge curves of the composite materials prepared in Test Examples 1 to 5 are as follows: Figure 3 As shown, the discharge specific capacities are 140mAh / g, 134mAh / g, 129mAh / g, 126mAh / g and 92mAh / g respectively.

[0100] The positive electrode sheet assembled hybrid capacitor prepared by the positive electrode materials of Application Examples 1 to Application Examples 4 and Comparative Examples 1 to Comparative Examples 3 was tested under 1C discharge (the discharge current was set to 1.3A and the voltage range was 4.2 to 2.5V). The discharge curve is shown in the attached figure. Figure 4 As shown in the attached Figure 4 It can be seen that the discharge capacity of the positive electrode sheet assembled hybrid capacitors prepared from the positive electrode materials of Examples 1 to 4 and Comparative Examples 1 to 3 at a rate of 1C is about 1.3Ah, the discharge voltage platform is 3.6V, and the battery mass is about 33g. According to the specific energy calculation formula E=(discharge capacity*platform voltage) / battery mass, the specific energy of the battery is calculated to be E=1.3Ah*3.6V / 33g=141.8Wh / kg.

[0101] The positive electrode sheet assembled hybrid capacitor prepared by the positive electrode materials of Application Examples 1 to Application Examples 4 and Comparative Examples 1 to Comparative Examples 3 was tested at 100C discharge (the discharge current was set to 110A and the voltage range was 4.2-2.5V). The discharge curve is shown in the attached figure. Figure 5 As shown in the attached Figure 5 It can be seen that the positive electrode sheet assembled hybrid capacitors prepared by the positive electrode materials of Application Examples 1 to Application Examples 4 have discharge capacity retention rates of 83.02%, 85.2%, 86.27% and 80.05% at 100C, respectively, which are much higher than the 100C discharge capacity retention rates of Comparative Examples 1 to 3 (67.27%, 70.12% and 60.1%, respectively), indicating that the composite positive electrode material prepared by this patent improves the rate performance of the hybrid capacitor.

[0102] The positive electrode sheet assembled hybrid capacitor prepared by the positive electrode materials of Application Examples 1 to Application Examples 4 and Comparative Examples 1 to Comparative Examples 3 was tested for discharge at 1000C (the discharge current was set to 1000A and the voltage range was 4.2 to 2.5V). The discharge curve is shown in the attached figure. Figure 6 As shown in the attached Figure 6 It can be seen that the discharge power of the hybrid capacitor assembled with the positive electrode sheets prepared with the positive electrode materials of Application Examples 1 to 4 is about 2800W, the battery mass is about 33g, and the specific power is >80kW / kg, which is much higher than the discharge specific power of Comparative Examples 1 to 3, indicating that the composite positive electrode material prepared by this patent improves the power performance of the hybrid capacitor.

Claims

1. A hybrid capacitor composite positive electrode material, characterized in that: The invention comprises nano-microstructured lithium cobalt oxide particles and nitrogen-doped activated carbon in a mass ratio of 80-95:5-20, wherein the nano-microstructured lithium cobalt oxide particles are micron-sized lithium cobalt oxide particles with a particle size of 2-5 μm formed by combining nano-sized lithium cobalt oxide particles, and the gram specific capacity of the nitrogen-doped activated carbon is greater than 35 mAh / g.

2. The method for preparing a hybrid capacitor composite positive electrode material according to claim 1, characterized in that The following steps are involved: S1. Preparation of nitrogen-doped activated carbon The quinoa is crushed and carbonized, and then Ca(OH)2 or K2CO3 is added, ground and mixed, and then a nitrogen source is added, ground and mixed to obtain a mixture, which is then carbonized to obtain a product, and the product is acid-washed to neutrality, washed and dried to obtain nitrogen-doped activated carbon; S2. Preparation of nanostructured lithium cobalt oxide particles Dissolve the cobalt source in deionized water to prepare a concentration of 0.1-0.5 mol / L Co 2+ aqueous solution, the prepared Co 2+ The aqueous solution is treated and then spray-dried to obtain a precursor, and the precursor is calcined at 400°C to 600°C under oxygen protection to obtain cobalt tetroxide; the cobalt tetroxide and lithium carbonate are ground and mixed, and then calcined at 600°C to 1000°C under oxygen protection, and nano-microstructured lithium cobalt oxide particles are obtained after grinding; S3. Preparation of hybrid capacitor composite positive electrode materials The nitrogen-doped activated carbon prepared by S1 and the nano-microstructured lithium cobalt oxide particles prepared by S2 were mixed in a mass ratio, placed in a high-energy ball mill in an agate jar, and ball-milled at a speed of 300-600 r / min for 2-8 h to obtain a composite positive electrode material based on ultrafast ion / electron synergistic energy storage effect.

3. The preparation method according to claim 2, characterized in that: The nitrogen source includes one or more of pyridine, urea, melamine, acrylamide, polyacrylamide, and polyvinyl pyrrolidone.

4. The preparation method according to claim 2, characterized in that: The cobalt source is selected from one or more of cobalt nitrate hexahydrate, cobalt acetate tetrahydrate, cobalt carbonate, cobalt chloride hexahydrate, and cobalt sulfate heptahydrate.

5. The preparation method according to claim 4, characterized in that: The molar ratio of cobalt element to lithium element in S2 is 1:1.02-1.

06.

6. The preparation method according to claim 2, characterized in that: The product in S1 was acid washed with 0.1 mol / L hydrochloric acid.

7. The preparation method according to claim 2, characterized in that: The parameters of spray drying in S2 are: spray inlet temperature 160°C to 180°C, feed rate 400 to 600 mL / h, and the precursor after spray drying.

8. The preparation method according to claim 2, characterized in that: The preparation steps of the nitrogen-doped activated carbon are specifically as follows: S1-1, wash quinoa with deionized water and dry it at 100°C to 120°C, grind it and sieve the powder through a 100-mesh standard sieve, heat it to 400°C to 600°C under nitrogen protection and carbonize it for 3 to 6 hours at a heating rate of 5°C / min, and grind it to obtain quinoa carbon powder; S1-2, grinding and mixing quinoa carbon powder and Ca(OH)2 or K2CO3 at a mass ratio of 1:1 to 3 to obtain a mixture A; grinding and mixing a nitrogen source and the mixture A at a mass ratio of 1:1 to 3 to obtain a mixture B; S1-3, heating the mixture B to 700°C-900°C under nitrogen protection and carbonizing for 2-4h at a heating rate of 5°C / min and a nitrogen flow rate of 0.4-0.6L / min to obtain a product; The product was acid-washed until the solution was neutral, then rinsed with deionized water and dried at 100° C. to obtain nitrogen-doped activated carbon.

9. The preparation method according to claim 8, characterized in that: The calcination time of the precursor in S2 is 2 to 4 hours, and the calcination time of the mixture of cobalt tetroxide and lithium carbonate is 6 to 12 hours.

10. The preparation method according to claim 9, characterized in that: The heating rate during calcination in S2 is 5°C / min, and the oxygen flow rate is 0.4-0.6 L / min.

Citation Information

Patent Citations

  • Anode material for super capacitor battery and preparing method thereof

    CN101335346A

  • Nickel cobalt lithium aluminate positive material and preparation method thereof

    CN103985856A

  • Preparation method of broad-spectrum and ultrahigh adsorption capacity activated carbon material

    CN107954424A

  • Spray drying preparation method of lithium transition metal acid salt cathode material and lithium ion battery using same

    CN112635747A

  • Lithium cobaltate aggregate, cobalt oxide aggregate, method for manufacturing the same and lithium cell using lithium cobaltate aggregate

    JP2002060225A