Low-on-resistance semiconductor power device and preparation method thereof

By etching trenches on the semiconductor substrate and depositing high-purity silicon and germanium epitaxial layers, controlling temperature and gas flow, the problem of P-type materials expansation in traditional high-temperature epitaxial is solved, and low on-resistance and high performance are achieved Preparation of semiconductor power devices.

CN118943006AActive Publication Date: 2024-11-12THING ELEMENT SEMICON TECH (QINGDAO) CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202410991029.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-12
Estimated Expiration
2044-07-23

Smart Images

  • Figure CN118943006A_ABST
    Figure CN118943006A_ABST
Patent Text Reader

Abstract

The invention relates to a preparation method of a low-on-resistance semiconductor power device. The preparation method comprises the following steps: etching a semiconductor substrate to form a groove; depositing high-purity undoped silicon in the groove to form an intrinsic silicon epitaxial layer; depositing a germanium-silicon epitaxial layer on the intrinsic silicon epitaxial layer, controlling the temperature below 800 DEG C, and controlling the germanium content lt; 20%, boron concentration lt; the preparation method comprises the following steps of: performing a low-pressure chemical vapor deposition (LPCVD) method, a plasma enhanced chemical vapor deposition (PECVD) method, a molecular beam epitaxy (MBE) method, a liquid phase epitaxy (LPE) method or a physical vapor deposition (PVD) method; wherein the total gas pressure in the LPCVD method is less than 200 torr. By controlling the flow of silane and germane gas, the germane gas accounts for less than 20% of the total gas flow. According to the invention, the technical problem that the substrate resistance is affected due to external expansion of the P-type semiconductor material in the traditional high-temperature epitaxy process is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of semiconductor technology, and in particular relates to a low on-resistance semiconductor power device and a preparation method thereof. Background Art

[0002] The development of semiconductor power devices has been moving towards increasing breakdown voltage and reducing on-resistance. With the proposal and development of superjunction theory, semiconductor power devices have lower on-resistance under the same withstand voltage conditions, greatly breaking through the traditional "silicon limit". At present, the manufacturing process of superjunction devices mainly includes multiple epitaxy technology, deep trench etching and filling technology, and high-energy particle injection technology.

[0003] The emergence of deep trench etch filling technology solves the problem of uneven superjunction structure formed in multiple epitaxial processes and has become the mainstream process choice for superjunction device manufacturing. However, when using deep trench etch filling technology, the traditional single high-temperature epitaxial process has some problems. During the epitaxial process, high temperature will cause the P-type semiconductor material to expand into the silicon on both sides of the deep trench, thereby affecting the resistivity of the substrate. This phenomenon leads to unstable device performance and limits the further improvement of superjunction devices. Summary of the invention

[0004] In view of the deficiencies existing in the related art, the present invention provides a low on-resistance semiconductor power device and a method for preparing the same, which solves the technical problem that the substrate resistance is affected by the expansion of P-type semiconductor materials in the traditional high-temperature epitaxial process.

[0005] In a possible embodiment, a method for preparing a low on-resistance semiconductor power device is provided, comprising the following steps: etching a groove on a semiconductor substrate; depositing high-purity undoped silicon in the groove to form an intrinsic silicon epitaxial layer; depositing a germanium silicon epitaxial layer on the intrinsic silicon epitaxial layer, controlling the temperature to be below 800°C, controlling the germanium content of the germanium silicon epitaxial layer to be less than 20%, and the boron concentration to be less than 1E18 cm -3 The deposition method includes any one of the following: low pressure chemical vapor deposition (LPCVD), plasma enhanced chemical vapor deposition (PECVD), molecular beam epitaxy (MBE), liquid phase epitaxy (LPE), physical vapor deposition (PVD); wherein the total gas pressure in the low pressure chemical vapor deposition (LPCVD) method is less than 200 torr; wherein the low pressure chemical vapor deposition method controls the germanium content of the germanium silicon epitaxial layer to be less than 20% and includes: introducing silane (SiH4) gas and germane (GeH4) gas into the reaction chamber and controlling the flow rate of the silane gas; controlling the flow rate of the germane gas so that the proportion of the germane gas in the total gas flow rate is less than 20%; and adjusting the temperature in the reaction chamber to keep it below 800°C.

[0006] In one possible embodiment, the low pressure chemical vapor deposition method controls the boron concentration of the germanium silicon epitaxial layer to be less than 1E18 cm -3 The method comprises: introducing borane (B2H6) gas into a reaction chamber during the deposition of a germanium silicon epitaxial layer; adjusting the flow rate of the borane gas to keep the boron concentration at less than 1E18 cm -3 .

[0007] In one possible embodiment, high-purity undoped silicon is deposited in the groove to form an intrinsic silicon epitaxial layer, including: performing a preheat treatment in a reaction chamber to allow the substrate surface to reach a deposition temperature; introducing high-purity silane (SiH4) gas into the reaction chamber; and adjusting the temperature in the reaction chamber to below 800°C to allow the intrinsic epitaxial layer to reach a set thickness.

[0008] In one possible implementation, the total gas pressure in the low pressure chemical vapor deposition (LPCVD) method is less than 200 torr.

[0009] In a possible implementation, the low pressure chemical vapor deposition method controls the germanium content of the germanium silicon epitaxial layer to be less than 20%.

[0010] In a possible embodiment, a low on-resistance semiconductor power device is provided, comprising: a semiconductor substrate; a groove etched on the semiconductor substrate; a high-purity undoped intrinsic silicon epitaxial layer in the groove; a germanium silicon epitaxial layer in the groove, the germanium silicon epitaxial layer being deposited on the intrinsic silicon epitaxial layer; wherein the high-purity undoped intrinsic silicon epitaxial layer and the germanium silicon epitaxial layer in the groove are prepared by a method for preparing a low on-resistance semiconductor power device.

[0011] Based on the above technical scheme, the preparation method of the low on-resistance semiconductor power device of the present invention, by etching grooves on the semiconductor substrate, depositing high-purity undoped silicon to form an intrinsic silicon epitaxial layer, and depositing a germanium silicon epitaxial layer on the intrinsic silicon epitaxial layer, solves the problem of the traditional method that a single high-temperature epitaxy causes the P-type semiconductor material to expand into the silicon on both sides of the deep trench during the epitaxy process, so as to achieve the effect of accurately controlling the epitaxial morphology, and can realize the production of superjunction devices with smaller cell sizes, and a single intrinsic semiconductor epitaxy can effectively avoid the influence of deep trench sidewall defects on epitaxial filling. BRIEF DESCRIPTION OF THE DRAWINGS

[0012] The drawings described herein are used to provide a further understanding of the present invention and constitute a part of this application. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:

[0013] Figure 1 A schematic diagram of the preparation process of a low on-resistivity semiconductor power device according to an embodiment.

[0014] In the figure:

[0015] 10. Intrinsic silicon epitaxial layer; 20. Silicon germanium epitaxial layer; 30. Substrate; 40. Trench. DETAILED DESCRIPTION

[0016] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0017] In the description of the present invention, it should be understood that the terms "center", "lateral", "longitudinal", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside" and the like indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present invention.

[0018] The terms "first", "second", and "third" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the technical features indicated. Thus, a feature defined as "first", "second", and "third" may explicitly or implicitly include one or more of the features.

[0019] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a direct connection, or an indirect connection through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0020] In order to solve the technical problem that the substrate resistance is affected by the outward expansion of P-type semiconductor materials in the traditional high-temperature epitaxial process, the present application provides a low on-resistance semiconductor power device and a preparation method thereof.

[0021] According to the first aspect of the present application, a method for preparing a low on-resistance semiconductor power device is provided. Figure 1The method comprises the following steps: etching a groove 40 on a semiconductor substrate 30; depositing high-purity undoped silicon in the groove to form an intrinsic silicon epitaxial layer 10; depositing a germanium silicon epitaxial layer 20 on the intrinsic silicon epitaxial layer 10, controlling the temperature below 800°C, controlling the germanium content of the germanium silicon epitaxial layer to be less than 20%, and the boron concentration to be less than 1E18 cm -3 The deposition method includes any one of the following: low pressure chemical vapor deposition (LPCVD), plasma enhanced chemical vapor deposition (PECVD), molecular beam epitaxy (MBE), liquid phase epitaxy (LPE), physical vapor deposition (PVD); wherein the total gas pressure in the low pressure chemical vapor deposition (LPCVD) method is less than 200 torr; wherein the low pressure chemical vapor deposition method controls the germanium content of the germanium silicon epitaxial layer to be less than 20% and includes: introducing silane (SiH4) gas and germane (GeH4) gas into the reaction chamber and controlling the flow rate of the silane gas; controlling the flow rate of the germane gas so that the proportion of the germane gas in the total gas flow rate is less than 20%; and adjusting the temperature in the reaction chamber to keep it below 800°C.

[0022] In the above scheme, first, a groove is etched on the semiconductor substrate to provide an appropriate structure to accommodate the subsequently deposited materials. Then, high-purity undoped silicon is deposited in the groove to form an intrinsic silicon epitaxial layer, ensuring the high purity and low defect density of the substrate. Next, a germanium silicon epitaxial layer is deposited on the intrinsic silicon epitaxial layer. By controlling the deposition temperature below 800°C, for example, 720°C, and adjusting the germanium gas flow rate, the germanium content is kept below 20% to ensure that the germanium silicon epitaxial layer has the doping concentration required to meet the charge balance. Using a low-pressure chemical vapor deposition method, the total gas pressure is controlled below 200 torr, which further optimizes the quality and performance of the epitaxial layer. Through a series of precisely controlled deposition steps, a semiconductor power device with low on-resistance is formed. See Figure 1 In the figure, the three figures are schematic diagrams of depositing an intrinsic silicon epitaxial layer 10 in the trench, depositing a silicon germanium epitaxial layer 20 and after an annealing process.

[0023] This method can reduce the on-resistance of semiconductor power devices, improve the working efficiency and performance stability of the devices, and further reduce the size of the device cell. By controlling the temperature and gas flow during the deposition process, a high-quality germanium silicon epitaxial layer can be obtained to ensure its excellent electrical properties.

[0024] When depositing the germanium silicon epitaxial layer, different deposition methods can be selected, such as plasma enhanced chemical vapor deposition (PECVD), molecular beam epitaxy (MBE), liquid phase epitaxy (LPE) or physical vapor deposition (PVD), and adjusted according to specific needs and equipment conditions. For different production environments, the deposition parameters can be further optimized by adjusting the temperature and gas flow in the reaction chamber. In addition to silane and germane, other suitable gases can be selected as reaction source materials to achieve similar technical effects.

[0025] In one possible embodiment, the low pressure chemical vapor deposition method controls the boron concentration of the germanium silicon epitaxial layer to be less than 1E18 cm -3 The method comprises: introducing borane (B2H6) gas into a reaction chamber during the deposition of a germanium silicon epitaxial layer; adjusting the flow rate of the borane gas to keep the boron concentration at less than 1E18 cm -3 .

[0026] This method introduces borane (B2H6) gas during the deposition of the germanium silicon epitaxial layer to achieve precise control of the boron concentration in the epitaxial layer. Boron, as a dopant, can adjust the electrical properties of semiconductor materials. By controlling the flow rate of borane gas, the boron concentration is maintained at 1E18 cm -3 In the following, it can be ensured that the conductive properties of the silicon germanium epitaxial layer meet the design requirements.

[0027] By controlling the boron concentration, the electrical properties of the germanium silicon epitaxial layer can be improved, the on-resistance of the device can be reduced, and the working efficiency and reliability of the power device can be improved. The low-pressure chemical vapor deposition method is used to make the entire process more controllable and meet the needs of large-scale production.

[0028] In addition to using borane (B2H6) gas as a doping source, other suitable dopants such as boron trifluoride (BF3) can also be selected. By adjusting the type and flow of the dopant, the electrical properties of the epitaxial layer can be further optimized. The deposition method can also choose other suitable technologies, such as molecular beam epitaxy (MBE) or plasma enhanced chemical vapor deposition (PECVD), to adapt to different production environments and needs.

[0029] In one possible embodiment, high-purity undoped silicon is deposited in the groove to form an intrinsic silicon epitaxial layer, including: performing a preheat treatment in a reaction chamber to allow the substrate surface to reach a deposition temperature; introducing high-purity silane (SiH4) gas into the reaction chamber; and adjusting the temperature in the reaction chamber to below 800°C to allow the intrinsic epitaxial layer to reach a set thickness.

[0030] In the above scheme, a high-purity intrinsic silicon epitaxial layer is formed by controlling the temperature and gas flow in the reaction chamber. First, a preheat treatment is performed in the reaction chamber to make the substrate surface reach a suitable deposition temperature. Then, high-purity silane (SiH4) gas is introduced into the reaction chamber, and a high-purity undoped silicon layer is formed in the groove by chemical vapor deposition. By adjusting the temperature in the reaction chamber below 800°C, the intrinsic epitaxial layer reaches a set thickness, effectively avoiding the influence of deep groove sidewall defects on epitaxial filling, and ensuring the uniformity and high quality of the epitaxial layer.

[0031] This method can effectively control the purity and thickness of the silicon epitaxial layer and improve the electrical properties and structural integrity of the epitaxial layer. Through preheating and temperature control, the introduction of impurities and lattice defects are reduced, and the conductivity and reliability of power devices are improved. In addition, the use of high-purity silane as a reaction source ensures the high purity and low defect density of the epitaxial layer, which is suitable for the manufacture of high-performance semiconductor devices.

[0032] During the preheat treatment and deposition process, different heating methods can be selected, such as infrared heating or resistance heating, to adapt to different equipment conditions. High-purity silane (SiH4) gas can also be replaced with other high-purity silicon sources, such as dichlorosilane (SiH2Cl2) or trichlorosilane (SiHCl3), according to specific process requirements. The deposition temperature range can be appropriately adjusted according to material properties and equipment conditions to further optimize the performance of the epitaxial layer.

[0033] In one possible implementation, the total gas pressure in the low pressure chemical vapor deposition (LPCVD) method is lower than 200 torr.

[0034] For example, it may be 120 torr.

[0035] This method makes the chemical vapor deposition process more stable and controllable by controlling the total gas pressure below 200 torr. Under low pressure conditions, molecular collisions of the reaction gas are reduced and the deposition rate is precisely controlled, which is conducive to the formation of high-quality germanium silicon epitaxial layers.

[0036] By controlling the total gas pressure below 200 torr, the uniformity and quality of the SiGe epitaxial layer can be further improved, defects and stress can be reduced, and the electrical performance and reliability of semiconductor devices can be improved. In addition, low pressure conditions help reduce reaction temperature and energy consumption, increasing the economy and environmental friendliness of the process.

[0037] The total gas pressure setting can be adjusted according to the specific equipment and process requirements, usually ranging from 100 torr to 200 torr. Under certain conditions, lower pressures can also be selected to optimize the deposition process. In addition, different deposition methods (such as PECVD, MBE, etc.) may have different requirements for gas pressure, and the process can be adjusted according to specific needs.

[0038] In a possible implementation, the low pressure chemical vapor deposition method controls the germanium content of the germanium silicon epitaxial layer to be less than 20%.

[0039] The method maintains the germanium content in the germanium silicon epitaxial layer below 20%, for example, 15%, by precisely controlling the flow rate of germanium (GeH4) gas. The specific steps include simultaneously introducing silane (SiH4) gas and germanium (GeH4) gas into the reaction chamber, and adjusting the flow rate ratio of the two gases so that the proportion of germanium gas in the total gas flow rate reaches a set value.

[0040] By introducing a germanium content of less than 20%, the epitaxial temperature can be effectively reduced, so that the P-type material does not expand at all, and the doping concentration of the epitaxial material is guaranteed to be the set value to achieve charge balance and improve the conductivity and stability of the device. The optimization of the germanium content can effectively reduce the epitaxial temperature, so that the P-type material does not expand at all, improve the performance of semiconductor power devices, and extend their service life, which is suitable for the manufacture of high-performance electronic devices.

[0041] The germanium content can be controlled within a certain range according to specific needs, such as between 10% and 20%, to adapt to different application scenarios and device requirements. The gas source for introducing germanium can also choose other suitable compounds, such as germanium tetrafluoride (GeF4), and adjust according to specific process requirements. Different deposition methods (such as MBE, LPE, etc.) may have different ways of controlling the germanium content, which can be optimized according to specific circumstances.

[0042] In a possible embodiment, a low on-resistance semiconductor power device is provided, characterized in that it includes: a semiconductor substrate 30; a groove 40 etched on the semiconductor substrate; a high-purity undoped intrinsic silicon epitaxial layer 10 in the groove; a germanium silicon epitaxial layer 20 in the groove, the germanium silicon epitaxial layer being deposited on the intrinsic silicon epitaxial layer; wherein the high-purity undoped intrinsic silicon epitaxial layer and the germanium silicon epitaxial layer in the groove are prepared by the preparation method of a low on-resistance semiconductor power device of any of the above-mentioned embodiments.

[0043] The semiconductor power device is prepared by etching a groove on a semiconductor substrate and sequentially depositing a high-purity undoped intrinsic silicon epitaxial layer and a germanium silicon epitaxial layer in the groove. Through the above steps, a semiconductor power device with low on-resistance is formed, and its electrical performance and structural integrity are optimized.

[0044] The above preparation method can significantly reduce the on-resistance of semiconductor power devices and improve their working efficiency and performance stability. The precise control of high-purity undoped intrinsic silicon epitaxial layer and germanium silicon epitaxial layer ensures the high quality and low defect density of the device, which is suitable for the manufacture of high-performance electronic devices.

[0045] The present invention proposes a low-temperature germanium-silicon epitaxial growth technology. By using germanium-silicon material for secondary epitaxy under conditions below 800°C, the low-temperature epitaxial growth ensures the metastable state of the entire epitaxial layer, without dislocations in the channel, and accurately controls the epitaxial layer with good thickness / concentration uniformity in the vertical and horizontal directions, effectively avoiding the expansion of P-type semiconductor materials. At the same time, using germanium-silicon material instead of traditional silicon material can effectively reduce the temperature required for epitaxy, further avoiding the expansion of P-type semiconductor materials.

[0046] Low-temperature epitaxy is used to complete deep trench backfill, which effectively prevents P-type semiconductor material from expanding into the silicon on both sides of the deep trench. Germanium silicon material is used instead of traditional silicon material for epitaxy, which effectively reduces the temperature required for epitaxy and further prevents P-type semiconductor material from expanding. One intrinsic semiconductor epitaxy and one low-temperature germanium silicon epitaxy are used to ensure that P-type semiconductor material does not expand at all, and one intrinsic semiconductor epitaxy can effectively prevent the influence of deep trench sidewall defects on epitaxial filling. Low-temperature epitaxial technology is applied to semiconductor power devices to complete the preparation of super junction structure, which solves the problem of P-type semiconductor material of super junction device expanding into silicon on both sides of the deep trench after one high-temperature epitaxy, thereby changing the substrate resistivity. The problem of premature sealing of the deep trench opening by P-type epitaxial material in deep trench etching and filling technology of super junction device is solved, thereby forming a complete deep trench backfill.

[0047] By adopting low-temperature epitaxial growth technology of 800℃ and below; using germanium silicon material for epitaxy; avoiding external expansion, there is no restriction on P-type semiconductor material, which can be diborane, etc.; there is no restriction on the depth-to-width ratio of the trench etched before epitaxial growth; there is no restriction on the type of carrier wafer, and the thickness can be 50um~800um; there is no restriction on the type of device using this technology, which can be a semiconductor power device.

[0048] Finally, it should be noted that: the various embodiments in this specification are described in a progressive manner, and each embodiment focuses on the differences from other embodiments. The same or similar parts between the various embodiments can be referenced to each other.

[0049] The above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention is described in detail with reference to the preferred embodiments, ordinary technicians in the field should understand that the specific implementation methods of the present invention can still be modified or some technical features can be replaced by equivalents without departing from the spirit of the technical solution of the present invention, which should be included in the scope of the technical solution for protection of the present invention.

Claims

1. A method for preparing a low on-resistance semiconductor power device, characterized in that: The steps include: Etching a groove on a semiconductor substrate; Depositing high-purity undoped silicon in the trench to form an intrinsic silicon epitaxial layer; A germanium-silicon epitaxial layer is deposited on the intrinsic silicon epitaxial layer. The temperature is controlled below 800°C. The germanium content of the germanium-silicon epitaxial layer is controlled to be less than 20%, and the boron concentration is controlled to be less than 1E18 cm -3 , the deposition method includes any of the following: low pressure chemical vapor deposition (LPCVD), plasma enhanced chemical vapor deposition (PECVD), molecular beam epitaxy (MBE), liquid phase epitaxy (LPE), physical vapor deposition (PVD); Wherein the total gas pressure in the low pressure chemical vapor deposition (LPCVD) method is less than 200 torr; The low pressure chemical vapor deposition method controls the germanium content of the germanium silicon epitaxial layer to be less than 20%, comprising: Introducing silane (SiH4) gas and germane (GeH4) gas into the reaction chamber and controlling the flow rate of the silane gas; Control the flow rate of germane gas so that the proportion of germane gas in the total gas flow rate is less than 20%; The temperature in the reaction chamber was adjusted to keep it below 800°C.

2. The method for preparing a low on-resistance semiconductor power device according to claim 1, characterized in that: in, Low-pressure chemical vapor deposition method to control the boron concentration of silicon germanium epitaxial layer to less than 1E18cm -3 The method comprises: introducing borane (B2H6) gas into the reaction chamber during the deposition of the germanium silicon epitaxial layer; adjusting the flow rate of the borane gas to keep the boron concentration at less than 1E18cm -3 .

3. The method for preparing a low on-resistivity semiconductor power device according to claim 2, characterized in that: in, Depositing high-purity undoped silicon in the trench to form an intrinsic silicon epitaxial layer includes: Performing preheating in the reaction chamber to allow the substrate surface to reach a deposition temperature; Introducing high purity silane (SiH4) gas into the reaction chamber; The temperature in the reaction chamber is adjusted to below 800° C. so that the intrinsic epitaxial layer reaches a set thickness.

4. The method for preparing a low on-resistivity semiconductor power device according to claim 3, characterized in that: in, The total gas pressure in the low pressure chemical vapor deposition (LPCVD) method is below 200 torr.

5. The method for preparing a low on-resistivity semiconductor power device according to claim 4, characterized in that: The low pressure chemical vapor deposition method controls the germanium content of the germanium silicon epitaxial layer to be less than 20%.

6. A low on-resistance semiconductor power device, characterized in that: include; Semiconductor substrate; A high-purity undoped intrinsic silicon epitaxial layer in the trench; a silicon germanium epitaxial layer in the trench, the silicon germanium epitaxial layer being deposited on the intrinsic silicon epitaxial layer; Wherein, the high-purity undoped intrinsic silicon epitaxial layer and the germanium silicon epitaxial layer in the trench are prepared by the method for preparing a low on-resistivity semiconductor power device according to any one of claims 1 to 5.

Citation Information

Patent Citations

  • Semiconductor device and manufacturing method thereof

    CN103681338A

  • PMOS structure and formation method thereof

    CN105374684A

  • Improvement method for dislocation defects of embedded silicon-germanium epitaxy

    CN105529266A

  • Epitaxial preparation method of source and drain of gate-all-around structure and gate-all-around structure

    CN113889436A

  • Preparation method of deep trench structure and deep trench structure

    CN117877974A