Wafer level packaging method and wafer level packaging structure

By preparing organic solderability protective layer and flux solder layer on wafer prefabricated parts, it directly contacts the metal pad to form welding points, solving the problems of high thickness and high cost in traditional packaging, and achieving a more efficient wafer level Package.

CN118943025APending Publication Date: 2024-11-12RUISI MICROSYSTEMS (YANTAI) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411158018.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

In traditional wafer-level packaging methods, the PAD lead-out structure needs to be defined and formed by using a lithography process, resulting in high packaging thickness and increased cost.

Method used

The organic solderability protective layer is prepared on the surface of the wafer prefabricated parts, and a solder layer containing flux is prepared on the surface. The welding layer is contacted with the metal pad to form a solder point, and the wafer-level packaging is completed, avoiding the protection layer etching window opening treatment.

Benefits of technology

The packaging thickness is reduced, the preparation efficiency is improved, the process cost is reduced, and the preparation process of the welding layer is simplified.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118943025A_ABST
    Figure CN118943025A_ABST
Patent Text Reader

Abstract

The invention discloses a wafer-level packaging method and a wafer-level packaging structure, which are applied to the field of wafer packaging, and the method comprises the steps: providing a wafer prefabricated member; preparing an organic solderable protection layer on the upper surface of the wafer prefabricated member to at least cover the metal bonding pad on the upper surface of the wafer prefabricated member; a welding layer containing scaling powder is prepared on the surface, at least partially corresponding to the metal bonding pad, of the organic solderable protection layer, and the scaling powder is obtained by dissolving and removing the organic solderable protection layer. According to the invention, the organic solderable protection layer is prepared on the upper surface of the wafer prefabricated member, so that the metal bonding pad in the wafer prefabricated member is prevented from being contacted and oxidized with the outside, the thickness of the protection layer is lower than that of the protection layer prepared at present, and the thickness of the whole device can be reduced after the welding layer is prepared subsequently; part of the organic solderable protection layer is dissolved through the soldering layer containing the soldering flux so that the organic solderable protection layer can make contact with the metal bonding pad and form the soldering point, etching and windowing of the protection layer are not needed when the soldering layer is prepared, definition of the metal bonding pad can be completed at the same time through one-time preparation of the soldering layer, and the preparation efficiency is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of wafer packaging, and in particular to a wafer-level packaging method and a wafer-level packaging structure. Background Art

[0002] Wafer Level Package (WLP) is a miniaturized packaging technology applied to wafers, and the package size is equal to the die size. In traditional WLP packaging, the PAD (metal window) is led out in the form of Solder Ball (metal solder ball) or Copper Pillar (copper pillar bump), and the height is usually greater than 50 microns. In modern module packaging, the packaging thickness of the device prepared by the above packaging process is relatively high, and whether the Solder Ball or Copper Pillar method is used, the PAD needs to be defined by the photolithography process, and then the Solder Ball and Copper Pillar are formed by steel screen printing or electroplating, which increases the cost of the WLP process.

[0003] Therefore, how to provide a method for reducing the thickness of device packaging produced by the WLP process while reducing the packaging cost of the WLP process is a technical problem that those skilled in the art need to solve urgently. Summary of the invention

[0004] In view of this, the purpose of the present invention is to provide a wafer-level packaging method and a wafer-level packaging structure, which solves the problem that the preparation of the pad lead-out structure in the prior art requires the use of a photolithography process to etch and open windows in the oxide protection layer outside the pad, which results in a relatively complicated process and a relatively high thickness of the final prepared packaging structure.

[0005] In order to solve the above technical problems, the present invention provides a wafer-level packaging method, comprising:

[0006] Providing a wafer preform; the wafer preform is a wafer device that has completed the chip preparation process and includes a metal pad exposed on the outermost surface;

[0007] Preparing an organic solderability protective layer on the upper surface of the wafer preform to at least cover the metal pad located on the upper surface of the wafer preform;

[0008] A welding layer containing flux is prepared on the surface of the organic solderability protective layer that at least partially corresponds to the metal pad. The flux is a flux that dissolves and removes the organic solderability protective layer, so that the welding layer completes the metal pad definition, contacts the metal pad and forms a welding point, thereby completing the wafer-level packaging of the wafer device.

[0009] Optionally, the thickness of the organic solderability protection layer is 0.1 micrometer to 0.5 micrometer.

[0010] Optionally, preparing an organic solderability protective layer on the upper surface of the wafer preform includes:

[0011] Applying an organic solderability protective agent on the upper surface of the wafer preform;

[0012] The coated organic solderability protective agent is baked to prepare the organic solderability protective layer.

[0013] Optionally, the step of baking the applied organic solderability protective agent to prepare the organic solderability protective layer comprises:

[0014] The applied organic solderability protective agent is initially baked at a temperature of 80 to 100 degrees for a duration of 1 to 2 minutes to preliminarily solidify the organic solderability protective agent;

[0015] The preliminarily cured organic solderability protective agent is baked for a second time, with the baking temperature being 150 to 200 degrees and the duration being 30 to 60 minutes, so that the organic solderability protective agent is completely cured to obtain the organic solderability protective layer.

[0016] Optionally, the welding layer is solder paste.

[0017] Optionally, preparing a solder paste containing flux on a surface of the organic solderability protection layer at least partially corresponding to the metal pad so that the solder paste contacts the metal pad and forms a solder joint, thereby completing wafer-level packaging of the wafer device, including:

[0018] On the surface of the organic solderability protective layer at least partially corresponding to the metal pad, preparing a solder paste containing flux, and using a reflow process to solder the solder paste to the metal pad to form a solder joint, thereby completing the wafer-level packaging of the wafer device;

[0019] When the solder paste is soldered to the metal pad using a reflow process, the heat generated by the reflow process is used to activate the solder flux in the solder paste to accelerate the dissolution of the organic solderability protective layer that the solder flux contacts.

[0020] Optionally, preparing a solder paste containing flux on a surface of the organic solderability protection layer at least partially corresponding to the metal pad so that the solder paste contacts the metal pad and forms a solder joint, thereby completing wafer-level packaging of the wafer device, including:

[0021] On the surface of the organic solderability protection layer at least partially corresponding to the metal pad, solder paste containing flux is prepared by steel screen printing so that the solder paste contacts the metal pad and forms a soldering point, thereby completing the wafer-level packaging of the wafer device.

[0022] Optionally, preparing a soldering layer containing a solder flux on a surface of the organic solderability protection layer at least partially corresponding to the metal pad comprises:

[0023] The welding layer is formed into an arc shape along the extension direction of the surface of the organic solderability protective layer, or the welding layer is formed into a rounded shape at the corner of the contour edge.

[0024] Optionally, after completing the wafer-level packaging of the wafer device, the method further includes:

[0025] The wafer-level packaged devices are cut to obtain packaged chips.

[0026] The present invention also provides a wafer-level packaging structure, which is prepared by the above-mentioned wafer-level packaging method, comprising:

[0027] A wafer preform, an organic solderability protective layer and a soldering layer containing a soldering flux; the soldering flux is a soldering flux that dissolves and removes the organic solderability protective layer;

[0028] The wafer preform is a wafer device that has completed the chip preparation process and includes a metal pad exposed on the outermost surface;

[0029] The organic solderability protection layer is at least laid on the upper surface of the metal pad of the wafer preform, and the organic solderability protection layer corresponds to at least a portion of the metal pad, and an opening is formed on the organic solderability protection layer corresponding to at least a portion of the metal pad after the flux dissolves to define the metal pad;

[0030] The welding layer contacts the metal pad through the opening and forms a welding point.

[0031] Optionally, the wafer preform is a wafer device having a cavity structure formed in a region corresponding to an active device;

[0032] The metal layer conductively connected to the outside and located beside the cavity structure is led out through a rewiring process, and a rewiring metal conductively connected to the metal layer is formed on the upper side of the cavity structure as the metal pad.

[0033] The present invention also provides a chip packaging module, including the wafer-level packaging structure as described above, and a plurality of packaged chips obtained after cutting.

[0034] It can be seen that the wafer-level packaging method provided by the present invention includes providing a wafer preform, which is a wafer device that has completed the chip preparation process and includes a metal pad exposed on the outermost surface; preparing an organic solderability protective layer on the upper surface of the wafer preform to at least cover the metal pad located on the upper surface of the wafer preform; preparing a welding layer containing a flux on the surface of the organic solderability protective layer that at least partially corresponds to the metal pad, the flux being a flux that dissolves and removes the organic solderability protective layer, so that the welding layer completes the metal pad definition, contacts the metal pad and forms a welding point, thereby completing the wafer-level packaging of the wafer device. The present invention prepares an organic solderability protective layer on the upper surface of the wafer preform to prevent the metal pad in the wafer preform from being oxidized by contact with the outside. Compared with the protective layer currently prepared, the thickness of the protective layer is lower, and the thickness of the overall device can be reduced after the subsequent preparation of the welding layer. The welding layer containing flux dissolves part of the organic solderability protective layer so that it can contact the metal pad and form a welding point. When preparing the welding layer, there is no need to etch and open a window in the protective layer. The definition of the metal pad can be completed at the same time by preparing the welding layer once, thereby improving the preparation efficiency.

[0035] In addition, the present invention also provides a wafer-level packaging structure, which also has the above-mentioned beneficial effects. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.

[0037] Figure 1 It is a schematic diagram of a cavity device structure of a wafer-level package that uses a metal solder ball to lead out a metal pad in the prior art;

[0038] Figure 2 It is a schematic diagram of a cavity device structure of a wafer-level package that uses a metal welding cap to lead out a metal welding pad in the prior art;

[0039] Figure 3 A schematic diagram of a non-cavity device structure of a wafer-level package that uses a metal solder ball to lead out a metal pad in the prior art;

[0040] Figure 4 A flowchart of a wafer-level packaging method provided by an embodiment of the present invention;

[0041] Figure 5 This is an example diagram of a process for preparing a cavity device for wafer-level packaging using metal solder balls to lead out metal pads in the prior art;

[0042] Figure 6 A schematic structural diagram of an organic solderability protective layer prepared on the upper surface of a wafer preform in a wafer-level packaging method provided by an embodiment of the present invention;

[0043] Figure 7 A schematic structural diagram of a wafer-level packaging structure provided by an embodiment of the present invention;

[0044] Figure 8 A flow chart of another wafer-level packaging method provided by an embodiment of the present invention;

[0045] Fig. 9 A schematic structural diagram of another wafer-level packaging structure provided by an embodiment of the present invention;

[0046] Figures 1 to 3 , Figures 5 to 7 ,as well as Fig. 9 In the figure, the reference numerals are described as follows:

[0047] 10-substrate, 20-metal interconnection layer, 21-protective layer, 22-active device layer, 30-metal pad, 31-metal layer conductively connected to the outside, 32-package sidewall, 33-package top, 40-organic solderability protective layer, 41-PI layer, 50-welding layer, 51-metal solder ball, 52-metal solder cap. DETAILED DESCRIPTION

[0048] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0049] Wafer Level Package (WLP) is a miniaturized packaging technology applied to wafers, and the package size is equal to the die size. In traditional WLP packaging, the lead-out of PAD (metal window) is in the form of Solder Ball (metal solder ball) or Copper Pillar (copper pillar bump), and the height is usually greater than 50 microns. In modern module packaging, the package thickness of the device prepared by the above packaging process is relatively high, and whether the Solder Ball or Copper Pillar method is used, the PAD needs to be defined by the photolithography process, and then the Solder Ball and Copper Pillar are formed by steel screen printing or electroplating, which increases the cost of the WLP process.

[0050] For details, please refer to Figure 1 and Figure 2 , Figure 1 The figure is a schematic diagram of a cavity device structure of a wafer-level package that uses a metal solder ball to lead out a metal pad in the prior art. Figure 2 The figure is a schematic diagram of a cavity device structure of a wafer-level package that uses a metal solder cap to lead out a metal solder pad in the prior art. Figure 1 and Figure 2 All of them are wafer devices that form a cavity structure, and in this embodiment, the metal layer 31 that is conductively connected to the outside is led out to the upper side of the cavity structure through the RDL process. In this embodiment, all the RDL metals prepared in the RDL process can be used as metal pads 30, but preferably, in the wafer device that forms a cavity structure, the RDL metal formed on the upper side of the package top 33 after the RDL process is generally used as the metal pad 30. Taking the SAW (surface acoustic wave) filter as an example, the manufacture of the SAW filter is divided into the front-end and the back-end. In the front-end process of the SAW filter, the preparation of the metal interconnection layer 20, the metal layer 31 that is conductively connected to the outside, and the protective layer 21 is completed. In the back-end process, the cavity package pad is mainly formed, the package side wall 32 is formed by photolithography in the non-circuit area, and then the package top 33 is formed by photolithography on the package side wall 32, so as to form a cavity above the circuit, and then the metal layer 31 connected to the outside is exposed by photolithography, and the metal layer 31 connected to the outside is led out to the upper side of the package top 33 by RDL (rewiring) process, and the RDL is coated with an oxidation protection layer, such as a PI (polyimide) layer 41, and then the PI layer 41 is photolithographically exposed to expose the metal pad 30, and the preparation is as follows. Figure 1 The metal solder ball 51 in the Figure 2 The metal welding cap 52 in the chip moves the metal layer 31 connected to the outside from the edge of the chip to the inside of the chip, so that the metal pad 30 is moved inward, reducing the area of ​​a single chip. The above chip is an unpackaged functional chip after wafer cutting. Figure 3 , Figure 3 The schematic diagram of the structure of a non-cavity device in wafer-level packaging using metal solder balls to lead out metal pads in the prior art. Figure 3 The active device layer 22 includes a metal interconnect layer 20 formed on the surface of the substrate 10 .

[0051] Therefore, how to provide a method for reducing the thickness of device packaging produced by the WLP process while reducing the packaging cost of the WLP process is a technical problem that those skilled in the art need to solve urgently.

[0052] The present invention prepares an organic solderability protective layer on the upper surface of the wafer preform to prevent the metal pad in the wafer preform from being oxidized by contact with the outside. Compared with the protective layer currently prepared, the thickness of the protective layer is lower, and the thickness of the overall device can be reduced after the subsequent preparation of the welding layer. The welding layer containing flux dissolves part of the organic solderability protective layer so that it can contact the metal pad and form a welding point. When preparing the welding layer, there is no need to etch and open a window in the protective layer. The definition of the metal pad can be completed at the same time by preparing the welding layer once, thereby improving the preparation efficiency.

[0053] Please refer to Figure 4 , Figure 4 A flowchart of a wafer-level packaging method provided by an embodiment of the present invention. The method may include:

[0054] S101: providing a wafer preform; the wafer preform is a wafer device that has completed the chip preparation process and includes a metal pad 30 exposed on the outermost surface.

[0055] The execution subject of this embodiment is a wafer-level packaging device. It should be noted that in this embodiment, the wafer preform completes the chip preparation process and includes a metal pad 30 exposed on the outermost surface for conductively leading out the prepared chip active area. In a feasible embodiment, the wafer preform completes the chip preparation, including preparing a metal interconnection layer 20, or other conductive interconnection layers, that is, the above-mentioned chip preparation process refers to the process of making an integrated circuit on the substrate 10 through a series of processing steps starting from the substrate 10. In this embodiment, the focus is on completing the preparation of the metal pad 30, so that when performing subsequent processes, the wafer is packaged, and the metal pad 30 is smoothly led out to complete the wafer-level packaging of the device. This embodiment does not limit the specific structure of the metal pad 30. For example, the metal pad 30 can be a metal pad 30 directly set on the surface of the wafer, or the metal pad 30 can also be a metal pad 30 processed by a rewiring (RDL) process. In addition, in order to prevent the surface of the prepared metal pad 30 from being oxidized by contact with the external air, an oxidation protection layer needs to be provided to protect the metal structure. In order to ensure that the metal pad 30 can be connected to the outside, an opening needs to be provided in the oxidation protection layer, and a metal lead-out structure is provided by using the opening to lead the metal pad 30 out to connect to the outside. The metal lead-out structure is generally provided as a metal solder ball 51 or a metal solder column. In this embodiment, it is not limited to which specific metal lead-out structure is used to lead out the metal pad 30. For example, a metal solder ball 51 can be provided to lead out the metal pad 30, or a metal solder column can be provided to lead out the metal pad 30, or in order to reduce the thickness of the prepared wafer-level package, a metal solder cap can be used, that is, a thinner metal solder layer can be prepared by steel screen printing as a metal lead-out structure. It should be noted that the metal pad 30 is currently led out by a metal solder cap, and the metal solder cap can be set to the order of 10 microns. It should be further pointed out that there are certain limitations in reducing the height of the solder layer in the actual manufacturing process. For devices like SAW filter (surface acoustic wave filter), BAW filter (bulk acoustic wave) or other devices with a small number of pins, the height of the soldering layer can be reduced, thereby significantly reducing the height of the wafer device. During the molding process, because the pad pitch is relatively large, it will not affect the filling of the molding compound (packaging material), but for other dies with more pins (unpackaged chips after wafer cutting), the soldering layer cannot be lowered too much to avoid insufficient filling of the packaging material during the packaging process when the pad pitch is small and the soldering layer is low.

[0056] The wafer level packaging method in the prior art can refer to Figure 5 , Figure 5The present invention is a flow chart of a cavity device for preparing a wafer-level package using a metal solder ball to lead out a metal pad in the prior art. The process includes, in sequence, wafer material, preparation and formation of a package side wall 32, preparation and formation of a package top 33 above the package side wall 32, preparation and completion of RDL wiring, preparation of a PI layer 41 on the upper surface of the whole wafer, opening a window in the PI layer 41 corresponding to the position of the metal pad 30 after RDL wiring, using an etching process to expose part of the metal pad 30, and preparing a metal solder ball 51 conductively connected to the metal pad 30 at the window position to lead out the metal pad 30. In the present application, the wafer material can be selected to complete the chip preparation process, and the wafer device including the metal pad 30 exposed on the outermost surface, that is, the wafer preform in the present application, and the steps of preparing and forming a package side wall 32, preparing and forming a package top 33 above the package side wall 32, and completing RDL wiring can be added to prepare a wafer device with a cavity structure.

[0057] Specifically, in different products, there are differences in the structure between the incoming wafers and the provided wafer preforms. For example, for conventional chips, such as logic chips or amplifier chips, after the chip preparation process is completed, the wafer obtained is a structure with metal pads on the surface, which is the incoming wafer, that is, the wafer preform, and then coated with an organic solderability protective layer, and then coated with a welding layer to achieve the welding lead-out of the metal pad; and for SAW filters or BAW filters, which require cavities. The incoming wafer is the wafer device (such as Figure 5 A), and then Figure 5 The process is obtained Figure 5 C, and then the metal layer 31 connected to the outside is rewired to the upper surface of the package top 33 by RDL as a metal pad 30. The wafer device structure obtained at this time is used as a wafer preform. S102: Prepare an organic solderability protective layer 40 on the upper surface of the wafer preform to at least cover the metal pad 30 located on the upper surface of the wafer preform.

[0058] It should be noted that this embodiment can refer to Figure 6 , Figure 6 A schematic diagram of a structure in which an organic solderability protective layer is prepared on the upper surface of a wafer preform in a wafer-level packaging method provided by an embodiment of the present invention. Figure 6 For the corresponding Figure 5 The device obtained by completing RDL wiring in step S102 is performed, wherein the organic solderability protective layer is as follows Figure 6As shown in . In this embodiment, since it is only involved in the process of preparing the metal pad 30, it is necessary to use the photolithography process to etch and open the window of the oxide protection layer prepared on the surface of the metal pad 30. Therefore, in this step, the organic solderability protection layer 40 can be prepared only on the surface of the metal pad 30, or the organic solderability protection layer 40 can be prepared on the upper surface of the whole wafer preform, and the upper surface of the wafer preform is the surface corresponding to the exposure of the metal pad 30. Further, in order to reduce the amount of organic solderability protection layer 40, while ensuring the regularity and convenience of removing and opening the window of the organic solderability protection layer 40 to lead out the metal pad 30, the organic solderability protection layer 40 can be prepared only on the surface of the partial area where the metal pad 30 needs to be led out. After that, when preparing the through hole in the organic solderability protection layer 40 to expose part of the metal pad 30, it is not necessary to consider the control of the opening size, and it is only necessary to remove the entire organic solderability protection layer 40, thereby improving the convenience of preparation.

[0059] Furthermore, in order to reduce the thickness of the oxidation protection layer protecting the metal pad 30 and thus reduce the thickness of the entire wafer device, the thickness of the organic solderability protection layer 40 can be set to 0.1 micrometer to 0.5 micrometer.

[0060] In a feasible embodiment, to ensure that the organic solderability protective layer is successfully prepared, the above-mentioned preparation of the organic solderability protective layer 40 on the upper surface of the wafer preform may include:

[0061] Step S11: applying an organic solderability protective agent on the upper surface of the wafer preform;

[0062] Step S12: baking the coated organic solderability protective agent to prepare an organic solderability protective layer 40 .

[0063] It should be noted that in this embodiment, the organic solderability protective layer 40 is prepared by coating and baking to ensure that the organic solderability protective layer 40 is successfully prepared and improve the stability of the contact between the organic solderability protective layer 40 and the surface of the wafer preform. The organic solderability protective agent can be set to be an organic acid or an organic compound as the main component, and benzotriazole (BTA) and its derivatives are usually used to form a thin protective film to prevent metal surface oxidation and improve welding performance. The organic solderability protective layer formed can be specifically set to a thickness of less than 1 micron, while the conventionally set PI layer 41 has a thickness of 5 to 30 microns.

[0064] Further, in order to improve the preparation efficiency of the organic solderability protective layer 40 prepared on the upper surface of the wafer preform, the above-mentioned baking of the coated organic solderability protective agent to prepare the organic solderability protective layer 40 may include:

[0065] Step S21: performing a primary baking on the applied organic solderability protective agent, the baking temperature is 80 to 100 degrees, and the duration is 1 to 2 minutes, so that the organic solderability protective agent is initially cured;

[0066] Step S22 : performing secondary baking on the preliminarily cured organic solderability protective agent, with the baking temperature being 150 to 200 degrees and the duration being 30 to 60 minutes, so that the organic solderability protective agent is completely cured to obtain an organic solderability protective layer 40 .

[0067] It should be noted that in this embodiment, the organic solderability protective agent is first baked using specified baking parameters to initially solidify the organic solderability protective agent, and then the initially solidified organic solderability protective agent is secondarily baked using corresponding baking parameters to prepare an organic solderability protective layer 40. This embodiment uses a secondary baking method to prepare the organic solderability protective layer 40, which is easy to shape and improves the preparation efficiency, avoiding the problem of unstable molding and low pass rate of the organic solderability protective layer 40 formed by direct single baking.

[0068] S103: Prepare a welding layer 50 containing flux on the surface of the organic solderability protective layer 40 that at least partially corresponds to the metal pad 30. The flux is the flux that dissolves and removes the organic solderability protective layer 40, so that the welding layer 50 completes the definition of the metal pad 30, contacts with the metal pad 30 and forms a welding point, thereby completing the wafer-level packaging of the wafer device.

[0069] This embodiment can refer to Figure 7 , Figure 7 A schematic diagram of the structure of a wafer-level packaging structure provided by an embodiment of the present invention. In this embodiment, a welding layer 50 containing a flux is prepared on the surface of the organic solderability protective layer 40 corresponding to at least part of the metal pad 30, and the flux is used to dissolve and remove the organic solderability protective layer 40 in contact, so as to form a through hole in the organic solderability protective layer 40 that exposes at least part of the metal pad 30, and the above-mentioned welding layer 50 is in contact with the exposed metal pad 30 and welded to form a welding point, and the metal pad 30 is led out by the welding layer 50 to complete the wafer-level packaging of the wafer device. In this embodiment, the welding layer 50 is prepared in one step, and the organic solderability protective layer 40 in contact can be dissolved and removed by the flux in the welding layer 50 to complete the definition of the metal pad 30, without etching the protective layer to open a window, and the welding layer 50 is in contact with the metal pad 30 to form a welding point, thereby improving the preparation efficiency.

[0070] The present embodiment does not limit the specific components of the soldering flux, for example, it can be configured to include rosin, active substances, solvents, film formers and surfactants, wherein the rosin can form a protective film and a soldering flux; the active substances can be configured to be organic acids and amine substances for removing oxides, and the amine substances are used to enhance the soldering effect; the solvent can be selected from isopropyl alcohol for dissolving and dispersing other components; the film former can be selected from acrylic resin for improving the stability of residues after soldering; the surfactant can be configured to be polyethylene glycol for reducing surface tension.

[0071] Furthermore, in order to ensure the stability and adaptability of the soldering layer 50 , the soldering layer 50 may be configured as solder paste.

[0072] In this embodiment, the welding layer 50 can be set as solder paste, that is, the solder paste containing the above-mentioned solder flux can be applied on the surface of the organic solderability protective layer 40 corresponding to at least part of the metal pad 30 by means of steel screen printing, and the organic solderability protective layer 40 that is in contact is removed by dissolving the solder flux, so that the solder paste contacts the exposed metal pad 30, and the two are welded to form a welding point at the contact position. To facilitate welding, the solder paste can be set as a low-temperature solder paste in the case of adapting to the subsequent wafer preparation process.

[0073] Further, in order to improve the convenience of soldering the solder paste to the metal pad 30, the solder paste containing flux is prepared on the surface of the organic solderability protection layer 40 corresponding to at least a portion of the metal pad 30, so that the solder paste contacts the metal pad 30 and forms a soldering point, and the wafer-level packaging of the wafer device is completed, which may include:

[0074] A solder paste containing flux is prepared on the surface of the organic solderability protection layer 40 corresponding to at least a portion of the metal pad 30, and the solder paste is soldered to the metal pad 30 using a reflow process to form a solder joint, thereby completing wafer-level packaging of the wafer device;

[0075] When soldering the solder paste to the metal pad 30 using the reflow process, the heat generated by the reflow process is used to activate the solder flux in the solder paste to accelerate the dissolution of the organic solderability protective layer 40 that the solder flux contacts.

[0076] In this embodiment, the solder paste and the metal pad 30 are soldered by a reflow process to form a soldering point at the solder paste and the metal pad 30. It should be noted that in this embodiment, the heat generated by the reflow process is used to activate the flux in the solder paste to increase the rate at which the flux dissolves the organic solderability protective layer 40 in contact with it, thereby improving the efficiency of wafer-level packaging.

[0077] Further, in order to improve the convenience of preparing solder paste and reduce the thickness of the prepared solder paste, the solder paste containing flux is prepared on the surface of the organic solderability protection layer 40 corresponding to at least a portion of the metal pad 30, so that the solder paste contacts the metal pad 30 and forms a welding point, and the wafer-level packaging of the wafer device is completed, which may include:

[0078] On the surface of the organic solderability protection layer 40 at least partially corresponding to the metal pad 30, a solder paste containing flux is prepared by screen printing so that the solder paste contacts the metal pad 30 and forms a solder joint, thereby completing the wafer-level packaging of the wafer device.

[0079] In this embodiment, the solder paste is prepared by steel screen printing, which can improve the preparation efficiency and ensure that the thickness of the printed solder paste is lower than the thickness of the metal solder ball 51 or the metal solder column prepared in the traditional way. In addition, it should be further explained that in this embodiment, the height of the final formed solder layer 50 can be controlled by controlling the amount of solder paste. After the final forming, the height and shape of the solder layer 50 can be observed by X-ray. When a lower solder layer 50 is used, for example, a solder layer 50 with a height of less than 20 microns, the wafer-level package can be analyzed by decap (chip unsealing) or slicing, and it can be observed whether the surface of the metal structure after RDL wiring is not covered by an oxidation protective layer.

[0080] Further, in order to ensure the stability of the prepared welding layer 50 and avoid the prepared welding layer 50 from having an irregular shape, the above-mentioned preparation of the welding layer 50 containing flux on the surface of the organic solderability protection layer 40 at least partially corresponding to the metal pad 30 may include:

[0081] Along the extension direction of the surface of the organic solderability protection layer 40 , the welding layer 50 is formed into an arc shape, or the welding layer 50 has a rounded corner at the contour edge.

[0082] It should be noted that, in the present embodiment, the welding layer 50 is set to be in an arc shape or a rounded shape at the corners of the contour edge along the extension direction of the surface of the organic solderability protective layer 40. The surface tension of the formed welding layer 50 can be used to limit the welding layer 50, and the size of the welding layer 50 diffused outward in all directions can be ensured to be similar, thereby improving the regularity of the welding layer 50.

[0083] Furthermore, in a feasible embodiment, after completing the wafer-level packaging of the wafer device, the above method may further include:

[0084] The wafer-level packaged devices are cut to obtain packaged chips.

[0085] The device that has completed wafer-level packaging in this embodiment needs to be cut and processed to obtain a packaged chip before being connected to an external structure.

[0086] The wafer-level packaging method provided by the embodiment of the present invention includes providing a wafer preform, wherein the wafer preform is a wafer device having a metal interconnection layer 20 and a metal pad 30 connected to the outside after completing the wafer front-end process; preparing an organic solderability protection layer 40 on the upper surface of the wafer preform to at least cover the metal pad 30 located on the upper surface of the wafer preform; preparing a welding layer 50 containing a flux on the surface of the organic solderability protection layer 40 at least partially corresponding to the metal pad 30, wherein the flux is a flux that dissolves and removes the organic solderability protection layer 40, so that the welding layer 50 completes the definition of the metal pad 30, contacts with the metal pad 30 and forms a welding point, thereby completing the wafer-level packaging of the wafer device. The present invention prepares an organic solderability protective layer 40 on the upper surface of the wafer preform to prevent the metal pad 30 in the wafer preform from being oxidized by contact with the outside. Compared with the currently prepared oxidation protective layer, the thickness of the oxidation protective layer is lower, and the thickness of the overall device can be reduced after the subsequent preparation of the welding layer 50. The welding layer 50 containing flux dissolves part of the organic solderability protective layer 40 so that it can contact the metal pad 30 and form a welding point. When preparing the welding layer 50, there is no need to etch and open a window in the oxidation protective layer. The definition of the metal pad can be completed at the same time by preparing the welding layer once, thereby improving the preparation efficiency.

[0087] In addition, the embodiment of the present invention sets the thickness of the organic solderability protection layer 40 to 0.1 micron to 0.5 micron, and can utilize the properties of the organic solderability protection layer 40 itself to reduce the thickness of the oxidation protection layer compared with the prior art while ensuring that the metal structure is protected from oxidation, thereby reducing the overall thickness of the wafer device after wafer-level packaging; the organic solderability protection layer 40 is prepared by coating and baking to ensure that the organic solderability protection layer 40 is successfully prepared and to improve the stability of the contact between the organic solderability protection layer 40 and the surface of the wafer preform; the organic solderability protection layer 40 is prepared by secondary baking to facilitate molding and improve the manufacturing efficiency, thereby avoiding the problem of unstable molding and low qualified rate of the organic solderability protection layer 40 formed by direct single baking; the welding layer 50 is set to solder paste to ensure welding The stability and adaptability of layer 50; soldering the solder paste and the metal pad 30 by the reflow process, and activating the flux in the solder paste by the heat generated by the reflow process to increase the rate at which the flux dissolves into the organic solderability protective layer 40 in contact, thereby improving the efficiency of wafer-level packaging; preparing the solder paste by steel screen printing can improve the preparation efficiency, and at the same time can ensure that the thickness of the printed solder paste is lower than the thickness of the metal solder ball 51 or metal solder column prepared by the traditional method; setting the welding layer 50 along the extension direction of the surface of the organic solderability protective layer 40 to an arc shape or a rounded shape at the corner of the contour edge can improve the regularity of the welding layer 50; after completing the wafer-level packaging of the wafer device, the wafer-level packaged device is cut to obtain a packaged chip, so as to obtain the packaged chip and connect it to the external structure.

[0088] In a feasible embodiment, the above wafer-level packaging method may specifically include the following steps, which can be referred to as Figure 8 , Figure 8 Flow chart of another wafer-level packaging method provided by an embodiment of the present invention:

[0089] Step S1: Wafer incoming material. Provide a wafer preform; the wafer preform is a wafer device that has completed the wafer front-end process and has a metal interconnect layer and a metal pad connected to the outside. The wafer device of the wafer incoming material in this embodiment can be selected from SAW filters, BAW (Bulk Acoustic Wave) filters, and other MEMS (micro-electromechanical system) sensors, and can be selected from devices that need to form a cavity package.

[0090] Step S2: Forming the package sidewall. Step S2 is to use a photosensitive dry film to cover the entire wafer, and then perform photolithography and development according to the pattern, leaving only the dry film at the package sidewall position. The package sidewall is generally formed outside the active device to form a supporting package sidewall.

[0091] Step S3: Form the package top above the package sidewall. Step S3 is to use a photosensitive dry film to cover the entire wafer, and then use photolithography to expose the metal layer and steps connected to the outside for conductive connection, so as to facilitate the production of RDL metal.

[0092] Step S4: Electroplating to form RDL wiring. In this embodiment, the metal layer located outside the package sidewall and electrically connected to the outside is led out to the upper side of the package top through the RDL process to form a metal pad.

[0093] Step S5: Prepare an organic solderability protective layer on the upper surface of the whole wafer. Use a spin coater to evenly coat the OSP solution on the surface of the wafer, and spin it at high speed to evenly distribute the solution and form a thin film; then use a hot plate to bake the wafer to ensure the uniformity and adhesion of the film layer and remove solvent residues. It is generally implemented in two steps. The recommended temperature for the initial baking is 80-100 degrees and the time is 1-2 minutes, so that the OSP film layer is initially cured. The second step is curing and drying, the temperature is about 150 to 200 degrees, and the baking time is 30-60 minutes to completely cure the OSP (organic solderability protective layer) film layer.

[0094] Step S6: Print solder paste at the position of the corresponding metal pad using a steel screen. Compared with the traditional solution, in this embodiment, the metal pad window opening and solder paste printing are combined into one step. The flux contained in the solder paste is used. The active ingredients of the flux can dissolve the OSP layer, exposing the surface of the metal pad, so that the solder paste can directly contact the metal pad. The metal pad can be set as a copper metal pad. After reflow soldering, an alloy is formed between copper and tin, and a solder joint is obtained. In the area outside the corresponding metal pad, because there is no printed solder paste, the OSP layer is not directly affected by the flux and remains intact, continuing to play its role in preventing copper oxidation. In addition, the shape of the window corresponding to the metal pad position can be circular, square or rectangular, but whether it is a square or a rectangle, the preferred design is that the corners are rounded to prevent irregular diffusion of solder.

[0095] The wafer-level packaging structure provided by an embodiment of the present invention is introduced below. The wafer-level packaging structure described below and the wafer-level packaging method described above can refer to each other.

[0096] Please refer to Figure 7 , Figure 7 A schematic structural diagram of a wafer-level packaging structure provided by an embodiment of the present invention may include:

[0097] Wafer preform, organic solderability protective layer 40 and soldering layer 50 containing solder flux; the solder flux is a solder flux that dissolves and removes the organic solderability protective layer 40;

[0098] The wafer preform is a wafer device that has completed the chip preparation process and includes a metal pad 30 exposed on the outermost surface;

[0099] The organic solderability protection layer 40 is at least laid on the upper surface of the metal pad 30 of the wafer preform, and the organic solderability protection layer 40 corresponds to at least a portion of the metal pad 30, and an opening is formed by dissolving the flux to define the metal pad 30;

[0100] The soldering layer 50 contacts the metal pad 30 through the opening and forms a soldering point.

[0101] It should be noted that, in the present embodiment, the welding layer 50 is a welding layer 50 containing flux, and the flux is a flux that can dissolve and remove the organic solderability protective layer 40 when in contact with the organic solderability protective layer 40. Furthermore, the organic solderability protective layer 40 is at least laid on the upper surface of the metal pad 30 of the wafer preform, and the organic solderability protective layer 40 corresponds to at least a portion of the area at the metal pad 30, and an opening is formed in the organic solderability protective layer 40 obtained by dissolving the organic solderability protective layer 40 with the flux mentioned above, so that the welding layer 50 can be welded to the metal pad 30 through the opening to form a welding point, and the metal pad 30 is led out using the welding layer 50. The above-mentioned process of defining the metal pad 30 and the process of contacting the welding layer 20 with the metal pad 30 are simultaneously completed by a step of preparing the welding layer. Further, the present embodiment can refer to Fig. 9 , Fig. 9 A schematic structural diagram of another wafer-level packaging structure provided by an embodiment of the present invention. Fig. 9 For wafer devices without a cavity structure, a wafer-level packaging structure is obtained using the preparation method of the present application.

[0102] Furthermore, in order to ensure the adaptability of the wafer-level packaging structure, the wafer preform is a wafer device having a cavity structure formed in the corresponding active device area;

[0103] The metal layer 31 conductively connected to the outside and located beside the cavity structure is led out through a rewiring process, and a rewiring metal conductively connected to the metal layer is formed on the upper side of the cavity structure as a metal pad 30.

[0104] It should be noted that the metal pad 30 in this embodiment is formed by a rewiring process in which a metal layer 31 conductively connected to the outside is led out to the upper side of the cavity structure. The rewiring process in this embodiment specifically adopts fan-in rewiring.

[0105] The wafer-level packaging structure provided by the embodiment of the present invention includes a wafer preform, an organic solderability protection layer 40 and a welding layer 50 containing flux, the welding flux is a welding flux for dissolving and removing the organic solderability protection layer 40, the wafer preform is a wafer device having a metal interconnection layer 20 and a metal pad 30 connected to the outside after completing the wafer front-end process; the organic solderability protection layer 40 is at least laid on the upper surface of the metal pad 30 of the wafer preform, and the organic solderability protection layer 40 corresponds to at least a part of the area at the metal pad 30, and an opening obtained by dissolving the flux is formed; the welding layer 50 contacts the metal pad 30 through the opening to form a welding point. The present invention prepares an organic solderability protective layer 40 on the upper surface of the wafer preform to prevent the metal pad 30 in the wafer preform from contacting with the outside and oxidizing. Compared with the currently prepared oxidation protective layer, the thickness of the oxide protective layer is lower, and the thickness of the overall device can be reduced after the subsequent preparation of the welding layer 50. The welding layer 50 containing flux dissolves part of the organic solderability protective layer 40 so as to contact with the metal pad 30 and form a welding point. When preparing the welding layer 50, there is no need to etch and open a window in the oxide protective layer, thereby improving the preparation efficiency. In addition, the embodiment of the present invention ensures the adaptability of the wafer-level packaging structure by setting the metal pad 30 to undergo a rewiring process, and leading the metal layer 31 that is conductively connected to the outside to the metal pad 30 formed on the upper side of the cavity structure.

[0106] The chip packaging module provided in an embodiment of the present invention is introduced below. The chip packaging module described below and the wafer-level packaging structure described above can be referred to each other.

[0107] The chip packaging module provided by the embodiment of the present invention may include a plurality of packaged chips obtained after cutting the wafer-level packaging structure as described above.

[0108] In this embodiment, the wafer-level packaging structure as described above is cut to obtain a plurality of packaged chips, so as to facilitate the subsequent connection preparation process for the single chip.

[0109] In this specification, each embodiment is described in a progressive manner, and each embodiment focuses on the differences from other embodiments. The same or similar parts between the embodiments can be referred to each other. For the device disclosed in the embodiment, since it corresponds to the method disclosed in the embodiment, the description is relatively simple, and the relevant parts can be referred to the method part.

[0110] In addition, it should be noted that, in this article, relationships such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprises" or any other variations are intended to cover non-exclusive inclusion, so that a process, method, article or device that includes a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.

[0111] The above is a detailed introduction to a wafer-level packaging method and a wafer-level packaging structure provided by the present invention. Specific examples are used in this article to illustrate the principles and implementation methods of the present invention. The description of the above embodiments is only used to help understand the method of the present invention and its core idea; at the same time, for general technical personnel in this field, according to the idea of ​​the present invention, there will be changes in the specific implementation method and application scope. In summary, the content of this specification should not be understood as a limitation on the present invention.

Claims

1. A wafer-level packaging method, characterized in that: include: Provide wafer preforms; The wafer preform is a wafer device that has completed the chip preparation process and includes a metal pad (30) exposed on the outermost surface; Preparing an organic solderability protection layer (40) on the upper surface of the wafer preform to at least cover the metal pad (30) located on the upper surface of the wafer preform; A welding layer (50) containing solder flux is prepared on the surface of the organic solderability protective layer (40) at least partially corresponding to the metal pad (30), wherein the solder flux is the solder flux that dissolves and removes the organic solderability protective layer (40), so that the welding layer (50) completes the definition of the metal pad (30), contacts the metal pad (30) and forms a welding point, thereby completing the wafer-level packaging of the wafer device.

2. The wafer-level packaging method according to claim 1, characterized in that: The thickness of the organic solderability protection layer (40) is 0.1 micrometer to 0.5 micrometer.

3. The wafer-level packaging method according to claim 1, characterized in that: Preparing an organic solderability protective layer (40) on the upper surface of the wafer preform comprises: Applying an organic solderability protective agent on the upper surface of the wafer preform; The applied organic solderability protective agent is baked to prepare the organic solderability protective layer (40).

4. The wafer-level packaging method according to claim 3, characterized in that: The step of baking the coated organic solderability protective agent to prepare the organic solderability protective layer (40) comprises: The applied organic solderability protective agent is initially baked at a temperature of 80 to 100 degrees for a duration of 1 to 2 minutes to preliminarily solidify the organic solderability protective agent; The preliminarily cured organic solderability protective agent is subjected to secondary baking at a temperature of 150 to 200 degrees for a duration of 30 to 60 minutes, so that the organic solderability protective agent is completely cured to obtain the organic solderability protective layer (40).

5. The wafer-level packaging method according to claim 1, characterized in that: The welding layer (50) is solder paste.

6. The wafer-level packaging method according to claim 5, characterized in that: On the surface of the organic solderability protection layer (40) at least partially corresponding to the metal pad (30), a solder paste containing a solder flux is prepared so that the solder paste contacts the metal pad (30) and forms a solder joint, thereby completing the wafer-level packaging of the wafer device, comprising: Preparing a solder paste containing a solder flux on a surface of the organic solderability protection layer (40) that at least partially corresponds to the metal pad (30), and using a reflow soldering process to solder the solder paste to the metal pad (30) to form a soldering point, thereby completing wafer-level packaging of the wafer device; When the solder paste is soldered to the metal pad (30) using a reflow soldering process, the heat generated by the reflow soldering process is used to activate the solder flux in the solder paste, thereby accelerating the dissolution of the organic solderability protective layer (40) that the solder flux contacts.

7. The wafer-level packaging method according to claim 5, characterized in that: On the surface of the organic solderability protection layer (40) at least partially corresponding to the metal pad (30), a solder paste containing a solder flux is prepared so that the solder paste contacts the metal pad (30) and forms a solder joint, thereby completing the wafer-level packaging of the wafer device, comprising: On the surface of the organic solderability protection layer (40) at least partially corresponding to the metal pad (30), a solder paste containing a solder flux is prepared by means of steel screen printing, so that the solder paste contacts the metal pad (30) and forms a soldering point, thereby completing the wafer-level packaging of the wafer device.

8. The wafer-level packaging method according to claim 1, characterized in that: The step of preparing a soldering layer (50) containing solder flux on a surface of the organic solderability protection layer (40) at least partially corresponding to the metal pad (30) comprises: The welding layer (50) is prepared to be in an arc shape along the extension direction of the surface of the organic solderability protective layer (40), or the welding layer (50) is prepared to be in a rounded shape at the corner of the contour edge.

9. The wafer-level packaging method according to claim 1, characterized in that: After completing the wafer-level packaging of the wafer device, the method further includes: The wafer-level packaged devices are cut to obtain packaged chips.

10. A wafer-level packaging structure, characterized in that: Prepared by the wafer-level packaging method according to any one of claims 1 to 9, comprising: A wafer preform, an organic solderability protective layer (40) and a soldering layer (50) containing a soldering flux; the soldering flux is a soldering flux that dissolves and removes the organic solderability protective layer (40); The wafer preform is a wafer device that has completed the chip preparation process and includes a metal pad (30) exposed on the outermost surface; The organic solderability protection layer (40) is at least laid on the upper surface of the metal pad (30) of the wafer preform, and the organic solderability protection layer (40) corresponds to at least a partial area of ​​the metal pad (30), and is formed with an opening defined by the metal pad (30) after the flux is dissolved; The welding layer (50) contacts the metal pad (30) through the opening to form a welding point.

11. The wafer-level packaging structure according to claim 10, characterized in that: The wafer preform is a wafer device having a cavity structure formed in the active device area; A metal layer (31) conductively connected to the outside and located beside the cavity structure is led out through a rewiring process, and a rewiring metal conductively connected to the metal layer is formed on the upper side of the cavity structure to serve as the metal pad (30).

12. A chip packaging module, characterized in that: The invention comprises a wafer-level packaging structure as claimed in any one of claims 10 to 11, and a plurality of packaged chips obtained after cutting.