Vacuum-solid device low lead wire arc processing method, lead wire arc structure and EBAPS device

By using low-lead arc control method in EBAPS devices, using BSOB mode and capillary chopper to set bonded leads, and controlling the close-fit distance to 0.3mm, solving the problems of device resolution differences and short-circuit breakdown in the prior art. Improves the tensile strength and imaging effect of the device.

CN118943150APending Publication Date: 2024-11-12NORTH NIGHT VISION TECH

Patent Information

Application Number
CN202410991841.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

There are technical bottlenecks in the control of close-fit distances in existing EBAPS devices, resulting in large differences in resolution and theoretical values. The low-lead arc welding method cannot be effectively applied to vacuum-solid devices, which can easily lead to device short circuit or breakdown.

Method used

Using the low-lead line arc control method, by installing bonding pads in the ceramic shell and welding at high temperature, bonding leads are set using BSOB mode and capillary chopper, including raised sections, depression sections, inverted sections, and platform For sections and descending sections, control the close attachment distance to 0.3mm and below to avoid direct contact between the side walls of the metal pads, and reduce the risk of breakdown and short circuit.

Benefits of technology

Reliable regulation of the close-attachment distance of vacuum-solid devices is achieved, the arc throwing height is reduced, the lead tensile strength is improved, the device short circuit and breakdown risks are avoided, and the optical imaging effect and device safety are ensured.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118943150A_ABST
    Figure CN118943150A_ABST
Patent Text Reader

Abstract

The invention discloses a vacuum-solid device low lead wire arc processing method, a lead wire arc structure and an EBAPS device. The method comprises the following steps: 1) welding a bonding cushion block in a ceramic shell mounting cavity with a bonding pad by using a solder; uniformly coating solder on the cushion block, aligning the chip with the bonding pad with the cushion block, and then welding at high temperature; 2) as the position of the ceramic bonding pad is lower than that of the chip bonding pad, the ceramic bonding pad is set as a second welding spot, and the chip bonding pad is set as a first welding spot in order to facilitate operation; and 3) arranging a bonding lead between the first welding spot and the second welding spot through a capillary chopper in a BSOB mode. Compared with an existing structure line arc, the line throwing height of the low-profile line arc is obviously reduced, under the same indium sealing condition or the smaller close-fitting distance packaging condition, the device breakdown and short circuit risks are greatly reduced, meanwhile, no obvious bending structure exists on the obtained line arc line shape, the bonding line arc is smoother, and the tensile strength of the lead is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of EBAPS devices, and in particular to a low-lead wire arc processing method for vacuum-solid devices and an EBAPS device thereof. Background Art

[0002] EBAPS is a vacuum-solid hybrid device, including: a photocathode, an electron-sensitive CMOS chip and an integrated ceramic shell. The imaging process is as follows: the incident photons are converted into photoelectrons after passing through the photocathode. The photoelectrons gain energy under the action of the external electric field in a vacuum and bombard the surface of the electron-sensitive CMOS chip. Elastic and inelastic scattering occurs with the lattice atoms in the chip to produce a large number of electron-hole pairs. Then, the electron-hole pairs are collected by electrodes through diffusion and the action of the electric field, and finally an electronic image is output.

[0003] EBAPS relies on electron bombardment of CMOS chips to multiply electrons and achieve signal amplification. It has a high electron gain effect and can achieve single-photon imaging. It has broad application prospects in extremely weak light imaging. However, due to the influence of device technology, the resolution of existing EBAPS is significantly different from the theoretical value.

[0004] In order to improve the resolution of the device, the existing EBAPS devices basically adopt close-fitting packaging. Studies have found that the resolution of EBAPS devices is related to the performance of the photocathode and the electron-sensitive CMOS chip, and is also related to the vacuum electron transmission dispersion caused by the close distance between the photocathode and the CMOS chip. Generally, the closer the close distance, the shorter the transmission distance of electrons in a vacuum, which is more conducive to reducing the vacuum electron transmission dispersion. By adopting a smaller close distance, the risk of breakdown during the use of the device can be avoided by reducing the number of breakdown points in the device, improving the pressure resistance characteristics and cleanliness of the tube shell, etc.

[0005] At present, the performance of components such as photocathodes and electron-sensitive CMOS chips has reached a technical bottleneck. The proximity distance of existing chips is ≤0.6mm, which has a certain adjustment space. However, there are no relevant reports at home and abroad on how to optimize the process to further control the proximity distance of EBAPS devices.

[0006] In order to improve the resolution of the device, the close contact distance is controlled by controlling the height of the pad sandwiched between the chip and the cathode. Affected by the height of the pad, CMOS chip and metal solder, the height difference between chip 1 soldering and chip 2 soldering is large, usually ≥1600μm. In order to ensure the normal electrical function of the chip after bonding, the height of the gold wire arc of the chip is usually set to 250μm, and the lead adopts conventional arc setting parameters. When the close contact distance between the chip and the cathode is set to ≤0.35mm, when the device is working normally, a high voltage of more than 1000V is usually set between the photocathode and the CMOS chip, and the photocathode and the chip gold wire will contact short circuit or produce breakdown discharge. If the arc height is reduced, the gold wire arc will directly contact the side wall of the metal pad, causing the chip optical imaging short circuit.

[0007] CN 200680000569.1 discloses a method for forming a low-profile wire arc. The method actually limits the structure of welding leads between a first welding position and a second welding position, but does not disclose specific application objects and welding parameters, which makes the method impossible to implement. At the same time, the method does not introduce the effects that can be obtained after the welding wire setting adopts this structure. The method cannot be applied to the lead welding requirements of vacuum-solid devices.

[0008] Therefore, based on the need to improve the resolution of EBAPS, after experimental verification, the present invention discloses a low lead arc control method for vacuum-solid devices.

[0009] The information disclosed in the background technology section is only intended to enhance the understanding of the overall background of the invention and should not be regarded as an admission or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art. Summary of the invention

[0010] In response to the above technical problems, the present application provides a vacuum-solid device low lead arc processing method, lead arc structure, and EBAPS device. The method can realize the regulation of low lead arc in vacuum-solid devices. The method can realize reliable regulation of close contact distance on chips with ultra-high welding heights. After welding, it can avoid the device short circuit caused by the contact between the photocathode and the gold wire of the chip after the indium seal of the device, or the direct contact between the gold wire arc and the side wall of the metal pad caused by the reduction of the arc casting height, resulting in the chip optical imaging short circuit and other problems.

[0011] The present application provides a vacuum-solid device low lead wire arc processing method, comprising the following steps:

[0012] 1) bonding a pad in the mounting cavity of a ceramic housing, and soldering the bonding pad in the mounting cavity of a ceramic housing with a solder pad using solder; then evenly coating the solder on the pad, aligning the chip with the solder pad with the pad, and soldering at a high temperature;

[0013] 2) Since the ceramic pad is lower than the chip pad, for the convenience of operation, the ceramic pad is set as the second soldering point and the chip pad is set as the first soldering point;

[0014] 3) using a capillary cutter in BSOB mode to set a bonding wire between the first solder joint and the second solder joint;

[0015] The bonding lead includes: a convex section, a concave section, a reversal section, a platform section, and a descending section; one end of the convex section is connected to the first welding point and convex upward, and the other end of the convex end is connected to the concave section; the concave section is concave downward, and the other end of the concave section is connected to the reversal section; the reversal section extends obliquely in a direction away from the first welding point and is connected to one end of the platform section; the other end of the platform section is connected to the starting point of the descending section, and the other end of the descending section is connected to the second welding point;

[0016] The platform segment includes: a node K2 segment, and the descending segment includes: a node K3 segment; the node K2 segment is connected to the extended end of the reversal segment and extends toward the second welding point; the other end of the node K2 segment is connected to one end of the node K3 segment; the node K3 segment extends obliquely toward the second welding point and is connected to the second welding point.

[0017] Preferably, the height of the raised arc of the raised section is 100 to 180 μm; the height of the arc of the recessed section relative to the chip after recessing is 60 to 100 μm; the reversal angle of the arc of the reversal section is -35 to -45°, and the reversal distance relative to the first welding point is 0.5 to 3%.

[0018] Preferably, the length of the platform segment controlled by the node K2 parallel to the chip is 30% to 85% of the total length of the chip; and the platform angle of the node K2 segment is 10 to 50°.

[0019] Preferably, the descending section controlled by the node K3 is 1-20% of the total length of the chip; and the platform angle of the node K3 section is 1-40°.

[0020] Preferably, the platform angle of the node K2 segment is 30-40°; and the platform angle of the node K3 segment is 13-20°.

[0021] Preferably, the length of the node K2 segment parallel to the chip is 75-85% of the total length of the chip; and the length of the node K3 segment is 1-5% of the total length of the chip.

[0022] Preferably, in step 1), solder is provided on the contact surfaces of the pad and the ceramic shell; the solder is solidified after bonding and stacking; the solder is a high temperature resistant and low outgassing rate conductive solder; and the solder solidification condition is heating at 200-300° C. for 7-9 hours.

[0023] Preferably, “arranging a bonding wire between the first solder joint and the second solder joint by a capillary wedge” comprises the following steps:

[0024] 2.1) A capillary wedge is used to first form a solder ball on the second solder joint, and then a wedge is used to form a solder wire with a convex section height at the first solder joint vertical lead, and then the solder wire is further extended to set a solder wire with a concave section height, and then the solder wire is reversed in the opposite direction relative to the second solder joint lead position to set a reverse section;

[0025] 2.2) When the welding wire is reversed to a preset angle and has an arc, under the action of the capillary chopper, the lead moves toward the second welding point to set a platform segment. The movement position of the welding wire toward the second welding point is determined by the length of the node K2 segment and the node K3 segment and the node platform angle. When the welding wire position moves to the second welding point, under the action of the chopper, the welding wire moves downward and connects with the small ball on the second welding point to complete the welding.

[0026] The second welding point of the bonding wire is welded by a thermosonic wire bonding method.

[0027] Another aspect of the present application provides a low lead wire arc processing method, comprising: a convex section, a concave section, a reversal section, a platform section, and a descending section; one end of the convex section is connected to the first welding point and convex upward, and the other end of the convex end is connected to the concave section; the concave section is concave downward, and the other end of the concave section is connected to the reversal section; the reversal section extends obliquely in a direction away from the first welding point and is connected to one end of the platform section; the other end of the platform section is connected to the second welding point;

[0028] Platform section: controlled by node K2, descending section: controlled by node K3; node K2 section

[0029] (i.e., the platform segment) is connected to the extended end of the inversion segment and extends toward the second welding point; the other end of the node K2 segment is connected to one end of the node K3 segment; the node K3 segment extends obliquely toward the second welding point and is connected to the second welding point. The first welding point is disposed on the surface of the chip; the second welding point is disposed in the ceramic shell cavity.

[0030] Another aspect of the present application further provides an EBAPS device, comprising: the lead wire arc structure as described above, a ceramic shell and a chip accommodated in the ceramic shell, which is prepared by the method as described above;

[0031] The first welding point is arranged on the top surface of the chip; the second welding point is arranged in the mounting cavity of the ceramic shell; the first end of the lead wire arc structure is welded to the first welding point; and the second end of the lead wire arc structure is welded to the second welding point.

[0032] The beneficial effects of this application include:

[0033] 1) The low-lead wire arc processing method for vacuum-solid devices provided in the present application can form bonding leads that will not short-circuit after packaging the device, and after reducing the wire arc height, the device can be imaged normally. This method can reduce the close proximity distance of the bonding leads to 0.3mm or less. Compared with the wire arc of the existing structure, the height of the low-profile wire arc is significantly reduced, and the risk of breakdown and short circuit is greatly reduced. At the same time, there is no obvious bending structure on the wire arc shape, the bonding wire is smoother, and the tensile strength of the lead is improved. The tensile strength of the resulting welding wire is 15-16gf, which is significantly higher than the welding wire of the existing structure.

[0034] 2) The wire arc structure provided by the present application can effectively reduce the close contact distance of the device to 0.3mm or less, providing a new idea for improving the imaging effect of the device. The bonding wire line is smoother, avoiding the formation of bending stress points on the lead, which is beneficial to improving the tensile strength of the bonding effect. At the same time, due to the smooth line shape, the probability of contact between the lead and the pad is reduced, and the distance is controllable, so that while obtaining a smaller close contact distance, the device is guaranteed to be safe to use and not short-circuited.

[0035] 3) The EBAPS device provided in the present application has a close proximity distance of 0.3 mm or less, the bonding wire is smoother, the tensile strength of the lead is improved, and the risk of breakdown and short circuit is greatly reduced. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 A schematic diagram of the front cross-sectional structure of an EBAPS device provided in an embodiment of the present application;

[0037] Figure 2 Schematic diagram of the front and cross-sectional structure of the chip bonding fixture provided in the embodiment of the present application; a) is comparative example 2; b) is an embodiment;

[0038] Figure 3 The present application provides a schematic diagram of a partial enlarged structure of the lead wire arc in the embodiment and comparative example 2; a) is comparative example 2; b) is the embodiment;

[0039] Figure 4 The present application provides partial magnified photos of the lead wire arc in the embodiment and comparative example 2; the magnification is 10 times; a) is comparative example 2; b) is the embodiment;

[0040] Figure 5 This is an electron bombardment image of an EBAPS device with a close proximity distance of ≤0.3 mm obtained by the method in the embodiment of the present application;

[0041] Figure 6 A comparison curve of the tensile strength of a low-profile wire arc and a conventional wire arc obtained by the method in the embodiment of the present application;

[0042] Legend:

[0043] Pressing plate, top plate 4, frame 2, clamping part 11, pressing plate 3 DETAILED DESCRIPTION

[0044] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Generally, the components of the embodiments of the present invention described and shown in the drawings here can be arranged and designed in various different configurations.

[0045] Therefore, the following detailed description of the embodiments of the present invention provided in the accompanying drawings is not intended to limit the scope of the invention claimed for protection, but merely represents selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0046] The technical means that are not described in detail in this application and are not used to solve the technical problems of this application are all set according to the common knowledge in the field, and can be implemented in a variety of common knowledge settings.

[0047] See also Figures 1 to 5 The vacuum-solid device low lead arc processing method provided in the present application comprises the following steps:

[0048] 1) Chip welding: Figure 1 As shown, a mounting cavity is provided in the ceramic shell, a pad is accommodated in the mounting cavity, solder is provided on the surface where the pad connects with the bottom of the ceramic shell groove, and the pad is connected with the ceramic shell through the solder; a chip is provided on the top surface of the pad, and the chip is bonded to the pad through the solder layer. The solder used is a high temperature resistant conductive solder.

[0049] Solder is used to bond the bottom surface of the pad and the bottom of the inner groove of the ceramic shell, and then high-temperature resistant conductive solder is used to bond the chip and the pad. The solder curing condition is heated at 200-300℃ for 7-9h. The device structure after welding is as follows Figure 1 shown.

[0050] In order to prevent the melting of indium tin solder and overflow of the indium seal position, oxidation of the bonding wire, and to improve the bonding adhesion rate, in view of the advantages of thermosonic gold wire bonding, such as low bonding temperature, low pressure, ability to achieve complex arch wire shapes, no need for protective gas, simple operation, and easy formation of solder joints under arc discharge conditions, gold wire with a diameter of Φ20-30μm is used as the bonding wire, and the thermosonic wire bonding method is used to achieve the electrical performance connection of the device.

[0051] 2) Chip bonding: Place the chip to be bonded Figure 2The bonding is performed in the bonding fixture shown. The bonding fixture includes: a pressure plate, a top plate 4 and a frame 2. A plurality of mounting grooves 1 are arranged at intervals on the frame 2, and the chip to be bonded is accommodated in the mounting groove 1. The top plate 4 is connected to the bottom surface of the chip to be bonded. The pressure plate includes: a clamping portion 11 and a crimping plate 3; the periphery of both ends of the crimping plate 3 is clamped in the clamping portion 11 to control the up and down movement of the crimping plate 3. A through hole is provided on the crimping plate 3, and a through hole cover is provided on the mounting groove 1 to achieve the bonding after fixing the bonding position of the chip to be bonded in the groove, which can avoid displacement during bonding. When bonding the chip, preheat it for 1 to 10 minutes to heat it to 90 to 120°C before bonding.

[0052] 3) Set the low profile arc (bonding line) parameters: The arc shape is controlled by 3 nodes, and the specific parameters are set as follows: Figure 3 k1) in (b) includes: a convex section, a concave section, and a reversal section; one end of the convex section is connected to the first welding point; the other end of the convex section is connected to one end of the concave section; the other end of the concave section is connected to one end of the reversal section, and the reversal section extends obliquely away from the first welding point and is connected to one end of the platform section. The other end of the platform section is connected to one end of the descending section, and the other end of the descending section extends obliquely toward the second welding point and is connected to the second welding point.

[0053] The height of the raised arc set in the raised section is 160-180μm, and the height of the arc set in the recessed section relative to the chip after being recessed is 60-100μm; the reversal angle of the arc in the reversed section is -35--45° (negative numbers represent that the arc moves in the opposite direction of the second solder joint), and the reversal distance relative to the first solder joint is 0.5-3%, and the more preferred reversal angle is -40°. The reverse displacement is the branch part of the arc, which provides enhanced tension to support the entire arc from collapsing. The height of the raised arc, the height of the arc relative to the chip after being recessed, and the reversal angle can be determined based on the height difference and horizontal distance between the first and second solder joints.

[0054] The platform segment is mainly controlled by the node K2, and the descending segment is mainly controlled by the node K3. The node K2 segment (platform segment) is connected to the extended end of the reversal segment and extends toward the second welding point. The other end of the node K2 segment is connected to one end of the node K3 segment. The node K3 segment (descending segment) extends obliquely toward the second welding point and is connected to the second welding point.

[0055] The length of the node K2 segment in the platform segment parallel to the chip is 40% to 85% of the total length of the chip, and more preferably 75 to 85%. The platform length should not be too long, otherwise the arc will appear to be floating. The platform angle between the node K2 segment and the plane where the second welding point is located is 10 to 50°, and more preferably 30 to 40°. At node 3 ( Figure 3(b) k3), the length of node K3 parallel to the chip is 1-20% of the total length of the chip, more preferably 1-5%, and the platform angle between the node K3 segment and the plane where the second solder point is located is 10-40°, more preferably 13-20°.

[0056] The length of the node K2 of the platform segment represents the length of the arc line parallel to the chip, which is usually 40% to 85%, so that the length of the gold wire parallel to the second solder joint is just beyond the edge of the pad to prevent the device from short circuiting. It can be adjusted according to the arc length of the lead. The platform angle is usually 10 to 50 degrees. The platform angle of the node should not be too large, otherwise it will cause the gold wire to fluctuate between the second node and the first node, thereby affecting the bonding strength.

[0057] The angle of the node K3 section of the descending section and the node platform length. The platform angle should not be too large, usually 1° to 40°. If the node platform angle is too large, the arc will fluctuate greatly, thus affecting the bonding strength. The node platform length is relative to the length of the second solder joint, usually 1 to 20%. The longer the node platform, the more likely it is that the third node will be between the first and second nodes, making the entire arc descend too long, causing the arc to hit the side wall of the metal gasket, causing the risk of device short circuit. For specific structure, see Figure 3 b) Figure 4 b).

[0058] 4) Set welding parameters: set the first welding point on the chip, and define the welding pad of the ceramic tube shell as the second welding point.

[0059] 5) Wire bonding: In order to improve the bonding strength, the bonding wires on the device adopt the BSOB mode. First, the solder joint is set on the second solder joint, and then the bonding wire is set between the first solder joint and the second solder joint according to the above parameter requirements by a splitter.

[0060] When welding the wire, a capillary chopper is used to first form a weld on the second weld, and then the chopper is used to form a weld at the height of the convex section at the first weld perpendicular to the lead, and then the weld is reversed in the opposite direction relative to the lead position of the second weld to set a reversal section. In this process, since the reversal height and reversal angle of the weld are set according to the aforementioned parameters, when the weld is reversed to the preset angle, it has an arc. Under the action of the capillary chopper, the lead moves toward the second weld to set a platform section and a descending section. The position of the weld moving toward the second weld is determined by the node platform length and the node platform angle. When the weld moves to the second weld, under the action of the chopper, the weld moves downward to connect with the small ball on the second weld to complete the welding, and the following is obtained: Figure 3 The bonding wire structure shown in Figure b. The wires on the other side of the device are also welded in the same order.

[0061] 6) Post-weld inspection.

[0062] Comparative Example 1

[0063] The difference from Example 1 is that the arc parameters described in Comparative Example 2 are not adopted, the node K1 segment and its inversion length and inversion angle are not set at the first welding point, and the arc height is directly reduced to 100μm. The gold wire arc of the device will contact the pad, causing the device optical imaging to be short-circuited, and the proximity distance cannot be further reduced.

[0064] Comparative Example 2

[0065] See also Figure 4 a), Figure 3 a), welded by the process operation in Example 2 disclosed in CN 202311496775.8, a bending section and a hook section are provided on one end of the bonding wire, and the extended end of the hook section is bonded to the chip. The bending section extends obliquely toward the welding surface of the chip on the pad; the extended end of the bending end is connected to a section of the hook section; the hook section is bent and extended toward the welding surface of the chip. Due to the structure of the hook section and the existence of the bending section, when the bonding wire extends obliquely upward from the bending section, it is arranged close to the pad. If the height of the hook section and the bending section is reduced, the two are easily in contact and cause a short circuit, so this structure cannot reduce the lead height.

[0066] Result analysis:

[0067] By comparing Figure 3 The arc of the comparative example 2 shown ( Figure 3 a) and low profile line arc comparison diagram ( Figure 3 b), compared with the arc in comparative example 2, the height of the low-profile arc is significantly reduced, and the measured height reduction can reach 90μm. Through parameter optimization, the low-profile arc is smoother.

[0068] By comparison Figure 4 a) and b) show that the bonding wire obtained by the method provided by the present application has a smoother line shape, avoiding the formation of bending stress points on the wire, which is beneficial to improving the tensile strength of the bonding. At the same time, due to the smooth line shape, the probability of the wire contacting the pad is reduced, and the distance is controllable, so that the device can be used safely and without short circuit while obtaining a smaller close contact distance. Figure 4 Node K1 in b is smaller and therefore cannot be seen after zooming in.

[0069] After the bonding wires are set by the method in the embodiment, the close contact distance can be less than or equal to 300 μm. After the device is assembled, the assembly structure is to set the photocathode directly opposite the chip after the bonding wires, and the photocathode is made on the convex platform of the transparent window. The EBAPS device structure is obtained after the indium sealing device. Figure 1 As shown, and imaging test is performed. The imaging results are as follows Figure 5 As shown by Figure 5 It can be seen that the imaging resolution of the device is high. At the same time, this method can also avoid causing short circuits in the device. After reducing the arc height, the device optical imaging is normal. The imaging results are as follows Figure 5 shown.

[0070] According to the wire bonding shear strength test standard and the arc tensile strength of the device obtained in Comparative Example 2, 100 bonding wires were set on the EBAPS device according to the methods of the embodiment and Comparative Example 2, and 13 bonding wires were randomly selected for tensile strength test. The results are listed in Figure 6 In, by Figure 6 It can be seen that the tensile strength of the bonding wire of the bonding structure is higher than that of the bonding wire of the structure obtained in Comparative Example 2, the highest can reach 15-16gf, and the lowest is 13-14gf, and the tensile strength of nearly one solder joint overlaps with the tensile strength value of the wire type in Comparative Example 2, and the test results of the remaining solder wires are better than those of Comparative Example 2. It shows that after bonding by this method, the connection strength of the wire is not affected and is effectively strengthened.

[0071] Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments, or to make equivalent substitutions for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for processing low lead arcs of vacuum-solid devices, It is characterized in that The following steps are involved: 1) bonding a pad in the mounting cavity of a ceramic housing, and soldering the bonding pad in the mounting cavity of a ceramic housing with a solder pad using solder; then evenly coating the solder on the pad, aligning the chip with the solder pad with the pad, and soldering at a high temperature; 2) Since the ceramic pad is lower than the chip pad, for the convenience of operation, the ceramic pad is set as the second soldering point and the chip pad is set as the first soldering point; 3) using a capillary cutter in BSOB mode to set a bonding wire between the first solder joint and the second solder joint; The bonding lead includes: a convex section, a concave section, a reversal section, a platform section, and a descending section; one end of the convex section is connected to the first welding point and convex upward, and the other end of the convex end is connected to the concave section; the concave section is concave downward, and the other end of the concave section is connected to the reversal section; the reversal section extends obliquely in a direction away from the first welding point and is connected to one end of the platform section; the other end of the platform section is connected to the starting point of the descending section, and the other end of the descending section is connected to the second welding point; The platform segment includes: a node K2 segment, and the descending segment includes: a node K3 segment; the node K2 segment is connected to the extended end of the reversal segment and extends toward the second welding point; the other end of the node K2 segment is connected to one end of the node K3 segment; the node K3 segment extends obliquely toward the second welding point and is connected to the second welding point.

2. The low lead wire arc processing method of vacuum-solid device according to claim 1, It is characterized in that The height of the raised arc set in the raised section is 100-180 μm; the height of the arc set in the recessed section relative to the chip is 60-100 μm; the reversal angle of the reversal section arc is -35--45°, and the reversal distance is 0.5-3% relative to the first solder joint.

3. The low lead wire arc processing method of vacuum-solid device according to claim 1, It is characterized in that The length of the platform segment controlled by the node K2 parallel to the chip is 30% to 85% of the total length of the chip; the platform angle of the node K2 segment is 10 to 50°.

4. The low lead wire arc processing method of vacuum-solid device according to claim 1, It is characterized in that The descending section controlled by the node K3 is 1 to 20% of the total length of the chip; the platform angle of the node K3 section is 1 to 40°.

5. The low lead wire arc processing method of vacuum-solid device according to claim 1, It is characterized in that The platform angle of the node K2 segment is 30 to 40°; the platform angle of the node K3 segment is 13 to 20°.

6. The low lead wire arc processing method of vacuum-solid device according to claim 1, It is characterized in that The length of the node K2 segment parallel to the chip is 75-85% of the total length of the chip; the length of the node K3 segment is 1-5% of the total length of the chip.

7. The low lead wire arc processing method of vacuum-solid device according to claim 1, It is characterized in that In step 1), solder is arranged on the contact surface of the pad and the ceramic shell; the solder is solidified after bonding and stacking; the solder is a high temperature resistant and low outgassing rate conductive solder; the solder solidification condition is heating at 200-300° C. for 7-9 hours.

8. The low lead wire arc processing method of vacuum-solid device according to claim 1, It is characterized in that “Providing a bonding wire between a first solder joint and a second solder joint by a capillary wedge” comprises the following steps: 2.1) A capillary wedge is used to first form a solder ball on the second solder joint, and then a wedge is used to form a solder wire with a convex section height at the first solder joint vertical lead, and then the solder wire is further extended to set a solder wire with a concave section height, and then the solder wire is reversed in the opposite direction relative to the second solder joint lead position to set a reverse section; 2.2) When the welding wire is reversed to a preset angle and has an arc, under the action of the capillary chopper, the lead moves toward the second welding point to set a platform segment. The movement position of the welding wire toward the second welding point is determined by the length of the node K2 segment and the node K3 segment and the node platform angle. When the welding wire position moves to the second welding point, under the action of the chopper, the welding wire moves downward and connects with the small ball on the second welding point to complete the welding. The second welding point of the bonding wire is welded by a thermosonic wire bonding method.

9. A low lead wire arc processing method, It is characterized in that include: Raised section, sunken section, reversal section, platform section, descending section; One end of the raised section is connected to the first welding point and raised upward, and the other end of the raised end is connected to the recessed section; the recessed section is recessed downward, and the other end of the recessed section is connected to the inversion section; the inversion section extends obliquely in a direction away from the first welding point and is connected to one end of the platform section; the other end of the platform section is connected to the second welding point; The platform segment is controlled by the node K2, and the descending segment is controlled by the node K3. The node K2 segment (i.e., the platform segment) is connected to the extended end of the inversion segment and is extended toward the second welding point. The other end of the node K2 segment is connected to one end of the node K3 segment. The node K3 segment (i.e., the descending segment) is extended obliquely toward the second welding point and is connected to the second welding point. The first welding point is set on the chip surface. The second welding point is set in the ceramic shell cavity.

10. An EBAPS device, It is characterized in that include: The lead wire arc structure, the ceramic shell and the chip accommodated in the ceramic shell are manufactured by the method as claimed in claim 9; The first solder joint is arranged on the top surface of the chip; the second solder joint is arranged in the mounting cavity of the ceramic housing; The first end of the lead wire arc structure is welded to the first welding point; the second end of the lead wire arc structure is welded to the second welding point.

Citation Information

Patent Citations

  • Method and apparatus for forming a low profile wire loop

    CN101193724A

  • Manufacturing method of backside illuminated EBAPS

    CN117525170A

Cited By

  • Bus bar welding method and bus assembly

    CN120981012A