Semiconductor device and method of manufacturing the same

By using high etch resistance polycrystalline oxide semiconductor film and interlayer insulating layer covering technology in semiconductor devices, the electrical characteristics problems caused by the shape deviation of the oxide semiconductor film are solved, and the yield and field effect mobility are improved, so as to achieve Stable electrical characteristics and efficient manufacturing process.

CN118943201APending Publication Date: 2024-11-12JAPAN DISPLAY INC +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410576294.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-05-12
Filing Date
2024-05-10
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

In semiconductor devices using oxide semiconductor films, the oxide semiconductor film has little etch resistance and is difficult to control its shape, resulting in a decrease in electrical characteristics deviation and yield. Especially in the manufacture of large-area glass substrates, the electrical characteristics problems caused by shape deviation are serious. .

Method used

The oxide semiconductor layer with a polycrystalline structure is used to form an oxide semiconductor film with high etch resistance by sputtering or atomic layer deposition. During the etching process, the film thickness difference is controlled to be less than 1 nm to ensure the film in the channel region. Thickness consistency, and an interlayer insulating layer is used to cover the source electrode and the drain electrode to reduce shape deviation.

Benefits of technology

The stability of the oxide semiconductor film shape and consistency of electrical characteristics is achieved, the yield of the semiconductor device is improved, and the high field effect mobility is maintained, ensuring the stability and durability of electrical characteristics.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118943201A_ABST
    Figure CN118943201A_ABST
Patent Text Reader

Abstract

The invention relates to a semiconductor device and a manufacturing method thereof. The present invention provides a semiconductor device having a small variation in shape of an oxide semiconductor film and having stable electrical characteristics. The semiconductor device includes: a gate electrode; a gate insulating layer over the gate electrode; an oxide semiconductor layer having a polycrystalline structure over the gate insulating layer; a source electrode and a drain electrode over the oxide semiconductor layer; and an interlayer insulating layer that covers the source electrode and the drain electrode and is in contact with the oxide semiconductor layer, the oxide semiconductor layer includes a first region overlapping one of the source electrode and the drain electrode and a second region in contact with the interlayer insulating layer, and the difference between the film thickness of the first region and the film thickness of the second region is 1 nm or less.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] One embodiment of the present invention relates to a semiconductor device. In particular, one embodiment of the present invention relates to a semiconductor device using an oxide semiconductor film as a channel. In addition, one embodiment of the present invention relates to a method for manufacturing a semiconductor device. Background Art

[0002] In recent years, semiconductor devices that use oxide semiconductor films instead of silicon semiconductor films such as amorphous silicon, low-temperature polycrystalline silicon, and single-crystal silicon as channels have been developed (for example, see Patent Documents 1 to 6). Semiconductor devices including such oxide semiconductor films have a simple structure like semiconductor devices including amorphous silicon films, and can be manufactured on a glass substrate by a low-temperature process. In addition, it is known that semiconductor devices including oxide semiconductor films have higher field effect mobility than semiconductor devices including amorphous silicon films.

[0003] Prior art literature

[0004] Patent Literature

[0005] Patent Document 1: Japanese Patent Application Publication No. 2021-141338

[0006] Patent Document 2: Japanese Patent Application Publication No. 2014-099601

[0007] Patent Document 3: Japanese Patent Application Publication No. 2021-153196

[0008] Patent Document 4: Japanese Patent Application Publication No. 2018-006730

[0009] Patent Document 5: Japanese Patent Application Publication No. 2016-184771

[0010] Patent Document 6: Japanese Patent Application Publication No. 2021-108405 Summary of the invention

[0011] Problems to be solved by the invention

[0012] However, in conventional semiconductor devices including oxide semiconductor films, the oxide semiconductor films have low etching resistance and are difficult to control in shape. In particular, in semiconductor devices manufactured using large-area substrates such as glass substrates, the deviation in the shape of the oxide semiconductor film causes the deviation in the electrical characteristics of the semiconductor device, which is the main reason for the reduction in yield.

[0013] One object of one embodiment of the present invention is to provide a semiconductor device having stable electrical characteristics while suppressing shape deviation of an oxide semiconductor film. Another object of one embodiment of the present invention is to provide a method for manufacturing a semiconductor device having improved yield while suppressing shape deviation of an oxide semiconductor film.

[0014] Means for solving problems

[0015] A semiconductor device involved in one embodiment of the present invention includes: a gate electrode; a gate insulating layer above the gate electrode; an oxide semiconductor layer having a polycrystalline structure above the gate insulating layer; a source electrode and a drain electrode above the oxide semiconductor layer; and an interlayer insulating layer, which covers the source electrode and the drain electrode and is in contact with the oxide semiconductor layer, the oxide semiconductor layer includes a first region overlapping with one of the source electrode and the drain electrode, and a second region in contact with the interlayer insulating layer, and the difference between the film thickness of the first region and the film thickness of the second region is less than 1 nm.

[0016] A method for manufacturing a semiconductor device involved in one embodiment of the present invention includes: forming a gate electrode, forming a gate insulating layer on the gate electrode, forming an oxide semiconductor layer having a polycrystalline structure on the gate insulating layer, forming a source electrode and a drain electrode on the oxide semiconductor layer, and forming an interlayer insulating layer covering the source electrode and the drain electrode and in contact with the oxide semiconductor layer, wherein the oxide semiconductor layer includes a first region overlapping with one of the source electrode and the drain electrode, and a second region in contact with the interlayer insulating layer, and the difference between the film thickness of the first region and the film thickness of the second region is less than 1 nm. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 It is a schematic cross-sectional view showing the structure of a semiconductor device according to one embodiment of the present invention.

[0018] Figure 2 It is a schematic plan view showing the structure of a semiconductor device according to one embodiment of the present invention.

[0019] Figure 3 This is a flowchart illustrating a method for manufacturing a semiconductor device according to one embodiment of the present invention.

[0020] Figure 4 It is a schematic cross-sectional view showing a method for manufacturing a semiconductor device according to one embodiment of the present invention.

[0021] Figure 5 It is a schematic cross-sectional view showing a method for manufacturing a semiconductor device according to one embodiment of the present invention.

[0022] Figure 6It is a schematic cross-sectional view showing a method for manufacturing a semiconductor device according to one embodiment of the present invention.

[0023] Figure 7 It is a schematic cross-sectional view showing a method for manufacturing a semiconductor device according to one embodiment of the present invention.

[0024] Figure 8 It is a schematic cross-sectional view showing a method for manufacturing a semiconductor device according to one embodiment of the present invention.

[0025] Fig. 9 It is a schematic cross-sectional view showing a method for manufacturing a semiconductor device according to one embodiment of the present invention.

[0026] Fig.10 It is a schematic cross-sectional view showing a method for manufacturing a semiconductor device according to one embodiment of the present invention.

[0027] Fig.11 It is a schematic cross-sectional view showing a method for manufacturing a semiconductor device according to one embodiment of the present invention.

[0028] Fig.12 This is a schematic plan view schematically showing a display device according to one embodiment of the present invention.

[0029] Fig.13 This is a block diagram showing a circuit configuration of a display device according to one embodiment of the present invention.

[0030] Fig.14 : is a circuit diagram showing a pixel circuit of a display device according to one embodiment of the present invention.

[0031] Fig.15 It is a schematic cross-sectional view showing the structure of a display device according to one embodiment of the present invention.

[0032] Fig.16 : is a circuit diagram showing a pixel circuit of a display device according to one embodiment of the present invention.

[0033] Fig.17 It is a schematic cross-sectional view showing the structure of a display device according to one embodiment of the present invention.

[0034] Fig.18A This is a graph showing the electrical characteristics of Sample A in the Example.

[0035] Fig.18B This is a graph showing the electrical characteristics of sample B-1 in the example.

[0036] Fig.18C This is a graph showing the electrical characteristics of sample B-2 in the example.

[0037] Fig.18D This is a graph showing the electrical characteristics of sample C-1 in the example.

[0038] Fig.18E This is a graph showing the electrical characteristics of sample C-2 in the example.

[0039] Fig.19 This is a graph showing threshold values ​​calculated from the electrical characteristics of each sample in the example.

[0040] Fig. 20 This is a graph showing the field effect mobility (field effect mobility in the saturation region) calculated from the electrical characteristics of each sample in the example.

[0041] Description of Reference Numerals

[0042] 10: Semiconductor device, 20: Display device,

[0043] 11: substrate, 12C: wiring, 12GE: gate electrode, 12W: wiring, 14: gate insulating layer, 15: contact hole, 16: gate insulating layer, 22: oxide semiconductor film, 24: oxide semiconductor layer, 26: oxide semiconductor layer, 32C: wiring, 32D: drain electrode, 32S: source electrode, 32W: wiring, 34: interlayer insulating layer, 36: metal oxide film, 38: interlayer insulating layer, 39: insulating layer, 42C: common electrode, 44: insulating layer, 46C: electrode, 46P: pixel electrode,

[0044] 110: driving transistor, 120: selecting transistor, 210: holding capacitor, 211: signal line, 212: gate line, 213: anode power line, 214: cathode power line, 220: liquid crystal region, 240: sealing region, 260: terminal region, 300: array substrate, 301: pixel circuit, 302: source driving circuit, 303: gate driving circuit, 304: source wiring, 305: gate wiring, 306: terminal portion, 307: connecting wiring, 310: sealing portion, 311: liquid crystal element, 320: opposing substrate, 330: flexible printed circuit substrate, 340: chip, 350: holding capacitor, 362: insulating layer, 363: opening, 390: pixel electrode, 392: light-emitting layer, 394: common electrode DETAILED DESCRIPTION

[0045] Hereinafter, various embodiments of the present invention will be described with reference to the accompanying drawings. The following disclosure is only an example. While maintaining the gist of the invention, the configuration that can be easily conceived by those skilled in the art by appropriately changing the configuration of the embodiment is of course included in the scope of the present invention. In order to make the description clearer, the accompanying drawings sometimes schematically represent the width, film thickness, shape, etc. of each part compared to the actual method. However, the shape shown in the figure is only an example and does not limit the interpretation of the present invention. In this specification and the accompanying drawings, the same symbols are marked for the same components as those described previously with respect to the figures that have appeared, and the detailed description is sometimes appropriately omitted.

[0046] In this specification, "semiconductor device" refers to all devices that can function by utilizing semiconductor characteristics. A transistor and a semiconductor circuit are included in one embodiment of a semiconductor device. The semiconductor device of the embodiment shown below can be, for example, a display device, an integrated circuit (IC) such as a microprocessor (MPU), or a transistor used in a memory circuit.

[0047] In this specification, a "display device" refers to a structure that uses an electro-optical layer to display an image. For example, the term display device sometimes refers to a display panel including an electro-optical layer, or sometimes refers to a structure in which other optical components (such as polarization components, backlights, touch panels, etc.) are installed relative to a display unit. In the "electro-optical layer", as long as there is no technical contradiction, a liquid crystal layer, an electroluminescent (EL) layer, an electrochromic (EC) layer, and an electrophoretic layer may be included. Therefore, in the embodiment, as a display device, a liquid crystal display device including a liquid crystal layer and an organic EL display device including an organic EL layer are exemplified for description. Among them, the structure described in the embodiment can be applied to a display device including the above-mentioned other electro-optical layers.

[0048] In this specification, etc., the direction from the substrate toward the oxide semiconductor layer is referred to as "up" or "above". On the contrary, the direction from the oxide semiconductor layer toward the substrate is referred to as "down" or "below". Thus, for the sake of convenience, the terms "up" or "down" are used for description, but the up-and-down relationship between the substrate and the oxide semiconductor layer can also be configured in a direction different from that shown in the figure. In addition, the expression "oxide semiconductor layer on the substrate" is merely an explanation of the up-and-down relationship between the substrate and the oxide semiconductor layer, and other components may be arranged between the substrate and the oxide semiconductor layer. Up or down refers to the stacking order in a structure having a plurality of layers stacked, and in the case of a pixel electrode described as above a semiconductor device, it may also be a positional relationship in which the semiconductor device and the pixel electrode do not overlap when viewed from above. On the other hand, in the case of a pixel electrode described as vertically above a semiconductor device, it refers to a positional relationship in which the semiconductor device and the pixel electrode overlap when viewed from above. It should be noted that viewing from above refers to observing from a direction perpendicular to the surface of the substrate.

[0049] In this specification and the like, the term "film" and the term "layer" can be interchanged as appropriate.

[0050] In this specification, etc., the expression "α includes A, B, or C", "α includes any one of A, B, and C", or "α includes one selected from A, B, and C" does not exclude the case where α includes a plurality of combinations of A to C unless otherwise specified. In addition, these expressions do not exclude the case where α includes other constituent elements.

[0051] It should be noted that the following embodiments can be combined with each other as long as no technical contradiction occurs.

[0052] <First embodiment>

[0053] Reference Figures 1 to 11 A semiconductor device 10 according to an embodiment of the present invention will be described.

[0054] [Configuration of Semiconductor Device 10]

[0055] Reference Figure 1 and Figure 2 The configuration of a semiconductor device 10 according to one embodiment of the present invention will be described. Figure 1 It is a cross-sectional view showing a schematic structure of a semiconductor device 10 according to an embodiment of the present invention. Figure 2 It is a schematic plan view showing the structure of a semiconductor device 10 according to one embodiment of the present invention. Figure 1 The cross-sectional view shown corresponds to Figure 2 The cross section is shown along line A1-A2.

[0056] like Figure 1 As shown, the semiconductor device 10 is provided on the substrate 11. The semiconductor device 10 includes a gate electrode 12GE, gate insulating layers 14 and 16, an oxide semiconductor layer 26, a source electrode 32S, a drain electrode 32D, and interlayer insulating layers 34 and 38. In the case where the source electrode 32S and the drain electrode 32D are not particularly distinguished, they can be collectively referred to as a source electrode and a drain electrode 32. In addition, the gate electrode 12GE, the gate insulating layers 14 and 16, and the oxide semiconductor layer 26 are sometimes referred to as a transistor. The semiconductor device 10 is a so-called bottom-gate transistor in which the gate electrode 12GE is provided below the oxide semiconductor layer 26.

[0057] In this embodiment, a bottom-gate transistor is exemplified as the semiconductor device 10 , but the semiconductor device 10 is not limited to the bottom-gate transistor. For example, the semiconductor device 10 may be a dual-gate transistor in which gate electrodes are provided above and below the oxide semiconductor layer 26 .

[0058] The gate electrode 12GE is provided on the substrate 11. The gate insulating layers 14 and 16 are provided on the substrate 11 and the gate electrode 12GE. The gate insulating layers 14 and 16 have a stacked structure, and the gate insulating layer 16 is provided on the gate insulating layer 14. The oxide semiconductor layer 26 is provided on the gate insulating layers 14 and 16. The source electrode 32S and the drain electrode 32D are provided on the oxide semiconductor layer 26. The interlayer insulating layers 34 and 38 are provided on the oxide semiconductor layer 26 and the source electrode 32S and the drain electrode 32D. The interlayer insulating layers 34 and 38 have a stacked structure, and the interlayer insulating layer 38 is provided on the interlayer insulating layer 34. That is, the interlayer insulating layers 34 and 38 cover the source electrode 32S and the drain electrode 32D, and the interlayer insulating layer 34 is in contact with the oxide semiconductor layer 26.

[0059] It should be noted that, although not shown in the figure, a metal oxide layer may be provided between the gate insulating layer 16 and the oxide semiconductor layer 26. The metal oxide layer may also have the same pattern as the oxide semiconductor layer 26. For example, as the metal oxide layer, an oxide containing aluminum (such as aluminum oxide) may be used. The film thickness of the metal oxide layer is not less than 1 nm and not more than 10 nm, preferably not less than 1 nm and not more than 5 nm.

[0060] like Figure 2As shown, when viewed from above, the oxide semiconductor layer 26 overlaps with the gate electrode 12GE. The D1 direction is the direction connecting the source electrode 32S and the drain electrode 32D, and the D2 direction is the direction orthogonal to the D1 direction. In the semiconductor device 10, the channel length L corresponds to the length of the region (channel region) of the oxide semiconductor layer 26 between the source electrode 32S and the drain electrode 32D in the D1 direction, and the channel width W corresponds to the width of the channel region in the D2 direction. When viewed from above, the region of the oxide semiconductor layer 26 overlapping with the source electrode 32S is the source region, and the region of the oxide semiconductor layer 26 overlapping with the drain electrode 32D is the drain region. That is, the channel region is located between the source region and the drain region.

[0061] The wiring 12W and the wiring 32W function as gate wiring. The wiring 32W is electrically connected to the wiring 12W via the contact hole 15. The details will be described later. The wiring 12W is formed in the same layer as the gate electrode 12GE. In addition, the wiring 32W is formed in the same layer as the source electrode 32S and the drain electrode 32D. It should be noted that the wiring 32W is sometimes not provided on the wiring 12W.

[0062] The oxide semiconductor layer 26 is light-transmissive and has a polycrystalline structure including a plurality of crystal grains. The details will be described later. By using the Poly-OS (Poly-crystalline Oxide Semiconductor: polycrystalline silicon oxide semiconductor) technology, the oxide semiconductor layer 26 having a polycrystalline structure can be formed. Therefore, the oxide semiconductor contained in the oxide semiconductor layer 26 is sometimes described as Poly-OS below.

[0063] Poly-OS contains two or more metal elements including indium (i.e., indium and at least one or more metal elements other than indium), and the ratio of indium to the two or more metal elements is 50% or more. As metal elements other than indium, gallium (Ga), zinc (Zn), aluminum (Al), hafnium (Hf), yttrium (Y), zirconium (Zr) or lanthanide elements are used. As the oxide semiconductor layer 26, metal elements other than the above may also be used.

[0064] The crystal grain size of the crystal grains contained in the Poly-OS is 0.1 μm or more, preferably 0.3 μm or more, and more preferably 0.5 μm or more. The crystal grain size can be obtained by, for example, SEM observation, TEM observation, or electron backscattered diffraction (EBSD) of the oxide semiconductor layer 26 .

[0065] As described above, since the crystal grain size of the crystal grains included in the Poly-OS is 0.1 μm or more, in the oxide semiconductor layer 26 having a film thickness of 10 nm to 30 nm, there is a region including only one crystal grain along the film thickness direction.

[0066] Poly-OS has excellent etching resistance. The details will be described later, but Poly-OS has excellent etching resistance relative to the etching solution used in the formation of the source electrode 32S and the drain electrode 32D. Specifically, in the formation of the source electrode 32S and the drain electrode 32D, the oxide semiconductor layer 26 is hardly etched by the etching solution. Therefore, the film thickness of the first region (i.e., the source region or the drain region) of the oxide semiconductor layer 26 overlapping with one of the source electrode 32S and the drain electrode 32D is substantially the same as the film thickness of the second region (i.e., the channel region) of the oxide semiconductor layer 26 that does not overlap with the source electrode 32S and the drain electrode 32D. In other words, the difference between the film thickness of the first region and the film thickness of the second region is less than 1.0 nm, preferably less than 0.5 nm, and more preferably less than 0.2 nm.

[0067] The deviation in the shape of the oxide semiconductor layer may become the main reason for the instability of the electrical characteristics of the semiconductor device. In particular, the deviation in the film thickness of the channel region of the oxide semiconductor layer is significantly manifested in the form of the deviation in the electrical characteristics of the semiconductor device. For example, if the film thickness of the channel region is smaller than the set value, the current flowing between the source electrode and the drain electrode is reduced. Therefore, the on-current of the semiconductor device is reduced, and thus the field effect mobility is reduced. In addition, if the oxide semiconductor layer is etched during the formation of the source electrode and the drain electrode, not only the film thickness of the channel region is reduced, but also a recess is formed on the upper surface of the oxide semiconductor layer between the source electrode and the drain electrode. The interlayer insulating layer is formed in a manner that covers the recess formed on the upper surface of the oxide semiconductor layer, but if the interlayer insulating layer cannot fully cover the recess, a gap is formed between the oxide semiconductor layer and the interlayer insulating layer, or between the source electrode and the drain electrode and the interlayer insulating layer. In a semiconductor device in such a state, stable electrical characteristics cannot be obtained. That is, the yield of the semiconductor device is reduced due to the deviation in the shape of the oxide semiconductor layer.

[0068] In contrast, in the semiconductor device 10, the oxide semiconductor layer 26 includes Poly-OS and has high etching resistance. Therefore, in the formation of the source electrode 32S and the drain electrode 32D, the film thickness of the channel region is hardly reduced, and thus no recess is formed on the upper surface of the oxide semiconductor layer 26. Therefore, in the semiconductor device 10, the shape deviation of the oxide semiconductor layer 26 is small, and stable electrical characteristics can be obtained. For example, in the semiconductor device 10, even when the gate insulating layers 14 and 16 are formed with a film thickness of more than 400 nm to improve the withstand voltage, the field effect mobility has a small deviation, and a 15 cm 2 / Vs or more, and further 20cm 2 / Vs or above field effect mobility (field effect mobility in the linear region).

[0069] [Method of Manufacturing Semiconductor Device 10]

[0070] Reference Figure 3 to Figure 11 A method for manufacturing the semiconductor device 10 according to one embodiment of the present invention will be described. Figure 3 1 is a flowchart illustrating a method for manufacturing the semiconductor device 10 according to one embodiment of the present invention. Figures 4 to 11 1 is a schematic cross-sectional view showing a method for manufacturing a semiconductor device 10 according to an embodiment of the present invention. Figure 3 The steps of the flowchart shown.

[0071] exist Figure 3 In step S1001 (“GE formation”), a gate electrode 12GE is formed on the substrate 11 (see Figure 4 ).

[0072] As the substrate 11, a glass substrate, a quartz substrate, a sapphire substrate, or other light-transmitting rigid substrate is used. When the substrate 11 needs to be flexible, a polyimide substrate, an acrylic substrate, a siloxane-based substrate, a fluororesin substrate, or a substrate containing resin is used as the substrate 11. When a substrate containing resin is used as the substrate 11, in order to improve the heat resistance of the substrate 11, impurity elements may be introduced into the above-mentioned resin. In addition, when the semiconductor device 10 is used in an integrated circuit, as the substrate 11, a semiconductor substrate such as a silicon substrate, a silicon carbide substrate, a compound semiconductor substrate, or a conductive substrate such as a stainless steel substrate, which is not light-transmitting, may be used.

[0073] The gate electrode 12GE is formed by processing a conductive film formed by a sputtering method. As the gate electrode 12GE, a metal material can be used. For example, as the metal material of the gate electrode 12GE, aluminum (Al), titanium (Ti), chromium (Cr), cobalt (Co), nickel (Ni), molybdenum (Mo), hafnium (Hf), tantalum (Ta), tungsten (W), bismuth (Bi), silver (Ag), copper (Cu), and alloys thereof or compounds thereof can be used. As the gate electrode 12GE, the above metal materials can be used in a single layer or in a stacked manner.

[0074] exist Figure 3 In step S1002 (“GI formation”), gate insulating layers 14 and 16 are formed on the gate electrode 12GE (see Figure 4 The gate insulating layers 14 and 16 are formed by CVD (Chemical Vapor Deposition) or sputtering. As the gate insulating layers 14 and 16, an insulating material can be used. For example, silicon oxide (SiO x ), silicon oxynitride (SiO x N y ), Silicon Nitride (SiN x ), silicon oxynitride (SiN x O y ) and other inorganic insulating materials. x N y It is a silicon compound containing nitrogen (N) at a ratio (x>y) less than oxygen (O). SiN x O y It is a silicon compound containing oxygen at a ratio smaller than nitrogen (x>y).

[0075] It is preferred that a gate insulating layer 14 using an insulating material containing nitrogen and a gate insulating layer 16 using an insulating material containing oxygen are sequentially formed on the substrate 11. By using an insulating material containing nitrogen as the gate insulating layer 14, impurities diffusing from the substrate 11 to the oxide semiconductor layer 26 can be blocked. In addition, by using an insulating material containing oxygen as the gate insulating layer 16, oxygen can be released by heat treatment. The temperature of the heat treatment for releasing oxygen from the insulating material containing oxygen is, for example, below 500° C., below 450° C., or below 400° C. It should be noted that the insulating material containing oxygen can also release oxygen when heated in any step of the manufacturing process of the semiconductor device 10.

[0076] The film thickness of the gate insulating layer 14 is preferably greater than the film thickness of the gate insulating layer 16. For example, the film thickness of the gate insulating layer 14 is greater than 200 nm, greater than 300 nm, or greater than 400 nm. In addition, for example, the film thickness of the gate insulating layer 16 is greater than 50 nm, greater than 100 nm, or greater than 150 nm. The film thickness of the gate insulating layers 14 and 16 (that is, the total film thickness of the gate insulating layer 14 and the gate insulating layer 16) is preferably greater than 300 nm, but the film thickness of the gate insulating layers 14 and 16 is not limited thereto.

[0077] exist Figure 3 In step S1004 (“OS film formation”), an oxide semiconductor film 22 is formed on the gate insulating layers 14 and 16 (see Figure 5 The oxide semiconductor film 22 is formed by sputtering or atomic layer deposition (ALD). The oxide semiconductor film 22 has a film thickness of 10 nm to 50 nm, preferably 10 nm to 40 nm, and more preferably 10 nm to 30 nm.

[0078] As the oxide semiconductor film 22, a metal oxide having semiconductor properties can be used. For example, as the oxide semiconductor film 22, an oxide semiconductor containing two or more metal elements including indium (In) (that is, indium and at least one or more metal elements other than indium) can be used. In addition, the ratio of indium to the two or more metal elements is 50% or more. As metal elements other than indium, gallium (Ga), zinc (Zn), aluminum (Al), hafnium (Hf), yttrium (Y), zirconium (Zr) or lanthanide elements are used. As the oxide semiconductor film 22, it is preferred to contain a Group 13 element. It should be noted that, as the oxide semiconductor film 22, other metal elements other than the above may also be used.

[0079] When the oxide semiconductor film 22 is crystallized by OS annealing described later, the oxide semiconductor film 22 after film formation and before OS annealing preferably has an amorphous structure (for example, a structure with a small amount of crystalline components of the oxide semiconductor that is determined to be amorphous by the XRD method). That is, the oxide semiconductor film 22 is preferably formed under conditions that prevent the oxide semiconductor film 22 from being crystallized as much as possible immediately after film formation. For example, when the oxide semiconductor film 22 is formed by sputtering, the oxide semiconductor film 22 is formed while controlling the temperature of the object to be formed (the substrate 11 and the structure formed thereon).

[0080] If a film is formed on a film-forming object by sputtering, the ions generated in the plasma and the atoms recoiled by the sputtering target collide with the film-forming object, so the temperature of the film-forming object rises as the film-forming process is performed. If the temperature of the film-forming object rises during the film-forming process, the oxide semiconductor film 22 contains microcrystals in the state just after the film is formed. If the oxide semiconductor film 22 contains microcrystals, the crystal grain size cannot be increased by the subsequent OS annealing. In order to control the temperature of the film-forming object, for example, the film can be formed while the film is cooled. For example, the film-forming object can be cooled from the surface opposite to the film-forming surface in a manner such that the temperature of the film-forming surface of the film-forming object (hereinafter referred to as "film-forming temperature") is below 100°C, below 70°C, below 50°C, or below 30°C. In particular, the film-forming temperature of the oxide semiconductor film 22 is preferably below 50°C. By forming the oxide semiconductor film 22 while cooling the substrate 11, an oxide semiconductor film 22 with a small crystalline component can be obtained just after the film is formed.

[0081] In the sputtering process, an oxide semiconductor film 22 having an amorphous structure is formed under a condition where the oxygen partial pressure is less than 10%. If the oxygen partial pressure is high, microcrystals are included in the oxide semiconductor film 22 just after the film is formed due to the excess oxygen contained in the oxide semiconductor film 22. Therefore, it is preferred to form the oxide semiconductor film 22 under conditions where the oxygen partial pressure is low. The oxygen partial pressure is, for example, greater than 1% and less than 5%, preferably greater than 2% and less than 4%. Under conditions where the oxygen partial pressure is less than 1%, the distribution of oxygen in the film forming device tends to become uneven. As a result, the composition of oxygen in the oxide semiconductor film also becomes uneven, forming an oxide semiconductor film containing a large number of microcrystals, or forming an oxide semiconductor film that does not crystallize even after an OS annealing treatment is performed.

[0082] exist Figure 3 In step S1005 (“OS pattern formation”), a pattern of the oxide semiconductor layer 24 is formed (see Figure 6 ). The pattern of the oxide semiconductor layer 24 is formed using photolithography. For example, a resist mask (not shown) is formed on the oxide semiconductor film 22, and the oxide semiconductor film 22 is etched using the resist mask. As the etching of the oxide semiconductor film 22, wet etching or dry etching can be used. In wet etching, an acidic etching solution can be used. As the etching solution, for example, oxalic acid, PAN, sulfuric acid, hydrogen peroxide or hydrofluoric acid can be used. By etching, an oxide semiconductor layer 24 having a predetermined pattern can be formed. Then, the resist mask is removed.

[0083] The formation of the oxide semiconductor layer 24 having a predetermined pattern (i.e., patterning of the oxide semiconductor film 22) is preferably performed before OS annealing. The etching resistance of the Poly-OS after OS annealing is high, and it is difficult to perform patterning by etching. In addition, by performing OS annealing after forming the oxide semiconductor layer 24, damage generated during the formation of the oxide semiconductor layer 24 (e.g., oxygen defects in the oxide semiconductor layer 24, etc.) can be repaired.

[0084] exist Figure 3 In step S1006 (“OS annealing”), after the oxide semiconductor layer 24 is formed, the oxide semiconductor layer 24 is subjected to heat treatment (OS annealing), thereby forming the oxide semiconductor layer 26 (see Figure 7 ). In the OS annealing, the oxide semiconductor layer 24 is maintained at a predetermined reaching temperature for a predetermined time. The predetermined reaching temperature is 300° C. to 500° C., preferably 350° C. to 450° C. In addition, the holding time at the reaching temperature is 15 minutes to 120 minutes, preferably 30 minutes to 60 minutes. By performing the OS annealing, the oxide semiconductor layer 24 having an amorphous structure is crystallized to form an oxide semiconductor layer 26 having a polycrystalline structure. That is, the oxide semiconductor layer 26 including Poly-OS is formed by the OS annealing.

[0085] exist Figure 3 In step S1008 (“contact hole formation”), contact holes are formed in the gate insulating layers 14 and 16 (see Figure 8 ). Thus, the upper surface of the wiring 12W is exposed. It should be noted that when it is not necessary to connect the wiring 32W to the wiring 12W, the process of step S1008 may not be performed.

[0086] exist Figure 3 In step S1009 ("forming SD"), the source electrode 32S, the drain electrode 32D and the wiring 32W (see Fig. 9 ) The source electrode 32S, the drain electrode 32D, and the wiring 32W are formed by patterning a conductive film formed by sputtering using wet etching.

[0087] As the source electrode 32S and the drain electrode 32D, the same metal material as the gate electrode 12GE is used. That is, as the metal material of the conductive film for patterning, aluminum (Al), titanium (Ti), chromium (Cr), cobalt (Co), nickel (Ni), molybdenum (Mo), hafnium (Hf), tantalum (Ta), tungsten (W), bismuth (Bi), silver (Ag), copper (Cu), and their alloys or their compounds can be used. As a conductive film, the above-mentioned metal materials can be used in a single layer or in a stacked manner. In the case where the metal material is used in a single layer, for example, the conductive film has a single layer structure of MoW alloy, Ti or Cu. In addition, in the case of using a metal material in a stacked manner, for example, the conductive film has a stacked structure of Ti, Al and Ti (Ti / Al / Ti structure), a stacked structure of Cu and Ti (Cu / Ti structure), or a stacked structure of Ti, Cu and Ti (Ti / Cu / Ti structure). The source electrode 32S and the drain electrode 32D also have the same structure as the conductive film. In addition, the wiring 32W is formed simultaneously with the formation of the source electrode 32S and the drain electrode 32D. It should be noted that, in order to reduce the resistance of the wiring 32W, the conductive film preferably includes a low-resistance metal material such as Al or Cu. In addition, when the conductive film includes a metal material such as Cu, it is preferred to provide a barrier metal film including Ti, Mo, or MoW alloy between the oxide semiconductor layer 26 and the metal film including Cu.

[0088] Here, the formation of the source electrode 32S and the drain electrode 32D having a stacked structure is described by taking the Cu / Ti structure as an example. Ti is formed on the oxide semiconductor layer 26 as a first metal film in contact with the oxide semiconductor layer 26, and then Cu is formed on the first metal film as a second metal film. Next, a predetermined resist pattern is formed on the second metal film, and the second metal film and the first metal film are wet-etched using the resist pattern as a mask. Thus, a second metal layer containing Ti and a first metal layer containing Cu are formed by the second metal film and the first metal film, respectively.

[0089] In forming the source electrode 32S and the drain electrode 32D, a hydrogen peroxide-based etchant is used as an etchant for wet etching. The hydrogen peroxide-based etchant contains a chelating agent such as ethylenediaminetetraacetic acid (EDTA) or phosphoric acid.

[0090] Poly-OS has excellent etching resistance. Specifically, the etching rate of the etching solution used in the formation of the source electrode 32S and the drain electrode 32D is very small. This means that Poly-OS is hardly etched by the etching solution. In other words, in the semiconductor device 10, even if a conductive film is directly formed on the oxide semiconductor layer 26 and the conductive film is patterned to form the source electrode 32S and the drain electrode 32D, the channel region of the oxide semiconductor layer 26 is hardly etched. Therefore, the film thickness of the first region (i.e., the source region or the drain region) of the oxide semiconductor layer 26 overlapping with one of the source electrode 32S and the drain electrode 32D is substantially the same as the film thickness of the second region (i.e., the channel region) of the oxide semiconductor layer 26 that does not overlap with the source electrode 32S and the drain electrode 32D. In other words, the film thickness of the oxide semiconductor layer 26 can be controlled in such a way that the difference between the film thickness of the first region and the film thickness of the second region is less than 1.0 nm, preferably less than 0.5 nm, and more preferably less than 0.2 nm.

[0091] For example, the etching rate of the oxide semiconductor layer 26 with respect to the etching solution (liquid temperature: 30° C.) used in forming the source electrode 32S and the drain electrode 32D is less than 0.01 nm / sec, or less than 0.20 nm / min. That is, even if the etching time is 60 seconds, the film thickness of the oxide semiconductor layer 26 is reduced by less than 0.20 nm.

[0092] In a semiconductor device including an oxide semiconductor layer that does not have a polycrystalline structure such as IGZO, when a conductive film directly formed on the oxide semiconductor layer is patterned to form a source electrode and a drain electrode, the oxide semiconductor layer will also be etched due to wet etching in the patterning of the conductive film. Therefore, in the case of manufacturing a semiconductor device in which the film thickness of the channel region of the oxide semiconductor layer is less than 40nm, it is necessary to pre-form an oxide semiconductor film with a film thickness of about 90nm, and in the formation of the source electrode and the drain electrode, adjust the etching time so that the film thickness of the channel region becomes less than 40nm. However, when the etching rate is high, it is difficult to precisely control the film thickness of the channel region by the etching time. In this case, the deviation of the film thickness of the channel region becomes larger.

[0093] In addition, if the film thickness of the channel region is greatly reduced, a recess is formed on the upper surface of the oxide semiconductor layer. The interlayer insulating layer is formed in a manner that covers the recess formed on the upper surface of the oxide semiconductor layer, but if the depth of the recess is large, the interlayer insulating layer cannot fully cover the recess. That is, sometimes a gap is generated between the oxide semiconductor layer and the interlayer insulating layer, or between the source electrode and the drain electrode and the interlayer insulating layer. This will not only make the electrical characteristics of the semiconductor device unstable, but also become the main reason for reducing the reliability of the semiconductor device.

[0094] On the other hand, the oxide semiconductor layer 26 contains Poly-OS and has high etching resistance. Therefore, there is no need to consider the reduction in the film thickness of the oxide semiconductor film 22 caused by the etching solution used in the formation of the source electrode 32S and the drain electrode 32D, and the film thickness of the channel region of the oxide semiconductor layer 26 can be controlled only by the film formation of the oxide semiconductor film 22. Therefore, the oxide semiconductor film 22 can be formed with a film thickness of 10 nm to 50 nm, preferably 10 nm to 40 nm, and more preferably 10 nm to 30 nm. In addition, since the oxide semiconductor layer 26 has high etching resistance, the selectivity of the metal material that can be used as the source electrode 32S, the drain electrode 32D, and the wiring 32W is improved.

[0095] The oxide semiconductor layer 26 has excellent etching resistance, and therefore, the etching rate of the conductive film in the formation of the source electrode 32S and the drain electrode 32D can be increased. For example, the etching rate of the first metal film in contact with the oxide semiconductor layer 26 is 0.1 nm / sec or more, preferably 0.5 nm / sec or more, and more preferably 0.9 nm / sec or more. In addition, when the second metal film formed on the first metal film includes Cu, the etching rate of the second metal film is 1.0 nm / sec or more, preferably 2.0 nm / sec or more, and more preferably 3.0 nm / sec or more.

[0096] It should be noted that, in the formation of the source electrode 32S and the drain electrode 32D, the oxide semiconductor layer 26 is hardly etched, but depending on the type of etching solution, the gate insulating layer 16 is sometimes etched. For example, in order not to leave an unnecessary conductive film, over-etching is performed instead of appropriate etching. In this case, the gate insulating layer 16 exposed from the conductive film is etched. In the gate insulating layer 16, the difference between the film thickness of the region overlapping with the oxide semiconductor layer 26 and the film thickness of the region not overlapping with the oxide semiconductor layer 26 is 5 nm or more, 10 nm or more, or 15 nm or more. In addition, in order to prevent the film thickness of the gate insulating layer 16 from becoming too small and to control the over-etching time, in the gate insulating layer 16, the difference between the film thickness of the region overlapping with the oxide semiconductor layer 26 and the film thickness of the region not overlapping with the oxide semiconductor layer 26 is 50 nm or less, preferably 30 nm or less, and more preferably 20 nm or less.

[0097] exist Figure 3 In step S1010 ("SiOx formation"), an interlayer insulating layer 34 is formed on the oxide semiconductor layer 26, the source electrode 32S, and the drain electrode 32D. As the interlayer insulating layer 34, an insulating material containing oxygen is preferably used. For example, silicon oxide (SiO x ) or silicon oxynitride (SiO x Ny ) etc. In addition, as the interlayer insulating layer 34, it is preferable to use an insulating film with few defects. For example, when the oxygen composition ratio in the interlayer insulating layer 34 is compared with the oxygen composition ratio in an insulating film (hereinafter referred to as "other insulating film") having the same composition as the interlayer insulating layer 34, the oxygen composition ratio in the interlayer insulating layer 34 is closer to the stoichiometric ratio for the insulating film than the oxygen composition ratio in the other insulating film. For example, silicon oxide (SiO x ), the interlayer insulating layer 34 has a composition ratio closer to the stoichiometric ratio of silicon oxide (SiO 2 ) than the gate insulating layer 14. As the interlayer insulating layer 34, a layer in which no defects are observed when evaluated by an electron spin resonance method (ESR) may be used.

[0098] The interlayer insulating layer 34 can be formed using the same film forming method as the gate insulating layers 14 and 16. In order to increase the oxygen composition ratio in the interlayer insulating layer 34, the film can be formed at a relatively low temperature (for example, a film forming temperature of less than 350° C.). In addition, in order to form an insulating film with few defects as the interlayer insulating layer 34, the interlayer insulating layer 34 can also be formed at a film forming temperature of 350° C. or more. In addition, after the interlayer insulating layer 34 is formed, a process of injecting oxygen into a part of the interlayer insulating layer 34 can be performed.

[0099] The film thickness of the interlayer insulating layer 34 is not less than 50 nm and not more than 300 nm, not less than 60 nm and not more than 200 nm, or not less than 70 nm and not more than 150 nm.

[0100] exist Figure 3 In step S1011 (“MO film formation”), a metal oxide film 36 is formed on the interlayer insulating layer 34 (see Fig.10 ). The metal oxide film 36 is formed by a sputtering method or an atomic layer deposition method (ALD: Atomic Layer Deposition).

[0101] As the metal oxide film 36, a metal oxide film containing aluminum as a main component is used. For example, aluminum oxide (AlO x ), aluminum oxynitride (AlO x N y ), aluminum oxynitride (AlN x O y ), aluminum nitride (AlN x) and other inorganic insulating films. A metal oxide film with aluminum as the main component means that the ratio of aluminum contained in the metal oxide film is 1% or more of the entire metal oxide film. The ratio of aluminum contained in the metal oxide film 36 may be 5% or more and 70% or more, 10% or more and 60% or more, or 30% or more and 50% or less of the entire metal oxide film 36. The above ratios may be mass ratios or weight ratios.

[0102] The thickness of the metal oxide film 36 is not less than 1 nm and not more than 50 nm, preferably not less than 1 nm and not more than 30 nm. As the metal oxide film 36, aluminum oxide is preferably used. Aluminum oxide has a high barrier property to gases such as oxygen or hydrogen. Here, the barrier property refers to the function of inhibiting the permeation of gases such as oxygen or hydrogen through aluminum oxide. That is, this means that gases such as oxygen or hydrogen in the layer below the aluminum oxide film are not allowed to move to the layer above the aluminum oxide film. Alternatively, gases such as oxygen or hydrogen in the layer above the aluminum oxide film are not allowed to move to the layer below the aluminum oxide film.

[0103] exist Figure 3 In step S1012 (“oxidation annealing”), a heat treatment is performed on the oxide semiconductor layer 26 while the interlayer insulating layer 34 and the metal oxide film 36 are formed (see Fig.10 Here, the oxidation annealing can be performed at a temperature of, for example, 350° C. to 450° C. Thus, oxygen released from the interlayer insulating layer 34 is supplied to the oxide semiconductor layer 26. By providing the metal oxide film 36 so as to cover the substrate 11, it is possible to suppress the oxygen released from the interlayer insulating layer 34 from being released to the outside of the metal oxide film 36.

[0104] In the process from forming the oxide semiconductor layer 26 to forming the interlayer insulating layer 34 on the oxide semiconductor layer 26, a large number of oxygen defects are generated in the oxide semiconductor layer 26. However, by the oxidation annealing in step S1012, oxygen released from the interlayer insulating layer 34 is supplied to the oxide semiconductor layer 26, and the oxygen defects are repaired.

[0105] exist Figure 3 In step S1013 ("MO removal"), the metal oxide film 36 (see Fig.11 ). For example, the metal oxide film 36 may be removed using diluted hydrofluoric acid (DHF).

[0106] exist Figure 3 In step S1014 ("SiNx film formation"), an interlayer insulating layer 38 is formed on the interlayer insulating layer 34. As the interlayer insulating layer 38, an insulating material containing nitrogen is preferably used. For example, silicon nitride (SiN x ) or silicon oxynitride (SiN x Oy ) etc. The interlayer insulating layer 38 can be formed by using the same film forming method as that of the gate insulating layers 14 and 16 .

[0107] Through the above steps, it is possible to produce Figure 1 A semiconductor device 10 is shown.

[0108] As described above, in the manufacturing process of the semiconductor device 10, by forming the oxide semiconductor layer 26 containing Poly-OS having high etching resistance, the shape deviation of the oxide semiconductor layer 26 is suppressed. In particular, it is possible to reduce the deviation of the film thickness of the channel region of the oxide semiconductor layer 26. As a result, the semiconductor device 10 has stable electrical characteristics, and the yield of the semiconductor device 10 is improved.

[0109] <Second embodiment>

[0110] Reference Figure 12 to Figure 15 A display device 20 using the semiconductor device 10 according to one embodiment of the present invention will be described. In the following embodiment, a circuit configuration in which the semiconductor device 10 described in the first embodiment is applied to a liquid crystal display device will be described.

[0111] [Overview of Display Device 20]

[0112] Fig.12 1 is a schematic top view showing an overview of a display device 20 according to an embodiment of the present invention. Fig.12 As shown, the display device 20 includes an array substrate 300, a sealing portion 310, an opposing substrate 320, a flexible printed circuit substrate 330 (FPC 330), and an IC chip 340. The array substrate 300 and the opposing substrate 320 are bonded together by the sealing portion 310. A plurality of pixel circuits 301 are arranged in a matrix in a liquid crystal region 220 surrounded by the sealing portion 310. The liquid crystal region 220 is a region that overlaps with a liquid crystal element 311 described later when viewed from above.

[0113] The sealing region 240 provided with the sealing portion 310 is a region around the liquid crystal region 220. The FPC 330 is provided in the terminal region 260. The terminal region 260 is a region where the array substrate 300 is exposed from the counter substrate 320 and is provided outside the sealing region 240. The outside of the sealing region 240 refers to the region provided with the sealing portion 310 and the outside of the region surrounded by the sealing portion 310. The IC chip 340 is provided on the FPC 330. The IC chip 340 supplies a signal for driving each pixel circuit 301.

[0114] [Circuit Configuration of Display Device 20]

[0115] Fig.131 is a block diagram showing a circuit configuration of a display device 20 according to an embodiment of the present invention. Fig.13 As shown, a source driving circuit 302 is provided at a position adjacent to the liquid crystal region 220 in the second direction D2 (column direction) with respect to the pixel circuit 301, and a gate driving circuit 303 is provided at a position adjacent to the liquid crystal region 220 in the first direction D1 (row direction). The source driving circuit 302 and the gate driving circuit 303 are provided in the above-mentioned sealing region 240. However, the region where the source driving circuit 302 and the gate driving circuit 303 are provided is not limited to the sealing region 240, and may be any region as long as it is outside the region where the pixel circuit 301 is provided.

[0116] The source wiring 304 extends from the source driver circuit 302 in the second direction D2 and is connected to the plurality of pixel circuits 301 arranged in the second direction D2. The gate electrode 12GE extends from the gate driver circuit 303 in the first direction D1 and is connected to the plurality of pixel circuits 301 arranged in the first direction D1.

[0117] The terminal region 260 is provided with a terminal portion 306. The terminal portion 306 is connected to the source driver circuit 302 via a connection wiring 307. Similarly, the terminal portion 306 is connected to the gate driver circuit 303 via a connection wiring 307. The FPC 330 is connected to the terminal portion 306, so that an external device connected to the FPC 330 is connected to the display device 20, and each pixel circuit 301 provided in the display device 20 is driven by a signal from the external device.

[0118] The semiconductor device 10 described in the first embodiment is used as a transistor included in the pixel circuit 301 , the source driver circuit 302 , and the gate driver circuit 303 .

[0119] [Pixel Circuit 301 of Display Device 20]

[0120] Fig.14 is a circuit diagram showing a pixel circuit 301 of a display device 20 according to an embodiment of the present invention. Fig.14 As shown, the pixel circuit 301 includes components such as the semiconductor device 10, the storage capacitor 350, and the liquid crystal element 311. The semiconductor device 10 has a gate electrode 12GE, an oxide semiconductor layer 26, a source electrode 32S, and a drain electrode 32D. The gate electrode 12GE is connected to the gate wiring 305. The source electrode 32S is connected to the source wiring 304. The drain electrode 32D is connected to the storage capacitor 350 and the liquid crystal element 311.

[0121] [Configuration of Display Device 20]

[0122] Fig.15It is a schematic cross-sectional view of a display device 20 according to one embodiment of the present invention. Fig.15 The display device 20 shown uses the semiconductor device 10 .

[0123] like Fig.15 As shown, a gate electrode 12GE is provided on the substrate 11. Gate insulating layers 14 and 16 are provided on the gate electrode 12GE. An oxide semiconductor layer 26 is provided on the gate insulating layers 14 and 16. A source electrode 32S and a drain electrode 32D are provided on the oxide semiconductor layer 26.

[0124] Interlayer insulating layers 34 and 38 are provided on the source electrode 32S and the drain electrode 32D. An insulating layer 39 is provided on the interlayer insulating layers 34 and 38. The insulating layer 39 is provided to alleviate the unevenness caused by the semiconductor device 10. In the interlayer insulating layers 34, 38 and the insulating layer 39, a contact hole is formed in a manner to expose the upper surface of the source electrode 32S. A common electrode 42C provided in a manner shared by a plurality of pixels is provided on the insulating layer 39. An insulating layer 44 is provided on the common electrode 42C. An insulating layer 44 is provided inside the contact hole. By forming the insulating layer 44 using a silicon nitride film, it is possible to suppress the intrusion of moisture from the contact hole through the insulating layer 44. A pixel electrode 46P is provided on the insulating layer 44 and inside the contact hole. The pixel electrode 46P is connected to the drain electrode 32D.

[0125] In addition, wiring 12C is provided on substrate 11, and is connected to wiring 32C via contact holes provided in gate insulating layers 14 and 16. Wiring 12C and wiring 32C function as capacitor wiring. In addition, electrode 46C is provided on insulating layer 39 and inside the opening. A holding capacitor 350 is formed by common electrode 42C, insulating layer 44 and electrode 46C.

[0126] In this embodiment, the semiconductor device 10 is used in a configuration of the pixel circuit 301 , but the semiconductor device 10 may be used in a peripheral circuit including a source driver circuit 302 and a gate driver circuit 303 .

[0127] <Third embodiment>

[0128] Reference Fig.16 and Fig.17 A display device 20 using the semiconductor device 10 according to one embodiment of the present invention will be described. In this embodiment, the semiconductor device 10 described in the first embodiment is applied to a circuit structure of an organic EL display device. The overview and circuit structure of the display device 20 are similar to those of the semiconductor device 10 described in the first embodiment. Fig.12 and Fig.13 The situations shown are the same, so the description is omitted.

[0129] [Pixel Circuit 301 of Display Device 20]

[0130] Fig.16 1 is a circuit diagram showing a pixel circuit of a display device 20 according to an embodiment of the present invention. Fig.16 As shown, the pixel circuit 301 includes components such as a driving transistor 110, a selection transistor 120, a holding capacitor 210, and a light-emitting element DO. The driving transistor 110 and the selection transistor 120 have the same structure as the semiconductor device 10. The source electrode of the selection transistor 120 is connected to the signal line 211, and the gate electrode of the selection transistor 120 is connected to the gate line 212. The source electrode of the driving transistor 110 is connected to the anode power line 213, and the drain electrode of the driving transistor 110 is connected to one end of the light-emitting element DO. The other end of the light-emitting element DO is connected to the cathode power line 214. The gate electrode of the driving transistor 110 is connected to the drain electrode of the selection transistor 120. The holding capacitor 210 is connected to the gate electrode and the drain electrode of the driving transistor 110. A grayscale signal for determining the light intensity of the light-emitting element DO is supplied to the signal line 211. A signal for selecting a pixel row in which the grayscale signal is written is supplied to the gate line 212.

[0131] [Cross-sectional structure of display device 20]

[0132] Fig.17 It is a schematic cross-sectional view showing the structure of a display device 20 according to one embodiment of the present invention. Fig.17 The display device 20 shown in FIG. Fig.15 The display device 20 shown is similar, but Fig.17 The structure of the display device 20 shown above the insulating layer 39 is different from Fig.15 The structure of the display device 20 shown above the insulating layer 39 is different. Fig.17 The display device 20 shown in FIG. Fig.15 Description of the same configurations of the display device 20 will be omitted, and differences between the two will be described.

[0133] like Fig.17As shown, the display device 20 has a pixel electrode 390, a light-emitting layer 392 and a common electrode 394 (light-emitting element DO) above the insulating layer 39. The pixel electrode 390 is arranged on the insulating layer 39 and inside the contact hole formed in the interlayer insulating layers 34, 38 and the insulating layer 39. An insulating layer 362 is arranged on the pixel electrode 390. An opening 363 is arranged in the insulating layer 362. The opening 363 corresponds to the light-emitting area. That is, the insulating layer 362 defines the pixel. The light-emitting layer 392 and the common electrode 394 are arranged on the pixel electrode 390 exposed by the opening 363. The pixel electrode 390 and the light-emitting layer 392 are respectively arranged relative to each pixel. On the other hand, the common electrode 394 is arranged in a manner shared by multiple pixels. Different materials are used for the light-emitting layer 392 according to the display color of the pixel.

[0134] In the second embodiment and the third embodiment, the semiconductor device 10 described in the first embodiment is applied to a liquid crystal display device and an organic EL display device, but the semiconductor device 10 can also be applied to display devices other than these display devices (for example, self-luminous display devices or electronic paper display devices other than organic EL display devices). In addition, the semiconductor device 10 can be applied to small and medium-sized display devices to large display devices without special limitations. In addition, even when a large-area substrate is used for manufacturing, the deviation of the shape of the oxide semiconductor layer 26 in the semiconductor device 10 is small. Therefore, when the semiconductor device 10 is applied to the display device 20, the display unevenness can be reduced. In addition, the yield rate when manufacturing the display device 20 can be improved.

[0135] [Example]

[0136] A semiconductor device 10 according to an embodiment of the present invention will be described in detail based on examples. However, the semiconductor device 10 is not limited to the examples described below.

[0137] [Etching rate]

[0138] The etching solution used for forming the source electrode and the drain electrode was used to calculate the poly-OS contained in the oxide semiconductor layer, MoW, Ti, Al and Cu used as the source electrode and the drain electrode, and silicon oxide (SiO x ) and silicon nitride (SiN x )'s etching rate for each material.

[0139] The samples for which the etching rate was measured are described. A single film of each material was formed on a silicon wafer to obtain a sample of each material. It should be noted that in the Poly-OS sample, an OS annealing treatment was performed after the formation of the oxide semiconductor film having an amorphous structure to form an oxide semiconductor layer having a polycrystalline structure.

[0140] As etching solutions, GHP-3 (manufactured by Kanto Chemical Co., Ltd.) containing a chelating agent and BTF-3 (manufactured by Kanto Chemical Co., Ltd.) containing phosphoric acid were used to perform wet etching (room temperature) of each material. After wet etching, the film thickness of each material was measured. In each material, wet etching was performed under conditions with different etching times, and data of multiple film thicknesses with different etching times were obtained. A standard curve was prepared based on the data of etching time and film thickness, and the etching rate of each material was calculated. The calculated etching rates of each material are shown in Table 1. It should be noted that "less than 0.01 nm / sec" in Table 1 means that the film thickness before and after wet etching is roughly the same, and is hardly etched by wet etching.

[0141] [Table 1]

[0142] GHP-3 BTF-3 Poly-OS Less than 0.01nm / sec Less than 0.01nm / sec MoW 0.14nm / sec 0.09nm / sec Ti Less than 0.01nm / sec 0.93nm / sec Al 0.01nm / sec 0.92nm / sec Cu 1.83nm / sec 3.23nm / sec <![CDATA[SiO x ]]> Less than 0.01nm / sec 0.21nm / sec <![CDATA[SiN x ]]> Less than 0.01nm / sec 0.21nm / sec

[0143] When GHP-3 is used as an etching solution, the etching rate of MoW is 0.14 nm / sec, while the etching rate of Poly-OS is less than 0.01 nm / sec. This means that when MoW is used as the conductive film of the source electrode 32S and the drain electrode 32D of the semiconductor device 10 (more specifically, the first metal film in contact with the oxide semiconductor layer 26), the oxide semiconductor layer 26 is hardly etched in the formation of the source electrode 32S and the drain electrode 32D by wet etching using GHP-3. Specifically, when the source electrode 32S and the drain electrode 32D are a MoW alloy single layer structure or a Cu / MoW structure, the oxide semiconductor layer 26 is hardly etched by GHP-3.

[0144] In addition, when BTF-3 is used as an etching solution, the etching rates of Ti and Al are 0.93 nm / sec and 0.92 nm / sec, respectively, while the etching rate of Poly-OS is less than 0.01 nm / sec. This means that when Ti is used as the conductive film of the source electrode 32S and the drain electrode 32D of the semiconductor device 10 (more specifically, the first metal film in contact with the oxide semiconductor layer 26), the oxide semiconductor layer 26 is hardly etched during the formation of the source electrode 32S and the drain electrode 32D by wet etching using BTF-3. Specifically, when the source electrode 32S and the drain electrode 32D are a Ti single layer structure, a Cu / Ti structure, or a Ti / Al / Ti structure, the oxide semiconductor layer 26 is hardly etched by BTF-3.

[0145] It should be noted that when BTF-3 is used as the etching solution, SiO x and SiN xetched. This is because BTF-3 contains hydrofluoric acid. In contrast, Poly-OS also has high etching resistance to hydrofluoric acid, so Poly-OS is hardly etched by BTF-3 containing hydrofluoric acid. Therefore, in the formation of the source electrode 32S and the drain electrode 32D by wet etching using BTF-3, there is a case where the gate insulating layer 16 is etched more than the oxide semiconductor layer 26. In this case, in the gate insulating layer 16, the film thickness of the region that does not overlap with the oxide semiconductor layer 26 is smaller than the film thickness of the region that overlaps with the oxide semiconductor layer 26.

[0146] As shown in Table 1, Poly-OS is hardly etched by GHP-3 and BTF-3. Therefore, a resist pattern is formed on each material, and each material is wet-etched (at room temperature) using the resist pattern as a mask. After wet etching, the film thickness of each material is measured. The etching rate of each material is calculated based on the etching time and the film thickness. The calculated etching rate of each material is shown in Table 2. It should be noted that "less than 0.01 nm / min" in Table 2 means that it is hardly etched by wet etching with an etching time of 5 minutes.

[0147] [Table 2]

[0148] GHP-3 BTF-3 Poly-OS 0.15nm / min Less than 0.01nm / min MoW 8.45m / min 5.22nm / min Ti 0.11nm / min 56.07nm / min Al 0.80nm / min 55.05nm / min Cu 0.15nm / min Less than 0.01nm / min <![CDATA[SiO x ]]> Less than 0.01nm / min 12.75nm / min <![CDATA[SiN x ]]> Less than 0.01nm / min 12.87nm / min

[0149] By extending the etching time, as shown in Table 2, the etching rate of Poly-OS relative to GHP-3 can be calculated. Therefore, in the formation of the source electrode 32S and the drain electrode 32D based on wet etching using BTF-3, even in the case of overetching for 1 minute, in the oxide semiconductor layer 26, the difference between the film thickness of the source region or the drain region and the film thickness of the channel region is less than 1 nm. On the other hand, the etching rate of Poly-OS relative to BTF-3 cannot be calculated. This means that Poly-OS has a very high etching resistance relative to BTF-3. Therefore, in the formation of the source electrode 32S and the drain electrode 32D based on wet etching using BTF-3, when overetching is performed for 1 minute, the oxide semiconductor layer 26 containing Poly-OS is hardly etched, and the oxide semiconductor layer 26 containing SiO x The gate insulating layer 16 is etched by about 13 nm. In other words, in the oxide semiconductor layer 26, the difference between the film thickness of the source region or the drain region and the film thickness of the channel region is less than 1 nm, and in the gate insulating layer 16, the difference between the film thickness of the region overlapping with the oxide semiconductor layer 26 and the film thickness of the region not overlapping with the oxide semiconductor layer 26 is greater than 10 nm.

[0150] [Electrical characteristics]

[0151] According to the first embodiment Figure 3The semiconductor device 10 is manufactured according to the flowchart shown in the figure, and the electrical characteristics of the semiconductor device 10 are measured. In the manufacture of the semiconductor device 10, a Ti single layer structure is used as the source electrode 32S and the drain electrode 32D. It should be noted that in the manufacture of the semiconductor device 10, no Figure 3 In order to investigate the influence of overetching in the formation of the source electrode 32S and the drain electrode 32D, the Ti single layer structure was etched appropriately with a mixed solution of ammonia and hydrogen peroxide (NH3 / H2O2 solution), and then a plurality of samples with different overetching conditions were prepared. The conditions of each sample are shown in Table 3.

[0152] [Table 3]

[0153] Overetching conditions Sample A none Sample B-1 Use GHP-3 for 30 sec Sample B-2 Use GHP-3 for 60 sec Sample C-1 Use BTF-3 for 30 seconds Sample C-2 Use BTF-3 for 60 seconds

[0154] Figures 18A to 18E This is a graph showing the electrical characteristics of each sample in the example. Figures 18A to 18E In each graph, the horizontal axis represents the gate voltage (Vg), and the vertical axis represents the drain current (Id). Fig.19 This is a graph showing the threshold value (Vth) calculated from the electrical characteristics of each sample in the example. Fig. 20 This is a graph showing the field effect mobility (field effect mobility in the linear region) calculated from the electrical characteristics of each sample in the example. Table 4 shows the measurement conditions of the electrical characteristics.

[0155] [Table 4]

[0156]

[0157] Figures 18A to 18E The graphs of electrical characteristics of the samples shown in FIG. 1 and FIG. 2 show the measurement results of nine semiconductor devices 10 in an overlapping manner. Figures 18A to 18E It can be understood that the deviation of the electrical characteristics is small in any of the samples. Fig.19 and Fig. 20 As shown, the variation in threshold and field effect mobility is small in all samples. This is considered to be because the oxide semiconductor layer 26 is not etched when the source electrode 32S and the drain electrode 32D are formed, and the variation in the shape of the oxide semiconductor layer 26 is suppressed, thereby stabilizing the electrical characteristics.

[0158] exist Fig.19 The average value of the threshold value in each sample is also shown in FIG. Fig.19 It can be understood that the average values ​​of the threshold values ​​of the samples are all positive values, which indicates that the semiconductor device 10 is an enhancement type. Fig. 20 The average field effect mobility of each sample is also shown. Fig. 20 It can be understood that the average field effect mobility of the samples exceeds 25 cm 2 / Vs, indicating that the semiconductor device 10 has a 20cm 2 / Field effect mobility above Vs.

[0159] In sample B-1 and sample B-2, the over-etching time in the wet etching using GHP-3 is different, but the influence of the over-etching time is not observed. In addition, in sample C-1 and sample C-2, the over-etching time in the wet etching using BTF-3 is different, but the influence of the over-etching is not observed. In addition, the etching solution in the wet etching of samples B-1, B-2 and samples C-1, C-2 is different, but the influence of the difference in etching solution is not observed. The oxide semiconductor layer 26 including Poly-OS has excellent etching resistance, and in the manufacture of the semiconductor device 10 using the oxide semiconductor layer 26, the process margin can be expanded. As a result, in the manufacture of the semiconductor device 10, the yield is improved.

[0160] As embodiments of the present invention, the above-mentioned embodiments and variations can be appropriately combined for implementation as long as they do not contradict each other. In addition, solutions obtained by those skilled in the art by appropriately adding, deleting or changing the design of components based on the semiconductor devices and display devices of the embodiments and variations, or solutions obtained by adding, omitting or changing the conditions of processes as long as they have the gist of the present invention are included in the scope of the present invention.

[0161] Even if there are other effects different from the effects brought about by the above-mentioned embodiments, it can be understood that the effects that are clear from the description of this specification or the effects that can be easily predicted by those skilled in the art are brought about by the present invention.

Claims

1. A semiconductor device comprising: a gate electrode; a gate insulating layer on the gate electrode; an oxide semiconductor layer having a polycrystalline structure on the gate insulating layer; a source electrode and a drain electrode on the oxide semiconductor layer; and an interlayer insulating layer covering the source electrode and the drain electrode and contacting the oxide semiconductor layer, The oxide semiconductor layer includes a first region overlapping with one of the source electrode and the drain electrode, and a second region in contact with the interlayer insulating layer. The difference between the film thickness of the first region and the film thickness of the second region is 1 nm or less.

2. The semiconductor device according to claim 1, in, The source electrode and the drain electrode include a first metal layer, The etching rate of the first metal layer with respect to the etching solution used in forming the first metal layer is 0.1 nm / sec or more, The etching rate of the oxide semiconductor layer relative to the etching solution is less than 0.01 nm.

3. The semiconductor device according to claim 2, in, The source electrode and the drain electrode further include a second metal layer containing copper on the first metal layer, The etching rate of the second metal layer with respect to the etching solution is 0.5 nm / sec or more.

4. The semiconductor device according to claim 3, in, The first metal layer includes molybdenum.

5. The semiconductor device according to claim 3, in, The etching solution contains a chelating agent.

6. The semiconductor device according to claim 2, in, The etching rate of the first metal layer is greater than or equal to 0.5 nm / sec.

7. The semiconductor device according to claim 6, in, The source electrode and the drain electrode further include a second metal layer containing copper on the first metal layer, The etching rate of the second metal layer with respect to the etching solution is 1.0 nm / sec or more.

8. The semiconductor device according to claim 7, in, The first metal layer includes titanium.

9. The semiconductor device according to claim 7, in, The etching solution contains phosphoric acid.

10. The semiconductor device according to any one of claims 1 to 9, in, The oxide semiconductor layer contains indium and at least one metal element other than indium, The ratio of the indium to the indium and the at least one metal element is 50% or more.

11. A method for manufacturing a semiconductor device, comprising: include: Forming a gate electrode, forming a gate insulating layer on the gate electrode, forming an oxide semiconductor layer having a polycrystalline structure on the gate insulating layer, forming a source electrode and a drain electrode on the oxide semiconductor layer, forming an interlayer insulating layer covering the source electrode and the drain electrode and contacting the oxide semiconductor layer, The oxide semiconductor layer includes a first region overlapping with one of the source electrode and the drain electrode, and a second region in contact with the interlayer insulating layer. The difference between the film thickness of the first region and the film thickness of the second region is 1 nm or less.

12. The method for manufacturing a semiconductor device according to claim 11, in, The formation of the source electrode and the drain electrode includes: Forming a first metal film, forming a second metal film on the first metal film, The first metal film and the second metal film are etched using an etching solution to form a first metal layer and a second metal layer on the first metal layer. The etching rate of the first metal film relative to the etching solution is 0.1 nm / sec or more, The etching rate of the oxide semiconductor layer with respect to the etching solution is less than 0.01 nm / sec.

13. The method for manufacturing a semiconductor device according to claim 12, in, The second metal film includes copper, The etching rate of the second metal film with respect to the etching solution is 0.5 nm / sec or more.

14. The method for manufacturing a semiconductor device according to claim 13, in, The first metal film includes molybdenum.

15. The method for manufacturing a semiconductor device according to claim 13, in, The etching solution contains a chelating agent.

16. The method for manufacturing a semiconductor device according to claim 12, in, The etching rate of the first metal film is greater than or equal to 0.5 nm / sec.

17. The method for manufacturing a semiconductor device according to claim 16, in, The second metal film includes copper, The etching rate of the second metal film with respect to the etching solution is 1.0 nm / sec or more.

18. The method for manufacturing a semiconductor device according to claim 17, in, The first metal film includes titanium.

19. The method for manufacturing a semiconductor device according to claim 17, in, The etching solution contains phosphoric acid.

20. The method for manufacturing a semiconductor device according to any one of claims 11 to 19, in, The oxide semiconductor layer contains indium and at least one metal element other than indium, The ratio of the indium to the indium and the at least one metal element is 50% or more.

Citation Information

Patent Citations

  • Semiconductor device

    JP2016184771A

  • Semiconductor device and display device having semiconductor device

    JP2018006730A

  • Semiconductor device manufacturing method

    JP2021108405A

  • Manufacturing method for semiconductor device

    JP2021141338A

  • Semiconductor device

    JP2021153196A