High-response ultraviolet detector based on bismuth antimonide thin film and preparation method thereof
By using a high-response ultraviolet detector with bismuth antimonide film in photodetectors, the unutilized problem of bismuth antimonide material in ultraviolet imaging technology is solved, the effect of fast response speed and high detection rate is achieved, and the process is simplified process.
Patent Information
- Application Number
- CN202410998375.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-11-12
AI Technical Summary
In the high-response ultraviolet imaging technology of photodetectors, bismuth antimonide (BiSb) materials have not been studied and applied, resulting in technical gaps in this field.
Using a high-response ultraviolet detector based on bismuth antimonide film, the bismuth antimonide film is formed on the substrate and the driving electrode is plated. The dual-target joint sputtering method is used to cool the solid solution under an inert gas atmosphere to achieve high efficiency of the material. preparation.
It realizes an ultraviolet detector with fast response speed and high detection rate, which can cover most sun blind light areas, and is simple in process, less difficult in commercialization, and has the characteristics of small size and light weight.
Smart Images

Figure CN118943229A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of ultraviolet detectors, and in particular to a high-response ultraviolet detector based on a bismuth antimonide film and a preparation method thereof. Background Art
[0002] Ultraviolet (IR) photoelectric sensing systems can be used in forest fires, missile warning, ultraviolet imaging, confidential communications, space detection, electrical discharge detection, and criminal investigation. Solar-blind ultraviolet detectors do not require refrigeration devices and have good environmental adaptability.
[0003] Theoretical calculations show that the band gap of a single-layer bismuth antimonide (BiSb) thin film material is (~0.46 eV), and its band structure varies with the semi-metal composition, up to 4 meV. Bi and Sb have the same rhombohedral crystal structure, with lattice mismatch △a / a=5.4% and △c / c=5.1%, and all components form a continuous solid solution.
[0004] However, bismuth antimonide (BiSb) materials have not been studied in the high-response UV imaging technology of photodetectors. Summary of the invention
[0005] The embodiment of the present application provides a high-response ultraviolet detector based on bismuth antimonide film and a preparation method thereof, which proves that bismuth antimonide material can be applied to ultraviolet imaging technology, and has the advantages of fast response speed and high detection rate, and can cover most of the solar-blind light area.
[0006] In a first aspect, a high-response ultraviolet detector based on a bismuth antimonide film is provided, comprising:
[0007] substrate;
[0008] a bismuth antimonide thin film located on the substrate;
[0009] The driving electrode is located on the bismuth antimonide film.
[0010] In some embodiments, the bismuth antimonide film has a thickness of 50-100 nm.
[0011] In some embodiments, the antimony and bismuth contents in the bismuth antimonide film are 66% and 34%, respectively.
[0012] In some embodiments, the substrate is a silicon layer or a silicon layer deposited with silicon dioxide.
[0013] In some embodiments, when the substrate is a silicon layer deposited with silicon dioxide, the thickness of the silicon dioxide is 100 to 500 nm.
[0014] In some embodiments, the thickness of the substrate is 50 μm to 300 μm.
[0015] In some embodiments, the driving electrode is made of one or more of Ag, Au, C, Cu, Ti and In.
[0016] In a second aspect, a method for preparing a high-response ultraviolet detector based on a bismuth antimonide film as described above is provided, comprising:
[0017] On a substrate, antimony and bismuth targets are sputtered by dual-target co-sputtering to form a solid solution, and then cooled to room temperature in an inert gas atmosphere to obtain a bismuth antimonide film;
[0018] A driving electrode is plated on the bismuth antimonide film.
[0019] In some embodiments, the cooling rate is 5-10° C. / min.
[0020] In some embodiments, the inert gas is argon, the gas flow rate does not exceed 20 sccm, and the gas pressure is 0.5 Pa to 5 Pa;
[0021] And / or, when the dual targets are sputtered together, the temperature of the magnetron sputtering machine does not exceed 300° C., and the sputtering power is 10-100W.
[0022] The beneficial effects of the technical solution provided by this application include:
[0023] The embodiment of the present application provides a high-response ultraviolet detector based on bismuth antimonide film and a preparation method thereof, which proves that bismuth antimonide material can be applied to ultraviolet imaging technology and has the advantages of fast response speed and high detection rate, and can cover most of the solar-blind light area. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0025] Figure 1 Schematic diagram of a high-response ultraviolet detector based on bismuth antimonide film provided in an embodiment of the present application;
[0026] Figure 2 A graph showing the change of current over time of a high-response ultraviolet detector based on a bismuth antimonide film under light illumination provided in an embodiment of the present application;
[0027] Figure 3 This is a curve diagram of the change of current with voltage under light for a high-response ultraviolet detector based on bismuth antimonide film provided in an embodiment of the present application.
[0028] In the figure: 1. substrate; 2. bismuth antimonide film; 3. driving electrode. DETAILED DESCRIPTION
[0029] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.
[0030] The applicant discovered that both bismuth and antimony are semimetals, and have excellent thermal stability and high absorption coefficient of ultraviolet light. Although both bismuth and antimony are semimetals, due to the influence of energy band crossing, semiconductor rather than semimetal behavior can be observed.
[0031] Based on this, see Figure 1 As shown, an embodiment of the present application provides a high-response ultraviolet detector based on a bismuth antimonide film. The detector is a layered structure, specifically including a substrate 1, a bismuth antimonide film 2 and a driving electrode 3. The bismuth antimonide film 2 is located on the substrate 1, and the driving electrode 3 is located on the bismuth antimonide film 2.
[0032] The bandgap of bismuth antimonide film is about 0.46eV ~ 4meV, with a narrow bandgap that can be adjusted with the composition, which can cover most of the solar-blind light area. Sb and Bi are elements in adjacent periods of the VA group, and have many similar properties. The two can form Bi 100-x Sb x Solid solution, to achieve the regulation of the electrical properties of materials.
[0033] Preferably, the thickness of the bismuth antimonide film 2 is 50 to 100 nm; it can be understood that, within this value range, the thickness of the bismuth antimonide film 2 can be determined according to actual needs. For example, as an example, the thickness of the bismuth antimonide film 2 can be 50 nm, the thickness of the bismuth antimonide film 2 can be 60 nm, the thickness of the bismuth antimonide film 2 can be 70 nm, the thickness of the bismuth antimonide film 2 can be 100 nm, and so on.
[0034] Preferably, the antimony and bismuth contents in the bismuth antimonide film 2 are 66% and 34% respectively.
[0035] Preferably, the substrate 1 is a silicon layer deposited with silicon dioxide, that is, a layer of silicon dioxide is deposited on the silicon layer, and the silicon layer is located on the side of the silicon dioxide away from the bismuth antimonide film. The thickness of the silicon dioxide is 100-500 nm.
[0036] Preferably, the substrate 1 may also be a silicon layer.
[0037] Preferably, the thickness of the substrate 1 is 50 μm to 300 μm. It is understandable that within this value range, the thickness of the substrate 1 can be determined according to actual needs. For example, as an example, the thickness of the substrate 1 can be 50 μm, the thickness of the substrate 1 can be 60 μm, the thickness of the substrate 1 can be 100 μm, the thickness of the substrate 1 can be 300 μm, and so on.
[0038] Preferably, the driving electrode is made of one or more of Ag, Au, C, Cu, Ti and In.
[0039] Furthermore, the present application also provides a method for preparing a high-response ultraviolet detector based on a bismuth antimonide film, which comprises the following steps:
[0040] 101: On a substrate 1, antimony and bismuth targets are sputtered by co-sputtering of dual targets to form a solid solution, and the solid solution is directly cooled to room temperature in an inert gas atmosphere without annealing to obtain a bismuth antimonide film 2;
[0041] When the dual targets are sputtered together, the temperature of the magnetron sputtering machine does not exceed 300°C, and can usually be heated to 200°C. The sputtering power is 10-100W, preferably 25W. The sputtering time can be determined according to actual needs, such as 20s. Argon is used as the inert gas, and the gas flow rate does not exceed 20sccm, such as 16sccm. The gas pressure is 0.5Pa-5Pa; the cooling rate is 5-10°C / min
[0042] 103 : Plating a driving electrode 3 on the bismuth antimonide film 2 .
[0043] The detector has a simple manufacturing process, low commercialization difficulty, and good performance. It is small in size and light in weight.
[0044] Example 1
[0045] See also Figure 1 As shown, a high-response ultraviolet detector based on bismuth antimonide film is a layered structure, specifically including a substrate 1, a bismuth antimonide film 2 and a driving electrode 3. The bismuth antimonide film 2 is located on the substrate 1, and the driving electrode 3 is located on the bismuth antimonide film 2.
[0046] The bismuth antimonide film 2 has a thickness of 80 nm, and contains 66% and 34% antimony and 34% bismuth, respectively.
[0047] The substrate 1 is a silicon layer deposited with silicon dioxide, and has a thickness of 100 μm.
[0048] The driving electrode 3 is made of Ag.
[0049] See also Figure 2 As shown, this is a current versus time (IT) curve of the high-response UV detector under 254nm light. It can be seen that the response time is 80ms and the recovery time is 70ms, and the response speed is very fast.
[0050] See also Figure 3 As shown in the figure, the current versus voltage (IV) curve of the high-response UV detector is 254 nm. It can be seen from the figure that under the irradiation condition, the photocurrent is 100 times the dark current, and the detection rate calculated from this also reaches 10 13 The detection rate is very high.
[0051] In the description of the present application, it should be noted that the terms "upper", "lower", etc. indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present application and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present application. Unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be an indirect connection through an intermediate medium, or it can be a connection between the two elements. For those of ordinary skill in the art, the specific meanings of the above terms in the present application can be understood according to the specific circumstances.
[0052] It should be noted that, in this application, relational terms such as "first" and "second" are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the sentence "comprise a ..." do not exclude the presence of other identical elements in the process, method, article or device including the elements.
[0053] The above description is only a specific implementation of the present application, so that those skilled in the art can understand or implement the present application. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to the embodiments shown herein, but will conform to the widest range consistent with the principles and novel features applied for herein.
Claims
1. A high-response ultraviolet detector based on bismuth antimonide film, It is characterized in that It includes: Substrate (1); A bismuth antimonide thin film (2) located on the substrate (1); A driving electrode (3) is located on the bismuth antimonide film (2).
2. The high-response ultraviolet detector based on bismuth antimonide film as claimed in claim 1, Features: The thickness of the bismuth antimonide film (2) is 50-100 nm.
3. The high-response ultraviolet detector based on bismuth antimonide film as claimed in claim 1, Features: The antimony and bismuth contents in the bismuth antimonide film (2) are 66% and 34% respectively.
4. The high-response ultraviolet detector based on bismuth antimonide film as claimed in claim 1, Features: The substrate (1) is a silicon layer or a silicon layer deposited with silicon dioxide.
5. The high-response ultraviolet detector based on bismuth antimonide film as claimed in claim 4, Features: When the substrate (1) is a silicon layer deposited with silicon dioxide, the thickness of the silicon dioxide is 100 to 500 nm.
6. The high-response ultraviolet detector based on bismuth antimonide film as claimed in claim 1, Features: The thickness of the substrate (1) is 50 μm to 300 μm.
7. The high-response ultraviolet detector based on bismuth antimonide film according to claim 1, Features: The driving electrode (3) is made of one or more of Ag, Au, C, Cu, Ti and In.
8. A method for preparing a high-response ultraviolet detector based on bismuth antimonide film as claimed in claim 1, It is characterized in that It includes: On a substrate (1), antimony and bismuth targets are sputtered by dual-target co-sputtering to form a solid solution, and the solution is cooled to room temperature in an inert gas atmosphere to obtain a bismuth antimonide film (2); A driving electrode (3) is plated on the bismuth antimonide film (2).
9. The method for preparing a high-response ultraviolet detector based on a bismuth antimonide film according to claim 8, Features: The cooling rate is 5-10°C / min.
10. The method for preparing a high-response ultraviolet detector based on a bismuth antimonide film according to claim 8, Features: The inert gas is argon, the gas flow rate does not exceed 20 sccm, and the gas pressure is 0.5Pa~5Pa; And / or, when the dual targets are sputtered together, the temperature of the magnetron sputtering machine does not exceed 300° C., and the sputtering power is 10-100W.