SiC light-triggered thyristor with avalanche enhancement function and manufacturing method thereof
By constructing a high-field avalanche ionization promotion zone in SiC photo-triggered thyristor, and using high-field avalanche ionization to achieve photogenerated carrier multiplication, the problems of insufficient photoelectric gain and slow opening speed of SiC photo-triggered thyristor are solved, and higher photoelectric gain is achieved and faster activate speed.
Patent Information
- Application Number
- CN202410994466.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-11-12
AI Technical Summary
The insufficient photoelectric gain and slow opening speed of SiC photo-triggered thyristors limit their application promotion, especially because the high cost, large volume and high system complexity of high power ultraviolet lasers are contrary to the original intention of reducing system volume and complexity through light control. , and it is difficult to achieve the emission of high-power density ultraviolet light using UV LEDs with small size and low cost.
A SiC phototriggered thyristor with avalanche enhancement function was designed. By constructing a high-field avalanche ionization promotion zone under the optical gate level of the SiC phototriggered thyristor, the photogenerated carrier multiplication is achieved by using high-field avalanche ionization, and the photogain and gain is improved. Activation speed. The specific implementation includes preparing n+ buffer layer, p-type buffer layer, p-type long base region, p-type base region, junction terminal expansion, n short base region and p+ emission region in sequence on an n+ type 4H-SiC substrate, and passing Preparation of physical gas phase transport method and chemical vapor deposition method, combined with lithography, ion implantation, vacuum evaporation and other technologies.
It achieves a higher photoelectric gain and faster turn-on speed, improves the performance of SiC light-triggered thyristors, and solves the problems of insufficient photoelectric gain and slow turn-on speed of traditional SiC light-triggered thyristors.
Smart Images

Figure CN118943232A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of semiconductor devices, and in particular relates to a SiC light-triggered thyristor with an avalanche enhancement function. The invention also relates to a method for manufacturing the SiC light-triggered thyristor with an avalanche enhancement function. Background Art
[0002] Silicon carbide (SiC) has the characteristics of large bandgap, high thermal conductivity, large critical avalanche breakdown electric field strength, and high carrier saturation drift velocity. Power devices made of SiC have the advantages of high temperature resistance, radiation resistance, and strong anti-interference ability. SiC light-triggered thyristors use light-injected carriers to replace the gate electrical signals of traditional electrically controlled thyristors to achieve direct light control, which can effectively reduce the size and complexity of the system. However, in order to increase the opening speed of SiC thyristors, it is often necessary to use ultraviolet lasers to emit high-power density ultraviolet light to trigger the gate level of SiC thyristors. However, high-power ultraviolet lasers have the characteristics of high cost, large size, and complex system. The solution of using high-power ultraviolet lasers to increase the opening speed of SiC light-triggered thyristors is contrary to the original intention of reducing the size and complexity of the system through light control. It is difficult to achieve the emission of high-power density ultraviolet light using small and low-cost UV LEDs. Therefore, the mutual restriction relationship between ultraviolet light power density and the turning-on speed of SiC light-triggered thyristors has become the main limiting factor for the application and promotion of SiC light-triggered thyristors. Summary of the invention
[0003] The purpose of the present invention is to provide a SiC light-triggered thyristor with avalanche enhancement function, which solves the problems of insufficient photoelectric gain and slow opening speed of the SiC light-triggered thyristor in the prior art.
[0004] Another object of the present invention is to provide a method for manufacturing a SiC light-triggered thyristor with avalanche enhancement function.
[0005] The first technical solution adopted by the present invention is that a SiC light-triggered thyristor with avalanche enhancement function includes a material of n + Type 4H-SiC substrate, n + The surface of the 4H-SiC substrate is made with n + Buffer layer, n + The surface of the buffer layer is formed with a p-type buffer layer upward, and the surface of the p-type buffer layer is formed with a p-type buffer layer upward. - Type long base region, p - The surface of the p-type long base region is made with a p-type base region and a junction terminal extension. The junction terminal extension is located on both sides of the p-type base region. - The surface of the p-type base region is made with an n-type short base region, and the surface of the n-type short base region is made with a p-type long base region. + Emission area, p +The emitter region is located above the p-type base region, and the anode ohmic contact metal is located on the p + On the upper surface of the emitter region, the cathode ohmic contact metal is located at n + The lower surface of the 4H-SiC substrate, the upper surface of the anode ohmic contact metal is covered with the anode PAD metal, and the lower surface of the cathode ohmic contact metal is covered with the cathode PAD metal.
[0006] The first technical solution of the present invention is also characterized in that:
[0007] n + The thickness of the substrate 1 of type 4H-SiC is 50.0 μm to 350 μm, and the donor impurity concentration is 1.0×10 18 cm -3 ~2.0×10 22 cm -3 ;n + The buffer layer 2 has a thickness of 1 μm to 2.5 μm and an impurity concentration of 1.0×10 18 cm -3 ~2.0×10 22 cm -3 The thickness of the p-type buffer layer 3 is 1 μm to 2.5 μm, and the impurity concentration is 1.0×10 17 cm -3 ~3.0×10 17 cm -3 ;p - The thickness of the long base region 4 is 50.0 μm to 160 μm, and the impurity concentration is 1.0×10 13 cm -3 ~5.0×10 14 cm -3 .
[0008] The junction terminal extension 10 is located on both sides of the p-type base region 5, and the lateral spacing between the junction terminal extension 10 and the p-type base region 5 is 0.1 mm to 1.0 cm; the width of the p-type base region 5 is 0.8 mm to 3 mm, the thickness of the p-type base region 5 is 0.5 μm to 2 μm, and the doping concentration is 2.0×10 14 cm -3 ~8.0×10 15 cm -3 The thickness of the junction terminal extension 10 is 0.3 μm to 3.0 μm, the width of the junction terminal extension 10 is 50 μm to 500 μm, and the JTE impurity concentration is 1.0×10 15 cm -3 ~5.0×10 16 cm -3 The space charge modulation ring width is 0.5μm~2.0μm, the ring spacing is 1.0μm~5.0μm, and the impurity concentration is 1.0×10 16 cm-3 ~1.0×10 18 cm -3 ;
[0009] The thickness of the n short base region 9 is 1.5 to 2.5 μm, and the impurity concentration is 8.0×10 16 cm -3 ~2.5×10 17 cm -3 ;p + The emitter region 8 is in the form of a plurality of convex terraces and is located above the p-type base region 5. The number of convex terraces ranges from 1 to 1000. + The lateral distance between the emitter region 8 and the p-type base region 5 is 0-1.0 mm; + The width of the emission region 8 is 10 μm to 2 cm, the thickness is 1.5 μm to 3.0 μm, and the impurity concentration is 2.0×10 19 cm -3 ~2.0×10 22 cm -3 ;
[0010] The anode ohmic contact metal 11 is formed by a combination of Ti, Ni, and W, with a thickness of 150nm to 300nm; the cathode ohmic contact metal 12 is formed by a combination of Ti and Ni, with a thickness of 100nm to 300nm; the anode PAD metal 13 is formed by a combination of Al and Cu, with a thickness of 4μm to 10μm; the cathode PAD metal 14 is formed by Au, with a thickness of 2μm to 3μm.
[0011] The second technical solution adopted by the present invention is a method for manufacturing a SiC light-triggered thyristor with avalanche enhancement function, which is implemented according to the following steps:
[0012] Step 1, preparing an n+ type 4H-SiC substrate by physical vapor transport method PVT;
[0013] Step 2: Prepare n+ type substrates by chemical vapor deposition (CVD) on the surface of the n+ type substrate. + Buffer layer, p-type buffer layer, p - Type long base region;
[0014] Step 3: Photolithography and ion implantation are used to - A p-type base region is prepared by moving the surface of the type long base region downward;
[0015] Step 4: Using chemical vapor deposition (CVD) - The n-type epitaxial layer, p-type epitaxial layer and + Type epitaxial layer;
[0016] Step 5: Etch p by photolithography plus dry etching process +The n-type epitaxial layer is formed by etching the n-type epitaxial layer and exposing the upper surface of the n-type epitaxial layer. + Emitting region, n short base region;
[0017] Step 6: Photolithography and ion implantation are used to - The type long base region surface is downwardly prepared to extend the junction terminal;
[0018] Step 7: Perform high temperature activation annealing under the protection of the carbon film.
[0019] Step 8: Photolithography, vacuum evaporation, and stripping are used in sequence to form a + The anode ohmic contact metal is manufactured on the upper surface of the emitter region by photolithography, vacuum evaporation, and stripping. + A cathode ohmic contact metal is fabricated on the lower surface of a 4H-SiC substrate;
[0020] Step 9, the upper surface of the anode ohmic contact metal is covered with an anode PAD metal by photolithography, vacuum evaporation, and etching, and the lower surface of the cathode ohmic contact metal is covered with a cathode PAD metal by photolithography, vacuum evaporation, and etching;
[0021] Step 10: forming a passivation layer on the upper surface of the device by a PECVD method;
[0022] Step 11: Manufacturing SiC light-triggered thyristors with avalanche enhancement function is achieved through dotting, scribing, and packaging.
[0023] The second technical solution of the present invention is also characterized in that:
[0024] The growth temperature of the physical vapor transport method PVT in step 1 is 2100° C. to 2250° C.; the growth temperature of the chemical vapor deposition method CVD in step 2 is 1400° C. to 1500° C.;
[0025] In step 3, the ion implantation temperature is 450° C. to 550° C.;
[0026] The growth temperature of the chemical vapor deposition method CVD in step 4 is 1400° C. to 1500° C.;
[0027] The annealing temperature in step 7 is 1650°C to 1800°C.
[0028] The beneficial effect of the present invention is that, in the SiC light-triggered thyristor with avalanche enhancement function, a high-field avalanche ionization promotion zone is constructed on the upper surface of the long base region below the optical gate level of the SiC light-triggered thyristor by setting a p-base region 5, and the multiplication of photogenerated carriers is achieved through high-field avalanche ionization, thereby improving the optical gain, so that the SiC light-triggered thyristor with avalanche enhancement function of the present invention has a higher photoelectric gain and a faster opening speed than the traditional SiC light-triggered thyristor. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 Schematic diagram of the cross-sectional structure of the SiC light-triggered thyristor with avalanche enhancement function in Embodiment 1 of the present invention;
[0030] Figure 2 is completed + Buffer layer 2, p-type buffer layer 3, p - Schematic diagram of the cross-sectional structure of the epitaxial manufacturing process of the type long base region 4;
[0031] Figure 3 is a schematic cross-sectional structure diagram of the manufacturing process of the p-type base region 5 after ion implantation;
[0032] Figure 4 The n-type epitaxial layer 6 is completed, p + A schematic cross-sectional structure diagram of the epitaxial manufacturing process of the epitaxial layer 7;
[0033] Figure 5 is completed + A schematic diagram of the cross-sectional structure of the photolithography and etching manufacturing process of the emission region 8;
[0034] Figure 6 It is a schematic cross-sectional structure diagram of completing the photolithography and etching manufacturing process of the n short base region 9;
[0035] Figure 7 is a schematic cross-sectional structure diagram of a manufacturing process of a junction terminal extension 10 completed by ion implantation;
[0036] Figure 8 It is a cross-sectional structural schematic diagram of the manufacturing process of the anode ohmic contact metal 11 and the cathode ohmic contact metal 12;
[0037] Fig. 9 It is a cross-sectional structural schematic diagram of the manufacturing process of the anode PAD metal 13 and the cathode PAD metal 14 completed by vacuum evaporation;
[0038] Fig.10 Schematic diagram of the SiC light-triggered thyristor cell structure with avalanche enhancement function according to Embodiment 2 of the present invention;
[0039] Fig.11Schematic diagram of the SiC light-triggered thyristor cell structure with avalanche enhancement function according to Embodiment 3 of the present invention;
[0040] Fig.12 is a numerical simulation characteristic curve of the switch characteristics of the SiC light-triggered thyristor with avalanche enhancement function in Example 1 of the present invention;
[0041] In the figure, 1.n + Type 4H-SiC substrate, 2.n + Buffer layer, 3.p-type buffer layer, 4.p - 5.p-type base region, 6.n-type epitaxial layer, 7.p + Type epitaxial layer, 8.p + Emitter region, 9.n short base region, 10. Junction terminal extension, 11. Anode ohmic contact metal, 12. Cathode ohmic contact metal, 13. Anode PAD metal, 14. Cathode PAD metal. DETAILED DESCRIPTION
[0042] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments.
[0043] The SiC light-triggered thyristor with avalanche enhancement function of the present invention comprises a material of n + Type 4H-SiC substrate 1, n + The 4H-SiC substrate 1 is formed with n + Buffer layer 2, n + The surface of the buffer layer 2 is formed with a p-type buffer layer 3, and the surface of the p-type buffer layer 3 is formed with a p-type buffer layer 3. - Type long base region 4, p - The surface of the p-type base region 4 is provided with a p-type base region 5 and a junction terminal extension 10, and the junction terminal extension 10 is located on both sides of the p-type base region 5. - The surface of the p-type long base region 4 and the p-type base region 5 is formed with an n-type short base region 9 upwardly, and the surface of the n-type short base region 9 is formed with a p-type long base region 4 and the p-type base region 5 upwardly. + Emission zone 8, p + The emitter region 8 is located above the p-type base region 5, and the anode ohmic contact metal 11 is located above the p-type base region 5. + On the upper surface of the emitter region 8, the cathode ohmic contact metal 12 is located at n + The lower surface of the 4H-SiC substrate 1 is covered with an anode PAD metal 13 on the upper surface of the anode ohmic contact metal 11 , and the lower surface of the cathode ohmic contact metal 12 is covered with a cathode PAD metal 14 .
[0044] n + The thickness of the substrate 1 of type 4H-SiC is 50.0 μm to 350 μm, and the donor impurity concentration is 1.0×10 18 cm -3 ~2.0×1022 cm -3 ;n + The buffer layer 2 has a thickness of 1 μm to 2.5 μm and an impurity concentration of 1.0×10 18 cm -3 ~2.0×10 22 cm -3 The thickness of the p-type buffer layer 3 is 1 μm to 2.5 μm, and the impurity concentration is 1.0×10 17 cm -3 ~3.0×10 17 cm -3 ;p - The thickness of the long base region 4 is 50.0 μm to 160 μm, and the impurity concentration is 1.0×10 13 cm -3 ~5.0×10 14 cm -3 .
[0045] The junction terminal extension 10 is located on both sides of the p-type base region 5, and the lateral spacing between the junction terminal extension 10 and the p-type base region 5 is 0.1 mm to 1.0 cm; the width of the p-type base region 5 is 0.8 mm to 3 mm, the thickness of the p-type base region 5 is 0.5 μm to 2 μm, and the doping concentration is 2.0×10 14 cm -3 ~8.0×10 15 cm -3 The thickness of the junction terminal extension 10 is 0.3 μm to 3.0 μm, the width of the junction terminal extension 10 is 50 μm to 500 μm, and the JTE impurity concentration is 1.0×10 15 cm -3 ~5.0×10 16 cm -3 The space charge modulation ring width is 0.5μm~2.0μm, the ring spacing is 1.0μm~5.0μm, and the impurity concentration is 1.0×10 16 cm -3 ~1.0×10 18 cm -3 ;
[0046] The thickness of the n short base region 9 is 1.5 to 2.5 μm, and the impurity concentration is 8.0×10 16 cm -3 ~2.5×10 17 cm -3 ;p + The emitter region 8 is in the form of a plurality of convex terraces and is located above the p-type base region 5. The number of convex terraces ranges from 1 to 1000. + The lateral distance between the emitter region 8 and the p-type base region 5 is 0-1.0 mm; +The width of the emission region 8 is 10 μm to 2 cm, the thickness is 1.5 μm to 3.0 μm, and the impurity concentration is 2.0×10 19 cm -3 ~2.0×10 22 cm -3 ;
[0047] The anode ohmic contact metal 11 is formed by a combination of Ti, Ni, and W, with a thickness of 150nm to 300nm; the cathode ohmic contact metal 12 is formed by a combination of Ti and Ni, with a thickness of 100nm to 300nm; the anode PAD metal 13 is formed by a combination of Al and Cu, with a thickness of 4μm to 10μm; the cathode PAD metal 14 is formed by Au, with a thickness of 2μm to 3μm.
[0048] The method for manufacturing a SiC light-triggered thyristor with avalanche enhancement function is implemented according to the following steps:
[0049] Step 1, preparing an n+ type 4H-SiC substrate 1 by physical vapor transport method PVT;
[0050] Step 2: epitaxially prepare n+ type substrate 1 upward from the surface of n+ type substrate 1 by chemical vapor deposition (CVD). + Buffer layer 2, p-type buffer layer 3, p - Type long base region 4;
[0051] Step 3: Photolithography and ion implantation are used to - The p-type base region 5 is prepared downward from the surface of the p-type long base region 4;
[0052] Step 4: Using chemical vapor deposition (CVD) - The surface of the long base region 4 is epitaxially grown upward to prepare the n-type epitaxial layer 6, the p + Type epitaxial layer 7;
[0053] Step 5: Etch p by photolithography plus dry etching process + The n-type epitaxial layer 7 is formed to expose the upper surface of the n-type epitaxial layer 6; the n-type epitaxial layer 6 is etched again by photolithography and dry etching to form a p + Emitter region 8, n short base region 9;
[0054] Step 6: Photolithography and ion implantation are used to - The long base region 4 is provided with a junction terminal extension 10 downwardly from the surface;
[0055] Step 7: Perform high temperature activation annealing under the protection of the carbon film.
[0056] Step 8: Photolithography, vacuum evaporation, and stripping are used in sequence to form a +The anode ohmic contact metal 11 is manufactured on the upper surface of the emitter region 8 by sequentially photolithography, vacuum evaporation, and stripping. + A cathode ohmic contact metal 12 is fabricated on the lower surface of the 4H-SiC substrate 1, such as Figure 8 As shown;
[0057] Step 9: The upper surface of the anode ohmic contact metal 11 is covered with an anode PAD metal 13 by photolithography, vacuum evaporation, and etching, and the lower surface of the cathode ohmic contact metal 12 is covered with a cathode PAD metal 14 by photolithography, vacuum evaporation, and etching. Fig. 9 As shown;
[0058] Step 10: forming a passivation layer on the upper surface of the device by a PECVD method;
[0059] Step 11: Manufacturing SiC light-triggered thyristors with avalanche enhancement function is achieved through dotting, scribing, and packaging.
[0060] The growth temperature of the physical vapor transport method PVT in step 1 is 2100° C. to 2250° C.; the growth temperature of the chemical vapor deposition method CVD in step 2 is 1400° C. to 1500° C.;
[0061] In step 3, the ion implantation temperature is 450° C. to 550° C.;
[0062] The growth temperature of the chemical vapor deposition method CVD in step 4 is 1400° C. to 1500° C.;
[0063] The annealing temperature in step 7 is 1650°C to 1800°C.
[0064] Example 1
[0065] like Figure 1 The structure of the SiC light-triggered thyristor with avalanche enhancement function in embodiment 1 of the present invention is as follows: + The substrate 1 is a 4H-SiC substrate with a thickness of 150.0 μm and a donor impurity concentration of 1.0×10 18 cm -3 ;
[0066] n + The 4H-SiC substrate 1 is formed with n + Buffer layer 2, thickness is 2.0 μm, impurity concentration is 1.0×10 18 cm -3 ;
[0067] n + The p-type buffer layer 3 is formed on the surface of the buffer layer 2, with a thickness of 2.0 μm and an impurity concentration of 2.0×10 17 cm-3 ;
[0068] The p-type buffer layer 3 has a p - The long base region 4 has a thickness of 80.0 μm and an impurity concentration of 2.0×10 14 cm -3 ;
[0069] p - A p-type base region 5 and a junction terminal extension 10 are formed downwardly from the surface of the p-type base region 4. The junction terminal extension 10 is located on both sides of the p-type base region 5, and the lateral spacing between the two is 2.0 mm.
[0070] The width of the p-type base region 5 is 800.0 μm, the thickness of the p-type base region 5 is 0.8 μm, and the doping concentration is 5.0×10 15 cm -3 ;
[0071] The thickness of the junction termination extension 10 is 0.8 μm, the width of the junction termination extension 10 is 120 μm, and the JTE impurity concentration is 6.0×10 16 cm -3 The space charge modulation ring width is 1.0 μm, the ring spacing is 1.0 μm to 5.0 μm, and the impurity concentration is 1.0×10 17 cm -3 ;
[0072] p - The n-type long base region 4 and the p-type base region 5 are formed on the surface with an n-type short base region 9 having a thickness of 2.0 μm and an impurity concentration of 2.0×10 17 cm -3 ;
[0073] The surface of the n short base region 9 is made of p + Emission zone 8, p + The emitter region 8 is located above the p-type base region 5, and the lateral spacing between the two is 1.0 mm; + The width of the emitter region 8 is 650 μm, the thickness is 3.0 μm, and the impurity concentration is 2.0×10 19 cm -3 ;
[0074] Located in p + The anode ohmic contact metal 11 on the upper surface of the emitter region 8 is formed by a combination of Ti, Ni, and W, and has a thickness of 200 nm;
[0075] Located in + The cathode ohmic contact metal 12 on the lower surface of the substrate 1 of type 4H-SiC is formed by a combination of Ti and Ni and has a thickness of 200 nm;
[0076] The upper surface of the anode ohmic contact metal 11 is covered with an anode PAD metal 13, which is a combination of Al and Cu and has a thickness of 5 μm;
[0077] The lower surface of the cathode ohmic contact metal 12 is covered with a cathode PAD metal 14 made of Au and having a thickness of 2 μm;
[0078] like Figure 2-Figure 9 Embodiment 1 of the present invention provides a method for manufacturing a SiC light-triggered thyristor with avalanche enhancement function, which is implemented according to the following steps:
[0079] The n+ type 4H-SiC substrate 1 was prepared by physical vapor transport (PVT) at a growth temperature of 2150°C. Figure 2 ;
[0080] The n+ type substrate 1 is epitaxially prepared upward by chemical vapor deposition (CVD). + Buffer layer 2, p-type buffer layer 3, p - Type long base region 4, the growth temperature is 1450℃, such as Figure 2 ;
[0081] Through photolithography and 500℃ ion implantation, the - The p-type base region 5 is prepared from the surface of the p-type long base region 4 downward, such as Figure 3 ;
[0082] The chemical vapor deposition (CVD) method was used to deposit - The n-type epitaxial layer 6 is prepared by epitaxially growing the surface of the n-type long base region 4 upwards. + The epitaxial layer 7 is grown at a temperature of 1450°C. Figure 4 ;
[0083] The p + Type epitaxial layer 7, forming p + The emitter region 8 exposes the upper surface of the n-type epitaxial layer 6, such as Figure 5 ; Again, the photolithography and dry etching process is performed to etch the n-type epitaxial layer 6 to form an n short base region 9, such as Figure 6 ;
[0084] Through photolithography and ion implantation, - The type long base region 4 is surface downwardly prepared to extend the junction terminal 10, such as Figure 7 ;
[0085] High temperature activation annealing is carried out under the protection of carbon film, and the annealing temperature is 1750℃.
[0086] Through photolithography, vacuum evaporation and lift-off methods, the p + Anode ohmic contact metal 11 is fabricated on the upper surface of the emitter region 8. +A cathode ohmic contact metal 12 is fabricated on the lower surface of the 4H-SiC substrate 1, such as Figure 8 As shown;
[0087] By photolithography, vacuum evaporation and etching, the upper surface of the anode ohmic contact metal 11 is covered with an anode PAD metal 13, and the lower surface of the cathode ohmic contact metal 12 is covered with a cathode PAD metal 14. Fig. 9 As shown;
[0088] A passivation layer is formed on the upper surface of the device by a PECVD method;
[0089] The manufacturing of SiC light-triggered thyristors with avalanche enhancement function is achieved through dotting, scribing and packaging.
[0090] Example 2
[0091] like Fig.10 The structure of the SiC light-triggered thyristor with avalanche enhancement function in embodiment 2 of the present invention is as follows: + The substrate 1 is a 4H-SiC substrate with a thickness of 50.0 μm and a donor impurity concentration of 1.0×10 20 cm -3 ;
[0092] n + The 4H-SiC substrate 1 is formed with n + Buffer layer 2, thickness is 2.5 μm, impurity concentration is 1.0×10 20 cm -3 ;
[0093] n + The p-type buffer layer 3 is formed on the surface of the buffer layer 2, with a thickness of 2.5 μm and an impurity concentration of 3.0×10 17 cm -3 ;
[0094] The p-type buffer layer 3 has a p - The long base region 4 has a thickness of 160.0 μm and an impurity concentration of 1.0×10 13 cm -3 ;
[0095] p - A p-type base region 5 is formed downward from the surface of the type long base region 4. The width of the p-type base region 5 is 3.0 mm, the thickness of the p-type base region 5 is 2.0 μm, and the doping concentration is 2.0×10 14 cm -3 ;
[0096] p - The n-type long base region 4 and the p-type base region 5 are formed on the surface with an n-type short base region 9 having a thickness of 2.5 μm and an impurity concentration of 2.5×1017 cm -3 ;
[0097] The surface of the n short base region 9 is made of p + Emission zone 8, p + The emitter region 8 covers the upper surface of the n short base region 9; + The width of the emission region 8 is 1 cm, the thickness is 3.0 μm, and the impurity concentration is 2.0×10 20 cm -3 ;
[0098] Located in p + The anode ohmic contact metal 11 on the upper surface of the emitter region 8 is formed by a combination of Ti and Ni and has a thickness of 300 nm;
[0099] Located in + The cathode ohmic contact metal 12 on the lower surface of the substrate 1 of type 4H-SiC is formed by a combination of Ti, Ni, and W, and has a thickness of 300 nm;
[0100] The upper surface of the anode ohmic contact metal 11 is covered with an anode PAD metal 13 made of Al and having a thickness of 10 μm;
[0101] The lower surface of the cathode ohmic contact metal 12 is covered with a cathode PAD metal 14 made of Ag and having a thickness of 3 μm;
[0102] Embodiment 2 of the present invention provides a method for manufacturing a SiC light-triggered thyristor with avalanche enhancement function, which is implemented according to the following steps:
[0103] The n+ type 4H-SiC substrate 1 is prepared by physical vapor transport (PVT) method at a growth temperature of 2250° C.;
[0104] The n+ type substrate 1 is epitaxially prepared upward by chemical vapor deposition (CVD). + Buffer layer 2, p-type buffer layer 3, p - Type long base region 4, growth temperature is 1500℃;
[0105] Through photolithography and 550℃ ion implantation, the p - The p-type base region 5 is prepared downward from the surface of the p-type long base region 4;
[0106] The chemical vapor deposition (CVD) method was used to deposit - The surface of the n-type long base region 4 is epitaxially formed upward to prepare the n-type short base region 9, the p-type long base region 4, and the n-type short base region 9. + Emitter region 8, growth temperature is 1500°C;
[0107] High temperature activation annealing is carried out under the protection of carbon film, and the annealing temperature is 1800℃.
[0108] Through photolithography, vacuum evaporation and lift-off methods, the p + Anode ohmic contact metal 11 is fabricated on the upper surface of the emitter region 8. + A cathode ohmic contact metal 12 is manufactured on the lower surface of the 4H-SiC substrate 1;
[0109] The upper surface of the anode ohmic contact metal 11 is covered with an anode PAD metal 13, and the lower surface of the cathode ohmic contact metal 12 is covered with a cathode PAD metal 14 by photolithography, vacuum evaporation, and etching methods;
[0110] A passivation layer is formed on the upper surface of the device by a PECVD method;
[0111] The manufacturing of SiC light-triggered thyristors with avalanche enhancement function is achieved through dotting, scribing and packaging.
[0112] Example 3
[0113] like Fig.11 The structure of the SiC light-triggered thyristor with avalanche enhancement function in embodiment 3 of the present invention is as follows: + The substrate 1 is a 4H-SiC substrate with a thickness of 350.0 μm and a donor impurity concentration of 2.0×10 22 cm -3 ;
[0114] n + The 4H-SiC substrate 1 is formed with n + Buffer layer 2, thickness is 1.0 μm, impurity concentration is 2.0×10 22 cm -3 ;
[0115] n + The p-type buffer layer 3 is formed on the surface of the buffer layer 2, with a thickness of 1.0 μm and an impurity concentration of 1.0×10 17 cm -3 ;
[0116] The p-type buffer layer 3 has a p - The long base region 4 has a thickness of 50.0 μm and an impurity concentration of 5.0×10 14 cm -3 ;
[0117] p - A p-type base region 5 is formed downward from the surface of the type long base region 4. The width of the p-type base region 5 is 1.0 mm, the thickness of the p-type base region 5 is 0.5 μm, and the doping concentration is 8.0×10 15 cm -3 ;
[0118] p -The surface of the p-type long base region 4 and the p-type base region 5 is formed with an n-type short base region 9 with a thickness of 1.5 μm and an impurity concentration of 8.0×10 16 cm -3 ;
[0119] The surface of the n short base region 9 is made of p + Emission zone 8, p + The emitter region 8 covers the upper surface of the n short base region 9;
[0120] p + The emission region 8 is in the shape of a groove, with a total width of 0.5 cm, a thickness of 1.5 μm, and an impurity concentration of 2.0×10 22 cm -3 ;
[0121] Located in p + The anode ohmic contact metal 11 on the upper surface of the emitter region 8 is formed of Ni and has a thickness of 150 nm;
[0122] Located in + The cathode ohmic contact metal 12 on the lower surface of the substrate 1 of type 4H-SiC is formed by a combination of Ni and W and has a thickness of 100 nm;
[0123] The upper surface of the anode ohmic contact metal 11 is covered with an anode PAD metal 13 made of Cu and having a thickness of 4 μm;
[0124] The lower surface of the cathode ohmic contact metal 12 is covered with a cathode PAD metal 14 made of Au and having a thickness of 3 μm;
[0125] Embodiment 3 of the present invention is a method for manufacturing a SiC light-triggered thyristor with avalanche enhancement function, which is implemented according to the following steps:
[0126] The n+ type 4H-SiC substrate 1 is prepared by physical vapor transport (PVT) method at a growth temperature of 2100° C.;
[0127] The n+ type substrate 1 is epitaxially prepared upward by chemical vapor deposition (CVD). + Buffer layer 2, p-type buffer layer 3, p - Type long base region 4, growth temperature is 1400℃;
[0128] Through photolithography and ion implantation at 450℃, the - The p-type base region 5 is prepared downward from the surface of the p-type long base region 4;
[0129] The chemical vapor deposition (CVD) method was used to deposit - The surface of the n-type long base region 4 is epitaxially formed upward to prepare the n-type short base region 9, the p-type long base region 4, and the n-type short base region 9. + Emitter zone 8, growth temperature is 1400°C;
[0130] High temperature activation annealing is carried out under the protection of carbon film, and the annealing temperature is 1650℃.
[0131] Through photolithography, vacuum evaporation and lift-off methods, the p + Anode ohmic contact metal 11 is fabricated on the upper surface of the emitter region 8. + A cathode ohmic contact metal 12 is manufactured on the lower surface of the 4H-SiC substrate 1;
[0132] The upper surface of the anode ohmic contact metal 11 is covered with an anode PAD metal 13, and the lower surface of the cathode ohmic contact metal 12 is covered with a cathode PAD metal 14 by photolithography, vacuum evaporation, and etching methods;
[0133] A passivation layer is formed on the upper surface of the device by a PECVD method;
[0134] The manufacturing of SiC light-triggered thyristors with avalanche enhancement function is achieved through dotting, scribing and packaging.
[0135] In order to illustrate the advantages of the SiC light-triggered thyristor with avalanche enhancement function of the present invention, the SiC light-triggered thyristor with avalanche enhancement function of the above embodiment 1 was verified by using the Sentaurus TCAD computer numerical experiment platform. Fig.12 The turn-on characteristic curves of a SiC light-triggered thyristor with avalanche enhancement function and a traditional SiC light-triggered thyristor under the same light-triggering conditions in Example 1 of the present invention are shown in the figure. As can be seen from the figure, the turn-on speed of the SiC light-triggered thyristor with avalanche enhancement function of the present invention is faster than that of the traditional SiC light-triggered thyristor. In summary, the SiC light-triggered thyristor with avalanche enhancement function of the present invention improves the photoelectric gain and turn-on speed of the existing SiC light-triggered thyristor.
Claims
1. SiC light-triggered thyristor with avalanche enhancement function, It is characterized in that Including materials for n + Type 4H-SiC substrate (1), n + The type 4H-SiC substrate (1) is fabricated with n + Buffer layer (2), n + The surface of the buffer layer (2) is formed with a p-type buffer layer (3) facing upward, and the surface of the p-type buffer layer (3) is formed with a p-type buffer layer (3) facing upward. - Type long base region (4), p - A p-type base region (5) and a junction terminal extension (10) are formed downwardly on the surface of the p-type long base region (4). The junction terminal extension (10) is located on both sides of the p-type base region (5). - The surface of the p-type long base region (4) and the p-type base region (5) is formed with an n-type short base region (9) upwardly, and the surface of the n-type short base region 9 is formed with a p-type long base region (4) and the p-type base region (5) upwardly. + Emission zone (8), p + The emitter region (8) is located above the p-type base region (5), and the anode ohmic contact metal (11) is located on the p-type base region (5). + On the upper surface of the emitter region (8), the cathode ohmic contact metal (12) is located at n + The lower surface of the 4H-SiC substrate (1) is covered with an anode PAD metal (13) on the upper surface of the anode ohmic contact metal (11), and the lower surface of the cathode ohmic contact metal (12) is covered with a cathode PAD metal (14).
2. The SiC light-triggered thyristor with avalanche enhancement function according to claim 1, It is characterized in that The + The substrate (1) of type 4H-SiC has a thickness of 50.0 μm to 350 μm and a donor impurity concentration of 1.0×10 18 cm -3 ~2.0×10 22 cm -3 ;n + The buffer layer (2) has a thickness of 1 μm to 2.5 μm and an impurity concentration of 1.0×10 18 cm -3 ~2.0×10 22 cm -3 The p-type buffer layer (3) has a thickness of 1 μm to 2.5 μm and an impurity concentration of 1.0×10 17 cm -3 ~3.0×10 17 cm -3 ;p - The thickness of the long base region (4) is 50.0 μm to 160 μm, and the impurity concentration is 1.0×10 13 cm -3 ~5.0×10 14 cm -3 .
3. The SiC light-triggered thyristor with avalanche enhancement function according to claim 1, It is characterized in that The junction terminal extension (10) is located on both sides of the p-type base region (5), and the lateral spacing between the junction terminal extension (10) and the p-type base region (5) is 0.1 mm to 1.0 cm; the width of the p-type base region (5) is 0.8 mm to 3 mm, the thickness of the p-type base region (5) is 0.5 μm to 2 μm, and the doping concentration is 2.0×10 14 cm -3 ~8.0×10 15 cm -3 The thickness of the junction terminal extension (10) is 0.3 μm to 3.0 μm, the width of the junction terminal extension (10) is 50 μm to 500 μm, and the JTE impurity concentration is 1.0×10 15 cm -3 ~5.0×10 16 cm -3 The space charge modulation ring width is 0.5μm~2.0μm, the ring spacing is 1.0μm~5.0μm, and the impurity concentration is 1.0×10 16 cm -3 ~1.0×10 18 cm -3 .
4. The SiC light-triggered thyristor with avalanche enhancement function according to claim 1, It is characterized in that The n short base region (9) has a thickness of 1.5 to 2.5 μm and an impurity concentration of 8.0×10 16 cm -3 ~2.5×10 17 cm -3 ;p + The emitter region (8) is in the form of a plurality of convex terraces and is located above the p-type base region (5). The number of the convex terraces ranges from 1 to 1000. + The lateral distance between the emitter region (8) and the p-type base region 5 is 0 to 1.0 mm; + The emission region (8) has a width of 10 μm to 2 cm, a thickness of 1.5 μm to 3.0 μm, and an impurity concentration of 2.0×10 19 cm -3 ~2.0×10 22 cm -3 .
5. The SiC light-triggered thyristor with avalanche enhancement function according to claim 1, It is characterized in that The anode ohmic contact metal (11) is formed by a combination of Ti, Ni and W, with a thickness of 150nm to 300nm; the cathode ohmic contact metal (12) is formed by a combination of Ti and Ni, with a thickness of 100nm to 300nm; the anode PAD metal (13) is formed by a combination of Al and Cu, with a thickness of 4μm to 10μm; the cathode PAD metal (14) is formed by Au, with a thickness of 2μm to 3μm.
6. The method for manufacturing a SiC light-triggered thyristor with avalanche enhancement function according to any one of claims 1 to 5, It is characterized in that Follow these steps to implement: Step 1, preparing an n+ type 4H-SiC substrate (1) by physical vapor transport (PVT); Step 2: epitaxially prepare n+ type substrate (1) upward from the surface by chemical vapor deposition (CVD). + Buffer layer (2), p-type buffer layer (3), p - Type long base region (4); Step 3: Photolithography and ion implantation are used to - The p-type base region (5) is prepared from the surface of the p-type long base region (4) downward; Step 4: Using chemical vapor deposition (CVD) on p - The n-type epitaxial layer (6), the p-type epitaxial layer (7) and the n-type epitaxial layer (8) are sequentially formed by epitaxially growing the surface of the n-type long base region (4) upward. + Type epitaxial layer (7); Step 5: Etch p by photolithography plus dry etching process + The n-type epitaxial layer (7) is formed to expose the upper surface of the n-type epitaxial layer (6); the n-type epitaxial layer (6) is etched by photolithography and dry etching again to form a p-type epitaxial layer (7). + Emitter region (8), n short base region (9); Step 6: Photolithography and ion implantation are used to - The long base region (4) is formed downwardly from the surface to form a junction terminal extension (10); Step 7, performing high temperature activation annealing under the protection of the carbon film; Step 8: Photolithography, vacuum evaporation, and stripping are used in sequence to form a + The anode ohmic contact metal (11) is manufactured on the upper surface of the emission region (8), and the anode ohmic contact metal (11) is manufactured on the upper surface of the emission region (8) by photolithography, vacuum evaporation, and stripping. + A cathode ohmic contact metal (12) is fabricated on the lower surface of a 4H-SiC substrate (1); Step 9, the upper surface of the anode ohmic contact metal (11) is covered with an anode PAD metal (13) by photolithography, vacuum evaporation, and etching, and the lower surface of the cathode ohmic contact metal (12) is covered with a cathode PAD metal (14) by photolithography, vacuum evaporation, and etching; Step 10: forming a passivation layer on the upper surface of the device by a PECVD method; Step 11: Manufacturing of SiC light-triggered thyristors with avalanche enhancement function is achieved through dotting, scribing, and packaging.
7. The method for manufacturing a SiC light-triggered thyristor with avalanche enhancement function according to claim 6, It is characterized in that The growth temperature of the physical vapor transport method PVT in step 1 is 2100° C. to 2250° C.; the growth temperature of the chemical vapor deposition method CVD in step 2 is 1400° C. to 1500° C.
8. The method for manufacturing a SiC light-triggered thyristor with avalanche enhancement function according to claim 6, It is characterized in that The ion implantation temperature in step 3 is 450°C to 550°C.
9. The method for manufacturing a SiC light-triggered thyristor with avalanche enhancement function according to claim 6, It is characterized in that The growth temperature of the chemical vapor deposition method CVD in step 4 is 1400°C to 1500°C.
10. The method for manufacturing a SiC light-triggered thyristor with avalanche enhancement function according to claim 6, It is characterized in that The annealing temperature in step 7 is 1650°C to 1800°C.