Method for preparing high-quality CsPbBr3 film through two-step method in air

By spin-coating PbBr2 and CsBr in the air with two-step method, the problem of preparing high-quality CsPbBr3 films in the air is solved, and the preparation and cost saving of high-quality films are achieved, and the photoluminescent performance is improved.

CN118943258APending Publication Date: 2024-11-12CHINA JILIANG UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411028220.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The prior art is difficult to prepare high-quality cesium-based perovskite CsPbBr3 films in the air, and are easily affected by air humidity, resulting in poor film quality.

Method used

The two-step spin coating method is used to spin coating PbBr2 film in the air, and then spin coating is used to form CsPbBr3 film with isopropanol and deionized water mixed solvent to form CsPbBr3 film, and the spin coating speed and annealing temperature are adjusted to improve the crystallinity of the film and Uniformity.

Benefits of technology

The high-quality and uniform CsPbBr3 film is prepared in the air, which reduces production costs and improves the photoluminescence brightness and grain regularity of the film.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure FT_2
    Figure FT_2
  • Figure FT_3
    Figure FT_3
Patent Text Reader

Abstract

Aiming at the problem of how to prepare the high-quality CsPbBr3 thin film in the air, the invention provides a method for preparing the high-quality CsPbBr3 thin film by a two-step method, the preparation method is a two-step spin-coating method, PbBr2 is spin-coated in the air, then CsBr dissolved by a mixed solvent of isopropanol and deionized water is spin-coated on the PbBr2 thin film, and finally the CsPbBr3 thin film is formed. The high-quality CsPbBr3 film is prepared in the air by adjusting the ratio of isopropanol to deionized water in the CsBr mixed solvent. And the prepared film has the advantages of good uniformity, high crystal quality, few defect states and good photoluminescence characteristic.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of electroluminescence, and in particular to a method for preparing a high-quality CsPbBr3 thin film in air by a two-step method. Background Art

[0002] Perovskite material is an ABX3 type structural material. The A position is generally a metal cation such as a rare earth or alkaline earth element or a methylamine, a formamidinium cation, or a long-chain amine ion. The B position is a transition element ion (Pb, Sn, etc.), and the X position is a halogen ion (Cl - Br - ,I - One or more combinations thereof). Perovskite materials have very excellent optoelectronic properties, such as excellent carrier transport performance, high luminous efficiency and high color purity, and the luminescent wavelength (390-790nm) can be adjusted by doping with halogen ions. However, most perovskite films are mainly prepared in inert gases, which is not conducive to reducing production costs. In addition, since formamidine and methylamine perovskites are easily affected by air humidity, it is difficult to prepare high-quality perovskite crystals in the air. For cesium-based perovskite materials, especially CsPbBr3 materials, due to their all-inorganic characteristics, they have good air stability. However, when a one-step process is used to prepare cesium-based perovskite films in the air, the crystallization process is also easily affected by water vapor in the air, and the film quality is very poor. Summary of the invention

[0003] The invention aims at the problem of how to prepare a high-quality CsPbBr3 film in air, and provides a two-step method for preparing a high-quality CsPbBr3 film. The preparation method is a two-step spin coating method, firstly spin coating PbBr2 in air, and then spin coating CsBr dissolved in a mixed solvent of isopropyl alcohol and deionized water on the PbBr2 film, and finally forming a CsPbBr3 film. The prepared film has good uniformity, high crystal quality and few defect states.

[0004] To achieve the above object, the technical solution adopted by the present invention is:

[0005] A method for preparing high-quality CsPbBr3 thin film in air in two steps, the method for preparing high-quality CsPbBr3 thin film in air in two steps comprises spin coating PbBr2 and CsBr in sequence;

[0006] The CsBr precursor solution is prepared by mixing isopropanol and deionized water in different proportions;

[0007] The PbBr2 precursor solution uses N,N-dimethylformamide and dimethyl sulfoxide;

[0008] The light-emitting layer material is CsPbBr3.

[0009] In the present invention, all-inorganic CsPbBr3 is used as the light-emitting layer thin film material, PbBr2 is spin-coated in the air to form a PbBr2 thin film, and an isopropanol / deionized water mixed solvent solution of CsBr is spin-coated on the PbBr2 thin film to form a high-quality CsPbBr3 thin film. On the one hand, the quality of the first deposited PbBr2 film affects the quality of the final CsPbBr3 thin film, so that the CsPbBr3 thin film can be regulated. By regulating the crystallinity of the thin film, a thin film with regular grain size and uniform distribution is obtained. Compared with the CsPbBr3 thin film prepared by the traditional one-step spin coating method, the film quality is greatly improved.

[0010] Preferably, the PbBr2 precursor solution is N,N-dimethylformamide, because it has very good solubility for PbBr2, and the formed PbBr2 film is not affected by water and oxygen;

[0011] The annealing temperature and spin coating speed can be changed according to the actual morphology of the CsPbBr3 film;

[0012] The processing conditions of the PbBr2 film are spin coating and placement in an air environment;

[0013] The film carrier substrate is glass, and a layer of transparent PbBr2 film is first spin-coated. The initially deposited PbBr2 film affects the thickness of the CsPbBr3 film. If the PbBr2 film is thin, the film formed will be locally uneven. If the PbBr2 film is thick, the formed CsPbBr3 film will have many impurities, and some PbBr2 cannot be converted into CsPbBr3 film. After spin-coating PbBr2, proper annealing of PbBr2 is conducive to the subsequent reaction of the PbBr2 film with the CsBr solution to form a high-quality CsPbBr3 film. If the annealing temperature of the PbBr2 film is too high, the surface of the PbBr2 film will show more white spots, and the photoluminescence of the CsPbBr3 film obtained after the CsBr solution is coated is basically not bright. The thickness of the perovskite luminescent layer formed by the CsPbBr3 film is 100-300nm. Too thin will lead to the narrowing of the recombination center and low device efficiency. Too thick will reduce the current, affect the electroluminescence brightness, and waste materials.

[0014] The CsPbBr3 film can also be prepared by immersion. The prepared PbBr2 film can be directly placed in a container containing a CsBr solvent, and after immersion for a certain period of time, it is blown dry with an inert gas stream to obtain a CsPbBr3 film with regular grain size and uniform distribution.

[0015] The certain soaking time is: 1min-5min.

[0016] Preferably, the CsBr precursor solution is a mixed solvent of isopropanol / deionized water and the ratio of isopropanol to deionized water is 9:1. The isopropanol / deionized water mixed solvent promotes the dissolution of CsBr and affects the quality of the subsequent CsPbBr3 film. Using a single isopropanol solvent, due to the low solubility of CsBr in isopropanol, this may limit the concentration of CsBr in the precursor solution. Low-concentration CsBr solution may cause the growth rate of the film to be unstable, resulting in poor crystal quality, and the rapid volatilization of isopropanol makes the density of the formed CsPbBr3 film very poor; while using a single deionized water solvent, due to the high solubility of CsBr in deionized water, the reaction with PbBr2 is violent and uncontrollable, and the volatility of deionized water is relatively poor, so the CsPbBr3 film formed by dissolving CsBr in a single solvent has poor quality. When the ratio of deionized water in the mixed solvent of isopropanol and deionized water is more than 1:9, the excess deionized water can further increase the solubility of CsBr, but the reduction in the amount of isopropanol slows down the nucleation rate of the CsPbBr3 film, resulting in poor crystallinity and irregular grain size of the CsPbBr3 film. When the ratio of deionized water in the mixed solvent of isopropanol and deionized water is less than 1:9, the solubility of CsBr becomes lower, and the isopropanol that occupies the main solvent component will evaporate quickly, causing the CsPbBr3 film to show local unevenness. Therefore, the precursor solvent of CsBr requires a certain amount of deionized water and isopropanol to form a high-quality CsPbBr3 film.

[0017] Compared with the prior art, the present invention has the following beneficial effects:

[0018] (1) The perovskite film prepared by the two-step method can be spin-coated in air throughout the process, avoiding the use of an inert gas glove box and saving costs.

[0019] (2) The two-step method for preparing high-quality CsPbBr3 thin films in air of the present invention is simple, reduces the complexity of the preparation process, can use existing mature equipment and technology, and has better reproducibility of the film. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 The flowchart of the method for preparing high-quality CsPbBr3 thin film in air by two-step method of the present invention is shown in the figure, wherein a layer of PbBr2 is firstly spin-coated on the substrate; and CsBr is spin-coated in the second step to directly form a CsPbBr3 thin film.

[0021] Figure 2 This is a scanning electron microscope (SEM) image of a CsPbBr3 thin film prepared by the two-step method in Example 1 with a CsBr mixed solvent of (isopropanol: deionized water = 9:1).

[0022] Figure 3 This is a scanning electron microscope (SEM) image of a CsPbBr3 thin film prepared by the two-step method in Example 2 with the CsBr solvent being a single solvent (isopropanol).

[0023] Figure 4 This is a scanning electron microscope (SEM) image of the CsPbBr3 film prepared by the two-step method in Comparative Example 1 with a CsBr mixed solvent of (isopropanol: deionized water = 7:3).

[0024] Figure 5 This is a scanning electron microscope (SEM) image of the CsPbBr3 thin film prepared by the two-step method in Comparative Example 2 and the CsBr solvent is a single solvent (deionized water).

[0025] Figure 6 Graph showing the photoluminescence intensity of the embodiment and the comparative example. DETAILED DESCRIPTION

[0026] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention is further described in detail below in conjunction with embodiment. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention. Those skilled in the art can make modifications or equivalent substitutions based on the understanding of the technical scheme of the present invention without departing from the spirit and scope of the technical scheme of the present invention, and all should be included in the protection scope of the present invention.

[0027] The present invention discloses a method for preparing high-quality CsPbBr3 thin film in air by two-step method. The coating method is as follows: Figure 1 As shown: a layer of PbBr2 film is first prepared by spin coating in the air, and a CsBr solution mixed with deionized water and isopropanol is spin coated on the prepared PbBr2 film. The CsBr in the solution reacts with the PbBr2 film to generate high-quality CsPbBr3.

[0028] Example 1

[0029] The film preparation is described as: glass substrate / CsPbBr3 film, and the preparation method includes the following steps:

[0030] 1) The glass substrate was ultrasonically cleaned for 10 minutes using D90 cleaning solution, deionized water, anhydrous ethanol, and isopropanol in sequence, then dried using a nitrogen gun, and finally cleaned in a plasma cleaning machine for 15 minutes.

[0031] 2) Prepare the perovskite precursor solution: use 1 ml of N,N-dimethylformamide as solvent and 50 mg of PbBr2 as solute; use 0.9 ml of isopropanol and 0.1 ml of deionized water as solvent and 8 mg of CsBr as solute, stir at room temperature overnight for use.

[0032] The substrate treated in step 1 was transferred to a fume hood in an air environment, and placed on a spin coater bracket. The prepared PbBr2 precursor solution was evenly dropped on the substrate. The spin coater was adjusted to rotate at 6000 rpm for 50 seconds, and then heated on a hot plate at 50 degrees Celsius for 10 minutes to obtain a PbBr2 layer. The prepared substrate containing the PbBr2 layer was cooled to room temperature, and the prepared CsBr precursor solution was evenly dropped on the substrate, and rotated at 3000 rpm for 40 seconds to form a layer of CsPbBr3 perovskite film. The morphology of this layer was observed by scanning electron microscopy as follows: Figure 2 As shown, the grains are evenly distributed and the film quality is good.

[0033] The green light CsPbBr3 film prepared in this embodiment was irradiated with ultraviolet light, and the brightness was observed to find that the film was very bright. The SEM image was observed to find that the grains were large and there were more nuclei. The surface grains of the film were regular and evenly distributed, indicating that this ratio of precursor solution is helpful to form a high-quality CsPbBr3 film with increased grain size and regular grains.

[0034] Example 2

[0035] The film preparation is described as: glass substrate / CsPbBr3 film, and the preparation method includes the following steps:

[0036] 1) The glass substrate was ultrasonically cleaned for 10 minutes using D90 cleaning solution, deionized water, anhydrous ethanol, and isopropanol in sequence, then dried using a nitrogen gun, and finally cleaned in a plasma cleaning machine for 15 minutes.

[0037] 2) Prepare the perovskite precursor solution: use 1 ml of N,N-dimethylformamide as solvent and 50 mg of PbBr as solute; use 1 ml of isopropanol as solvent and 8 mg of CsBr as solute, stir at room temperature overnight for use.

[0038] The substrate treated in step 1 was transferred to a fume hood in an air environment, placed on a spin coater bracket, the prepared PbBr2 precursor solution was evenly dropped on the substrate, and rotated at 6000 rpm for 50 seconds, and then heated on a hot plate at 50 degrees Celsius for 10 minutes to obtain a PbBr2 layer. The prepared substrate containing the PbBr2 layer was cooled to room temperature, and the prepared CsBr precursor solution was evenly dropped on the substrate, and rotated at 3000 rpm for 40 seconds to form a perovskite film composed of CsPbBr3. The morphology of this layer was observed by scanning electron microscopy as follows Figure 2 As shown, a large number of agglomerated particles were produced.

[0039] The green light CsPbBr3 film prepared in this example was irradiated with an ultraviolet lamp, and the brightness was observed to find that the film was relatively bright, but the film was yellowish as a whole and uneven in some parts.

[0040] Comparative Example 1

[0041] The film preparation is described as: glass substrate / CsPbBr3 film, and the preparation method includes the following steps:

[0042] 1) The glass substrate was ultrasonically cleaned for 10 minutes using D90 cleaning solution, deionized water, anhydrous ethanol, and isopropanol in sequence, then dried using a nitrogen gun, and finally cleaned in a plasma cleaning machine for 15 minutes.

[0043] 2) Prepare the perovskite precursor solution: Prepare the perovskite precursor solution: use 1 ml of N,N-dimethylformamide as solvent and 50 mg of PbBr2 as solute; use 0.7 ml of isopropanol and 0.3 ml of deionized water as solvent and 8 mg of CsBr as solute, stir at room temperature overnight for use.

[0044] The substrate treated in step 1 was transferred to a fume hood in an air environment, and placed on a spin coater bracket. The prepared PbBr2 precursor solution was evenly dropped on the substrate, and the substrate was rotated at 6000 rpm for 50 seconds, and then heated on a hot plate at 50 degrees Celsius for 10 minutes to obtain a PbBr2 film. The prepared substrate containing the PbBr2 film was cooled to room temperature, and the prepared CsBr precursor solution was evenly dropped on the substrate, and the substrate was rotated at 3000 rpm for 40 seconds to form a layer of CsPbBr3 perovskite film.

[0045] The SEM image of the green CsPbBr3 film prepared in this comparative example shows that the grain distribution is relatively dispersed, and the whole is in a clustered state. This state may be that the PbBr2 has not reacted completely and is aggregated with the formed perovskite crystals. Its photoluminescence properties are as follows Figure 6 As shown, the brightness is lower than that of Examples 1 and 2, indicating that the ratio of isopropanol: deionized water in the CsBr precursor solution is 7:3, the crystallization effect is poor, the number of nuclei is small, and the formed perovskite grains are dispersed. The weak photoluminescence may be due to the fact that PbBr2 is not completely reacted by CsBr, resulting in its weak photoluminescence.

[0046] Comparative Example 2

[0047] The film preparation is described as: glass substrate / CsPbBr3 film, and the preparation method includes the following steps:

[0048] 1) The glass substrate was ultrasonically cleaned for 10 minutes using D90 cleaning solution, deionized water, anhydrous ethanol, and isopropanol in sequence, then dried using a nitrogen gun, and finally cleaned in a plasma cleaning machine for 15 minutes.

[0049] 2) Prepare the perovskite precursor solution: Prepare the perovskite precursor solution: use 1 ml of N,N-dimethylformamide as solvent and 50 mg of PbBr2 as solute; use 1 ml of deionized water as solvent and 8 mg of CsBr as solute, stir at room temperature overnight for use.

[0050] The substrate treated in step 1 was transferred to a fume hood in an air environment, and placed on a spin coater bracket. The prepared PbBr2 precursor solution was evenly dropped on the substrate, and the substrate was rotated at 6000 rpm for 50 seconds, and then heated on a hot plate at 50 degrees Celsius for 10 minutes to obtain a PbBr2 film. The prepared substrate containing the PbBr2 film was cooled to room temperature, and the prepared CsBr precursor solution was evenly dropped on the substrate, and the substrate was rotated at 3000 rpm for 40 seconds to form a layer of CsPbBr3 perovskite film.

[0051] The SEM image of the green CsPbBr3 film prepared in this comparative example shows that the grains are dispersed and appear long strips overall. This state may be due to the high proportion of water in the CsBr precursor, which affects the nucleation of the perovskite film and results in the failure to form good perovskite grains. Figure 6 As shown, the brightness is lower than that of Examples 1, 2 and Comparative Example 1, indicating that the crystallization effect of the CsPbBr3 thin film formed by the CsBr precursor solution using a single solvent water is very poor, and the number of nucleations is very small. Such grains may cause lattice strain, surface and grain boundary defects of the perovskite, which is not conducive to the preparation of green light CsPbBr3 thin films.

[0052] From Example 1 and Example 2, we can see that the solvent of CsBr can also be replaced by a single solvent, isopropanol, and a green light CsPbBr3 film can be prepared. After testing, the film prepared by the mixed solvent of isopropanol and water used in the CsBr precursor solution in Example 1 shows more regular grain size, better film morphology and higher photoluminescence intensity. The photoluminescence brightness of the optoelectronic devices prepared in Example 1 and Comparative Examples 1-2 and the surface morphology of the film were tested, and the results are shown in Table 1. Compared with Comparative Example 1, Example 1 uses a trace amount of water as the CsBr solvent, which has a better grain distribution and higher photoluminescence brightness, and forms more perovskite grains under the same scanning electron microscope, making the film grain size more regular. Compared with Comparative Example 2, Example 1 uses a small amount of water as the CsBr solvent, and the film formed by using a single solvent water in Comparative Example 2 has higher photoluminescence brightness, more regular grains, and better film surface morphology. In contrast, in Comparative Example 1 and Comparative Example 2, different proportions of water are added to the CsBr precursor solution. The morphology and luminescence performance of the CsPbBr3 film prepared by using only water as the CsBr solvent are worse. Figure 6The photoluminescence diagrams of the embodiments and the comparative examples are shown.

Claims

1. A method for preparing high-quality CsPbBr3 thin film in air by two steps, characterized in that: include: Prepare PbBr2 and CsBr perovskite precursor solutions respectively; A PbBr2 film is prepared by spin coating, the PbBr2 film is annealed, and a CsBr solution is spin coated on the PbBr2 film to obtain a perovskite film; The solvent of the PbBr2 precursor solution is dimethyl sulfoxide, N,N-dimethylformamide or a mixed solvent of the two, and the solvent of the CsBr perovskite precursor solution is a mixed solvent of isopropanol and deionized water.

2. The method for preparing high-quality CsPbBr3 thin film in air by two-step method according to claim 1, characterized in that: The preparation of PbBr2 and CsBr perovskite precursor liquids comprises: And / or, the CsBr is dissolved by adding isopropanol and deionized water in different proportions, and stirred at a certain temperature for a certain time; And / or, the PbBr2 is dissolved in a solvent and stirred at a certain temperature for a certain period of time.

3. The method for preparing high-quality CsPbBr3 thin film in air by two-step method according to claim 2, characterized in that: The certain stirring temperature is 30°C-80°C, and the certain time is 5 minutes-2 hours.

4. The method for preparing high-quality CsPbBr3 thin film in air by two-step method according to claim 1, characterized in that: The cleaning of the glass substrate comprises: First, the glass substrate is wiped with ethanol and deionized water, and the surface of the substrate is ultrasonically cleaned with an organic solvent to remove excess dust and grease on the surface, and finally dried with an inert gas.

5. The method for preparing high-quality CsPbBr3 thin film in air by two-step method according to any one of claims 1 to 4, characterized in that: Includes steps: Step 1, cleaning and plasma treating the glass substrate; Step 2: Spin-coat a certain concentration of PbBr2 solution on a glass substrate to prepare a thin film, and spin-coat a certain concentration of CsBr on the PbBr2 film, so that the two react chemically to prepare a CsPbBr3 perovskite film.

6. The method for preparing high-quality CsPbBr3 thin film in air by two-step method according to claim 5, characterized in that: Step 2 specifically includes: The PbBr2 film needs to be annealed at a certain temperature for a certain period of time to be prepared.

7. The method for preparing high-quality CsPbBr3 thin film in air by two-step method according to claim 5, characterized in that: The concentration of the PbBr2 solution is 10-100 mg / ml, and the concentration of the CsBr solution is 2-20 mg / ml.

8. The method for preparing high-quality CsPbBr3 thin film in air by two-step method according to claim 6, characterized in that: The certain annealing temperature is 50°C-150°C, and the certain time is 1 minute-3 hours.

9. The method for preparing high-quality CsPbBr3 thin film in air by two-step method according to any one of claims 1 to 4, characterized in that: CsBr is dissolved in a mixed solvent of deionized water and isopropanol with a ratio of 9:1-1:9.