Negative electrode for rechargeable lithium battery and rechargeable lithium battery including same
By using copolymer binder, Si-C composite and crystalline carbon in the negative electrode material of rechargeable lithium batteries, and using magnetic field orientation technology, the volume expansion problem of the negative electrode material during charging and discharging is solved, and the energy is improved Density and cycle life.
Patent Information
- Application Number
- CN202410269798.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-05-10
- Filing Date
- 2024-03-11
- Publication Date
- 2024-11-12
AI Technical Summary
The negative electrode materials of existing rechargeable lithium batteries have volume expansion problems during charging and discharging, which affects the energy density and cycle life.
The negative electrode active material layer including copolymer binder, Si-C composite and crystalline carbon is used to improve the orientation of the negative electrode active material through magnetic field orientation technology, reduce volume expansion, and enhance adhesion.
It effectively suppresses the volume expansion of the negative electrode material, improves the energy density and cycle life, and ensures the stability and adhesion of the negative electrode active material layer.
Smart Images

Figure CN118943293A_ABST
Abstract
Description
Technical Field
[0001] One or more embodiments of the present disclosure relate to a negative electrode for a rechargeable lithium battery and a rechargeable lithium battery including the negative electrode. Background Art
[0002] Rechargeable lithium batteries that have recently attracted attention as power sources for small portable electronic devices utilize an organic electrolyte solution and thus have a discharge voltage twice or more as high as that of batteries utilizing an alkaline aqueous solution and thus have a relatively high energy density.
[0003] Research on silicon negative active materials having a high discharge specific capacity of about 3400 mAh / g and capable of rapidly combining with lithium ions and rapidly charging and discharging has been actively conducted for rechargeable lithium batteries. Summary of the invention
[0004] One or more aspects of embodiments of the present disclosure relate to a negative electrode for a rechargeable lithium battery that exhibits good or suitable energy density and improved expansion characteristics.
[0005] One or more aspects of an embodiment of the present disclosure relate to a rechargeable lithium battery including the negative electrode.
[0006] Additional aspects will be set forth in part in the description which follows and, in part, will be obvious from the description, or may be learned by practice of the disclosed presented embodiments.
[0007] According to one or more embodiments of the present disclosure, a negative electrode for a rechargeable lithium battery includes: a current collector; and a negative active material layer, on the current collector, and including a copolymer binder, a Si-C composite first negative active material (e.g., in the form of particles) and a crystalline carbon second negative active material (e.g., in the form of particles), wherein the copolymer binder includes a first repeating unit derived from a (meth)acrylic monomer and a second repeating unit derived from a (meth)acrylonitrile monomer, and the negative electrode has a DD (divergence) value defined by Equation 1 of about 30 or greater.
[0008] Equation 1
[0009] DD(divergence)=(I a / I 总 )×100
[0010] in,
[0011] I a is the sum of the peak intensities at 2θ=42.4±0.2°, 43.4±0.2°, 44.6±0.2° and 77.5±0.2° measured by X-ray diffraction (XRD) using Cu Kα rays, and
[0012] I 总 It is the sum of peak intensities at 2θ=26.5±0.2°, 42.4±0.2°, 43.4±0.2°, 44.6±0.2°, 54.7±0.2° and 77.5±0.2° measured by XRD using Cu Kα rays.
[0013] According to one or more embodiments of the present disclosure, there is provided a rechargeable lithium battery including: a negative electrode; a positive electrode including a positive active material; and a non-aqueous electrolyte.
[0014] Other embodiments are included in the detailed description below.
[0015] The negative electrode of one or more embodiments of the present disclosure for a rechargeable lithium battery may exhibit improved expansion characteristics. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] The accompanying drawings are included to provide a further understanding of the disclosure and are incorporated in and constitute a part of this specification. The drawings illustrate example embodiments of the disclosure and together with the description serve to explain the principles of the disclosure.
[0017] Figure 1 is a schematic diagram showing the orientation of a negative active material on a negative electrode according to one or more embodiments of the present disclosure.
[0018] Figure 2 is a schematic diagram illustrating the orientation of a negative electrode according to one or more embodiments of the present disclosure.
[0019] Figure 3 A process for imparting orientation in negative electrode preparation according to one or more embodiments of the present disclosure is schematically illustrated.
[0020] Figure 4 is a schematic diagram illustrating the structure of a rechargeable lithium battery according to one or more embodiments of the present disclosure.
[0021] Figure 5 is an image of a disassembled rechargeable lithium battery cell according to Example 6 after formation charge and discharge.
[0022] Figure 6 is an image of a disassembled rechargeable lithium battery cell according to Reference Example 1 after undergoing formation charge and discharge. DETAILED DESCRIPTION
[0023] The present disclosure can be modified in many alternative forms, and therefore specific embodiments will be illustrated in the drawings and described in more detail. However, it should be understood that it is not intended to limit the present disclosure to the particular forms disclosed, but on the contrary, it is intended to cover all modifications, equivalents and substitutes falling within the spirit and scope of the present disclosure.
[0024] Hereinafter, embodiments of the present disclosure will be described in more detail. However, these embodiments are merely examples, and the present disclosure is not limited thereto, and the present disclosure is defined by the scope of the claims and their equivalents.
[0025] The terms used in the present disclosure are used to explain the embodiments, but are not intended to limit the present disclosure. As used herein, the singular forms "a", "an", and "the" are also intended to include the plural forms unless the context clearly indicates otherwise. In addition, when describing embodiments of the present disclosure, the use of "may" refers to "one or more embodiments of the present disclosure".
[0026] The term "combinations thereof" may include mixtures, stacks, composites, copolymers, alloys, blends, reactants of components.
[0027] The terms "comprises," "includes," or "has" are intended to indicate the presence of a certain characteristic, quantity, step, constituent element, or combination thereof, but it should be understood that the possibility of the presence or addition of one or more other characteristics, quantities, steps, constituent elements, or combinations thereof is not precluded.
[0028] In the present disclosure, when no definition is otherwise provided, it will be understood that when an element such as a layer, film, region, or substrate is referred to as being “on” another element, it can be directly on the other element or intervening elements may be present therebetween.
[0029] As used herein, "A and / or B" may mean "A or B or both of them (e.g., simultaneously)". In addition, the " / " used herein may be interpreted as "and" or as "or", depending on the circumstances. Expressions such as "at least one of...", "one of...", and "selected from..." when preceding / following a list of elements modify the entire list of elements without modifying individual elements of the list. For example, "at least one of a, b, and c", "at least one selected from a, b, and c", "at least one selected from a to c", etc. may mean only a, only b, only c, both a and b (e.g., simultaneously), both a and c (e.g., simultaneously), both b and c (e.g., simultaneously), all of a, b, and c, or variations thereof.
[0030] When an element such as a layer, film, region, and / or plate is referred to as being “on” or “over” another element, it may include the case where the element is “directly on” the other element, and may include the case where another element (e.g., an intervening element) is present between the element and the other element. In contrast, when an element is referred to as being “directly on” another element, there are no intervening elements.
[0031] As used herein, the term "particle size" or "particle diameter" may be an average particle diameter. If the particle has a spherical shape (e.g., when the particle has a spherical shape), the particle size / particle diameter may refer to the diameter of the particle, and if the particle has a non-spherical shape (e.g., when the particle has a non-spherical shape), the particle size / particle diameter may refer to the size (e.g., length) of the longer axis (e.g., major axis) of the particle.
[0032] When no definition is provided in the specification, the average particle size / particle size represents the average particle size / particle size (D50) of about 50 volume % in the cumulative volume in the particle size distribution. Particle size / particle size and average particle size (D50) can be measured by a method that is very suitable for those skilled in the art (e.g., by a particle size analyzer, or by a transmission electron microscope image, a scanning electron microscope image or a field emission scanning electron microscope (FE-SEM)). In certain embodiments, a dynamic light scattering measurement device can be used for data analysis, and the number of particles is counted for each size range, and according to the data, the average particle size / particle size (D50) value can be easily obtained by calculation. In certain embodiments, a laser diffraction method can be used. The particles to be measured can be distributed in a distribution solvent and introduced into a commercially available laser diffraction particle measurement device (e.g., MT 3000 available from Microtrac, Inc.), an ultrasonic wave of about 28kHz is irradiated with a power of 60W, and the average particle size / particle size (D50) of 50% standard particle distribution is calculated in a measuring device to obtain laser diffraction.
[0033] According to one or more embodiments, a negative electrode for a rechargeable lithium battery includes: a current collector (e.g., a negative electrode current collector); and a negative electrode active material layer, which is on the current collector and includes a copolymer binder, a Si-C composite first negative electrode active material (e.g., in the form of particles) and a crystalline carbon second negative electrode active material (e.g., in the form of particles).
[0034] The copolymer binder includes a first repeating unit derived from a (meth) acrylic monomer and a second repeating unit derived from a (meth) acrylonitrile monomer. In one or more embodiments, the copolymer binder may also include a third repeating unit derived from another monomer copolymerizable with the (meth) acrylic monomer and / or the (meth) acrylonitrile monomer.
[0035] In one or more embodiments, "(meth)" may mean including or excluding a methyl group. For example, (meth)acrylic acid means methacrylic acid or acrylic acid.
[0036] Based on the amount of 100wt% of the copolymer binder, the amount of the first repeating unit derived from the (meth) acrylic monomer may be about 35wt% to about 65wt% or about 40wt% to about 65wt%. In the copolymer binder, if the amount of the first repeating unit derived from the (meth) acrylic monomer is within this range (for example, when the amount of the first repeating unit derived from the (meth) acrylic monomer is within this range), the distribution of the negative active material can be further improved, and the storage stability of the negative active material composition (for example, the negative active material layer composition) used in the preparation of the negative electrode can be further improved.
[0037] Based on the amount of 100wt% of the copolymer binder, the amount of the second repeating unit derived from the (meth) acrylonitrile monomer may be about 35wt% to about 65wt% or about 35wt% to about 60wt%. In the copolymer binder, if the amount of the second repeating unit derived from the (meth) acrylonitrile monomer is within this range (for example, when the amount of the second repeating unit derived from the (meth) acrylonitrile monomer is within this range), the negative electrode can be more easily prepared, the negative active material layer can be more firmly adhered to the current collector, and the storage safety of the negative active material composition used in the preparation of the negative electrode can be further improved.
[0038] In one or more embodiments, the (meth)acrylic acid monomer may be (meth)acrylic acid, an alkali metal salt or alkaline earth metal salt of (meth)acrylic acid, an ammonium salt of (meth)acrylic acid, or one or more combinations thereof. The alkali metal salt or alkaline earth metal salt of (meth)acrylic acid may be sodium acrylate, lithium acrylate, potassium acrylate, calcium acrylate, magnesium acrylate, sodium (meth)acrylate, lithium (meth)acrylate, potassium (meth)acrylate, calcium (meth)acrylate, or one or more combinations thereof. The ammonium salt of (meth)acrylic acid may be an ammonia neutralization product of (meth)acrylic acid, a monoethanolamine neutralization product of (meth)acrylic acid, a diethanolamine neutralization product of (meth)acrylic acid, a hydroxylamine neutralization product of (meth)acrylic acid, or one or more combinations thereof.
[0039] In one or more embodiments, the copolymer binder may further include a third repeating unit derived from another monomer copolymerizable with the (meth)acrylic monomer and / or the (meth)acrylonitrile monomer.
[0040] The other monomers copolymerizable with the (meth) acrylic monomer and / or the (meth) acrylonitrile monomer may include hydroxyl-containing monomers or amide-containing monomers. The hydroxyl-containing monomer may be, for example, 2-hydroxyethyl (meth) acrylate, 2-hydroxypropyl (meth) acrylate, 4-hydroxybutyl (meth) acrylate, 2-hydroxyhexyl (meth) acrylate, 6-hydroxyhexyl (meth) acrylate, 8-hydroxyoctyl (meth) acrylate, 10-hydroxydecyl (meth) acrylate, 12-hydroxylauryl (meth) acrylate, (4-hydroxymethylcyclohexyl) methacrylate, N-hydroxymethyl (meth) acrylamide, N-hydroxy (meth) acrylamide, vinyl alcohol, allyl alcohol, 2-hydroxyethyl vinyl ether, 4-hydroxybutyl vinyl ether, diethylene glycol monovinyl ether, or one or more combinations thereof. The amide group-containing monomer can be, for example, acrylamide, methacrylamide, diethyl(meth)acrylamide, N-vinylpyrrolidone, N-vinyl-2-pyrrolidone, N-(meth)acryloylpyrrolidone, N,N-dimethylacrylamide, N,N-dimethylmethacrylamide, N,N-diethylacrylamide, N,N-diethylmethacrylamide, N,N'-methylenebisacrylamide, N,N-dimethylaminopropylacrylamide, N,N-dimethylaminopropylmethacrylamide, or one or more combinations thereof.
[0041] If the copolymer binder further includes a third repeating unit derived from another monomer copolymerizable with the (meth)acrylic monomer and / or the (meth)acrylonitrile monomer (for example, when the copolymer binder further includes a third repeating unit derived from another monomer copolymerizable with the (meth)acrylic monomer and / or the (meth)acrylonitrile monomer), the amount of the third repeating unit may be greater than 0 wt % and about 20 wt % or less, based on 100 wt % of the amount of the copolymer binder.
[0042] Here, in one or more embodiments, the amount of the first repeating unit or the second repeating unit may be appropriately adjusted. For example, in some embodiments, the amount of the first repeating unit or the second repeating unit may be about 35 wt % or more and less than about 65 wt %.
[0043] If the copolymer binder further includes a third repeating unit (eg, when the copolymer binder further includes a third repeating unit), electrode expansion of the negative electrode may be more effectively suppressed or reduced.
[0044] In one or more embodiments, the copolymer binder may be a water-soluble copolymer for dispersion stability of the copolymer. The copolymer binder may have a viscosity of about 500 mPa·s to about 3000 mPa·s, about 750 mPa·s to about 2500 mPa·s, about 750 mPa·s to about 2000 mPa·s, about 750 mPa·s to about 1500 mPa·s, or about 1000 mPa·s to about 1500 mPa·s in an aqueous solution having a solid content (e.g., amount) of about 7 wt%. If the viscosity of the copolymer binder in an aqueous solution having a solid content (e.g., amount) of about 7 wt% is within this range (e.g., when the viscosity of the copolymer binder in an aqueous solution having a solid content (e.g., amount) of about 7 wt% is within this range), the adhesion of the negative active material layer to the current collector may be further improved, and the cycle life characteristics of the rechargeable lithium battery may be further improved.
[0045] The viscosity can be measured using a Brookfield viscometer with a LV4 rotor at 20 to 530 rpm and room temperature (20 to 25° C.), but is not limited thereto. For example, the viscosity can be measured using a Brookfield viscometer with a LV4 rotor at 30 rpm and room temperature (25° C.).
[0046] In one or more embodiments, the copolymer binder may include a copolymer of acrylic acid and acrylonitrile.
[0047] In one or more embodiments, the copolymer binder may have a weight average molecular weight (Mw) of about 100,000 g / mol to about 1500,000 g / mol or about 500,000 g / mol to about 1,000,000 g / mol. In one or more embodiments, the weight average molecular weight (Mw) may be measured by GPC (gel permeation chromatography).
[0048] In one or more embodiments, the negative electrode may have a DD (Degree of Divergence) value defined by Equation 1 of about 30 or greater, about 30 to about 60, about 30 to about 55, about 35 to about 55, or about 40 to about 55.
[0049] Equation 1
[0050] DD(divergence)=(I a / I 总 )×100
[0051] In equation 1,
[0052] I a is the sum of the peak intensities at non-planar angles measured by XRD using Cu Kα radiation, and
[0053] I 总 It is the sum of the peak intensities at all angles measured by XRD using Cu Kα radiation.
[0054] When measured by XRD using Cu Kα rays, the non-plane angles represent 2θ=42.4±0.2°, 43.4±0.2°, 44.6±0.2°, and 77.5±0.2°, i.e., (100) plane, (101) R plane, (101) H plane, and (110) plane. In the art, graphite has a structure classified into a rhombus structure and a hexagonal structure having an ABAB type or kind of stacking order according to the stacking order of graphene layers, and the R plane represents the rhombus structure, while the H plane represents the hexagonal structure.
[0055] Therefore, I a It may be the sum of peak intensities at 2θ=42.4±0.2°, 43.4±0.2°, 44.6±0.2°, and 77.5±0.2° when measured by XRD using Cu Kα rays.
[0056] When measured by XRD using Cu Kα rays, all angles represent 2θ=26.5±0.2°, 42.4±0.2°, 43.4±0.2°, 44.6±0.2°, 54.7±0.2° and 77.5±0.2°, i.e., (002) plane, (100) plane, (101)R plane, (101)H plane, (004) plane and (110) plane. In some embodiments, the peak at 2θ=43.4±0.2° can also be considered to occur by overlapping the peak of the (101)R plane of the carbon-based material with another peak of the (111) plane of the current collector (e.g., Cu).
[0057] Therefore, I 总 It may be the sum of peak intensities at 2θ=26.5±0.2°, 42.4±0.2°, 43.4±0.2°, 44.6±0.2°, 54.7±0.2°, and 77.5±0.2° measured by XRD using Cu Kα rays.
[0058] In the art, peak intensity may represent the height of a peak or the integrated area of a peak, and according to one or more embodiments, the peak intensity represents the integrated area of a peak (ie, a peak integrated area value).
[0059] In one or more embodiments, XRD is measured under the measurement conditions of 2θ=10° to 80°, a scanning speed (° / s) (i.e., degrees per second) of 0.044 to 0.089, and a step size (° / step) of 0.013 to 0.039 by using Cu Kα rays as the target ray but removing the monochromator to improve the peak intensity resolution.
[0060] The DD value indicates that the negative electrode (negative electrode) active material included in the negative electrode active material layer is oriented at a set or predetermined angle, and a larger value indicates that the negative electrode (negative electrode) active material is well oriented. Figure 1 As schematically shown in FIG. 1 , when the negative electrode active material 3 is oriented to one side of the substrate 1 at an angle a, as the DD value increases, the angle a increases. In addition, in one or more embodiments, the DD value is maintained after charge and discharge.
[0061] In one or more embodiments, the DD value of the negative electrode may be about 30 or greater, about 30 to about 60, or about 30 to about 50. A DD value of the negative electrode of about 30 or greater indicates that the negative active material stands substantially perpendicular to the current collector at a set or predetermined angle, indicating that the negative active material layer of the negative electrode is an oriented layer (e.g., an anisotropic layer). For example, standing substantially vertically not only means standing at an angle of 90° relative to the current collector (e.g., relative to the surface of the current collector on which the negative active material layer is arranged), but also stands at an angle close to 90° (e.g., about 90°).
[0062] If the DD value of the negative electrode is less than 30 (for example, when the DD value of the negative electrode is less than 30), the negative active material layer corresponds to the non-oriented layer, or even if the negative active material layer corresponds to the oriented layer, the effect for suppressing expansion is not significant.
[0063] In one or more embodiments, the negative electrode active material 3a is positioned to the current collector 1 in the vertical direction, and therefore, during the charge and discharge of the battery including the negative electrode, volume expansion (such as Figure 2 ). Therefore, if a negative electrode active material including Si is used (for example, when a negative electrode active material including Si is used), the extreme volume expansion in the vertical direction that may occur can be effectively suppressed or reduced, which significantly reduces the thickness increase rate and prevents the negative electrode active material layer from being separated from the current collector. Therefore, the negative electrode active material including Si that can improve energy density can be easily applied to batteries.
[0064] Because the negative electrode according to one or more embodiments includes a copolymer binder as a binder, the volume expansion of the negative electrode can be more effectively suppressed or reduced, and flexibility and adhesion can be ensured in the preparation of the negative electrode. This allows the negative electrode active material layer to be prevented or reduced from detaching from the current collector even after the battery including the negative electrode is charged and discharged.
[0065] In one or more embodiments, the amount of the copolymer binder may be about 0.5 wt % to about 5 wt %, about 0.8 wt % to about 5 wt %, about 1.0 wt % to about 5 wt %, or about 1.2 wt % to about 4.0 wt %, based on the total weight of the negative active material layer (100 wt %). If the amount of the copolymer binder is within this range (e.g., when the amount of the copolymer binder is within this range), the volume expansion of the negative electrode during charging and discharging of the battery can be further reduced.
[0066] In one or more embodiments, the negative electrode active material may include a Si-C composite first negative electrode active material and a crystalline carbon second negative electrode active material, and the amount of Si may be about 1 wt% to about 20 wt% or about 3 wt% to about 20 wt% based on the total weight 100 wt% of the first negative electrode active material and the second negative electrode active material. If the negative electrode active material includes Si in an amount in the above range (for example, when the negative electrode active material includes Si in an amount in the above range), the energy density of the negative electrode can be further improved, and a high capacity can be obtained.
[0067] In one or more embodiments, the crystalline carbon second negative electrode active material (e.g., crystalline carbon-based active material) can be amorphous (e.g., irregularly shaped), plate-like, flaky, spherical or fibrous artificial graphite, natural graphite, or one or more combinations thereof.
[0068] The Si-C composite (i.e., Si-C composite negative electrode active material) may include Si and a carbon-based material. The carbon-based material may be amorphous carbon or crystalline carbon. In one or more embodiments, the Si-C composite may, for example, include a core containing Si particles and a carbon-based material around the core (e.g., around the core). The core may also include a carbon-based material. For example, in some embodiments, the Si-C composite may include a core in which Si particles are mixed with a first carbon-based material and a second carbon-based material around the core (e.g., around the core). The first carbon-based material may be different from or the same as the second carbon-based material, and may be amorphous carbon or crystalline carbon. Examples of Si-C composites may include secondary particles (i.e., aggregates) and an amorphous carbon coating layer around the aggregates (e.g., around the aggregates), and may include amorphous carbon filled between the aggregates to surround the surface of the primary particles, in which at least one Si nano primary particle is aggregated with crystalline carbon.
[0069] In the Si—C composite, the amount of Si may be adjusted to include Si in a range of about 1 wt % to about 20 wt % or about 3 wt % to about 20 wt % based on the total weight of the first and second negative active materials.
[0070] In one or more embodiments, Si (e.g., Si particles) may have a particle size of about 10 nm to about 30 μm (about 10 nm to about 1000 nm according to one or more embodiments, and about 20 nm to about 150 nm according to one or more embodiments). If the average particle size of silicon is within this range (e.g., when the average particle size of silicon is within this range), extreme volume expansion caused during charge and discharge can be suppressed or reduced, and destruction of the conductive path due to particle fragmentation can be prevented or reduced.
[0071] In one or more embodiments, the mixing ratio of the Si-C composite first negative electrode active material to the crystalline carbon second negative electrode active material may be a weight ratio of about 3:97 to about 10:90, about 3:97 to about 15:85, or about 7:93 to about 10:90. If the mixing ratio of the Si-C composite first negative electrode active material to the crystalline carbon second negative electrode active material is within this range (for example, when the mixing ratio of the Si-C composite first negative electrode active material to the crystalline carbon second negative electrode active material is within this range), a high energy density effect can be achieved, and a relatively high capacity can be obtained at the same time.
[0072] The amorphous carbon may be asphalt carbon, soft carbon, hard carbon, mesophase asphalt carbide, burned coke, carbon fiber, or one or more combinations thereof, and the crystalline carbon may be amorphous (e.g., irregularly shaped), plate-like, flaky, spherical or fibrous natural graphite, artificial graphite, or one or more combinations thereof.
[0073] In one or more embodiments, the DD value is obtained by charging and discharging a rechargeable lithium battery including a negative electrode, then disassembling the fully discharged rechargeable lithium battery to obtain the negative electrode, and measuring XRD of the negative electrode.
[0074] Charge and discharge were performed once or twice at about 0.1 C to about 0.2 C. The DD value of the negative active material layer was obtained by peeling the negative active material layer with a tape after charge and discharge to collect the negative active material layer and measuring XRD of the resulting negative active material layer attached to the current collector.
[0075] In one or more embodiments, the negative electrode active material layer may have a thickness of about 10 μm to about 100 μm. A negative electrode active material layer having a thickness within this range may have advantages associated with adhesion. In one or more embodiments, the negative electrode active material layer may be formed on at least one side of the current collector, for example, on either side or both (e.g., opposite) sides, and the thickness may be the thickness of one side of the negative electrode active material layer. For example, the thickness may be the thickness of the negative electrode active material layer on one side of the current collector. If the negative electrode active material layer is formed on both (e.g., opposite) sides of the current collector (e.g., when the negative electrode active material layer is formed on both (e.g., opposite) sides of the current collector), the entire thickness of the negative electrode active material layer included in the negative electrode may be about 20 μm to about 200 μm.
[0076] The thickness of the negative active material layer may refer to the thickness after pressurization and vacuum drying in the preparation of the negative electrode. The vacuum drying may be performed at a pressure of about 0.03 atm to about 0.06 atm at about 100°C to about 160°C.
[0077] If the negative active material layer includes a negative active material and a copolymer binder (eg, when the negative active material layer includes a negative active material and a copolymer binder), the amount of the negative active material may be about 96 wt % to about 99.2 wt % based on the total weight of the negative active material layer.
[0078] In one or more embodiments, the negative electrode active material layer may further include an aqueous binder. In the negative electrode active material layer, the amount of the copolymer binder may be about 0.8 wt % to about 5 wt % based on the total weight of the negative electrode active material layer, the amount of the negative electrode active material may be about 90 wt % to about 98.2 wt % based on the total weight of the negative electrode active material layer, and the amount of the aqueous binder may be about 1 wt % to about 5 wt % based on the total weight of the negative electrode active material layer.
[0079] In one or more embodiments, the negative electrode active material layer may further include a conductive material. In the negative electrode active material layer, the amount of the copolymer binder may be about 0.8 wt % to about 5 wt % based on the total weight of the negative electrode active material layer, the amount of the negative electrode active material may be about 85 wt % to about 97.2 wt % based on the total weight of the negative electrode active material layer, the amount of the conductive material may be about 1 wt % to about 5 wt % based on the total weight of the negative electrode active material layer, and the amount of the aqueous binder may be about 1 wt % to about 5 wt % based on the total weight of the negative electrode active material layer.
[0080] The aqueous binder can be styrene-butadiene rubber (SBR), acrylated styrene-butadiene rubber (ABR), acrylonitrile-butadiene rubber, acrylic rubber, butyl rubber, fluororubber, polyvinyl pyrrolidone, polypropylene, polyepichlorohydrin, polyphosphazene, ethylene propylene diene copolymer, polyvinyl pyridine, chlorosulfonated polyethylene, latex, polyester resin, acrylic resin, phenolic resin, epoxy resin, polyvinyl alcohol or one or more combinations thereof.
[0081] In some embodiments, the aqueous binder may also be a cellulose compound. The cellulose compound may be carboxymethyl cellulose, hydroxypropyl methyl cellulose, methyl cellulose or an alkali metal thereof. The alkali metal may be Na, K or Li.
[0082] Conductive materials may be included to provide electrode conductivity. Any electrically conductive material may be used as the conductive material unless it causes a chemical change. Non-limiting examples of conductive materials may be: carbon-based materials such as natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black and / or carbon fiber, etc.; metal-based materials of metal powder or metal fiber, including copper, nickel, aluminum and / or silver, etc.; conductive polymers such as polyphenylene derivatives; or one or more mixtures (and / or combinations) thereof.
[0083] The current collector may include one selected from copper foil, nickel foil, stainless steel foil, titanium foil, nickel foam, copper foam, a polymer substrate coated with a conductive metal, and one or more combinations thereof, but the embodiments of the present disclosure are not limited thereto.
[0084] Such a negative electrode according to one or more embodiments may be prepared by coating a negative active material layer composition on a current collector while applying a magnetic field. Figure 3 A method of preparing a negative electrode according to one or more embodiments is illustrated in more detail.
[0085] like Figure 3 As shown in , the magnet 7 is located under the current collector, the negative active material layer composition including the negative active material 3a is coated on the current collector, and it is dried to prepare the negative active material layer U1. The coating of the negative active material layer composition can be performed by moving the current collector in the coating direction while the magnet is located under the current collector. Therefore, a magnetic field (magnetic flux) of the magnet is formed in a direction perpendicular to the current collector, but the magnetic field is formed as a vector function at a set or predetermined angle according to the coating speed (speed of moving the current collector). In this way, the carbon-based negative active material included in the negative active material layer composition stands, that is, oriented at a set or predetermined angle relative to the current collector, and therefore, the negative active material layer is formed as an oriented layer (e.g., an anisotropic layer).
[0086] In one or more embodiments, the magnet may have a magnetic field strength of about 1000 Gauss to about 10000 Gauss (e.g., about 4000 Gauss to about 8000 Gauss or about 5000 Gauss to about 7000 Gauss). In some embodiments, the negative electrode active material layer composition may be coated on the current collector and maintained for about 3 seconds to about 15 seconds, that is, it may be exposed to a magnetic field for about 3 seconds to about 15 seconds. In one or more embodiments, the time of exposure to the magnetic field may be about 3 seconds to about 12 seconds. Depending on the time of exposure to the magnetic field, the DD value obtained may vary.
[0087] In addition, the DD value can also be obtained by adjusting the viscosity of the negative electrode active material layer composition.
[0088] In one or more embodiments, the viscosity of the negative electrode active material layer composition may be about 2000 cps to about 4000 cps, about 2000 cps to about 3500 cps, or about 2500 cps to about 3500 cps at room temperature (about 20° C. to about 25° C.). The viscosity of the negative electrode active material layer composition may be controlled or selected within this range.
[0089] The viscosity of the negative electrode active material layer composition lower than this range may cause an extreme increase in the verticality of the crystalline carbon-based negative electrode active material (for example, the crystalline carbon second negative electrode active material) included in the negative electrode active material layer, resulting in poor contact of the negative electrode active material particles, and thus, the electron transfer resistance of the negative electrode active material layer may increase, while a viscosity higher than this range may reduce the effect of orientation, thereby reducing the impregnation of the electrolyte.
[0090] In one or more embodiments, the negative electrode active material layer composition can be prepared by mixing the negative electrode active material and the copolymer binder in a solvent. In some embodiments, an aqueous binder can be further added to the negative electrode active material layer composition, or an aqueous binder and a conductive material can be further added to the negative electrode active material layer composition.
[0091] In one or more embodiments, the solvent may be water.
[0092] A rechargeable lithium battery according to one or more embodiments may include a negative electrode, a positive electrode, and an electrolyte.
[0093] The positive electrode may include a positive electrode current collector and a positive active material layer including a positive active material (eg, in the form of particles) formed on the positive electrode current collector.
[0094] The positive electrode active material may include one or more lithiated intercalation compounds that reversibly intercalate and deintercalate lithium ions, and in one or more embodiments, one or more composite oxides of metals selected from cobalt, manganese, nickel, and one or more combinations thereof and lithium may be utilized. For example, a compound represented by one or more of the following chemical formulas may be utilized. Li a A 1-b X b D 1 2 (0.90≤a≤1.8, 0≤b≤0.5); Li a A 1-b X b O 2-c1 D 1 c1 (0.90≤a≤1.8, 0≤b≤0.5, 0≤c1≤0.05); Li a E 1-b X b O 2-c1 D 1 c1 (0.90≤a≤1.8, 0≤b≤0.5, 0≤c1≤0.05); Li a E 2-b X b O 4-c1 D 1 c1 (0.90≤a≤1.8, 0≤b≤0.5, 0≤c1≤0.05); Li a Ni 1-b-c Co b X c D 1 α (0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.5, 0<α≤2); Li a Ni 1-b-c Co b X c O 2-α T α (0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.5, 0<α<2); Li a Ni 1-b-c Co b X c O 2-α T 2 (0.90≤a≤1.8, 0≤b≤0.5, 0≤c≤0.5, 0<α<2); Li a Ni 1-b-c Mn b X c D 1α (0.90≤a≤1.8,0≤b≤0.5,0≤c≤0.5,0<α≤2);Li a Ni 1-b-c Mr b X c O 2-α T α (0.90≤a≤1.8,0≤b≤0.5,0≤c≤0.5,0<α<2);Li a Ni 1-b-c Mr b X c O 2-α T 2 (0.90≤a≤1.8,0≤b≤0.5,0≤c≤0.5,0<α<2);Li a Ni b HAVE BEEN c G d O 2 (0.90≤a≤1.8,0≤b≤0.9,0≤c≤0.5,0.001≤d≤0.1);Li a Ni b Co c L 1 d G e O 2 (0.90≤a≤1.8,0≤b≤0.9,0≤c≤0.5,0≤d≤0.5,0≤e≤0.1);Li a NiG b O 2 (0.90≤a≤1.8,0.001≤b≤0.1);Li a CoG b O 2 (0.90≤a≤1.8,0.001≤b≤0.1);Li a Mr 1-b G b O 2 (0.90≤a≤1.8,0.001≤b≤0.1);Li a Mr 2 G b O 4 (0.90≤a≤1.8,0.001≤b≤0.1);Li a Mr 1-g G g NIGHT 4 (0.90≤a≤1.8,0≤g≤0.5);QO 2 ;QS 2 ;LiQS 2 ;V 2 O5 ;LiV 2 O 5 ;LiZO 2 ;LiNiVO 4 ;Li (3-f) J 2 (PO 4 ) 3 (0≤f≤2);Li (3-f) Fe 2 (PO 4 ) 3 (0≤f≤2); and Li a FePO 4 (0.90≤a≤1.8).
[0095] In the above chemical formula, A can be selected from nickel (Ni), cobalt (Co), manganese (Mn) and one or more combinations thereof; X can be selected from aluminum (Al), Ni, Co, Mn, chromium (Cr), iron (Fe), magnesium (Mg), strontium (Sr), vanadium (V), rare earth elements and one or more combinations thereof; D 1 may be selected from oxygen (O), fluorine (F), sulfur (S), phosphorus (P) and one or more combinations thereof; E may be selected from Co, Mn and combinations thereof; T may be selected from F, S, P and one or more combinations thereof; G may be selected from Al, Cr, Mn, Fe, Mg, lanthanum (La), cerium (Ce), Sr, V and one or more combinations thereof; Q may be selected from titanium (Ti), molybdenum (Mo), Mn and one or more combinations thereof; Z may be selected from Cr, V, Fe, scandium (Sc), yttrium (Y) and one or more combinations thereof; J may be selected from V, Cr, Mn, Co, Ni, copper (Cu) and one or more combinations thereof; L 1 Selected from Mn, Al and combinations thereof.
[0096] In one or more embodiments, the above-mentioned compound in the form of particles may have a coating layer on its surface, or may be mixed with another compound having a coating layer. The coating layer may include at least one coating element compound selected from the oxide of the coating element, the hydroxide of the coating element, the hydroxyl oxide of the coating element, the carbonate of the coating element, and the hydroxy carbonate of the coating element. The coating element compound for the coating layer may be amorphous or crystalline. The coating element included in the coating layer may include Mg, Al, Co, potassium (K), sodium (Na), calcium (Ca), Si, Ti, V, tin (Sn), germanium (Ge), gallium (Ga), boron (B), arsenic (As), zirconium (Zr) or one or more mixtures thereof. The coating layer can be set by utilizing these elements in the compound in a method that has no adverse effect on the properties of the positive active material. For example, the method may include any coating method (such as spraying and / or dipping, etc.), which will not be shown in more detail because it is very suitable for the relevant field.
[0097] In the positive electrode, the amount of the positive active material may be about 90 wt % to about 98 wt % based on the total weight of the positive active material layer.
[0098] In some embodiments, the positive electrode active material layer may further include a binder and a conductive material, and may include the binder and the conductive material in an amount of about 1 wt % to about 5 wt % based on the total amount of the positive electrode active material layer.
[0099] The binder improves the bonding properties between the positive electrode active material particles and between the positive electrode active material particles and the positive electrode current collector. Examples of the binder may be polyvinyl alcohol, carboxymethyl cellulose, hydroxypropyl cellulose, diacetyl cellulose, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, ethylene oxide-containing polymers, polyvinyl pyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, styrene-butadiene rubber, acrylated styrene-butadiene rubber, epoxy resin and / or nylon, etc., but the embodiments of the present disclosure are not limited thereto.
[0100] Conductive materials may be included to provide electrode conductivity. Any electrically conductive material may be used as the conductive material unless it causes a chemical change. Non-limiting examples of conductive materials may include: carbon-based materials such as natural graphite, artificial graphite, carbon black, acetylene black, Ketjen black and / or carbon fiber, etc.; metal-based materials of metal powder or metal fiber, including copper, nickel, aluminum and / or silver, etc.; conductive polymers such as polyphenylene derivatives; or one or more mixtures thereof.
[0101] The positive electrode current collector may be an aluminum foil, a nickel foil, or one or more combinations thereof, but the embodiments of the present disclosure are not limited thereto.
[0102] The positive electrode active material layer or the negative electrode active material layer can be formed by mixing the corresponding active material, the binder and the optional conductive material in a solvent to prepare an active material layer composition and coating the active material layer composition on the corresponding current collector. This active material layer preparation method is very suitable for the relevant field, so that a detailed description will not be provided in the present disclosure. In one or more embodiments, the solvent may be N-methylpyrrolidone and / or water, etc., but the embodiments of the present disclosure are not limited thereto. In some embodiments, the solvent for the negative electrode active material layer composition may be water.
[0103] The electrolyte may include a non-aqueous organic solvent and a lithium salt.
[0104] The nonaqueous organic solvent serves as a medium for transporting ions participating in the electrochemical reaction of the battery.
[0105] The non-aqueous organic solvent may include a carbonate solvent, an ester solvent, an ether solvent, a ketone solvent, an alcohol solvent or an aprotic solvent or a mixture thereof.
[0106] Carbonate solvents may include dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), ethyl methyl carbonate (MEC), ethylene carbonate (EC), propylene carbonate (PC) and / or butylene carbonate (BC) etc. Esters solvents may include methyl acetate, ethyl acetate, n-propyl acetate, dimethyl acetate, methyl propionate, ethyl propionate, propyl propionate, decanoic acid lactone, mevalonolactone and / or caprolactone etc. Ether solvents may include dibutyl ether, tetraethylene glycol dimethyl ether, diethylene glycol dimethyl ether, dimethoxyethane, 2-methyltetrahydrofuran and / or tetrahydrofuran etc. In addition, ketone solvents may include cyclohexanone etc. Alcohol solvents may include ethanol and / or isopropanol, etc., and aprotic solvents may include: nitriles, such as R-CN (wherein R is a C2 to C20 linear, branched or cyclic hydrocarbon, and may include a double bond, an aromatic ring or an ether bond); amides, such as dimethylformamide, etc.; dioxolanes, such as 1,3-dioxolane and / or 1,4-dioxolane, etc.; and / or cyclopentane sulfone, etc.
[0107] The non-aqueous organic solvent can be used alone or in a mixture. If the non-aqueous organic solvent is used in a mixture (e.g., when the non-aqueous organic solvent is used in a mixture), the mixing ratio can be controlled or selected according to the desired battery performance, and it can be very suitable for technicians in the relevant field.
[0108] In one or more embodiments, the carbonate solvent may include a mixture having a cyclic carbonate and a linear carbonate. The cyclic carbonate and the linear carbonate are mixed together in a volume ratio of about 1:1 to about 1:9, and when the mixture is used as a non-aqueous organic solvent for an electrolyte, it may have enhanced performance.
[0109] If a non-aqueous organic solvent is mixed and utilized (e.g., when a non-aqueous organic solvent is mixed and utilized), a mixed solvent of cyclic carbonate and chain carbonate, a mixed solvent of cyclic carbonate and propionate solvent, or a mixed solvent of cyclic carbonate, chain carbonate and propionate solvent can be utilized. The propionate solvent may include methyl propionate, ethyl propionate, propyl propionate, or one or more combinations thereof.
[0110] If utilizing a mixture of cyclic carbonate and linear carbonate or a mixture of cyclic carbonate and propionate solvent (e.g., when utilizing a mixture of cyclic carbonate and linear carbonate or a mixture of cyclic carbonate and propionate solvent), considering performance, it may be desirable to utilize the mixture in a volume ratio of about 1:1 to about 1:9. In certain embodiments, cyclic carbonate, linear carbonate and propionate solvent may be mixed and utilized in a volume ratio of 1:1:1 to 3:3:4. The mixing ratio of the solvent may also be appropriately adjusted according to desired or suitable properties.
[0111] In one or more embodiments, the non-aqueous organic solvent may further include an aromatic hydrocarbon solvent and a carbonate solvent. Here, the carbonate solvent and the aromatic hydrocarbon solvent may be mixed together in a volume ratio of about 1:1 to about 30:1.
[0112] The aromatic hydrocarbon organic solvent may be an aromatic hydrocarbon compound represented by Chemical Formula 1.
[0113] Chemical formula 1
[0114]
[0115] In Chemical Formula 1, R 1 To R 6 The radicals may be independently the same or different and may be independently selected from hydrogen, halogen, C1 to C10 alkyl, halogenated alkyl, and one or more combinations thereof.
[0116] Non-limiting examples of aromatic hydrocarbon organic solvents may be selected from benzene, fluorobenzene, 1,2-difluorobenzene, 1,3-difluorobenzene, 1,4-difluorobenzene, 1,2,3-trifluorobenzene, 1,2,4-trifluorobenzene, chlorobenzene, 1,2-dichlorobenzene, 1,3-dichlorobenzene, 1,4-dichlorobenzene, 1,2,3-trichlorobenzene, 1,2,4-trichlorobenzene, iodobenzene, 1,2-diiodobenzene, 1,3-diiodobenzene, 1,4-diiodobenzene, 1,2,3-triiodobenzene, 1,2,4-triiodobenzene, toluene, 2,4-fluorotoluene, and 1,2-dichlorobenzene. 3-difluorotoluene, 2,4-difluorotoluene, 2,5-difluorotoluene, 2,3,4-trifluorotoluene, 2,3,5-trifluorotoluene, chlorotoluene, 2,3-dichlorotoluene, 2,4-dichlorotoluene, 2,5-dichlorotoluene, 2,3,4-trichlorotoluene, 2,3,5-trichlorotoluene, iodotoluene, 2,3-diiodotoluene, 2,4-diiodotoluene, 2,5-diiodotoluene, 2,3,4-triiodotoluene, 2,3,5-triiodotoluene, xylene and one or more combinations thereof.
[0117] In one or more embodiments, the electrolyte may further include vinylene carbonate and / or an ethylene carbonate-based compound represented by Chemical Formula 2 as an additive for improving cycle life.
[0118] Chemical formula 2
[0119]
[0120] In chemical formula 2, R 7 and R 8 can be independently the same or different, and can be independently hydrogen, halogen, cyano (CN), nitro (NO 2 ) or fluorinated C1 to C5 alkyl, provided that R 7 and R 8 At least one of them is halogen, cyano (CN), nitro (NO 2 ) or a fluorinated C1 to C5 alkyl group, and R 7 and R 8 Not simultaneously (e.g., concurrently) hydrogen.
[0121] Non-limiting examples of ethylene carbonate compounds may include difluoroethylene carbonate, chloroethylene carbonate, dichloroethylene carbonate, bromoethylene carbonate, dibromoethylene carbonate, nitroethylene carbonate, cyanoethylene carbonate, and / or fluoroethylene carbonate, etc. The amount of the additive for improving the cycle life characteristics may be utilized within an appropriate or suitable range.
[0122] In one or more embodiments, the electrolyte may further include vinyl ethylene carbonate, propane sultone, succinonitrile, or one or more combinations thereof, and the utilization amount may be appropriately adjusted.
[0123] The lithium salt dissolved in the non-aqueous organic solvent supplies lithium ions to the rechargeable lithium battery, realizes the basic operation of the rechargeable lithium battery, and improves the transport of lithium ions between the positive electrode and the negative electrode. Non-limiting examples of the lithium salt may include a lithium ion selected from LiPF 6 , LiBF 4 、LiSbF 6 、LiAsF 6 、LiN(SO 2 C 2 F 5 ) 2 、Li(CF 3 SO 2 ) 2 N、LiN(SO 3 C 2 F 5 ) 2 、Li(FSO 2 ) 2 N(Lithium bis(fluorosulfonyl)imide: LiFSI), LiC 4 F 9 SO 3 、LiClO 4 、LiAlO 2 、LiAlCl 4 、LiPO 2 F 2 、LiN(C x F 2x+1 SO 2 )(C y F 2y+1 SO 2 )(wherein x and y are natural numbers, for example, integers from 1 to 20), lithium difluoro(bisoxalato)phosphate, LiCl, LiI, LiB(C 2 O 4 ) 2 One or both of lithium bis(oxalate)borate: LiBOB) and lithium difluoro(oxalate)borate (LiDFOB). The concentration of the lithium salt may be in the range of about 0.1 M to about 2.0 M. If the lithium salt is included in the above concentration range (e.g., when the lithium salt is included in the above concentration range), the electrolyte may have excellent or suitable performance and lithium ion mobility due to optimal or suitable electrolyte conductivity and viscosity.
[0124] In one or more embodiments, the rechargeable lithium battery may further include a separator between the negative electrode and the positive electrode, depending on the type (or type) of the battery. Non-limiting examples of separators may include polyethylene, polypropylene, polyvinylidene fluoride, and multilayers thereof having two or more layers (such as polyethylene / polypropylene double-layer separators, polyethylene / polypropylene / polyethylene three-layer separators, and polypropylene / polyethylene / polypropylene three-layer separators).
[0125] Figure 4 is an exploded perspective view of a rechargeable lithium battery according to one or more embodiments. The rechargeable lithium battery according to one or more embodiments is shown as a prismatic battery, but is not limited thereto and may include batteries of various shapes such as cylindrical batteries and / or pouch batteries.
[0126] Reference Figure 4 The rechargeable lithium battery 100 according to one or more embodiments may include an electrode assembly 40 manufactured by winding a separator 30 disposed between a positive electrode 10 and a negative electrode 20, and a case 50 accommodating the electrode assembly 40. An electrolyte may be impregnated in the positive electrode 10, the negative electrode 20, and the separator 30.
[0127] Hereinafter, examples and comparative examples of the present disclosure are described. However, these examples shall not be interpreted as limiting the scope of the present disclosure in any sense.
[0128] Example 1
[0129] 5 wt % of Si-C composite, 91 wt % of artificial graphite, 2 wt % of acrylic acid-acrylonitrile copolymer binder and 2 wt % of styrene-butadiene rubber were mixed in an aqueous solvent to prepare a negative electrode active material layer slurry having a viscosity of 3000 cps (at 25° C.). The viscosity was measured using a Brookfield viscometer with a LV4 rotor at 30 rpm and room temperature (25° C.).
[0130] The acrylic acid-acrylonitrile copolymer includes 44 wt % acrylic acid and 56 wt % acrylonitrile, and an aqueous solution (at 25° C.) in which the copolymer is added to water to have a solid content (eg, amount) of 7 wt % has a solution viscosity of 1200 mPa·s.
[0131] The Si-C composite includes a silicon core and a soft carbon amorphous coating layer on the surface of the silicon core, and based on the total weight of the Si-C composite (100wt%), the amount of the silicon core is 60wt%, and the amount of the soft carbon amorphous carbon layer is 40wt%. The silicon core is a silicon nanoparticle having an average particle size (D50) of 20nm, and the soft carbon amorphous carbon layer has an average thickness of 100nm.
[0132] The Cu foil current collector is positioned on a magnet with a magnetic field strength of 6000 Gauss while moving the Cu foil current collector, and the negative active material layer slurry is coated on the current collector to be exposed to the magnetic field for 8 seconds, pressurized and dried at a high temperature of 100° C. or higher to prepare a negative active material layer having a thickness of 80 μm, thereby obtaining a negative electrode.
[0133] 96wt% LiCoO 2 The positive active material, 2 wt% of carbon black conductive agent and 2 wt% of polyvinylidene fluoride binder were mixed in N-methylpyrrolidone solvent to prepare positive active material slurry. The positive active material slurry was coated on an Al current collector, dried and pressed to prepare a positive electrode.
[0134] A rechargeable lithium battery cell (full battery cell) was manufactured using the negative electrode, the positive electrode and the electrolyte. A mixed solvent of ethylene carbonate, ethyl methyl carbonate and dimethyl carbonate (volume ratio 20:10:70) was used and 1.5 M LiPF was dissolved therein. 6 to prepare the electrolyte.
[0135] Example 2
[0136] A negative electrode active material layer slurry having a viscosity of 3200 cps (at 25° C.) was prepared by substantially the same steps as in Example 1, except that 5 wt % of Si—C composite, 91 wt % of artificial graphite, 2 wt % of acrylic acid-acrylonitrile copolymer binder and 2 wt % of styrene-butadiene rubber were mixed in an aqueous solvent.
[0137] The Cu foil current collector was positioned on a magnet with a magnetic field strength of 6000 Gauss while being moved, and the negative active material layer slurry was coated on the current collector to be exposed to the magnetic field for 9 seconds, pressed and dried to prepare a negative active material layer having a thickness of 80 μm, thereby obtaining a negative electrode.
[0138] A rechargeable lithium battery cell was manufactured through substantially the same steps as those in Example 1 using the negative electrode as well as the positive electrode and electrolyte used in Example 1.
[0139] Example 3
[0140] A negative electrode active material layer slurry having a viscosity of 3400 cps (at 25° C.) was prepared by substantially the same steps as in Example 1, except that 5 wt % of Si—C composite, 91 wt % of artificial graphite, 2 wt % of acrylic acid-acrylonitrile copolymer binder and 2 wt % of styrene-butadiene rubber were mixed in an aqueous solvent.
[0141] The Cu foil current collector was positioned on a magnet with a magnetic field strength of 6000 Gauss while being moved, and the negative active material layer slurry was coated on the current collector to be exposed to the magnetic field for 10 seconds, pressed and dried to prepare a negative active material layer having a thickness of 80 μm, thereby obtaining a negative electrode.
[0142] A rechargeable lithium battery cell was manufactured through substantially the same steps as those in Example 1 using the negative electrode as well as the positive electrode and electrolyte used in Example 1.
[0143] Example 4
[0144] A negative electrode active material layer slurry having a viscosity of 3300 cps (at 25° C.) was prepared by substantially the same steps as in Example 1, except that 5 wt % of Si—C composite, 91 wt % of artificial graphite, 2 wt % of acrylic acid-acrylonitrile copolymer binder and 2 wt % of styrene-butadiene rubber were mixed in an aqueous solvent.
[0145] The Cu foil current collector was positioned on a magnet with a magnetic field strength of 6000 Gauss while being moved, and the negative active material layer slurry was coated on the current collector to be exposed to the magnetic field for 11 seconds, pressed and dried to prepare a negative active material layer having a thickness of 80 μm, thereby obtaining a negative electrode.
[0146] A rechargeable lithium battery cell was manufactured through substantially the same steps as those in Example 1 using the negative electrode as well as the positive electrode and electrolyte used in Example 1.
[0147] Example 5
[0148] A negative electrode active material layer slurry having a viscosity of 3500 cps (at 25° C.) was prepared by substantially the same steps as in Example 1, except that 5 wt % of Si—C composite, 91 wt % of artificial graphite, 2 wt % of acrylic acid-acrylonitrile copolymer binder and 2 wt % of styrene-butadiene rubber were mixed in an aqueous solvent.
[0149] The Cu foil current collector was positioned on a magnet with a magnetic field strength of 6000 Gauss while being moved, and the negative active material layer slurry was coated on the current collector to be exposed to the magnetic field for 12 seconds, pressed and dried to prepare a negative active material layer having a thickness of 80 μm, thereby obtaining a negative electrode.
[0150] A rechargeable lithium battery cell was manufactured through substantially the same steps as those in Example 1 using the negative electrode as well as the positive electrode and electrolyte used in Example 1.
[0151] Example 6
[0152] A negative electrode active material layer slurry having a viscosity of 3500 cps (at 25° C.) was prepared by substantially the same steps as in Example 1, except that 5 wt % of Si—C composite, 91.6 wt % of artificial graphite, 1.4 wt % of acrylic acid-acrylonitrile copolymer binder and 2 wt % of styrene-butadiene rubber were mixed in an aqueous solvent.
[0153] The Cu foil current collector was positioned on a magnet with a magnetic field strength of 6000 Gauss while being moved, and the negative active material layer slurry was coated on the current collector to be exposed to the magnetic field for 12 seconds, pressed and dried to prepare a negative active material layer having a thickness of 80 μm, thereby obtaining a negative electrode.
[0154] A rechargeable lithium battery cell was manufactured through substantially the same steps as those in Example 1 using the negative electrode as well as the positive electrode and electrolyte used in Example 1.
[0155] Comparative Example 1
[0156] 5 wt % of the Si-C composite used in Example 1, 91 wt % of artificial graphite, 2 wt % of an acrylic acid-acrylonitrile copolymer binder, and 2 wt % of styrene-butadiene rubber were mixed in an aqueous solvent to prepare a negative active material layer slurry having a viscosity of 3000 cps (at 25° C.).
[0157] The negative active material layer slurry was coated on a Cu foil current collector and dried to prepare a negative active material layer having a thickness of 80 μm, thereby obtaining a negative electrode.
[0158] A rechargeable lithium battery cell was manufactured through substantially the same steps as those in Example 1 using the negative electrode as well as the positive electrode and electrolyte used in Example 1.
[0159] Comparative Example 2
[0160] 5 wt % of the Si—C composite used in Example 1, 91 wt % of artificial graphite, 2 wt % of polyacrylic acid, and 2 wt % of styrene-butadiene rubber were mixed in a water solvent to prepare a negative active material layer slurry having a viscosity of 3500 cps (at 25° C.).
[0161] The Cu foil current collector was positioned on a magnet with a magnetic field strength of 6000 Gauss while being moved, and the negative active material layer slurry was coated on the current collector to be exposed to the magnetic field for 5 seconds, pressed and dried to prepare a negative active material layer having a thickness of 80 μm, thereby obtaining a negative electrode.
[0162] A rechargeable lithium battery cell was manufactured through substantially the same steps as those in Example 1 using the negative electrode as well as the positive electrode and electrolyte used in Example 1.
[0163] Comparison Example 3
[0164] 5 wt % of the Si—C composite used in Example 1, 91 wt % of artificial graphite, 2 wt % of polyacrylic acid, and 2 wt % of styrene-butadiene rubber were mixed in a water solvent to prepare a negative active material layer slurry having a viscosity of 3500 cps (at 25° C.).
[0165] The Cu foil current collector was positioned on a magnet with a magnetic field strength of 6000 Gauss while being moved, and the negative active material layer slurry was coated on the current collector to be exposed to the magnetic field for 8 seconds, pressed and dried to prepare a negative active material layer having a thickness of 80 μm, thereby obtaining a negative electrode.
[0166] A rechargeable lithium battery cell was manufactured through substantially the same steps as those in Example 1 using the negative electrode as well as the positive electrode and electrolyte used in Example 1.
[0167] Comparison Example 4
[0168] 5 wt % of the Si—C composite used in Example 1, 91 wt % of artificial graphite, 2 wt % of polyacrylic acid, and 2 wt % of styrene-butadiene rubber were mixed in a water solvent to prepare a negative active material layer slurry having a viscosity of 3300 cps (at 25° C.).
[0169] The Cu foil current collector was positioned on a magnet with a magnetic field strength of 6000 Gauss while being moved, and the negative active material layer slurry was coated on the current collector to be exposed to the magnetic field for 9 seconds, pressed and dried to prepare a negative active material layer having a thickness of 80 μm, thereby obtaining a negative electrode.
[0170] A rechargeable lithium battery cell was manufactured through substantially the same steps as those in Example 1 using the negative electrode as well as the positive electrode and electrolyte used in Example 1.
[0171] Comparative Example 5
[0172] 5 wt % of the Si—C composite used in Example 1, 91 wt % of artificial graphite, 2 wt % of polyacrylic acid, and 2 wt % of styrene-butadiene rubber were mixed in a water solvent to prepare a negative active material layer slurry having a viscosity of 3250 cps (at 25° C.).
[0173] The Cu foil current collector was positioned on a magnet with a magnetic field strength of 6000 Gauss while being moved, and the negative active material layer slurry was coated on the current collector to be exposed to the magnetic field for 10 seconds, pressed and dried to prepare a negative active material layer having a thickness of 80 μm, thereby obtaining a negative electrode.
[0174] A rechargeable lithium battery cell was manufactured through substantially the same steps as those in Example 1 using the negative electrode as well as the positive electrode and electrolyte used in Example 1.
[0175] Comparative Example 6
[0176] 5 wt % of the Si—C composite used in Example 1, 91 wt % of artificial graphite, 2 wt % of polyacrylic acid, and 2 wt % of styrene-butadiene rubber were mixed in a water solvent to prepare a negative active material layer slurry having a viscosity of 3300 cps (at 25° C.).
[0177] The Cu foil current collector was positioned on a magnet with a magnetic field strength of 6000 Gauss while being moved, and the negative active material slurry was coated on the current collector to be exposed to the magnetic field for 11 seconds, pressed and dried to prepare a negative active material layer having a thickness of 80 μm, thereby obtaining a negative electrode.
[0178] A rechargeable lithium battery cell was manufactured through substantially the same steps as those in Example 1 using the negative electrode as well as the positive electrode and electrolyte used in Example 1.
[0179] Comparative Example 7
[0180] 5 wt % of the Si—C composite used in Example 1, 91 wt % of artificial graphite, 2 wt % of polyacrylic acid, and 2 wt % of styrene-butadiene rubber were mixed in a water solvent to prepare a negative active material layer slurry having a viscosity of 3250 cps (at 25° C.).
[0181] The Cu foil current collector is positioned on a magnet with a magnetic field strength of 6000 Gauss while moving the Cu foil current collector, a negative electrode active material layer slurry is coated on the current collector to be exposed to the magnetic field for 12 seconds, pressed and dried at a high temperature of 100° C. or higher to prepare a negative electrode active material layer having a thickness of 80 μm, thereby obtaining a negative electrode.
[0182] A rechargeable lithium battery cell was manufactured through substantially the same steps as those in Example 1 using the negative electrode as well as the positive electrode and electrolyte used in Example 1.
[0183] Comparative Example 8
[0184] 5 wt % of the Si—C composite used in Example 1, 91 wt % of artificial graphite, and 4 wt % of carboxymethyl cellulose (CMC) were mixed in a water solvent to prepare a negative active material layer slurry having a viscosity of 3500 cps (at 25° C.).
[0185] The Cu foil current collector was positioned on a magnet with a magnetic field strength of 6000 Gauss while being moved, and the negative active material layer slurry was coated on the current collector to be exposed to the magnetic field for 5 seconds, pressed and dried to prepare a negative active material layer having a thickness of 80 μm, thereby obtaining a negative electrode.
[0186] A rechargeable lithium battery cell was manufactured through substantially the same steps as those in Example 1 using the negative electrode as well as the positive electrode and electrolyte used in Example 1.
[0187] Comparative Example 9
[0188] 5 wt % of the Si—C composite used in Example 1, 91 wt % of artificial graphite, and 4 wt % of carboxymethyl cellulose were mixed in a water solvent to prepare a negative active material layer slurry having a viscosity of 3300 cps (at 25° C.).
[0189] The Cu foil current collector was positioned on a magnet with a magnetic field strength of 6000 Gauss while being moved, and the negative active material layer slurry was coated on the current collector to be exposed to the magnetic field for 8 seconds, pressed and dried to prepare a negative active material layer having a thickness of 80 μm, thereby obtaining a negative electrode.
[0190] A rechargeable lithium battery cell was manufactured through substantially the same steps as those in Example 1 using the negative electrode as well as the positive electrode and electrolyte used in Example 1.
[0191] Comparative Example 10
[0192] 5 wt % of the Si—C composite used in Example 1, 91 wt % of artificial graphite, and 4 wt % of carboxymethyl cellulose were mixed in a water solvent to prepare a negative active material layer slurry having a viscosity of 3150 cps (at 25° C.).
[0193] The Cu foil current collector was positioned on a magnet with a magnetic field strength of 6000 Gauss while being moved, and the negative active material layer slurry was coated on the current collector to be exposed to the magnetic field for 9 seconds, pressed and dried to prepare a negative active material layer having a thickness of 80 μm, thereby obtaining a negative electrode.
[0194] A rechargeable lithium battery cell was manufactured through substantially the same steps as those in Example 1 using the negative electrode as well as the positive electrode and electrolyte used in Example 1.
[0195] Comparative Example 11
[0196] 5 wt % of the Si—C composite used in Example 1, 91 wt % of artificial graphite, and 4 wt % of carboxymethyl cellulose were mixed in a water solvent to prepare a negative active material layer slurry having a viscosity of 3100 cps (at 25° C.).
[0197] The Cu foil current collector was positioned on a magnet with a magnetic field strength of 6000 Gauss while being moved, and the negative active material layer slurry was coated on the current collector to be exposed to the magnetic field for 10 seconds, pressed and dried to prepare a negative active material layer having a thickness of 80 μm, thereby obtaining a negative electrode.
[0198] A rechargeable lithium battery cell was manufactured through substantially the same steps as those in Example 1 using the negative electrode as well as the positive electrode and electrolyte used in Example 1.
[0199] Comparative Example 12
[0200] 5 wt % of the Si—C composite used in Example 1, 91 wt % of artificial graphite, and 4 wt % of carboxymethyl cellulose were mixed in a water solvent to prepare a negative active material layer slurry having a viscosity of 3120 cps (at 25° C.).
[0201] The Cu foil current collector was positioned on a magnet with a magnetic field strength of 6000 Gauss while being moved, and the negative active material layer slurry was coated on the current collector to be exposed to the magnetic field for 11 seconds, pressed and dried to prepare a negative active material layer having a thickness of 80 μm, thereby obtaining a negative electrode.
[0202] A rechargeable lithium battery cell was manufactured through substantially the same steps as those in Example 1 using the negative electrode as well as the positive electrode and electrolyte used in Example 1.
[0203] Comparative Example 13
[0204] 5 wt % of the Si—C composite used in Example 1, 91 wt % of artificial graphite, and 4 wt % of carboxymethyl cellulose were mixed in a water solvent to prepare a negative active material layer slurry having a viscosity of 3050 cps (at 25° C.).
[0205] The Cu foil current collector was positioned on a magnet with a magnetic field strength of 6000 Gauss while being moved, and the negative active material layer slurry was coated on the current collector to be exposed to the magnetic field for 12 seconds, pressed and dried to prepare a negative active material layer having a thickness of 80 μm, thereby obtaining a negative electrode.
[0206] A rechargeable lithium battery cell was manufactured through substantially the same steps as those in Example 1 using the negative electrode as well as the positive electrode and electrolyte used in Example 1.
[0207] Comparative Example 14
[0208] A negative electrode active material layer slurry having a viscosity of 3250 cps (at 25° C.) was prepared by substantially the same steps as those in Example 1, except that 5 wt % of the Si—C composite utilized in Example 1, 91 wt % of artificial graphite, 2 wt % of an acrylic acid-acrylonitrile copolymer binder, and 2 wt % of styrene-butadiene rubber were mixed in an aqueous solvent.
[0209] The Cu foil current collector was positioned on a magnet with a magnetic field strength of 6000 Gauss while being moved, and the negative active material layer slurry was coated on the current collector to be exposed to the magnetic field for 5 seconds, pressed and dried to prepare a negative active material layer having a thickness of 80 μm, thereby obtaining a negative electrode.
[0210] A rechargeable lithium battery cell was manufactured through substantially the same steps as those in Example 1 using the negative electrode as well as the positive electrode and electrolyte used in Example 1.
[0211] Reference Example 1
[0212] A negative electrode active material layer slurry having a viscosity of 3500 cps (at 25° C.) was prepared by substantially the same steps as in Example 1, except that 5 wt % of Si—C composite, 92.3 wt % of artificial graphite, 0.7 wt % of acrylic acid-acrylonitrile copolymer and 2.0 wt % of styrene-butadiene rubber were mixed in an aqueous solvent.
[0213] The Cu foil current collector is positioned on a magnet with a magnetic field strength of 6000 Gauss while moving the Cu foil current collector, and the negative active material layer slurry is coated on the current collector to be exposed to the magnetic field for 12 seconds, pressed and dried at a high temperature of 100° C. or higher to prepare a negative active material layer having a thickness of 80 μm, thereby obtaining a negative electrode.
[0214] A rechargeable lithium battery cell was manufactured through substantially the same steps as those in Example 1 using the negative electrode as well as the positive electrode and electrolyte used in Example 1.
[0215] Experimental Example 1) Measurement of X-ray Diffraction Characteristics
[0216] The rechargeable lithium battery cells according to Examples 1 to 6, Comparative Examples 1 to 14, and Reference Example 1 were all charged and discharged twice at 0.1C, and fully discharged at 0.1C to 2.75V. The fully discharged battery cells were each disassembled to obtain a negative electrode. For each of these negative electrodes, an X'Pert (PANalytical BV) XRD device using Cu Kα rays as target rays was used, but in order to improve the peak intensity resolution, the monochromator device was removed, and then the XRD was measured. The measurement was carried out under the conditions of 2θ = 10° to 80°, scanning speed (° / s) = 0.06436, and step length of 0.026° / step.
[0217] According to the measured XRD results, the DD value of each layer was calculated, and the results are shown in Table 1.
[0218] Among the XRD results, the integrated areas of the peaks shown at 2θ=26.5±0.2° ((002) plane), 42.4±0.2° ((100) plane), 43.4±0.2° ((101) R plane), 44.6±0.2° ((101) H plane), 54.7±0.2° ((004) plane) and 77.5±0.2° ((110) plane) were measured, and the sum of the areas of the peaks shown at 2θ=42.4±0.2° ((100) plane), 43.4±0.2° ((101) R plane), 44.6±0.2° ((101) H plane) and 77.5±0.2° ((110) plane) was taken as I a , and the sum of the areas of the peaks shown at 2θ = 26.5 ± 0.2° ((002) plane), 42.4 ± 0.2° ((100) plane), 43.4 ± 0.2° ((101) R plane), 44.6 ± 0.2° ((101) H plane), 54.7 ± 0.2° ((004) plane) and 77.5 ± 0.2° ((110) plane) was taken as I 总 , and by calculating these values we obtain DD(I a / I 总 ).
[0219] The binder types or species, slurry viscosities, and conditions for applying a magnetic field in Examples 1 to 6, Comparative Examples 1 to 14, and Reference Example 1 are summarized in Table 1. In Table 1, P(AA-AN) represents acrylic acid-acrylonitrile copolymer, SBR represents styrene-butadiene rubber, PAA represents acrylic acid, and CMS represents carboxymethyl cellulose.
[0220] Table 1
[0221]
[0222]
[0223] Experimental Example 2) Evaluation of the thickness of the negative electrode
[0224] The initial thickness of the negative electrode according to Examples 1 to 6, Comparative Examples 1 to 14, and Reference Example 1 was measured respectively. In addition, the rechargeable lithium battery cells according to Examples 1 to 6 and Comparative Examples 1 to 14 were each charged at SOC 30 (charged to 30% of the charge capacity based on 100% of the full battery charge capacity), the negative electrode was removed from the battery cell, and then the thickness of the negative electrode was measured.
[0225] The thickness expansion of the negative electrode was measured by Equation 2. The results are shown in Table 2 as a thickness increase rate.
[0226] Equation 2
[0227] Thickness expansion ratio (%) = {(thickness after charge and discharge - initial thickness) / initial thickness} × 100
[0228] Table 2
[0229]
[0230]
[0231] As shown in Table 2, when the Examples and Comparative Examples having the same DD value are compared, the thickness increase rate of the Examples is low.
[0232] Examples 1 to 6 using the P(AA-AN) copolymer binder all had DD values of 30 or more and showed a low thickness increase rate.
[0233] However, Comparative Example 1 in which a P(AA-AN) copolymer binder was used but a magnetic field was not applied exhibited a high thickness increase rate, and Comparative Example 2 in which a magnetic field was applied but a PAA binder was used had a DD value less than 30 and exhibited a high thickness increase rate.
[0234] Comparative Examples 3 and 4 had DD values of 30 or more, but both showed slightly high thickness increase rates using the PAA binder.
[0235] Comparative Examples 8 and 14, which used a CMC binder or a P(AA-AN) binder but had a DD value of less than 30, both showed a high thickness increase rate.
[0236] Reference Example 1 had a DD value of 51, but used 0.7 wt % (which was too little) of the P(AA-AN) binder, resulting in low adhesion, and thus, separation occurred during charge and discharge, making it impossible to measure the thickness increase rate.
[0237] Experimental Example 3) Evaluation of Separation
[0238] The rechargeable lithium battery cells according to Examples 1 to 6, Comparative Examples 1 to 14, and Reference Example 1 were each subjected to formation charge and discharge at 0.1C, and then the battery cells were disassembled. Among these results, the image of the battery cell according to Example 6 was Figure 5 , and an image of a battery cell according to Reference Example 1 is shown in Figure 6 Shown in.
[0239] like Figure 5 and Figure 6 As shown in , Example 6 shows that the negative electrode active material layer is well or substantially adhered to the current collector even after charge and discharge, while Reference Example 1 shows that the negative electrode active material layer is mostly or substantially separated from the current collector.
[0240] As used herein, the terms "substantially," "about," or the like are used as terms of approximation and not as terms of degree, and are intended to take into account the inherent deviations of measured or calculated values that one of ordinary skill in the art will recognize. "About," as used herein, includes the stated value and means within an acceptable range of deviations of a particular value as determined by one of ordinary skill in the art taking into account the measurement in question and the errors associated with the measurement of a particular quantity (i.e., the limitations of the measurement system). For example, "about" can mean within one or more standard deviations, or within ±30%, ±20%, ±10%, ±5% of the stated value.
[0241] Any numerical range listed here is intended to include all sub-ranges of the same numerical precision contained in the listed range. For example, the range of "1.0 to 10.0" is intended to include all sub-ranges between the listed minimum value 1.0 and the listed maximum value 10.0 (including the listed minimum value 1.0 and the listed maximum value 10.0), that is, having a minimum value equal to or greater than 1.0 and a maximum value equal to or less than 10.0, such as 2.4 to 7.6. Any maximum numerical limit listed here is intended to include all lower numerical limits contained therein, and any minimum numerical limit listed in this specification is intended to include all higher numerical limits contained therein. Therefore, the applicant reserves the right to modify this specification (including claims) to explicitly list any sub-ranges contained in the range explicitly listed here.
[0242] The battery management system (BMS) device and / or any other related device or component according to the embodiments of the present disclosure described herein can be implemented using any suitable hardware, firmware (e.g., a dedicated integrated circuit), software, or a combination of software, firmware, and hardware. For example, the various components of the device can be formed on an integrated circuit (IC) chip or on separate IC chips. In addition, the various components of the device can be implemented on a flexible printed circuit film, a tape carrier package (TCP), a printed circuit board (PCB), or formed on a substrate. In addition, the various components of the device can be processes or threads running on one or more processors in one or more computing devices, and the one or more computing devices execute computer program instructions and interact with other system components to perform the various functions described herein. The computer program instructions are stored in a memory, which can be implemented in a computing device using a standard memory device (such as a random access memory (RAM) as an example). The computer program instructions can also be stored in other non-temporary computer-readable media (such as a CD-ROM, a flash drive, etc. as an example). In addition, it should be recognized by those skilled in the art that the functions of various computing devices can be combined or integrated into a single computing device without departing from the scope of the present disclosure, or the functions of a specific computing device can be distributed to one or more other computing devices.
[0243] Although the present disclosure has been described in conjunction with what are presently considered to be practical example embodiments, it will be understood that the present disclosure is not limited to the disclosed embodiments, but on the contrary, is intended to cover one or more suitable modifications and equivalent arrangements included within the spirit and scope of the appended claims and their equivalents. Therefore, the foregoing embodiments should be understood as merely examples and not to limit the present disclosure in any way.
Claims
1. A negative electrode for a rechargeable lithium battery, the negative electrode comprising: current collector; as well as a negative electrode active material layer, on the current collector, and comprising a copolymer binder, a Si-C composite first negative electrode active material, and a crystalline carbon second negative electrode active material, in, The copolymer binder comprises a first repeating unit derived from a (meth)acrylic monomer and a second repeating unit derived from a (meth)acrylonitrile monomer, and The divergence value of the negative electrode defined by Equation 1 is 30 or greater, Equation 1 Divergence = (I a / I 总 )×100, in, I a is the sum of the peak intensities at 2θ=42.4±0.2°, 43.4±0.2°, 44.6±0.2°, 77.5±0.2° measured by X-ray diffraction using Cu Kα radiation, and I 总 It is the sum of the peak intensities at 2θ=26.5±0.2°, 42.4±0.2°, 43.4±0.2°, 44.6±0.2°, 54.7±0.2°, and 77.5±0.2° measured by X-ray diffraction using Cu Kα rays.
2. The negative electrode for a rechargeable lithium battery according to claim 1, wherein The divergence value of the negative electrode is 30 to 60.
3. The negative electrode for a rechargeable lithium battery according to claim 1, wherein The amount of the first repeating unit derived from the (meth)acrylic monomer is about 35 wt % to about 65 wt % based on 100 wt % of the copolymer binder.
4. The negative electrode for a rechargeable lithium battery according to claim 1, wherein The amount of the second repeating unit derived from the (meth)acrylonitrile monomer is 35 wt % to 65 wt % based on 100 wt % of the copolymer binder.
5. The negative electrode for a rechargeable lithium battery according to claim 1, wherein The copolymer binder further includes a third repeating unit derived from another monomer copolymerizable with the (meth)acrylic monomer and / or the (meth)acrylonitrile monomer.
6. The negative electrode for a rechargeable lithium battery according to claim 5, wherein The amount of the third repeating unit is greater than 0 wt % and 20 wt % or less, based on 100 wt % of the amount of the copolymer binder.
7. The negative electrode for a rechargeable lithium battery according to claim 1, wherein The copolymer binder is a copolymer of acrylic acid and acrylonitrile.
8. The negative electrode for a rechargeable lithium battery according to claim 1, wherein The amount of the copolymer binder is 0.5 wt % to 5 wt % based on 100 wt % of the total weight of the negative active material layer.
9. The negative electrode for a rechargeable lithium battery according to claim 1, wherein The amount of Si is 1 wt % to 20 wt % based on 100 wt % of the total amount of the Si—C composite first negative electrode active material and the crystalline carbon second negative electrode active material.
10. The negative electrode for a rechargeable lithium battery according to claim 1, wherein Based on 100 wt % of the total amount of the Si—C composite first negative electrode active material and the crystalline carbon second negative electrode active material, the amount of Si is 3 wt % to 20 wt %.
11. The negative electrode for a rechargeable lithium battery according to claim 1, wherein The mixing ratio of the Si-C composite first negative electrode active material to the crystalline carbon second negative electrode active material is 3:97 to 10:90 by weight.
12. The negative electrode for a rechargeable lithium battery according to claim 1, wherein The negative electrode active material layer has a thickness of 10 μm to 100 μm.
13. The negative electrode for a rechargeable lithium battery according to claim 1, wherein The peak intensity is the peak integrated area value.
14. The negative electrode for a rechargeable lithium battery according to claim 1, wherein The copolymer binder has a viscosity of 500 to 3000 mPa·s in an aqueous solution having a solid content of 7 wt %.
15. The negative electrode for a rechargeable lithium battery according to claim 1, wherein The crystalline carbon second negative electrode active material is artificial graphite or natural graphite in an irregular shape, plate-like, flaky, spherical or fibrous shape, or a combination thereof.
16. The negative electrode for a rechargeable lithium battery according to claim 1, wherein The Si-C composite first negative electrode active material includes Si and a carbon material.
17. The negative electrode for a rechargeable lithium battery according to claim 1, wherein The negative electrode is prepared by the following steps: arranging a magnet under the current collector; coating a negative electrode active material layer composition on the current collector, the negative electrode active material layer composition comprising the Si-C composite first negative electrode active material and the crystalline carbon second negative electrode active material; and drying the coated negative electrode active material layer composition, and The magnet has a strength of a magnetic field in a range of 1000 Gauss to 10000 Gauss.
18. The negative electrode for a rechargeable lithium battery according to claim 17, wherein After the step of coating the negative electrode active material layer composition, the coated negative electrode active material layer composition is exposed to the magnetic field for 3 seconds to 15 seconds.
19. The negative electrode for a rechargeable lithium battery according to claim 17, wherein The negative active material layer composition has a viscosity of 2000 cps to 4000 cps at room temperature.
20. A rechargeable lithium battery, comprising: The negative electrode according to any one of claims 1 to 19; A positive electrode, including a positive active material; as well as Non-aqueous electrolytes.