Bipolar composite electrode plate, preparation method of bipolar composite electrode plate, lithium ion battery and manufacturing method of lithium ion battery
By using the PVD process to deposit metal layers and plating protective layers on polymer substrates, the preparation process of bipolar composite electrode sheets is simplified, the problems of complex process and high cost are solved, the performance and efficiency of lithium-ion batteries are improved, and the performance and efficiency of lithium-ion batteries are achieved. Lower manufacturing costs and higher battery performance.
Patent Information
- Application Number
- CN202411031828.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-11-12
AI Technical Summary
The existing bipolar composite electrode sheets are complicated in the process of preparation and have high production costs. Due to the uneven surface of lithium metal, it is difficult to achieve uniform deposition, resulting in lithium dendrites, reducing battery capacity and short circuits. The existing lithium-ion batteries are The process route is long and the manufacturing cost is high.
The first metal layer, the second metal layer and the lithium metal layer are deposited on the polymer substrate by physical vapor deposition (PVD) process, and the protective layer is plated on the surface of the lithium metal layer to simplify the process flow, ensure uniform deposition of lithium metal and reduce the Equipment quantity and process steps.
The simplified preparation process of bipolar composite electrode sheet is realized, the energy density and output voltage of lithium-ion batteries are improved, the cycle performance is enhanced, the manufacturing cost is reduced, and the protection layer is used to avoid lithium metal corrosion, which improves the efficiency and battery capacity of Coulomb .
Smart Images

Figure CN118943304A_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to the field of battery technology, and in particular to a bipolar composite electrode sheet and a preparation method thereof, as well as a lithium ion battery and a manufacturing method thereof. Background Art
[0002] With the rapid development of the new energy industry, the market has put forward higher requirements for the use of lithium-ion batteries. Improving energy density and improving cycle performance are the main directions. The current collector is one of the important components of lithium-ion batteries, which is used to carry active materials, collect and conduct electrons. Aluminum foil and copper foil have good conductivity and can meet the battery's demand for current conduction. However, aluminum foil and copper foil have disadvantages such as large mass and high cost. Compared with traditional aluminum foil and copper foil current collectors, composite current collectors have the advantages of high conductivity, low cost and light weight. However, the existing unipolar composite current collectors need to be coated with positive and negative electrode materials respectively to obtain unipolar positive and negative electrode sheets. When assembling the battery, it is necessary to ensure the alignment of the positive and negative electrode sheets. If the alignment is deviated, it will cause low cell capacity and poor cycle performance due to lithium precipitation. In addition, the control accuracy of the winding machine / stacking machine is very high during the battery assembly process. This process limits the assembly efficiency and the process is complicated. The bipolar composite current collector is composed of two layers of metal foil (such as copper foil and aluminum foil) with a layer of polymer material in between. This structure allows the current to flow on both sides of the current collector, realizing the integration of the positive and negative electrodes on the same current collector to form a bipolar composite electrode sheet. Compared with the monopolar composite electrode sheet, the bipolar composite electrode sheet has the advantages of high space utilization, uniform current distribution, low internal resistance, and simple manufacturing process.
[0003] However, in the preparation process of the existing bipolar composite electrode sheet, the positive electrode material and the negative electrode material are generally coated on the two surfaces of the bipolar composite current collector respectively. After coating, baking, cold pressing and other operations are required respectively. The process is complicated. Any poor control of any step will affect the yield of the battery cell, and the production cost is high. In addition, lithium metal has the advantages of extremely high specific capacity, extremely low standard redox potential and very small density, and has always been considered as one of the most ideal negative electrode materials. However, due to the uneven surface of metallic lithium, it is difficult for the existing method to make lithium metal deposit evenly on the surface of the current collector, which easily leads to the formation of lithium dendrites at the negative electrode. Lithium dendrites will not only reduce the battery capacity, but also pierce the diaphragm, causing the battery short circuit; and the lithium in the existing lithium negative electrode is easily corroded by air, organic solvents, etc., affecting the battery capacity and coulomb efficiency. Therefore, the existing bipolar composite electrode sheet generally uses other negative electrode materials such as graphite instead of lithium metal negative electrode, which reduces the battery energy density. Moreover, the existing lithium-ion battery process has a long production route and high manufacturing cost.
[0004] Therefore, how to provide a bipolar composite electrode sheet and a preparation method thereof, as well as a lithium-ion battery and a manufacturing method thereof, so as to shorten the process route and reduce the manufacturing cost without reducing the battery performance, is a problem that needs to be solved urgently. Summary of the invention
[0005] In view of the above technical problems, the present disclosure provides a bipolar composite electrode sheet and a preparation method thereof, as well as a lithium-ion battery and a manufacturing method thereof, to solve or at least alleviate at least one technical problem existing in the above bipolar composite electrode sheet, lithium-ion battery and a preparation method thereof.
[0006] According to a specific embodiment of the present disclosure, in a first aspect, the present disclosure provides a method for preparing a bipolar composite electrode sheet, comprising the following steps:
[0007] Step (S1), depositing a first metal layer on one side of a polymer substrate by a physical vapor deposition (PVD) process as a positive electrode current collector; and depositing a second metal layer on the other side of the polymer substrate as a negative electrode current collector;
[0008] Step (S2), depositing a lithium metal layer on a side of the second metal layer away from the polymer substrate by a PVD process, wherein the lithium metal layer serves as a negative electrode;
[0009] Step (S3), plating a protective layer on the surface of the lithium metal layer to protect the lithium metal layer; and
[0010] Step (S4), coating a positive electrode material on a side of the first metal layer away from the polymer substrate to form a positive electrode.
[0011] Optionally, in step (S1), a first metal layer is deposited on one side of the polymer substrate by a PVD process, comprising the following steps: attaching the polymer substrate to a sample stage, installing the sample stage in a deposition chamber, placing the first metal layer vapor in a crucible or an evaporation boat; adjusting the vacuum degree in the deposition chamber to 10 -4 Pa~10 -5 Pa, the sample stage rotation speed is 8-12 r / min; and heating is performed to evaporate the steam of the first metal layer and deposit it on one side of the polymer substrate to form the first metal layer.
[0012] Optionally, in step (S1), a second metal layer is deposited on the other side of the polymer substrate by a PVD process, comprising the following steps: pasting the polymer substrate onto a sample stage, installing the sample stage in a deposition chamber, placing the second metal layer vapor in a crucible or an evaporation boat; adjusting the vacuum degree in the deposition chamber to 10 -4 Pa~10 -5Pa, the sample stage rotation speed is 8-12 r / min; and heating is performed to evaporate the steam of the second metal layer and deposit it on the other side of the polymer substrate to form the second metal layer.
[0013] Optionally, an electron gun heating method is used to evaporate the steam material of the first metal layer or the steam material of the second metal layer.
[0014] Optionally, the material of the first metal layer is aluminum, and the evaporation rate of the first metal layer is 15 to 30 angstroms per second.
[0015] Optionally, the material of the second metal layer is copper, and the evaporation rate of the second metal layer is 5 to 15 angstroms per second.
[0016] Optionally, a lithium metal layer is deposited on a side of the second metal layer away from the polymer substrate by a PVD process, comprising the following steps: placing the lithium metal in a crucible or an evaporation boat with the second metal layer facing the opening of the crucible or the evaporation boat, and adjusting the vacuum degree in the deposition chamber to 10 -4 Pa~10 -5 Pa, the sample stage rotation speed is 8-12 r / min; and heating is performed to evaporate lithium metal and deposit it on one side of the second metal layer, and the evaporation speed of the lithium metal layer is 20-50 angstroms / second.
[0017] Optionally, in step (S1), before depositing the first metal layer and the second metal layer on both sides of the polymer substrate, a first primer layer and a second primer layer are respectively deposited on both sides of the polymer substrate to increase the bonding force between the polymer substrate and the first metal layer and the second metal layer; then, the first metal layer is deposited on the side of the first primer layer away from the polymer substrate by a PVD process as a positive electrode current collector; and the second metal layer is deposited on the side of the second primer layer away from the polymer substrate as a negative electrode current collector.
[0018] Optionally, vacuum evaporation or magnetron sputtering is used to deposit the first primer layer and the second primer layer on both sides of the polymer substrate respectively.
[0019] Optionally, the materials of the first bottom layer and the second bottom layer include Ni, Cr, Zn, Co, Ti and their corresponding oxides, AlO x And at least one of SiO2.
[0020] According to a specific embodiment of the present disclosure, in a second aspect, the present disclosure provides a bipolar composite electrode sheet, which is obtained by using any of the above-mentioned methods for preparing a bipolar composite electrode sheet, and the bipolar composite electrode sheet comprises:
[0021] Polymer substrate;
[0022] A first metal layer is disposed on one side of the polymer substrate;
[0023] A second metal layer is disposed on the other side of the polymer substrate;
[0024] A lithium metal negative electrode is disposed on a side of the second metal layer away from the polymer substrate;
[0025] A protective layer is disposed on a side of the lithium metal negative electrode away from the polymer substrate; and
[0026] The positive electrode material layer is arranged on a side of the first metal layer away from the polymer substrate.
[0027] Optionally, the bipolar composite electrode sheet also includes a first coating layer and a second coating layer, wherein the first coating layer is arranged between the polymer substrate and the first metal layer to increase the bonding force between the polymer substrate and the first metal layer; the second coating layer is arranged between the polymer substrate and the second metal layer to increase the bonding force between the polymer substrate and the second metal layer.
[0028] Optionally, the thickness of the first metal layer is 0.5-3 μm.
[0029] Optionally, the second metal layer has a thickness of 0.5-3 μm.
[0030] Optionally, the thickness of the lithium metal negative electrode is 0.5 to 2.5 μm.
[0031] Optionally, the thickness of the protective layer is 10-30 nm.
[0032] Optionally, the thickness of the protective layer is 15-20 nm.
[0033] Optionally, the thickness of the first coating layer is 3 to 30 nm.
[0034] Optionally, the second primer layer has a thickness of 3-30 nm.
[0035] Optionally, the material of the protective layer includes AlO x 、Li3N、LiPON、LixSiO y 、LiZrO x , Li 1.5 Al 0.5 Ge 1.5 (PO4)3 or at least one of the composite materials, wherein the composite material includes a rigid LLZTO inorganic material and a flexible lithiated naphthalene sulfide organic material, wherein the rigid LLZTO inorganic material serves as a skeleton and the flexible lithiated naphthalene sulfide organic material serves as a filler.
[0036] Optionally, the materials of the first bottom layer and the second bottom layer include Ni, Cr, Zn, Co, Ti and their corresponding oxides, AlO x And at least one of SiO2.
[0037] According to a specific embodiment of the present disclosure, in a third aspect, the present disclosure provides a method for manufacturing a lithium-ion battery, comprising:
[0038] A bipolar composite electrode sheet obtained by any of the above-mentioned methods for preparing a bipolar composite electrode sheet;
[0039] Winding or laminating the bipolar composite electrode sheet and the separator together;
[0040] The wound or stacked bipolar composite electrode sheets and diaphragms are placed in a shell, and the shell is sealed after the electrolyte is injected into the shell.
[0041] According to a specific embodiment of the present disclosure, in a fourth aspect, the present disclosure provides a lithium-ion battery obtained by using the lithium-ion battery manufacturing method.
[0042] Compared with the prior art, the above solution of the embodiment of the present disclosure has at least the following beneficial effects:
[0043] (1) The preparation method of the bipolar composite electrode sheet provided by the present invention adopts the PVD process to complete the deposition of the first metal layer, the second metal layer and the lithium negative electrode. That is, the production process of the composite current collector and the negative electrode can be directly completed by PVD deposition. During the preparation process, only the positive electrode material is coated once, which reduces the number of equipment used; the traditional negative electrode coating, baking, cold pressing and stacking or winding alignment assembly processes are eliminated, simplifying the process flow; and when assembling the battery, the positive and negative electrodes do not need to be aligned, the battery assembly is simple, and the process difficulty is reduced. Moreover, the use of lithium metal with high specific capacity, low standard redox potential, low density and good conductivity as the negative electrode can improve the energy density and output voltage of lithium-ion batteries; improve the electronic conductivity of the negative electrode, which is conducive to the rapid transmission of charge; and the lithium metal layer can also be used as a lithium supplement, which can supplement the irreversible capacity loss of the negative electrode during the first charging process, and can supplement Li + In addition, by plating a protective layer on the surface of the lithium metal negative electrode, the lithium in the lithium metal negative electrode can be isolated from the air and organic solvents, etc., to prevent the lithium in the lithium metal layer from being corroded by the air and organic solvents, resulting in irreversible consumption of lithium, thereby reducing the initial coulombic efficiency, battery capacity, etc.
[0044] (2) The material of the protective layer has high ionic conductivity and high modulus, which can improve the interfacial compatibility between the electrolyte and metallic lithium, induce uniform nucleation of metallic lithium, and deposit lithium in a layer-by-layer growth manner, effectively promoting the uniform deposition of lithium.
[0045] (3) In the preparation method of the bipolar composite electrode sheet provided by the present disclosure, when vacuum evaporating the lithium metal layer, the evaporation rate is controlled to be 20 to 50 angstroms per second, which can reduce the overall deviation of the deposition rate during the film formation period, so as to achieve the purpose of uniform deposition of lithium metal on the surface of the second metal layer, and the surface of the obtained lithium metal layer is flat. In addition, by controlling the film formation time, the thickness of the obtained lithium metal negative electrode is 0.5 to 2.5 μm, which can improve the energy density and output voltage of the battery without causing waste of lithium metal.
[0046] (4) The embodiment of the present disclosure deposits the first bottom layer and the second bottom layer on both sides of the polymer substrate respectively, thereby improving the bonding force between the polymer substrate and the first metal layer and the second metal layer, further improving the stability of the bipolar composite electrode sheet, and improving the cycle performance of the lithium-ion battery.
[0047] (5) The embodiment of the present disclosure adopts a composite current collector, and the first metal layer and the second metal layer are deposited on both sides of the polymer substrate. The thickness of the first metal layer and the second metal layer is preferably 0.5 to 3 μm. Under the premise of not affecting the conductivity and electrochemical stability of the current collector, the mass, volume and cost of the current collector are significantly reduced compared with traditional aluminum foil and copper foil current collectors. BRIEF DESCRIPTION OF THE DRAWINGS
[0048] The drawings herein are incorporated into the specification and constitute a part of the specification, showing embodiments consistent with the present disclosure, and together with the specification, are used to explain the principles of the present disclosure. Obviously, the drawings described below are only some embodiments of the present disclosure, and for ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work. In the drawings:
[0049] Figure 1 is a flow chart of a method for preparing a bipolar composite electrode sheet in some embodiments of the present disclosure;
[0050] Figure 2 Schematic diagram of the cross-sectional structure of a bipolar composite electrode sheet in some embodiments of the present disclosure;
[0051] Figure 3 Schematic diagram of the cross-sectional structure of a bipolar composite electrode sheet in some embodiments of the present disclosure;
[0052] Figure 4 The present invention is a flowchart of a method for manufacturing a lithium-ion battery in some embodiments of the present invention.
[0053] The reference numerals in the specific implementation manner are as follows:
[0054] Bipolar composite electrode sheet 10;
[0055] Protective layer 1, lithium metal negative electrode 2, second metal layer 3, polymer substrate 4, first metal layer 5, positive electrode material layer 6, first primer layer 7, second primer layer 8. DETAILED DESCRIPTION
[0056] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention will be further described in detail below with reference to the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0057] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which the present disclosure belongs; the terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the present disclosure.
[0058] It should also be noted that the terms "include", "comprises" or any other variations thereof are intended to cover non-exclusive inclusion, so that a product or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such product or device. In the absence of more restrictions, the elements defined by the sentence "comprises a" do not exclude the presence of other identical elements in the product or device including the elements.
[0059] In the description of the embodiments of the present invention, the orientations or positional relationships indicated by the technical terms "upper", "lower", "thickness", etc. are based on the orientations or positional relationships shown in the accompanying drawings and are only for the convenience of describing the embodiments of the present invention and simplifying the description. They do not indicate or imply that the devices or elements referred to must have a specific orientation, be constructed and operated in a specific orientation. Therefore, they cannot be understood as limitations on the embodiments of the present invention.
[0060] In the description of the embodiments of the present invention, the term "and / or" is only a description of the association relationship of associated objects, indicating that three relationships may exist. For example, A and / or B may represent: A exists alone, A and B exist at the same time, and B exists alone. In addition, the character " / " in this article generally indicates that the associated objects before and after are in an "or" relationship.
[0061] In the description of the embodiments of the present invention, the symbol “~” represents the two endpoint data before and after the “~” and all data between the two endpoints. For example, A~B represents all data greater than or equal to A and less than or equal to B.
[0062] Reference to "embodiments" in this disclosure means that a particular feature, structure, or characteristic described in conjunction with the embodiments may be included in at least one embodiment of the disclosure. The appearance of the phrase in various places in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described in this disclosure may be combined with other embodiments.
[0063] In the preparation process of the existing bipolar composite electrode sheet, the positive electrode material and the negative electrode material are generally coated on the two surfaces of the bipolar composite current collector respectively. After coating, baking, cold pressing and other operations are required respectively. The process is complicated. Any poor control of any step will affect the yield of the battery cell. In addition, multiple coatings require a large number of equipment and high production costs. In addition, although lithium metal has the advantages of extremely high specific capacity, extremely low standard redox potential and very small density, it has always been considered as one of the most ideal negative electrode materials. However, due to the uneven surface of metallic lithium, the existing coating method is difficult to make lithium metal deposit evenly on the surface of the current collector, which easily leads to the formation of lithium dendrites at the negative electrode. Lithium dendrites will not only reduce the battery capacity, but also may pierce the diaphragm, causing the battery short circuit, and the lithium in the lithium negative electrode is easily corroded by air, organic solvents, etc., affecting the battery capacity. Therefore, lithium metal negative electrodes have not been practically applied in lithium-ion batteries. The existing bipolar composite electrode sheets generally use other negative electrode materials such as graphite instead of lithium metal negative electrodes, which reduces the battery energy density. Moreover, the existing lithium-ion battery process has a long production route and high manufacturing cost.
[0064] In order to solve the above technical problems, the inventors have found through research that the preparation process of the lithium metal negative electrode and how to isolate the lithium ions in the lithium metal negative electrode from air and organic solvents can be considered to reduce the generation of lithium dendrites in the lithium metal negative electrode and the consumption of lithium in the lithium metal negative electrode; and the assembly process of the obtained bipolar composite electrode sheet is simple.
[0065] The present invention uses a PVD process to complete the deposition of the first metal layer, the second metal layer and the lithium negative electrode. That is, the production process of the composite current collector and the negative electrode is directly completed through PVD deposition. In the preparation process of the bipolar composite electrode sheet, only the positive electrode material is coated once, which reduces the number of equipment used; the traditional negative electrode coating, baking, cold pressing and stacking or winding alignment assembly processes are omitted, simplifying the process flow; and when assembling the battery, the positive and negative electrodes do not need to be aligned, the battery assembly is simple, and the process difficulty is reduced. Moreover, the use of lithium metal with high specific capacity, low standard redox potential, low density and good conductivity as the negative electrode can improve the energy density and output voltage of lithium-ion batteries; improve the electronic conductivity of the negative electrode, which is conducive to the rapid transmission of charge; and the lithium metal layer can also be used as a lithium supplement, which can supplement the irreversible capacity loss of the negative electrode during the first charging process, and can supplement Li +In addition, by plating a protective layer on the surface of the lithium metal negative electrode, the lithium in the lithium metal negative electrode can be isolated from the air and organic solvents, etc., to prevent the lithium in the lithium metal layer from being corroded by the air and organic solvents, resulting in irreversible consumption of lithium, thereby reducing the initial coulombic efficiency, battery capacity, etc.
[0066] The optional embodiments of the present disclosure are described in detail below with reference to the accompanying drawings.
[0067] See also Figure 1 The present disclosure provides a method for preparing a bipolar composite electrode sheet, comprising the following steps:
[0068] Step (S1), depositing a first metal layer on one side of a polymer substrate by a PVD process as a positive electrode current collector; depositing a second metal layer on the other side of the polymer substrate as a negative electrode current collector;
[0069] Step (S2), depositing a lithium metal layer on a side of the second metal layer away from the polymer substrate by a PVD process, wherein the lithium metal layer serves as a negative electrode;
[0070] Step (S3), plating a protective layer on the surface of the lithium metal layer to protect the lithium metal layer; and
[0071] Step (S4), coating a positive electrode material on a side of the first metal layer away from the polymer substrate to form a positive electrode.
[0072] In step (S1), the PVD process includes vacuum evaporation, magnetron sputtering, ion plating, etc. In some embodiments, the deposition order of the first metal layer and the second metal layer can be adjusted according to actual needs.
[0073] The first metal layer is deposited on one side of the polymer substrate by a PVD process, comprising the following steps: pasting the polymer substrate onto a sample stage, installing the sample stage in a deposition chamber, placing the first metal layer vaporized material in a crucible or an evaporation boat; adjusting the vacuum degree in the deposition chamber to 10 -4 Pa~10 -5 Pa, the sample stage rotation speed is 8-12 r / min; and heating is performed to evaporate the steam of the first metal layer and deposit it on one side of the polymer substrate to form the first metal layer.
[0074] The second metal layer is deposited on the other side of the polymer substrate by a PVD process, including the following steps: placing the vapor of the second metal layer in a crucible or an evaporation boat; adjusting the vacuum degree in the deposition chamber to 10 -4 Pa~10 -5Pa, the sample stage rotation speed is 8-12 r / min; and heating is performed to evaporate the steam of the second metal layer and deposit it on the other side of the polymer substrate to form the second metal layer.
[0075] The evaporation rate of the first metal layer and the evaporation rate of the second metal layer can be adjusted by program-controlled power. In some embodiments, the material of the first metal layer is metal aluminum, and the evaporation rate of the first metal layer is 15 to 30 angstroms / second. The melting point of aluminum is relatively low. This evaporation rate range can quickly evaporate a uniform aluminum film on the surface of the polymer substrate; the material of the second metal layer is copper, and the evaporation rate of the second metal layer is 5 to 15 angstroms / second. The melting point of copper is relatively high, and the energy required for evaporation is relatively high. If the evaporation rate is too fast, it is easy to burn the polymer substrate. The evaporation rate of 5 to 15 angstroms / second can reduce the heat brought by copper vapor to the polymer substrate, so that the second metal layer is formed more densely on the polymer substrate. In some more preferred embodiments, the material of the first metal layer is metal aluminum, and the evaporation rate of aluminum is preferably 20 angstroms / second; the material of the second metal layer is metal copper, and the evaporation rate of copper is preferably 10 angstroms / second.
[0076] The heating method for evaporating the steam of the first metal layer or the second metal layer can be selected according to actual needs. In some embodiments, the steam of the first metal layer or the second metal layer is evaporated by electron gun heating.
[0077] During the vacuum evaporation process, the uniformity of the deposition of the first metal layer and the second metal layer is ensured by rotating the sample stage. The thickness of the first metal layer and the second metal layer is controlled by controlling the vacuum evaporation film forming time. If the thickness of the first metal layer and the second metal layer is too large, for example, greater than 3μm, the mass and volume of the battery cell will increase, the volume energy density of the battery cell will be reduced, and the cost will be increased; if the thickness of the first metal layer and the second metal layer is too small, for example, less than 0.5μm, the conductivity and electrochemical stability of the current collector in the battery cell will be affected. In some embodiments, the thickness of the first metal layer and the second metal layer is preferably 0.5 to 3μm. In this embodiment, the thickness of the first metal layer and the second metal layer is 1μm.
[0078] The polymer substrate can be a polymer material commonly used in composite current collectors. As an example, the material of the polymer substrate includes but is not limited to polyethylene terephthalate (PET), o-phenylphenol, polypropylene, polyimide, polyvinyl chloride, etc. If the polymer substrate is too thin, it cannot play a good supporting role; if the polymer substrate is too thick, it will increase the volume of the composite current collector and the difficulty of welding the middle ear of the battery cell. In some embodiments, the thickness of the polymer substrate is 3 to 20 μm. In this embodiment, the polymer substrate is a PET film with a thickness of 6 μm.
[0079] In some embodiments, before depositing the first metal layer and the second metal layer on both sides of the polymer substrate, a first primer layer and a second primer layer are respectively deposited on both sides of the polymer substrate to increase the bonding strength between the polymer substrate and the first metal layer and the second metal layer, respectively; then, the first metal layer is deposited on the side of the first primer layer away from the polymer substrate by a PVD process as a positive electrode current collector; and the second metal layer is deposited on the side of the second primer layer away from the polymer substrate as a negative electrode current collector.
[0080] The first bottom layer and the second bottom layer can be deposited on both sides of the polymer substrate by vacuum evaporation or magnetron sputtering. The materials of the first bottom layer and the second bottom layer can be the same or different. Preferably, the materials of the first bottom layer and the second bottom layer both include Ni, Cr, Zn, Co, Ti and their corresponding oxides, AlO x More preferably, the materials of the first base layer and the second base layer both include corresponding oxides of Ni, Cr, Zn, Co or Ti, AlO x The oxide is more conducive to forming COX (Ni, Cr, Zn, Co or Ti) bonding, and improving the bonding force between the polymer substrate and the first metal layer and the second metal layer.
[0081] If the thickness of the first bottom layer and the second bottom layer is too large, for example, greater than 30 nm, the magnetron sputtering energy during the preparation of the first bottom layer and the second bottom layer is relatively large, which will greatly reduce the strength of the polymer substrate and increase the cost; if the thickness of the first bottom layer and the second bottom layer is too small, for example, less than 3 nm, it cannot be uniformly formed into a film, and an island-shaped or dot-shaped bottom layer is formed, which has little effect on increasing the bonding force between the polymer substrate and the first metal layer and the second metal layer. In some embodiments, the thickness of the first bottom layer and the second bottom layer is 3 to 30 nm. In some preferred embodiments, the thickness of the first bottom layer and the second bottom layer is 5 to 20 nm.
[0082] It can be understood that before depositing the first metal layer and the second metal layer on both sides of the polymer substrate, depositing the first primer layer and the second primer layer on both sides of the polymer substrate respectively is an optional step, and whether to deposit the first primer layer and the second primer layer on both sides of the polymer substrate can be selected according to actual needs.
[0083] In step (S2), depositing a lithium metal layer on the side of the second metal layer away from the polymer substrate by a PVD process includes: placing lithium metal in a crucible or an evaporation boat, with the second metal layer facing the opening of the crucible or the evaporation boat, and adjusting the vacuum degree in the deposition chamber to 10 -4 Pa~10 -5Pa, the sample stage rotation speed is 8-12 r / min; and heating is performed to evaporate lithium metal and deposit it on one side of the second metal layer, and the evaporation speed of the lithium metal layer is 20-50 angstroms / second.
[0084] The evaporation rate of the lithium metal layer is 20 to 50 angstroms per second. Lithium metal has a low melting point and is particularly easy to form vapor. The evaporation rate fluctuates greatly. If the evaporation rate is low, it is difficult to achieve uniform deposition. The evaporation rate of the lithium metal layer in the embodiment of the present disclosure is 20 to 50 angstroms per second, which can reduce the overall deviation of the deposition rate during film formation and achieve uniform deposition. In this embodiment, the evaporation rate of the lithium metal layer is 50 angstroms per second.
[0085] The PVD process is used to complete the deposition of the first metal layer, the second metal layer and the lithium negative electrode. That is, the production process of the composite current collector and the negative electrode can be directly completed through PVD deposition, which reduces the number of equipment used, eliminates the traditional negative electrode coating, baking and stacking or winding alignment assembly processes, and simplifies the process flow. In addition, the use of lithium metal as the negative electrode can increase the energy density and output voltage of the battery; improve the electronic conductivity of the negative electrode, which is conducive to the rapid transmission of charge; and the lithium metal layer can also be used as a lithium supplement, which can supplement the irreversible capacity loss of the negative electrode during the first charging process, and can supplement Li + concentration, so as to achieve the purpose of improving the initial coulombic efficiency and battery capacity.
[0086] In some embodiments, the thickness of the lithium metal layer is preferably, but not limited to, 0.5 to 2.5 μm. In this embodiment, the thickness of the lithium metal layer is 1 μm.
[0087] In step (S3), the protective layer can be deposited on the surface of the lithium metal layer by a PVD process. In some embodiments, the protective layer is deposited on the surface of the lithium metal layer by a vacuum evaporation technique.
[0088] The protective layer covers the surface of the lithium metal layer, which can isolate the lithium metal in the lithium metal negative electrode from air and organic solvents, etc., to prevent the lithium in the lithium metal layer from being corroded by air and organic solvents, causing irreversible consumption of lithium, and thereby reducing the initial coulombic efficiency, battery capacity, etc.
[0089] The material of the protective layer is preferably a rigid material with high ionic conductivity and high modulus, or a composite material of a rigid material with high ionic conductivity and high modulus and a flexible organic material, which can effectively promote the uniform deposition of metallic lithium and inhibit the growth of dendrites. In some embodiments, the material of the protective layer includes but is not limited to AlO x 、Li3N、LiPON、LixSiO y 、LiZrO x , Li 1.5 Al 0.5 Ge1.5 (PO4)3 or at least one of a composite material, the composite material comprising a rigid LLZTO inorganic material and a flexible lithiated naphthalene organic material, the rigid LLZTO inorganic material as a skeleton, and the flexible lithiated naphthalene organic material as a filler. In some preferred embodiments, the material of the protective layer is Al2O3, Al2O3 is used to improve the interface compatibility between the electrolyte and metallic lithium, and the high Young's modulus Al2O3 can induce uniform nucleation of metallic lithium and deposit lithium in a layer-by-layer growth manner, effectively promoting uniform deposition of lithium. If the thickness of the protective layer is too thin, it will not play a protective role; if it is too thick, it will affect the lithium ion channel. In some embodiments, the thickness of the protective layer is 10 to 30 nm. Preferably, the thickness of the protective layer is 15 to 20 nm.
[0090] In step (S4), the method for coating the positive electrode material on one side of the first metal layer can adopt the common coating method of the positive electrode material layer of the existing lithium ion battery. For example, blade coating, roller transfer coating, etc. After coating the positive electrode material layer, the positive electrode is formed by baking, cold pressing and other processes. The positive electrode material includes a positive electrode active material, a conductive agent and a binder. In some embodiments, the positive electrode active material, the conductive agent, and the binder are dispersed in a solvent (such as N-methylpyrrolidone) to form a positive electrode slurry; the positive electrode slurry is coated on the first metal layer, and after drying, cold pressing and other processes, the positive electrode can be obtained.
[0091] The positive electrode material includes a positive electrode active material, a binder and a conductive agent. The positive electrode active material, the binder and the conductive agent can be respectively the positive electrode active material, the binder and the conductive agent known in the positive electrode materials of lithium ion batteries. As an example, the positive electrode active material can be but is not limited to LiCoO2, LiNiO2, LiMnO2, LiMn2O4, LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2、LiNi 0.5 Co 0.2 Mn 0.3 O2、LiNi 0.5 Co 0.25 Mn 0.25 O2、LiNi 0.6 Co 0.2 Mn 0.2 O2、LiNi 0.8 Co 0.1 Mn 0.1 O2、LiNi 0.85 Co 0.15 Al 0.05O2, LiFePO4, LiMnPO4, etc.; the binder can be but not limited to polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), vinylidene fluoride-tetrafluoroethylene-propylene terpolymer, vinylidene fluoride-hexafluoropropylene-tetrafluoroethylene terpolymer, tetrafluoroethylene-hexafluoropropylene copolymer and fluorine-containing acrylate resin, etc.; the conductive agent can be but not limited to superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene or carbon nanofibers, etc. In this embodiment, the positive electrode material includes, by mass percentage: 90wt% lithium iron phosphate, 2-5wt% PVDF and 5-8wt% carbon nanotubes and conductive carbon black.
[0092] In the preparation process of the bipolar composite electrode sheet of the disclosed embodiment, only the positive electrode material is coated once, eliminating the traditional negative electrode coating, baking and other processes, simplifying the process flow. In addition, when assembling the battery, the positive and negative electrodes do not need to be aligned, the battery assembly is simple, and the process difficulty is reduced.
[0093] See also Figure 2 , the embodiment of the present disclosure provides a bipolar composite electrode sheet 10, which is obtained by any of the above-mentioned methods for preparing a bipolar composite electrode sheet. The bipolar composite electrode sheet 10 includes: a protective layer 1, a lithium metal negative electrode 2, a second metal layer 3, a polymer substrate 4, a first metal layer 5 and a positive electrode material layer 6 are stacked in sequence. The first metal layer 3 is arranged on one side of the polymer substrate 4, the second metal layer 3 is arranged on the other side of the polymer substrate 4, the lithium metal negative electrode 2 is arranged on the side of the second metal layer 3 away from the polymer substrate 4, the protective layer 1 is arranged on the side of the lithium metal negative electrode 2 away from the polymer substrate 4, and the positive electrode material layer 6 is arranged on the side of the first metal layer 5 away from the polymer substrate 4.
[0094] See also Figure 3 In some embodiments, the bipolar composite electrode sheet 10 also includes a first bottom layer 7 and a second bottom layer 8. The first bottom layer 7 is arranged between the polymer substrate 4 and the first metal layer 5 to increase the bonding force between the polymer substrate 4 and the first metal layer 5; the second bottom layer 8 is arranged between the polymer substrate 4 and the second metal layer 3 to increase the bonding force between the polymer substrate 4 and the second metal layer 3.
[0095] In some embodiments, the thickness of the first metal layer 5 and the second metal layer 3 is preferably 0.5-3 μm. In this embodiment, the thickness of the first metal layer 5 and the second metal layer 3 is 1 μm. In some embodiments, the material of the first metal layer 5 is aluminum, and the material of the second metal layer 3 is copper.
[0096] In some embodiments, the thickness of the lithium metal negative electrode 2 is preferably 0.5-2.5 μm. In this embodiment, the thickness of the lithium metal negative electrode 2 is preferably 1 μm.
[0097] In some embodiments, the material of the protective layer 1 is not limited to at least one of the following materials: AlO x 、Li3N、LiPON、LixSiO y 、LiZrO x , Li 1.5 Al 0.5 Ge 1.5 ((PO4)3 or a composite material including a rigid LLZTO inorganic material and a flexible lithiated naphthalene sulfone organic material, wherein the rigid LLZTO inorganic material serves as a skeleton and the flexible lithiated naphthalene sulfone organic material serves as a filler. In some preferred embodiments, the material of the protective layer 1 is Al2O3. In some preferred embodiments, the thickness of the protective layer 1 is 10 to 30 nm. In some preferred embodiments, the thickness of the protective layer 1 is 15 to 20 nm.
[0098] In some embodiments, the materials of the first base layer 7 and the second base layer 8 both include Ni, Cr, Zn, Co, Ti and their corresponding oxides, AlO x Preferably, the materials of the first base layer 7 and the second base layer 8 both include corresponding oxides of Ni, Cr, Zn, Co or Ti, AlO x and at least one of SiO2. Oxides are more conducive to forming COX (Ni, Cr, Zn, Co or Ti) bonds, and improving the bonding force between the polymer substrate and the first metal layer and the second metal layer. In some embodiments, the thickness of the first base layer 7 and the second base layer 8 is 3 to 30 nm.
[0099] The protective layer 1, lithium metal negative electrode 2, second metal layer 3, polymer substrate 4, first metal layer 5, positive electrode material layer 6, first primer layer 7 and second primer layer 8 of this embodiment are respectively the same as the protective layer, lithium metal negative electrode, second metal layer, polymer substrate, first metal layer, positive electrode material, first primer layer and second primer layer described in the preparation method of the bipolar composite electrode sheet in the aforementioned embodiment, including all the technical features described in the aforementioned embodiment, which will not be repeated here.
[0100] See also Figure 4 The present disclosure provides a method for manufacturing a lithium-ion battery, comprising the following steps:
[0101] Step (I), obtaining a bipolar composite electrode sheet 10 by using any of the above-mentioned methods for preparing a bipolar composite electrode sheet;
[0102] Step (II), winding or laminating the bipolar composite electrode sheet 10 and the separator together;
[0103] Step (III) is to place the wound or stacked bipolar composite electrode sheets and the separator in a shell, inject electrolyte into the shell, and then seal the shell.
[0104] In the bipolar composite electrode sheet of the embodiment of the present disclosure, the positive electrode and the negative electrode are integrated on the same current collector. When winding, the distance between the first metal layer and the second metal layer in the thickness direction of the diaphragm is small, which reduces the volume of the battery cell, and makes the current distribution uniform and the internal resistance small. Compared with the winding or stacking method of the traditional electrode sheet, the present disclosure only winds a single electrode during battery assembly, and there is no need to consider the alignment of the positive and negative electrodes, which greatly simplifies the battery assembly process; and avoids the traditional assembly method. The deviation when aligning the positive and negative electrodes is prone to occur, resulting in low battery cell capacity, lithium precipitation leading to poor cycle performance, etc.; and the control accuracy requirements for the winding machine or stacking machine during the battery assembly process are relatively low.
[0105] The separator, electrolyte and shell may be the separator, electrolyte and shell known in lithium-ion batteries, respectively.
[0106] The disclosed embodiment also provides a lithium-ion battery obtained by using any of the above-mentioned methods for manufacturing a lithium-ion battery.
[0107] The following is an introduction to the preparation process, test methods and test data of the specific embodiments and comparative examples of the present disclosure:
[0108] Embodiment 1:
[0109] Paste the PET film onto the sample stage, then install the sample stage on the base in the deposition chamber, place the aluminum vapor in the evaporation boat, and adjust the vacuum degree in the deposition chamber to 10 before evaporation. -4 Pa~10 -5 Pa, the sample stage rotation speed is 10r / min; the electron gun heating method is used for evaporation, the evaporation rate is 20 angstroms / second, and a 1μm aluminum metal layer is deposited on one side of the PET film; the copper vapor material is placed in the evaporation boat, and the electron gun heating method is used for evaporation, and the evaporation rate is 10 angstroms / second, and a 1μm copper metal layer is deposited on the other side of the PET film; the lithium vapor material is placed in the evaporation boat, and a 1μm thick lithium metal layer is evaporated on the surface of the copper metal layer at a evaporation rate of 50 angstroms / second; then a 10nm thick AlO is plated on the surface of the lithium metal layer x ; The positive electrode material is coated on the surface of the aluminum metal layer, and the positive electrode material uses 90wt% lithium iron phosphate, 2-5wt% PVDF and 5-8wt% carbon nanotubes and conductive carbon black to obtain a bipolar composite electrode sheet.
[0110] Then the bipolar composite electrode sheet and the separator are wound together, placed in a housing after winding, and then injected with electrolyte to assemble a lithium-ion battery. The electrolyte uses commercial electrolyte HR9212.
[0111] Embodiment 2:
[0112] Example 2 is basically the same as Example 1, and the only difference is that the thickness of the protective layer is different, as shown in Table 1.
[0113] Embodiment 3:
[0114] Example 3 is basically the same as Example 1, and the only difference is that the thickness of the protective layer is different, as shown in Table 1.
[0115] Embodiment 4:
[0116] Example 4 is basically the same as Example 1, and the only difference is that the thickness of the protective layer is different, as shown in Table 1.
[0117] Embodiment 5:
[0118] Example 5 is basically the same as Example 3, with the only difference being that 5 nm NiCr is deposited between the polymer substrate and the first metal layer as the first primer layer, and 5 nm NiCr is deposited between the polymer substrate and the second metal layer as the second primer layer, as shown in Table 1 for details.
[0119] Embodiment 6:
[0120] Example 6 is basically the same as Example 3, with the only difference being that 5 nm Cr is deposited between the polymer substrate and the first metal layer as the first primer layer, and 5 nm Cr is deposited between the polymer substrate and the second metal layer as the second primer layer, as shown in Table 1 for details.
[0121] Comparative Example 1:
[0122] Comparative Example 1 is substantially the same as Example 1, with the only difference being that no protective layer is deposited on the surface of the lithium metal layer, as shown in Table 1 for details.
[0123] Comparative Example 2:
[0124] A conventional aluminum foil with a thickness of 9 μm is used as a positive electrode current collector, a conventional copper foil with a thickness of 6 μm is used as a negative electrode current collector, a lithium metal negative electrode with a thickness of 1 μm is arranged on the surface of the copper foil to obtain a negative electrode sheet, and a positive electrode material is coated on the surface of the aluminum foil. The positive electrode material uses 90 wt% lithium iron phosphate, 2-5 wt% PVDF and 5-8 wt% carbon nanotubes and conductive carbon black to obtain a positive electrode sheet.
[0125] Then, the positive electrode sheet, the separator and the negative electrode sheet are stacked and placed in a housing, and then an electrolyte is injected to assemble a lithium-ion battery. The electrolyte uses a commercial electrolyte HR9212.
[0126] Comparative Example 3:
[0127] Comparative Example 3 is basically the same as Comparative Example 2, except that: AlO is plated on the surface of the lithium metal negative electrode with a thickness of 15 nm. x layer.
[0128] After the lithium ion batteries obtained in Examples 1-4 and Comparative Examples 1-3 were cycled for 100 cycles, the cycle capacity retention rate and coulombic efficiency were tested, and the test data are shown in Table 1. The capacity retention rate is the capacity retention rate after 100 cycles, the test temperature is 25°C, and the charge and discharge rate is 0.2C.
[0129] Table 1 Relevant data and test results of the electrode sheet composition of each embodiment and comparative example
[0130]
[0131] Comparative Example 2 is a conventional aluminum foil and copper foil current collector with a relatively large thickness used in the existing process, with lithium metal as the negative electrode and no protective layer. From the results of Comparative Example 2, it can be seen that after 100 cycles, the capacity retention rate and coulombic efficiency of the lithium-ion battery are severely attenuated. Compared with Comparative Example 2, Examples 1-4 have greatly improved capacity retention rate and coulombic efficiency. This shows that compared with the conventional process of using lithium metal as the negative electrode in the prior art, the bipolar composite electrode sheet and its preparation process disclosed in the present invention, which use lithium metal as the negative electrode and plate a protective layer on the surface of the lithium negative electrode, can greatly improve the cycle performance of lithium-ion batteries.
[0132] Comparative Example 3 uses thicker conventional aluminum foil and copper foil current collectors. Compared with Comparative Example 3 in Table 1, the capacity retention rate and coulombic efficiency of Example 2 are substantially the same, which indicates that the embodiment of the present invention can greatly reduce the weight, volume, and manufacturing cost of the electrode sheet and simplify the process flow without affecting the performance of the lithium-ion battery.
[0133] Compared with Comparative Example 1, the capacity retention rate and coulombic efficiency of the lithium-ion battery in Examples 1-4 in Table 1 are significantly increased, indicating that the provision of a protective layer on the surface of the lithium metal negative electrode in the present disclosure can prevent the lithium in the lithium metal layer from being corroded by air and organic solvents, resulting in irreversible consumption of lithium, thereby improving the coulombic efficiency and cycle performance of the lithium-ion battery.
[0134] Compared with Example 3, the coulombic efficiency of the lithium-ion battery in Examples 5 and 6 in Table 1 remains basically unchanged, and the capacity retention rate is significantly increased after 100 cycles. This indicates that by providing a first primer layer between the polymer substrate and the first metal layer, and providing a second primer layer between the polymer substrate and the second metal layer, the bonding force between the polymer substrate and the first metal layer and the second metal layer can be significantly improved without reducing the coulombic efficiency of the battery, thereby improving the stability of the bipolar composite electrode sheet and the cycle performance of the lithium-ion battery.
[0135] From the above results and analysis, it can be concluded that the bipolar composite electrode sheet disclosed in the present invention can shorten the process route, reduce manufacturing costs, and simplify the difficulty of battery assembly without reducing the performance of lithium-ion batteries or even improving battery performance.
[0136] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present disclosure, rather than to limit them; although the present disclosure has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein by equivalents; and these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present disclosure, and they should all be included in the scope of the claims and specification of the present disclosure. In particular, as long as there is no structural conflict, the various technical features mentioned in the various embodiments can be combined in any way. The present disclosure is not limited to the specific embodiments disclosed herein, but includes all technical solutions that fall within the scope of the claims.
Claims
1. A method for preparing a bipolar composite electrode sheet, characterized in that: The following steps are involved: Step (S1), depositing a first metal layer on one side of a polymer substrate by a PVD process as a positive electrode current collector; depositing a second metal layer on the other side of the polymer substrate as a negative electrode current collector; Step (S2), depositing a lithium metal layer on a side of the second metal layer away from the polymer substrate by a PVD process, wherein the lithium metal layer serves as a negative electrode; Step (S3), plating a protective layer on the surface of the lithium metal layer to protect the lithium metal layer; and Step (S4), coating a positive electrode material on a side of the first metal layer away from the polymer substrate to form a positive electrode.
2. The method for preparing a bipolar composite electrode sheet according to claim 1, characterized in that: In the step (S1), a first metal layer is deposited on one side of the polymer substrate by a PVD process, and a second metal layer is deposited on the other side of the polymer substrate, comprising the following steps: The polymer substrate is pasted onto the sample stage, and then the sample stage is installed in the deposition chamber, and the evaporation material of the first metal layer or the second metal layer is placed in the crucible or the evaporation boat; Adjust the vacuum level in the deposition chamber to 10 -4 Pa~10 -5 Pa, the sample stage rotation speed is 8-12r / min; and The first metal layer is heated to evaporate the material and deposit it on one side of the polymer substrate to form the first metal layer; or the second metal layer is heated to evaporate the material and deposit it on the other side of the polymer substrate to form the second metal layer.
3. The method for preparing a bipolar composite electrode sheet according to claim 2, characterized in that: The material of the first metal layer is aluminum, and the evaporation rate of the first metal layer is 15 to 30 angstroms per second; and / or the material of the second metal layer is copper, and the evaporation rate of the second metal layer is 5 to 15 angstroms per second.
4. The method for preparing a bipolar composite electrode sheet according to claim 2, characterized in that: In the step (S2), a lithium metal layer is deposited on a side of the second metal layer away from the polymer substrate by a PVD process, comprising the following steps: Place the lithium metal vapor in a crucible or an evaporation boat, with the second metal layer facing the opening of the crucible or the evaporation boat, and adjust the vacuum degree in the deposition chamber to 10 -4 Pa~10 -5 Pa, the sample stage rotation speed is 8-12r / min; and The heating causes the lithium metal vapor to evaporate and deposit on the side of the second metal layer away from the polymer substrate. The evaporation rate of the lithium metal layer is 20 to 50 angstroms per second.
5. The method for preparing a bipolar composite electrode sheet according to any one of claims 1 to 4, characterized in that: In the step (S1), before depositing the first metal layer and the second metal layer on both sides of the polymer substrate, it also includes depositing a first primer layer and a second primer layer on both sides of the polymer substrate, respectively, to increase the bonding force between the polymer substrate and the first metal layer and the second metal layer; then depositing the first metal layer on the side of the first primer layer away from the polymer substrate through a PVD process as a positive electrode current collector; and depositing the second metal layer on the side of the second primer layer away from the polymer substrate as a negative electrode current collector.
6. A bipolar composite electrode sheet, characterized in that: The bipolar composite electrode sheet is prepared by the method for preparing the bipolar composite electrode sheet according to any one of claims 1 to 5, wherein the bipolar composite electrode sheet comprises: Polymer substrate; A first metal layer is disposed on one side of the polymer substrate; A second metal layer is disposed on the other side of the polymer substrate; A lithium metal negative electrode is disposed on a side of the second metal layer away from the polymer substrate; A protective layer is disposed on a side of the lithium metal negative electrode away from the polymer substrate; and The positive electrode material layer is arranged on a side of the first metal layer away from the polymer substrate.
7. The bipolar composite electrode sheet according to claim 6, characterized in that: The thickness of the first metal layer and the thickness of the second metal layer are 0.5 to 3 μm; and / or the thickness of the lithium metal negative electrode is 0.5 to 2.5 μm; and / or the thickness of the protective layer is 10 to 30 nm; and / or the thickness of the first base layer and the second base layer is 3 to 30 nm.
8. The bipolar composite electrode sheet according to claim 6 or 7, characterized in that: The material of the protective layer includes AlO x 、Li3N、LiPON、LixSiO y 、LiZrO x , Li 1.5 Al 0.5 Ge 1.5 (PO4)3 or at least one of the composite materials, wherein the composite material includes a rigid LLZTO inorganic material and a flexible lithiated naphthalene sulfide organic material, wherein the rigid LLZTO inorganic material serves as a skeleton and the flexible lithiated naphthalene sulfide organic material serves as a filler.
9. A method for manufacturing a lithium ion battery, characterized in that: include: A bipolar composite electrode sheet obtained by the preparation method according to any one of claims 1 to 5; Winding or laminating the bipolar composite electrode sheet and the separator together; The wound or stacked bipolar composite electrode sheets and diaphragms are placed in a shell, and the shell is sealed after electrolyte is injected into the shell.
10. A lithium ion battery, characterized in that: The lithium ion battery is obtained by the lithium ion battery manufacturing method as claimed in claim 9.