Lithium ion battery positive electrode material, positive electrode plate and lithium ion battery

By combining the positive electrode material of lithium battery, using the combination of nickel, cobalt, manganese ternary materials and other nickel, cobalt, manganese ternary materials and the second positive electrode active material, combined with the carbon cladding layer, the metal dissolution problem is solved, the circulation and storage performance of lithium battery is improved, and the volume is controlled Expansion.

CN118943312APending Publication Date: 2024-11-12ENVISION DYNAMICS TECH (JIANGSU) CO LTD +3
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202310532776.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-11
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The problem of metal dissolution in the positive electrode active material of lithium batteries leads to damage to the interface of solid electrolytic media, affecting the cycling performance, storage performance and volume expansion of the battery, especially at high temperatures.

Method used

The first positive electrode active material such as nickel-cobalt-manganese ternary material, lithium iron phosphate, etc. is combined with the second positive electrode active material. By adjusting its mass ratio and particle size distribution, the carbon cladding layer is added to form an inert barrier layer to reduce metal dissolution. .

Benefits of technology

Effectively improve the circulation and storage performance of lithium batteries, reduce the metal Mn dissolution amount, improve the volume expansion control of the battery, ensure that the capacity retention rate is greater than 81% after 500 cycles of 45℃ and the storage capacity retention rate is greater than 60℃. 84%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118943312A_ABST
    Figure CN118943312A_ABST
Patent Text Reader

Abstract

The invention provides a lithium ion battery positive electrode material, a positive electrode plate and a lithium ion battery, the lithium ion battery positive electrode material at least comprises: a first positive electrode active material, the first positive electrode active material comprises any one or more of a nickel cobalt manganese ternary material, lithium iron phosphate, lithium iron manganese phosphate, a lithium-rich manganese-based material, lithium cobalt oxide or lithium nickel manganese oxide; the chemical general formula of the second positive electrode active material is LixM1-yNyO4-z, x is more than or equal to 0.05 and less than or equal to 6, y is more than or equal to 0 and less than or equal to 1, z is more than or equal to 0 and less than or equal to 2, the element M comprises any one or more of Fe, Ni or Co, and the element N comprises any one or more of Al, Mn, Ti, Si or Cu. The invention provides a lithium ion battery positive electrode material, a positive electrode plate and a lithium ion battery. The lithium ion battery positive electrode material and the positive electrode plate can effectively improve metal dissolution and improve the performance of the battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium ion batteries, and in particular to a lithium ion battery positive electrode material, a positive electrode sheet and a lithium battery. Background Art

[0002] Lithium transition metal oxides are a promising positive electrode active material for lithium batteries due to their low price and high specific capacity. However, many positive electrode active materials for lithium batteries (such as lithium manganese oxide, nickel-cobalt-manganese ternary materials, lithium iron manganese phosphate, lithium iron phosphate or lithium phosphate, etc.) have the problem of metal dissolution, which will cause metal deposition at the negative electrode, thereby causing the destruction or thickening of the solid electrolyte interface (SEI). This in turn affects battery performance, such as causing the battery's cycle performance, storage performance and gas production performance to deteriorate, and this phenomenon is more significant at high temperatures. Summary of the invention

[0003] The present invention provides a lithium ion battery positive electrode material, a positive electrode plate and a lithium ion battery, which can effectively improve the problem of metal dissolution, thereby improving the storage performance and cycle performance of the battery and improving the volume expansion of the battery.

[0004] To solve the above technical problems, the present invention is achieved through the following technical solutions:

[0005] The present invention provides a lithium ion battery positive electrode material, comprising at least the following components:

[0006] A first positive electrode active material, wherein the first positive electrode active material includes any one or more of a nickel-cobalt-manganese ternary material, lithium iron phosphate, lithium iron manganese phosphate, a lithium-rich manganese-based material, lithium cobalt oxide, or lithium nickel manganese oxide;

[0007] The second positive electrode active material has a chemical formula of Li x M 1-y N y O 4-z , wherein 0.05≤x≤6, 0≤y≤1, 0≤z≤2, the element M includes any one or more of Fe, Ni or Co, and the element N includes any one or more of Al, Mn, Ti, Si or Cu.

[0008] In one embodiment of the present invention, the mass ratio of the first positive electrode active material to the second positive electrode active material is 90:10 to 99:1.

[0009] In one embodiment of the present invention, the median particle size D of the first positive electrode active material is 50 The median particle size D of the second positive electrode active material 50 The ratio is 1.25-12.5.

[0010] In one embodiment of the present invention, the median particle size D of the second positive electrode active material is 50 The median particle size D of the first positive electrode active material is 1 μm-10 μm. 50 0.8μm-9.2μm.

[0011] In one embodiment of the present invention, the surface of the first positive electrode active material is coated with a carbon layer, and the coating amount of the carbon is 1%-3% of the mass of the first positive electrode active material.

[0012] In one embodiment of the present invention, the chemical formula of the nickel-cobalt-manganese ternary material is LiNi x Co y Mn 1-x-y O2, where 0.9≤x≤1, 0≤y≤0.06.

[0013] In one embodiment of the present invention, the general chemical formula of the lithium manganese iron phosphate is LiMn x Fe 1-x PO4, where 0.5≤x≤1.

[0014] In one embodiment of the present invention, the general chemical formula of the lithium-rich manganese-based material is Li 1+x Mn a Ni b O 2-c , where 0<x≤0.3, 0.5<a≤1, 0≤b<0.5, x+a+b+c=1.

[0015] The present invention also provides a positive electrode sheet, comprising the above-mentioned lithium-ion battery positive electrode material.

[0016] The present invention also provides a lithium-ion battery, comprising the above-mentioned positive electrode plate.

[0017] In one embodiment of the present invention, the amount of metal Mn dissolved in the lithium-ion battery is ≤500 ppm.

[0018] In summary, the present invention provides a lithium ion battery positive electrode material, a positive electrode sheet and a lithium ion battery, which can effectively improve the distribution uniformity of particles, so that the compaction density of the positive electrode sheet reaches 2.44-3.68g / cm 3 , thereby improving the processing quality of the pole piece. It can effectively improve the metal dissolution of the battery, thereby effectively improving the cycle performance and storage performance of the battery, and improving the volume expansion of the battery. The prepared lithium battery has a capacity retention rate of more than 81% after 500 cycles at 45°C, a storage capacity retention rate of more than 84% at 60°C, a storage volume growth rate of less than 8% at 60°C, and a metal Mn dissolution amount of ≤500ppm in the lithium-ion battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for describing the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative work.

[0020] Figure 1 FIG. 1 is a schematic diagram of the structure of a lithium battery in one embodiment of the present invention.

[0021] Figure 2 Graph showing the cycle performance of the lithium battery in Example 1 of the present invention and Comparative Example 1.

[0022] Description of labels:

[0023] 100, positive electrode plate; 200, separator; 300, negative electrode plate; 400, electrolyte. DETAILED DESCRIPTION

[0024] The following describes the embodiments of the present invention through specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention.

[0025] It should be understood that the present invention can be implemented in different forms and should not be construed as being limited to the embodiments set forth herein. On the contrary, providing these embodiments will make disclosure thorough and complete, and will fully convey the scope of the present invention to those skilled in the art. If not otherwise specified, the "%" and "parts" shown in the following examples refer to "mass %" and "mass parts" respectively.

[0026] The technical solution of the present invention is further described in detail below in conjunction with several embodiments and drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0027] Lithium transition metal oxide is a promising positive electrode active material for lithium batteries due to its low price and high specific capacity. Lithium batteries made from lithium transition metal oxide are widely used in portable electronic products such as mobile phones, tablet computers, laptops and digital cameras, as well as in transportation tools such as electric bicycles and electric vehicles. The present invention provides a lithium ion battery positive electrode material, a positive electrode sheet and a lithium ion battery, which can improve the cycle performance and storage performance of the battery and can be applied to various electronic products and electric vehicle fields.

[0028] The present invention provides a positive electrode material for a lithium-ion battery, comprising a first positive electrode active material and a second positive electrode active material, wherein the first positive electrode active material comprises any one or more of a nickel-cobalt-manganese ternary material, lithium iron phosphate, lithium iron manganese phosphate, a lithium-rich manganese-based material, lithium cobalt oxide, or lithium nickel manganese oxide. The chemical formula of the second positive electrode active material is Li x M 1-y N y O 4-z , wherein 0.05≤x≤6, 0≤y≤1, 0≤z≤2, element M includes any one or more of Fe, Ni or Co, and element N includes any one or more of Al, Mn, Ti, Si or Cu. The first positive electrode active material and the second positive electrode active material are compounded, and the second positive electrode active material can be used as an inert barrier layer to alleviate the dissolution of metal (such as Mn) in the first positive electrode active material, so that the amount of metal Mn dissolved in the final prepared lithium battery is ≤500ppm, thereby effectively improving the long-term performance of the battery, such as improving the battery's cycle performance, storage performance, and gas production performance.

[0029] In one embodiment of the present invention, the second positive electrode active material Li x M 1-y N y O 4-z When the content of lithium is within a preset range, that is, 0.05≤x≤1, the second positive electrode active material has a high electrochemical activity and can improve the performance stability of the lithium battery. When the content of lithium is too low and is 0, that is, x=0, M 1-y N y O 4-z As a metal oxide, it will be corroded by the hydrofluoric acid formed in the electrolyte, resulting in poor cycle performance of the battery. When the lithium content is too high, that is, x is greater than 1, the electrochemical activity of the second positive electrode active material is high, and the volume expansion and contraction during the cycle will also cause poor battery stability.

[0030] In one embodiment of the present invention, the median particle size D of the second positive electrode active material 50 For example, it is 1 μm to 10 μm. And the median particle size D of the first positive electrode active material is 50The median particle size D of the second positive electrode active material 50 The ratio of the first positive electrode active material to the second positive electrode active material is, for example, 1.25-12.5. 50 When the ratio is within this range, the particles of the first positive electrode active material are filled between the particles of the second positive electrode active material, and the two particles are evenly distributed, which can effectively improve the compaction density of the positive electrode sheet, thereby effectively improving the processing quality of the positive electrode sheet and thus improving the performance of the battery. 50 The ratio is too large, the median particle size D of the second positive electrode active material 50 If the particle size is too small and less than 1 μm, the specific surface area of ​​the second positive electrode active material will be too high, which will affect the processing performance of the electrode sheet and further affect the battery performance. 50 The ratio is too small, and the median particle size D 50 If it is too large and greater than 10 μm, the first positive electrode active material will be distributed relatively unevenly in the electrode sheet, thereby affecting the battery performance.

[0031] In one embodiment of the present invention, in the first positive electrode active material, the chemical formula of the nickel-cobalt-manganese ternary material (NCM) is, for example, LiNi x Co y Mn 1-x-y O2, where 0.9≤x≤1, 0≤y≤0.06. The general chemical formula of lithium manganese iron phosphate is, for example, LiMn x Fe 1-x PO4, wherein 0.5≤x≤1. The general chemical formula of lithium-rich manganese-based materials (LRMO) is, for example, Li 1+x Mn a Ni b O 2-c , wherein 0<x≤0.3, 0.5<a≤1, 0≤b<0.5, x+a+b+c=1. In one embodiment of the present invention, the median particle size D of the first positive electrode active material is 50 For example, 0.8 μm-9.2 μm.

[0032] In one embodiment of the present invention, for example, a carbon (C) layer can be coated on the surface of the first positive electrode active material, and the carbon coating amount is, for example, 1%-3% of the mass of the first positive electrode active material. Further, the carbon coating amount is, for example, 1.2%-2% of the mass of the first positive electrode active material. The carbon coating amount within the above range can improve the conductivity of the first positive electrode active material, thereby improving the rate performance of the battery. At the same time, the dissolution of metal Mn in the first positive electrode active material can be reduced, thereby improving the cycle performance of the battery. If the carbon coating amount is too low and is less than 1% of the mass of the first positive electrode active material, the coating effect is poor and the dissolution of the metal cannot be effectively blocked. If the carbon coating amount is too high and is higher than 3% of the mass of the first positive electrode active material, the active sites are reduced. In one embodiment of the present invention, for example, one or more uniform carbon (C) layers are coated on the surface of the first positive electrode active material, and the area of ​​the first positive electrode active material coated by the carbon layer is 100% of the surface area of ​​the first positive electrode active material. In other embodiments, the area of ​​the first positive electrode active material covered by the carbon layer may also be less than 100% of the surface area of ​​the first positive electrode active material.

[0033] In one embodiment of the present invention, the mass ratio of the first positive electrode active material to the second positive electrode active material is, for example, 90:10 to 99:1. When the mass ratio of the first positive electrode active material to the second positive electrode active material is within this range, it can not only improve the problem of metal dissolution in the first positive electrode active material, but also increase the energy density of the second positive electrode active material, thereby ensuring that various performances of the battery are improved. When the mass ratio of the first positive electrode active material to the second positive electrode active material is less than 90:10, the mass proportion of the first positive electrode active material is too low, resulting in the energy density of the battery being affected, and the particles of the first positive electrode active material are relatively unevenly distributed in the electrode sheet, thereby affecting the long-term performance of the battery. When the mass ratio of the first positive electrode active material to the second positive electrode active material is greater than 99:1, the mass proportion of the first positive electrode active material is too low, and the metal dissolution problem cannot be effectively solved, resulting in insignificant improvement in battery performance.

[0034] See also Figure 1As shown, the present invention also proposes a positive electrode plate, including the above-mentioned lithium-ion battery positive electrode material. In one embodiment of the present invention, the positive electrode plate 100 includes a positive electrode current collector, a conductive agent, a binder and the above-mentioned lithium-ion battery positive electrode material. Among them, the positive electrode current collector can be selected from aluminum foil, etc. The conductive agent is selected from any one or more of conductive carbon black (Super P, SP), acetylene black, carbon nanotubes (Carbon Nanotube, CNT) and graphene, etc. The binder is selected from any one or more of polyvinylidene fluoride (Polyvinylidene Fluoride, PVDF), polyamide (Polyamide, PA), polyacrylonitrile (Polyacrylonitrile, PAN), polyacrylate (polyacrylate), polyvinylether (polyvinylether), polymethyl methacrylate (Polymethyl Methacrylate, PMMA), polyhexafluoropropylene (Polyhexafluoropropylene) or styrene butadiene rubber (Polymerized Styrene Butadiene Rubber, SBR), etc.

[0035] See also Figure 1 As shown, in this embodiment, the positive electrode current collector is selected from aluminum foil, the conductive agent is selected from SP, the binder is selected from PVDF, and the positive electrode material is selected from LiMn 0.6 Fe 0.4 PO4@C and Li 0.5 In this embodiment, 98% of LiMn 0.6 Fe 0.4 PO4@C with 2% Li 0.5 NiO2 is mixed to form secondary particles. After the particles, SP and PVDF are mixed in a weight ratio of, for example, 97:1.5:1.5, N-methylpyrrolidone (NMP) is added, and the mixture is stirred in a vacuum mixer until the system is uniform to obtain a positive electrode slurry. The positive electrode slurry is evenly coated on an aluminum foil, and the aluminum foil is placed in a blast drying oven and dried at 120°C for 10 minutes. The dried electrode sheet is rolled and cut to form a positive electrode sheet 100.

[0036] See also Figure 1 As shown, the present invention also proposes a lithium-ion battery, which includes the above-mentioned positive electrode sheet 100, separator 200, negative electrode sheet 300 and electrolyte 400, the positive electrode sheet 100 and the negative electrode sheet 300 are located on both sides of the separator 200, and the positive electrode sheet 100, separator 200 and negative electrode sheet 300 are immersed in the electrolyte 400.

[0037] See also Figure 1 As shown, in one embodiment of the present invention, the negative electrode plate 300 includes a negative electrode current collector, a conductive agent, a binder and a negative electrode active material. Among them, the negative electrode current collector can be selected from copper foil, etc. The conductive agent is selected from any one or more of conductive carbon black (Super P, SP), acetylene black, carbon nanotube (Carbon Nanotube, CNT) and graphene, etc. The binder is selected from any one or more of polyvinylidene fluoride (Polyvinylidene Fluoride, PVDF), polyamide (Polyamide, PA), polyacrylonitrile (Polyacrylonitrile, PAN), polyacrylate (polyacrylate), polyvinylether (polyvinylether), polymethyl methacrylate (Polymethyl Methacrylate, PMMA), polyhexafluoropropylene (Polyhexafluoropropylene) or styrene butadiene rubber (Polymerized Styrene Butadiene Rubber, SBR), etc. The negative electrode active material is any one or more of natural graphite, artificial graphite, crystalline carbon, amorphous carbon or carbon composite material.

[0038] See also Figure 1 As shown, in this embodiment, the negative electrode active material is selected from artificial graphite, the conductive agent is selected from SP, the binder is selected from styrene-butadiene rubber, and the thickener is selected from sodium carboxymethyl cellulose. In this embodiment, artificial graphite, conductive carbon black, sodium carboxymethyl cellulose and styrene-butadiene rubber are mixed at a mass ratio of 96:1:1:2, deionized water is added, and a negative electrode slurry is obtained under the action of a vacuum mixer. The negative electrode slurry is evenly coated on the negative electrode current collector copper foil, the copper foil is placed in a blast drying oven, and dried at 120°C for 10 minutes, and the dried electrode sheet is rolled and cut to prepare a negative electrode sheet 300.

[0039] See also Figure 1 As shown, in one embodiment of the present invention, the diaphragm 200 is selected from a polyethylene film (PE) or a polypropylene film (PP), etc. The thickness of the diaphragm 200 is, for example, 9 to 18 μm, the air permeability is, for example, 180 to 380 s / 100 mL, and the porosity is, for example, 30 to 50%.

[0040] See also Figure 1As shown, in one embodiment of the present invention, the electrolyte 400 includes, for example, a lithium salt and an organic solvent. The lithium salt is selected from, for example, any one or more of lithium hexafluorophosphate (LiPF6), lithium difluorophosphate (LiPO2F2), lithium bis(fluorosulfonyl)imide (LiFSi), lithium tetrafluoroborate (LiBF4), lithium difluoro(oxalato)borate (1-), LiDFOB, or lithium bis(oxalate)borate (LiBOB). In this embodiment, the lithium salt is selected from, for example, LiPF6. In one embodiment of the present invention, the content of the lithium salt is, for example, 4 to 24 wt% of the total mass of the electrolyte 400, and the content of the organic solvent is, for example, 96 to 76 wt% of the total mass of the electrolyte 400. The organic solvent is selected from any one or more of ethylene carbonate (EC), dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC) or polycarbonate (PC).

[0041] See also Figure 1 As shown, in one embodiment of the present invention, the positive electrode sheet 100, the separator 200 and the negative electrode sheet 300 are stacked in sequence, so that the separator 200 is located between the positive electrode and the negative electrode to play a role of isolation. Then, the stack is wrapped with an aluminum plastic film, transferred to a vacuum oven and dried at 100-130°C, and sealed after injecting the electrolyte 400, and the amount of the injected electrolyte is, for example, 3.0g / Ah. After the injection, after the formation and aging process, a soft-pack battery with a capacity of, for example, 1Ah, that is, a lithium-ion battery, is finally prepared.

[0042] Hereinafter, the present invention will be explained in more detail by citing examples, which should not be construed as limiting. Appropriate modifications may be made within the scope consistent with the gist of the present invention, all of which fall within the technical scope of the present invention.

[0043] Example 1

[0044] Positive electrode material preparation: 98% LiMn 0.6 Fe 0.4 PO4@C with 2% median particle size D 508.3μm Li 0.5 NiO2 mixed.

[0045] Preparation of positive electrode: After mixing the above positive electrode active materials, SP and PVDF in a weight ratio of 97:1.5:1.5, NMP was added and stirred in a vacuum mixer until the system was uniform to obtain positive electrode slurry. The positive electrode slurry was evenly coated on aluminum foil, which was placed in a blast drying oven and dried at 120°C for 10 minutes. The dried electrode was rolled and cut to make positive electrode sheets.

[0046] Preparation of lithium battery: The positive electrode plate, the separator and the negative electrode plate are stacked in sequence, the stack is wrapped with aluminum-plastic film, the electrolyte is injected and sealed, and after the formation and aging process, a soft-pack battery with a capacity of 1Ah, i.e., a lithium-ion battery, is finally prepared.

[0047] Example 2

[0048] LiMn 0.6 Fe 0.4 PO4@C was changed to LiFePO4@C, and other operations were the same as those in Example 1.

[0049] Example 3

[0050] LiMn 0.6 Fe 0.4 PO4@C to LiNi 0.9 Co 0.06 Mn 0.04 O2, other operations are the same as those in Example 1.

[0051] Example 4

[0052] LiMn 0.6 Fe 0.4 PO4@C to Li 1.1 Ni 0.45 Mn 0.55 O 2.1 @C, other operations are the same as those in Example 1.

[0053] Example 5

[0054] LiMn 0.6 Fe 0.4 PO4@C was replaced by LiCoO2@C, and other operations were the same as those in Example 1.

[0055] Example 6

[0056] LiMn 0.6 Fe 0.4 PO4@C to LiNi 1.5 Mn 0.5O4@C, other operations are the same as those in Example 1.

[0057] Example 7

[0058] Li 0.5 NiO2 to Li 0.5 FeO2, other operations are the same as in Example 1.

[0059] Example 8

[0060] Li 0.5 NiO2 to Li 0.5 CoO2, other operations are the same as those in Example 1.

[0061] Example 9

[0062] Li 0.5 NiO2 to Li 0.3 NiO2, other operations are the same as those in Example 1.

[0063] Example 10

[0064] Li 0.5 NiO2 to Li 0.7 NiO2, other operations are the same as those in Example 1.

[0065] Embodiment 11

[0066] Li 0.5 NiO2 is changed to LiNiO2, and other operations are the same as those in Example 1.

[0067] Example 12

[0068] Li 0.5 NiO2 was changed to NiO2, and other operations were the same as those in Example 1.

[0069] Embodiment 13

[0070] Li 0.5 NiO2 to Li 0.3 FeO2, other operations are the same as in Example 1.

[0071] Embodiment 14

[0072] Li 0.5 NiO2 to Li 0.7 FeO2, other operations are the same as in Example 1.

[0073] Embodiment 15

[0074] Li 0.5 NiO2 is changed to LiFeO2, and other operations are the same as those in Example 1.

[0075] Example 16

[0076] Li 0.5 NiO2 to Li 0.3 CoO2, other operations are the same as those in Example 1.

[0077] Embodiment 17

[0078] Li 0.5 NiO2 to Li 0.7 CoO2, other operations are the same as those in Example 1.

[0079] Embodiment 18

[0080] Li 0.5 NiO2 is changed to LiCoO2, and other operations are the same as those in Example 1.

[0081] Embodiment 19

[0082] Li 0.5 NiO2 is changed to CoO2, and other operations are the same as those in Example 1.

[0083] Embodiment 20

[0084] Li 0.5 The median particle size of NiO2 is D 50 The diameter is changed to 1.2 μm, and the other operations are the same as those in Example 1.

[0085] Embodiment 21

[0086] Li 0.5 The median particle size of NiO2 is D 50 The diameter was changed to 4.5 μm, and the other operations were the same as those in Example 1.

[0087] Embodiment 22

[0088] Li 0.5 The median particle size of NiO2 is D 50 The thickness was changed to 0.5 μm, and the other operations were the same as those in Example 1.

[0089] Embodiment 23

[0090] Li 0.5 The median particle size of NiO2 is D 50 The diameter is changed to 12.6 μm, and the other operations are the same as those in Example 1.

[0091] Embodiment 24

[0092] LiMn 0.6 Fe 0.4 PO4@C and Li0.5 The mass ratio of NiO2 was changed to 99:1, and the other operations were the same as in Example 1.

[0093] Embodiment 25

[0094] LiMn 0.6 Fe 0.4 PO4@C and Li 0.5 The mass ratio of NiO2 was changed to 95:5, and the other operations were the same as in Example 1.

[0095] Embodiment 26

[0096] LiMn 0.6 Fe 0.4 PO4@C and Li 0.5 The mass ratio of NiO2 was changed to 93:7, and the other operations were the same as in Example 1.

[0097] Embodiment 27

[0098] LiMn 0.6 Fe 0.4 PO4@C and Li 0.5 The mass ratio of NiO2 was changed to 90:10, and the other operations were the same as in Example 1.

[0099] Embodiment 28

[0100] LiMn 0.6 Fe 0.4 PO4@C and Li 0.5 The mass ratio of NiO2 was changed to 99.5:0.5, and the other operations were the same as in Example 1.

[0101] Embodiment 29

[0102] LiMn 0.6 Fe 0.4 PO4@C and Li 0.5 The mass ratio of NiO2 was changed to 88:12, and the other operations were the same as in Example 1.

[0103] Comparative Example 1

[0104] The positive electrode active material is LiMn 0.6 Fe 0.4 PO4@C, other operations are the same as those in Example 1.

[0105] Comparative Example 2

[0106] The positive electrode active material is LiFePO4@C, and other operations are the same as those in Example 1.

[0107] Comparative Example 3

[0108] The positive electrode active material is LiNi 0.9 Co 0.06 Mn 0.04 O2@C, other operations are the same as those in Example 1.

[0109] Comparative Example 4

[0110] The positive electrode active material is Li 1.1 Ni 0.45 Mn 0.55 O 2.1 @C, other operations are the same as those in Example 1.

[0111] Comparative Example 5

[0112] The positive electrode active material is LiCoO2@C, and other operations are the same as those in Example 1.

[0113] Comparative Example 6

[0114] The positive electrode active material is LiNi 1.5 Mn 0.5 O4@C, other operations are the same as those in Example 1.

[0115] The pole piece compaction density test is to take a bare foil with a diameter of 14mm and a foil containing active substances, weigh their masses, and record them as m1 and m2 respectively. The thickness of the foil is recorded as d1. Rolling is performed using a pressure of 12MPa, and the thickness after rolling is measured and recorded as d2. The pole piece compaction density under 12MPa is: (m2-m1) / (Π*0.07*0.07) / (d2-d1). Under the same pressure, the higher the pole piece compaction, the lower the elongation, which means that the processing performance of this active substance is better.

[0116] The cycle test is carried out in the range of 2.5V-4.2V, at 45℃, with 500 cycles of charge and discharge at 1C, and the capacity ratio of the 500th cycle to the 1st cycle is recorded as its capacity retention rate.

[0117] The storage test is performed at 60°C with a full charge of 4.2V, and the capacity ratio on the 30th day to the 1st day is recorded as the storage capacity retention rate.

[0118] The storage volume growth rate test is performed at 60°C with 4.2V full charge storage, and the volume difference between the 30th day and the 1st day is recorded. This value divided by the volume on the first day is the storage volume growth rate.

[0119] The test of the dissolution amount of metal Mn is to disassemble the battery cell after the cycle is completed and use the ICP method (inductively coupled plasma) to test the metal element content of the negative electrode plate.

[0120] The positive electrode active materials in each embodiment and each comparative example were used to prepare lithium batteries, and the performance of the lithium batteries was tested. The test results are shown in Table 1.

[0121] Table 1. Performance of lithium batteries in various embodiments and comparative examples

[0122]

[0123]

[0124]

[0125]

[0126] See also Figure 1 As shown in Table 1, in combination with Examples 1-6 and Comparative Examples 1-6, in Comparative Examples 1-6, the first positive electrode active material such as LiMn is used alone. 0.6 Fe 0.4 PO4@C, LiFePO4@C, LiNi 0.9 Co 0.06 Mn 0.04 O2@C、Li 1.1 Ni 0.45 Mn 0.55 O 2.1 @C, LiCoO2@C or LiNi 1.5 Mn 0.5 O4@C, the battery capacity retention rate after 500 cycles at 45°C was 91.3%, 93.3%, 86.5%, 91.4%, 84.8% or 78.8% respectively. In Examples 1-6, a second positive electrode active material, such as Li 0.5 NiO2, the battery's 45°C cycle 500 cycle capacity retention rate reached 92.8%, 94.3%, 88.4%, 93.4%, 86.2% and 81.9% respectively, which was 1%-3.1% higher than that of the battery using the first positive electrode active material alone, and the 60°C storage capacity retention rate of the lithium battery was improved, and the 60°C storage volume growth rate was reduced. In Comparative Example 1, the measured metal Mn dissolution amount was 600ppm, while the metal Mn dissolution amount of Example 1 was only 200ppm. According to Figure 1 As shown, in Comparative Example 1, only LiMn 0.6 Fe 0.4 PO4@C is used as the active material, while LiMn 0.6 Fe 0.4 PO4@C and Li 0.5NiO2 mixed, the capacity retention rate of the lithium battery in Example 1 after 500 cycles at 45°C is significantly higher. It can be seen that by adding the second positive electrode active material to the first positive electrode active material for compounding, the second positive electrode active material can effectively alleviate the phenomenon of metal dissolution in the first positive electrode active material, thereby effectively improving various performances of the battery.

[0127] Please refer to Table 1, combining Examples 24-27 with Examples 28-29, in Example 28, LiMn 0.6 Fe 0.4 PO4@C and Li 0.5 The mass ratio of NiO2 is 99.5:0.5, and the battery's 45°C cycle 500 cycle capacity retention rate, 60°C storage capacity retention rate and 60°C storage volume growth rate are 91.7%, 89.8% and 6.4% respectively. In Example 29, LiMn 0.6 Fe 0.4 PO4@C and Li 0.5 The mass ratio of NiO2 is 88:12, and the battery's 45°C cycle 500 cycle capacity retention rate, 60°C storage capacity retention rate, and 60°C storage volume growth rate are 91.7%, 89.9%, and 6.3%, respectively. 0.6 Fe 0.4 PO4@C and Li 0.5 When the mass ratio of NiO2 is 90:10-99:1, the performance of the battery is improved. For example, the capacity retention rate after 500 cycles at 45°C can reach up to 93.5%, the storage capacity retention rate at 60°C can reach up to 91.2%, and the storage volume growth rate at 60°C can be reduced to 5.1%. It can be seen that when the mass ratio of the first positive electrode active material to the second positive electrode active material is 90:10-99:1, the two particles are evenly distributed and the battery performance is the best. When the content of the second positive electrode active material is too low and less than 1%, it is impossible to effectively improve the metal dissolution of the first positive electrode active material. When the content of the second positive electrode active material is too high and higher than 10%, it will cause the first positive electrode active material to be unevenly distributed in the electrode sheet. Both of these situations will affect the performance of the battery.

[0128] Please refer to Table 1, combining Example 1 and Examples 20-21 with Examples 22-23, in Example 22, Li 0.5 The median particle size of NiO2 is D 50 The cell thickness is 0.5 μm, and the battery capacity retention rate after 500 cycles at 45°C, the storage capacity retention rate at 60°C, and the storage volume growth rate at 60°C are 91.9%, 89.7%, and 6.6%, respectively. 0.5 The median particle size of NiO2 is D 50The cell thickness is 12.6 μm, and the battery capacity retention rate after 500 cycles at 45°C, the storage capacity retention rate at 60°C, and the storage volume growth rate at 60°C are 92.1%, 90.5%, and 6.5%, respectively. 0.5 The median particle size of NiO2 is D 50 The median particle size D of the second positive electrode active material is 1-10 μm, and the performance of the battery is improved. For example, the capacity retention rate after 500 cycles at 45 ° C can reach 92.8%, the storage capacity retention rate at 60 ° C can reach 90.8%, and the storage volume growth rate at 60 ° C can be reduced to 5.3%. 50 When the median particle size D of the second positive electrode active material is 1-10 μm, the two particles are evenly distributed and the battery performance is optimal. 50 When the particle size is too small and less than 1 μm, the specific surface area of ​​the particles is too high, which affects the processing of the electrode sheet. 50 When the diameter is too large and greater than 10 μm, the first positive electrode active material will be unevenly distributed. Both of these situations will affect the performance of the battery.

[0129] As shown in Table 1, the positive electrode active material proposed in the present invention is prepared into a positive electrode sheet, and the compaction density of the positive electrode sheet reaches 2.44-3.68 g / cm 3 The positive electrode sheet is prepared into a lithium battery. The capacity retention rate of the lithium battery after 500 cycles at 45°C can reach 90.8%-94.3%, the storage capacity retention rate at 60°C can reach 90.4%-92.8%, and the storage volume growth rate at 60°C can be reduced to 3.5%-5.3%.

[0130] In summary, the present invention provides a lithium-ion battery positive electrode material, a positive electrode plate and a lithium-ion battery, which can effectively improve the metal dissolution of the battery and other problems by adding a second positive electrode active material to a nickel-cobalt-manganese ternary material, lithium iron phosphate, lithium iron manganese phosphate or a lithium-rich manganese-based material and other positive electrode active materials, so that the dissolution amount of metal Mn is less than 500ppm, thereby improving the stability of various battery performances. By selecting the median particle size of the second positive electrode active material and selecting the mass ratio of the two active materials, it is ensured that the particles of the two active materials are evenly distributed, thereby improving the processing quality of the plate, thereby improving the volume energy density of the battery, thereby improving the cycle performance and storage performance of the battery, and improving the volume expansion of the battery.

[0131] The above description is only a preferred embodiment of the present application and an explanation of the technical principles used. Those skilled in the art should understand that the scope of the invention involved in the present application is not limited to the technical solution formed by a specific combination of the above-mentioned technical features, but should also cover other technical solutions formed by any combination of the above-mentioned technical features or their equivalent features without departing from the inventive concept, such as a technical solution formed by replacing the above-mentioned features with (but not limited to) technical features with similar functions disclosed in this application.

[0132] Except for the technical features described in the specification, the remaining technical features are known technologies to those skilled in the art. In order to highlight the innovative features of the present invention, the remaining technical features will not be described here in detail.

Claims

1. A positive electrode material for a lithium ion battery, characterized in that: At least the following components are included: A first positive electrode active material, wherein the first positive electrode active material includes any one or more of a nickel-cobalt-manganese ternary material, lithium iron phosphate, lithium iron manganese phosphate, a lithium-rich manganese-based material, lithium cobalt oxide, or lithium nickel manganese oxide; The second positive electrode active material has a chemical formula of Li x M 1-y N y O 4-z , wherein 0.05≤x≤6, 0≤y≤1, 0≤z≤2, the element M includes any one or more of Fe, Ni or Co, and the element N includes any one or more of Al, Mn, Ti, Si or Cu.

2. The lithium-ion battery positive electrode material according to claim 1, characterized in that The mass ratio of the first positive electrode active material to the second positive electrode active material is 90:10 to 99:

1.

3. The positive electrode material for lithium-ion batteries according to claim 1, characterized in that: The median particle size D of the first positive electrode active material 50 The median particle size D of the second positive electrode active material 50 The ratio is 1.25-12.

5.

4. The lithium-ion battery positive electrode material according to claim 1, characterized in that The median particle size D of the first positive electrode active material 50 The median particle size D of the second positive electrode active material is 0.8 μm-9.2 μm. 50 1μm-10μm.

5. The lithium-ion battery positive electrode material according to claim 1, characterized in that: The surface of the first positive electrode active material is coated with a carbon layer, and the coating amount of the carbon is 1%-3% of the mass of the first positive electrode active material.

6. The lithium-ion battery positive electrode material according to claim 1, characterized in that: The general chemical formula of the nickel-cobalt-manganese ternary material is LiNi x Co y Mn 1-x-y O2, where 0.9≤x≤1, 0≤y≤0.

06.

7. The positive electrode material for lithium-ion batteries according to claim 1, characterized in that: The general chemical formula of the lithium manganese iron phosphate is LiMn x Fe 1-x PO4, where 0.5≤x≤1.

8. The lithium-ion battery positive electrode material according to claim 1, characterized in that: The general chemical formula of the lithium-rich manganese-based material is Li 1+x Mn a Ni b O 2-c , where 0<x≤0.3, 0.5<a≤1, 0≤b<0.5, x+a+b+c=1.

9. A positive electrode sheet, characterized in that: The invention comprises a lithium-ion battery positive electrode material as claimed in any one of claims 1 to 8.

10. A lithium ion battery, characterized in that: Comprising the positive electrode sheet as described in claim 9.

11. A lithium ion battery according to claim 10, characterized in that: The amount of metal Mn dissolved in the lithium ion battery is ≤500ppm.

Citation Information

Cited By

  • Positive plate, battery comprising positive plate and electric device

    CN120809740A

  • Nonaqueous electrolyte secondary battery positive electrode and nonaqueous electrolyte secondary battery

    WO2026071174A1