Layered oxide positive electrode material and preparation method thereof, positive plate and sodium ion battery

By adopting the dual fluorination strategy of fluorine doping and sodium fluoride coating in layered oxide positive electrode materials, the problem of instability of the material in the air is solved, its air stability and circulation performance are improved, and sodium is improved Performance and energy density of ion batteries.

CN118943330APending Publication Date: 2024-11-12JIANGSU ZENIO NEW ENERGY BATTERY TECH CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411025738.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

After exposure to the air, the layered oxide positive electrode material causes structural and chemical integrity loss due to reaction with carbon dioxide and moisture, lacks air stability, and affects the performance and cycling performance of sodium ion batteries.

Method used

The layered oxide material is used to dopant fluorine and form a sodium fluoride coating layer on its surface. The electronegativity and stability of the material are improved by trace F doping and NaF coating layer, inhibit the reaction of water molecules in the air, and The residual alkali on the surface is safely and effectively converted into a NaF coating by ion exchange.

Benefits of technology

It significantly improves the air stability and circulation performance of the material, improves the average working voltage and overall energy density of the material, and improves the processing performance and conductivity of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118943330A_ABST
    Figure CN118943330A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of batteries, in particular to a layered oxide positive electrode material, a preparation method thereof, a positive plate and a sodium ion battery. The layered oxide positive electrode material comprises a substrate and a coating layer arranged on at least part of the surface of the substrate, the substrate comprises a fluorine-doped layered oxide; and the coating layer comprises sodium fluoride. According to the double-fluorinated layered oxide material provided by the invention, the air stability of the layered oxide material is improved, the structure of the material is greatly stabilized, the average working voltage of the material is improved, and the overall energy density of the material is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of battery technology, and in particular to layered oxide positive electrode materials and preparation methods thereof, positive electrode sheets and sodium ion batteries. Background Art

[0002] With the increasing demand for energy and growing concerns about the environment, sodium-ion batteries have received great attention in recent years as a potential alternative to lithium-ion batteries, thanks to their low cost, environmentally friendly and abundant raw materials. In particular, O3-type layered oxide cathode materials have attracted widespread attention in the market due to their high capacity and abundant precursor resources. However, the poor air stability of these materials is a major obstacle to their commercialization. Both carbon dioxide and moisture can cause the cathode materials to deteriorate even after a few hours of exposure to air, resulting in a loss of structural and chemical integrity. The air stability of cathode materials is critical to battery manufacturing, storage, performance and long-term cycling. Summary of the invention

[0003] In view of this, the present invention provides a layered oxide positive electrode material and a preparation method thereof, a positive electrode sheet and a sodium ion battery. The layered oxide positive electrode material effectively improves the air stability of the material, and the double fluorination modification stabilizes the material structure and improves the cycle performance of the material.

[0004] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0005] In a first aspect, the present invention provides a layered oxide positive electrode material, the layered oxide positive electrode material comprising a substrate, and a coating layer disposed on at least a portion of the surface of the substrate;

[0006] The substrate includes a fluorine-doped layered oxide;

[0007] The coating includes sodium fluoride.

[0008] In an embodiment of the present invention, the chemical formula of the fluorine-doped layered oxide is Na x Ni i Fe j Mn k M m O 2-y F y ,

[0009] Wherein, M is at least one of Li, B, Mg, Al, K, Ca, Ti, Co, V, Cr, Cu, Zn, Zr, Nb and Sn;

[0010] 0.6 < x ≤ 1, 0 < i ≤ 0.4, 0 < j ≤ 0.5, 0 < k ≤ 0.6, 0 < m ≤ 0.2, 0.03 ≤ y ≤ 0.15; and i + j + k + m = 1.

[0011] In the embodiment of the present invention, there is no residual alkali between the matrix and the coating layer.

[0012] In the embodiment of the present invention, the residual alkali includes sodium carbonate and sodium hydroxide.

[0013] Preferably, the thickness of the coating layer is 6 - 20 nm.

[0014] More preferably, the thickness of the coating layer is 8 - 15 nm.

[0015] In a second aspect, the present invention provides a method for preparing the above-mentioned layered oxide cathode material, comprising the following steps:

[0016] S1, Mix the Ni i Fe j Mn k M m (OH)2 precursor, sodium source, and fluorine source evenly to obtain a mixture; perform a first sintering on the mixture and cool it naturally to obtain a fluorine-doped layered oxide.

[0017] S2, Mix the fluorine-doped layered oxide with an ammonium fluoride solution, after a chemical reaction, filter and dry it to obtain a fluorine-doped layered oxide material initially coated with sodium fluoride; perform a second sintering on the fluorine-doped layered oxide material initially coated with sodium fluoride to obtain a layered oxide cathode material.

[0018] In the embodiment of the present invention, the sodium source includes but is not limited to at least one of sodium carbonate, sodium hydroxide, sodium acetate, sodium oxalate, and sodium nitrate.

[0019] In the embodiment of the present invention, the fluorine source includes but is not limited to at least one of sodium fluoride, ammonium fluoride, and ammonium bifluoride.

[0020] Preferably, the molar ratio of sodium in the Ni i Fe j Mn k M m (OH)2 precursor, sodium in the sodium source, and fluorine in the fluorine source is 1:(1.03 - 1.05):(0.03 - 0.15).

[0021] Preferably, the concentration of the ammonium fluoride solution is 0.3 - 0.8 mol / L.

[0022] In the embodiment of the present invention, the solvent of the ammonium fluoride solution is at least one of methanol, tetrahydrofuran, and dimethylformamide.

[0023] Preferably, the mass ratio of the fluorine-doped layered oxide to the ammonium fluoride solution is 1:(10-20).

[0024] Preferably, in step S1, the heating rate of the first sintering is 1-10°C / min, the holding temperature of the first sintering is 750-1100°C, and the time of the first sintering is 8-20h.

[0025] In an embodiment of the present invention, in step S2, there is residual alkali on the surface of the fluorine-doped layered oxide, and the above chemical reaction is a chemical reaction between the residual alkali on the surface of the fluorine-doped layered oxide and ammonium fluoride.

[0026] Preferably, in step S2, the temperature of the chemical reaction is 10-30° C., and the time of the chemical reaction is 20-40 min.

[0027] Preferably, in step S2, the heating rate of the second sintering is 1-10°C / min, the holding temperature of the second sintering is 400-600°C, and the time of the second sintering is 4-8h.

[0028] In a third aspect, the present invention provides a positive electrode sheet, which includes the above-mentioned layered oxide positive electrode material, and / or the layered oxide positive electrode material prepared by the above-mentioned preparation method.

[0029] In a fourth aspect, the present invention provides a sodium ion battery comprising the above-mentioned positive electrode sheet.

[0030] Compared with the prior art, the present invention has the following beneficial effects:

[0031] The present invention adopts a double fluorination strategy of fluorine doping and fluoride coating layered oxide materials to improve the air stability of layered oxide materials. At the same time, the double fluorination strategy adopted by the present invention greatly stabilizes the material structure and improves the material's cycle performance. The strategy of using double fluorinated layered oxide positive electrode materials in the present invention has the following advantages:

[0032] 1. The bulk material is doped with trace amounts of F, and the highly electronegative F is used to stabilize the Na-O layer and the transition metal-oxygen (TM-O) layer, which improves the structural stability of the material during the process of sodium ion insertion and extraction, and at the same time improves the overall electronegativity of the material, inhibiting the H + and Na in the material + Proton exchange reaction occurs, thereby improving material properties;

[0033] 2. When the sodium-based layered oxide cathode material naturally cools down after sintering, it will react with carbon dioxide and water molecules in the air to automatically generate residual alkali (sodium carbonate and sodium hydroxide). Reaction with ammonium fluoride can convert the residual alkali (Na2CO3, NaOH) on the surface of the layered oxide material into a NaF coating layer, which, on the one hand, reduces the overall alkalinity of the material and is beneficial to improving the processing performance of the material; on the other hand, NaF is poorly soluble in water and is more stable in the air than residual alkali (Na2CO3, NaOH). The introduction of the NaF coating layer improves the air stability of the material; the introduction of the NaF coating layer also avoids the positive electrode contact between the material and the electrolyte, inhibiting the generation of side reactions;

[0034] 3. NaF has good electrical conductivity. Converting the residual alkali on the surface of the material into a NaF coating layer also improves the overall electrical conductivity of the material and improves the rate performance of the material;

[0035] 4. Common NaF generation reactions inevitably produce dangerous HF gas. The present invention provides an ion exchange method to directly convert the residual alkali on the surface of the material into a NaF coating layer. This method is safer and more effective.

[0036] 5. Double fluorination (trace F doping and NaF coating) strategy. Thanks to the strong electronegativity of F, the average working voltage of the material is also improved, which is also beneficial to improving the overall energy density of the material.

[0037] In summary, the double fluorinated layered oxide material provided by the present invention not only improves the air stability of the layered oxide material, but also greatly stabilizes the structure of the material, increases the average operating voltage of the material, and improves the overall energy density of the material. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] Figure 1 Schematic diagram of a double fluorinated layered oxide material; wherein 1 represents a substrate; 2 represents a coating layer;

[0039] Figure 2 X-ray diffraction patterns of the unexposed air sample and the exposed air environment sample of Example 1;

[0040] Figure 3 X-ray diffraction patterns of the samples not exposed to air and the samples exposed to air environment in Comparative Example 2. DETAILED DESCRIPTION

[0041] The present invention discloses a layered oxide positive electrode material and a preparation method thereof, a positive electrode sheet and a sodium ion battery. Those skilled in the art can refer to the content of this article and appropriately improve the process parameters to achieve the same. It should be particularly noted that all similar substitutions and modifications are obvious to those skilled in the art, and they are all deemed to be included in the present invention. The methods and applications of the present invention have been described through preferred embodiments, and relevant personnel can obviously modify or appropriately change and combine the methods and applications described herein without departing from the content, spirit and scope of the present invention to implement and apply the technology of the present invention.

[0042] In the description of the present invention, it should be noted that the terms "first", "second", etc. are only used for descriptive purposes, and do not indicate or imply relative importance.

[0043] In the description of the present invention, a list of items connected by the term "at least one of" or other similar terms may mean any combination of the listed items. For example, if items A, B are listed, the phrase "at least one of A, B" means only A; only B; or A and B. In another example, if items A, B, C are listed, the phrase "at least one of A, B, C" means only A; or only B; only C; A and B (excluding C); A and C (excluding B); B and C (excluding A); or all of A, B, and C. Item A may include a single element or multiple elements. Item B may include a single element or multiple elements. Item C may include a single element or multiple elements.

[0044] The endpoints and any values ​​of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range or the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.

[0045] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.

[0046] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.

[0047] If there is no special explanation, the "include" and "comprising" mentioned in this application are open-ended or closed-ended. For example, the "include" and "comprising" may mean that other components not listed may also be included or only the listed components may be included or only the listed components may be included.

[0048] Specifically, the present invention adopts the following technical solutions:

[0049] In a first aspect, the present invention provides a layered oxide cathode material, which includes a matrix and a coating layer disposed on at least a part of the surface of the matrix;

[0050] The matrix includes a fluorine-doped layered oxide;

[0051] The coating layer includes sodium fluoride.

[0052] In an embodiment of the present invention, the chemical formula of the fluorine-doped layered oxide is Na x Ni i Fe j Mn k M m O 2-y F y ,

[0053] wherein M is at least one of Li, B, Mg, Al, K, Ca, Ti, Co, V, Cr, Cu, Zn, Zr, Nb, and Sn;

[0054] 0.6 < x ≤ 1, 0 < i ≤ 0.4, 0 < j ≤ 0.5, 0 < k ≤ 0.6, 0 < m ≤ 0.2, 0.03 ≤ y ≤ 0.15; and i + j + k + m = 1.

[0055] In an embodiment of the present invention, x, i, j, k, m, and y are respectively the molar ratios of the corresponding elements.

[0056] In an embodiment of the present invention, when 0.6 < x ≤ 0.8, the fluorine-doped layered oxide is a P2-phase layered oxide; when 0.8 < x ≤ 1, the fluorine-doped layered oxide is an O3-phase layered oxide.

[0057] In the present invention, 0.03 ≤ y ≤ 0.15. When the fluorine doping ratio is too high, the specific capacity of the material will be affected; when the fluorine doping ratio is too low, the Na-O layer and the transition metal-oxygen (TM-O) layer cannot be effectively stabilized, and the role of structural stability cannot be achieved.

[0058] In an embodiment of the present invention, there is no residual alkali between the matrix and the coating layer. In an embodiment of the present invention, the residual alkali on the surface of the matrix raw material is used as a sodium source for preparing sodium fluoride in the coating layer.

[0059] In an embodiment of the present invention, the residual alkali includes sodium carbonate and sodium hydroxide.

[0060] Preferably, the thickness of the coating layer is 6 - 20 nm. Exemplarily, the thickness of the coating layer is any value among 6 nm, 8 nm, 10 nm, 12 nm, 14 nm, 15 nm, 16 nm, 18 nm, 20 nm or any value within the range composed of any two of the above values.

[0061] Preferably, the coating layer has a thickness of 8 to 15 nm.

[0062] In a second aspect, the present invention provides a method for preparing the above-mentioned layered oxide positive electrode material, comprising the following steps:

[0063] S1, Ni i Fe j Mn k M m The (OH)2 precursor, the sodium source and the fluorine source are uniformly mixed to obtain a mixture; the mixture is first sintered and naturally cooled to obtain a fluorine-doped layered oxide;

[0064] S2, mixing the fluorine-doped layered oxide with the ammonium fluoride solution, filtering and drying after chemical reaction to obtain the fluorine-doped layered oxide material initially coated with sodium fluoride; performing a second sintering on the fluorine-doped layered oxide material initially coated with sodium fluoride to obtain a layered oxide positive electrode material.

[0065] In an embodiment of the present invention, the sodium source includes but is not limited to at least one of sodium carbonate, sodium hydroxide, sodium acetate, sodium oxalate, and sodium nitrate.

[0066] In an embodiment of the present invention, the fluorine source includes but is not limited to at least one of sodium fluoride, ammonium fluoride, and ammonium bifluoride.

[0067] Preferably, Ni i Fe j Mn k M m The molar ratio of the (OH)2 precursor, the sodium in the sodium source, and the fluorine in the fluorine source is 1:(1.03-1.05):(0.03-0.15). Exemplarily, the molar ratio of the precursor, the sodium in the sodium source, and the fluorine in the fluorine source is any of 1:1.04:0.08, 1:1.04:0.03, 1:1.04:0.15, 1:1.03:0.15, 1:1.05:0.03, or any value within the range consisting of any two of the above values.

[0068] Preferably, the concentration of the ammonium fluoride solution is 0.3-0.8 mol / L. Exemplarily, the concentration of the ammonium fluoride solution is any value among 0.3 mol / L, 0.4 mol / L, 0.5 mol / L, 0.6 mol / L, 0.7 mol / L, 0.8 mol / L, or any value within the range consisting of any two of the above values.

[0069] In the embodiment of the present invention, the solvent of the ammonium fluoride solution is at least one of methanol, tetrahydrofuran and dimethylformamide. The ammonium fluoride solution cannot use water as a solvent, otherwise the layered oxide will react with water, resulting in a decrease in material performance.

[0070] Preferably, the mass ratio of the fluorine-doped layered oxide to the ammonium fluoride solution is 1:(10-20). Exemplarily, the mass ratio of the fluorine-doped layered oxide to the ammonium fluoride solution is any value among 1:10, 1:11, 1:12, 1:13, 1:14, 1:15, 1:16, 1:17, 1:18, 1:19, 1:20 or any value within the range consisting of any two of the above values.

[0071] In an embodiment of the present invention, the mixing in step S1 is performed by ball milling at a rotation speed of 300 to 800 r / min for 0.5 to 5 h.

[0072] Preferably, in step S1, the heating rate of the first sintering is 1-10°C / min, the holding temperature of the first sintering is 750-1100°C, and the time of the first sintering is 8-20h. Exemplarily, the heating rate of the first sintering is any value in 1°C / min, 2°C / min, 3°C / min, 4°C / min, 5°C / min, 6°C / min, 7°C / min, 8°C / min, 9°C / min, 10°C / min, or any value in the range of any two of the above values, the holding temperature of the first sintering is any value in 750°C, 800°C, 850°C, 900°C, 950°C, 1000°C, 1050°C, 1100°C, or any value in the range of any two of the above values, and the time of the first sintering is any value in 8h, 10h, 12h, 14h, 16h, 18h, 20h, or any value in the range of any two of the above values.

[0073] In an embodiment of the present invention, in step S2, there is residual alkali on the surface of the fluorine-doped layered oxide, and the above chemical reaction is a chemical reaction between the residual alkali on the surface of the fluorine-doped layered oxide and ammonium fluoride. The fluorine-doped layered oxide, the positive electrode material of the sodium ion battery, will react with carbon dioxide and water molecules in the air to automatically generate residual alkali (sodium carbonate and sodium hydroxide) during sintering and cooling. Therefore, in step S2, there are residual alkalis such as sodium carbonate and sodium hydroxide on the surface of the fluorine-doped layered oxide raw material. The present invention uses a chemical reaction between ammonium fluoride and two residual alkalis to prepare a sodium fluoride coating layer, and the chemical reaction equation is as follows:

[0074] Ion exchange reaction equation: 2NH4F+Na2CO3→2NaF+(NH4)2CO3

[0075] Acid-base neutralization reaction equation: NH4F+NaOH→NaF+NH3+H2O

[0076] Preferably, in step S2, the temperature of the chemical reaction is 10-30°C, and the time of the chemical reaction is 20-40min. Exemplarily, the temperature of the chemical reaction is any value in 10°C, 12°C, 14°C, 16°C, 18°C, 20°C, 22°C, 24°C, 26°C, 28°C, 30°C, or any value in the range of any two of the above values. In a specific embodiment of the present invention, the temperature of the chemical reaction is room temperature; the time of the chemical reaction is any value in 20min, 22min, 24min, 26min, 28min, 30min, 32min, 34min, 36min, 38min, 40min, or any value in the range of any two of the above values. When the reaction time of the chemical reaction is too short, the residual alkali and ammonium fluoride cannot fully react, and an effective sodium fluoride coating layer cannot be formed, which leads to an insignificant improvement in the air stability of the material, affecting the rate and cycle performance of the material; when the reaction time of the chemical reaction is too long, the sodium fluoride coating layer formed is too thick, affecting the gram capacity of the material.

[0077] In an embodiment of the present invention, the steps of reacting the residual alkali on the surface of the fluorine-doped layered oxide with the ammonium fluoride solution, filtering, and drying in step S2 are all performed in a fume hood.

[0078] Preferably, in step S2, the heating rate of the second sintering is 1 to 10°C / min, the holding temperature of the second sintering is 400 to 600°C, and the time of the second sintering is 4 to 8h. Exemplarily, the heating rate of the second sintering is any value in 1°C / min, 2°C / min, 3°C / min, 4°C / min, 5°C / min, 6°C / min, 7°C / min, 8°C / min, 9°C / min, 10°C / min or any value in the range of any two of the above values, the holding temperature of the second sintering is any value in 400°C, 450°C, 500°C, 550°C, 600°C or any value in the range of any two of the above values, and the time of the second sintering is any value in 4h, 5h, 6h, 7h, 8h or any value in the range of any two of the above values.

[0079] In a third aspect, the present invention provides a positive electrode sheet, which includes the above-mentioned layered oxide positive electrode material, and / or the layered oxide positive electrode material prepared by the above-mentioned preparation method.

[0080] In an embodiment of the present invention, the positive electrode sheet includes a positive electrode current collector and a positive electrode active material layer disposed on at least one surface of the positive electrode current collector in a thickness direction.

[0081] In an embodiment of the present invention, the positive electrode active material layer includes the layered oxide positive electrode material of the present invention, a conductive agent and a binder.

[0082] Preferably, the mass ratio of the layered oxide positive electrode material, the conductive agent and the binder is (80-98): (1-10): (1-10). Exemplarily, the mass ratio of the layered oxide positive electrode material, the conductive agent and the binder is 80:10:10, 90:6:4, 98:1:1, etc.

[0083] In the embodiment of the present invention, the conductive agent includes but is not limited to at least one of Super P, acetylene black, Ketjen black, and conductive graphite. In addition to the several specific substances listed above, other types of conductive agents recognized by those skilled in the art are within the protection scope of the present invention.

[0084] In the embodiment of the present invention, the binder includes but is not limited to at least one of polyvinylidene fluoride (PVDF), styrene butadiene rubber (SBR), sodium carboxymethyl cellulose (CMC), polyacrylate (LA), and polyacrylic acid binder (PAA). In addition to the several specific substances listed above, other types of binders recognized by those skilled in the art are within the scope of protection of the present invention.

[0085] The present application has no particular limitation on the method for preparing the positive electrode sheet. Those skilled in the art can prepare the positive electrode sheet according to conventional preparation methods as long as the purpose of the present application can be achieved.

[0086] In a fourth aspect, the present invention provides a sodium ion battery comprising the above-mentioned positive electrode sheet.

[0087] In the embodiment of the present invention, the battery structure includes but is not limited to button batteries, soft-pack batteries, cylindrical batteries, etc.

[0088] The present application has no particular restrictions on the negative electrode sheet, separator, and electrolyte in the battery, and those skilled in the art can select them according to actual needs as long as the purpose of the present application can be achieved.

[0089] The reagents, instruments or materials used in the present invention can be obtained through commercial channels.

[0090] The present invention will be further described below in conjunction with embodiments:

[0091] Embodiment 1:

[0092] like Figure 1 As shown, the layered oxide positive electrode material of this embodiment includes a substrate 1 and a coating layer 2 arranged on the surface of the substrate. The substrate includes a fluorine-doped layered oxide, and its chemical formula is NaNi 0.28 Fe 0.33 Mn 0.34 Ti 0.05 O 1.95 F 0.05The coating layer includes sodium fluoride, the sodium source of which is the residual alkali on the surface of the substrate, and the residual alkali includes sodium carbonate and sodium hydroxide; the thickness of the coating layer is 8 to 15 nm.

[0093] The preparation method of the layered oxide positive electrode material of this embodiment is as follows:

[0094] 1. Ni 0.28 Fe 0.33 Mn 0.34 Ti 0.05 The (OH)2 precursor, sodium acetate and ammonium fluoride were placed in a ball mill at a speed of 300 r / min for 2 h to fully mix them according to the molar ratio of 1:1.04:0.08; the mixed powder was placed in a muffle furnace and solid-phase sintered at 900 °C for 12 h at a heating rate of 5 °C / min, and the layered oxide material NaNi was obtained after natural cooling and grinding. 0.28 Fe 0.33 Mn 0.34 Ti 0.05 O 1.92 F 0.08 of black powder.

[0095] 2. Layered oxide material NaNi 0.28 Fe 0.33 Mn 0.34 Ti 0.05 O 1.95 F 0.05 The black powder was placed in a 0.5 mol / L ammonium fluoride solution (the solvent was methanol) for 30 min (the mass ratio of the added layered oxide to the ammonium fluoride solution was 1:15), filtered and dried to obtain a fluorine-doped layered oxide material initially coated with NaF; then it was placed in a muffle furnace and sintered at 550 °C at a heating rate of 5 °C / min for 5 h, and then naturally cooled to obtain a doubly fluorinated NaF@NaNi 0.28 Fe 0.33 Mn 0.34 Ti 0.0 5O 1.92 F 0.08 Material.

[0096] Embodiment 2:

[0097] The only difference between this embodiment and embodiment 1 is that Ni 0.28 Fe 0.33 Mn 0.34 Ti 0.05 The molar ratio of (OH)2 precursor to sodium acetate and ammonium fluoride is 1:1.04:0.03; the final material is NaF@NaNi 0.28 Fe 0.33 Mn 0.34 Ti 0.05 O1.97 F 0.03 .

[0098] Embodiment 3:

[0099] The only difference between this embodiment and embodiment 1 is that Ni 0.28 Fe 0.33 Mn 0.34 Ti 0.05 The molar ratio of (OH)2 precursor to sodium acetate and ammonium fluoride is 1:1.04:0.15; the final material is NaF@NaNi 0.28 Fe 0.33 Mn 0.34 Ti 0.05 O 1.85 F 0.15 .

[0100] Embodiment 4:

[0101] The only difference between this embodiment and Embodiment 1 is that the reaction time of the layered oxide and the ammonium fluoride solution is 20 minutes.

[0102] Embodiment 5:

[0103] The only difference between this embodiment and Embodiment 1 is that the reaction time of the layered oxide and the ammonium fluoride solution is 40 minutes.

[0104] Embodiment 6:

[0105] The only difference between this embodiment and embodiment 1 is that the precursor used is Ni 0.25 Fe 0.33 Mn 0.34 Cu 0.08 (OH)2, the final material is NaF@NaNi 0.25 Fe 0.33 Mn 0.34 Cu 0.08 O 1.92 F 0.08 .

[0106] Embodiment 7:

[0107] The only difference between this embodiment and embodiment 1 is that the precursor used is Ni 0.30 Fe 0.33 Mn 0.34 Zn 0.04 (OH)2, the final material is NaF@NaNi 0.30 Fe 0.33 Mn 0.34 Zn 0.04 O 1.92 F 0.08 .

[0108] Comparative Example 1

[0109] Compared with Example 1, this comparative example does not carry out fluorine doping and sodium fluoride coating, and the preparation method is as follows:

[0110] Ni 0.28 Fe 0.33 Mn 0.34 Ti 0.05 The (OH)2 precursor and sodium acetate were placed in a ball mill at a speed of 300 r / min for 2 h in a molar ratio of 1:1.04 to fully mix them; the mixed powder was placed in a muffle furnace and solid-phase sintered at 900 °C for 12 h at a heating rate of 5 °C / min, and the layered oxide material NaNi was obtained after natural cooling and grinding. 0.28 Fe 0.33 Mn 0.34 Ti 0.05 O2 is a black powder.

[0111] Comparative Example 2

[0112] Compared with Example 1, this comparative example only performs fluorine doping without sodium fluoride coating, and the preparation method is as follows:

[0113] Ni 0.28 Fe 0.33 Mn 0.34 Ti 0.05 The (OH)2 precursor, sodium acetate and ammonium fluoride were placed in a ball mill at a speed of 300 r / min for 2 h to fully mix them according to the molar ratio of 1:1.04:0.08; the mixed powder was placed in a muffle furnace and solid-phase sintered at 900 °C for 12 h at a heating rate of 5 °C / min, and the layered oxide material NaNi was obtained after natural cooling and grinding. 0.28 Fe 0.33 Mn 0.34 Ti 0.05 O 1.92 F 0.08 of black powder.

[0114] Comparative Example 3

[0115] Compared with Example 1, this comparative example only performs sodium fluoride coating without fluorine doping, and the preparation method is as follows:

[0116] 1. Ni 0.28 Fe 0.33 Mn 0.34 Ti 0.05The (OH)2 precursor and sodium acetate were placed in a ball mill at a speed of 300 r / min for 2 h in a molar ratio of 1:1.04 to fully mix them; the mixed powder was placed in a muffle furnace and solid-phase sintered at 900 °C for 12 h at a heating rate of 5 °C / min, and the layered oxide material NaNi was obtained after natural cooling and grinding. 0.28 Fe 0.33 Mn 0.34 Ti 0.05 O2 is a black powder.

[0117] 2. Layered oxide material NaNi 0.28 Fe 0.33 Mn 0.34 Ti 0.05 The black powder of O2 was placed in a 0.5 mol / L ammonium fluoride solution (the solvent was methanol) and reacted for 30 min (the mass ratio of the added layered oxide to the ammonium fluoride solution was 1:15), then filtered and dried to obtain the layered oxide material initially coated with NaF; then placed in a muffle furnace and sintered at 550 °C at a heating rate of 5 °C / min for 5 h, and then naturally cooled to obtain NaF@NaNi 0.28 Fe 0.33 Mn 0.34 Ti 0.05 O2. Comparative Example 4:

[0118] The only difference between this comparative example and Example 1 is that Ni 0.28 Fe 0.33 Mn 0.34 Ti 0.05 The molar ratio of (OH)2 precursor to sodium acetate and ammonium fluoride is 1:1.04:0.2; the final material is NaF@NaNi 0.28 Fe 0.33 Mn 0.34 Ti 0.05 O 1.8 F 0.2 .

[0119] Comparative Example 5:

[0120] The only difference between this comparative example and Example 1 is that the reaction time of the layered oxide and the ammonium fluoride solution is 10 minutes.

[0121] Comparative Example 6:

[0122] The only difference between this comparative example and Example 1 is that the reaction time of the layered oxide and the ammonium fluoride solution is 60 minutes.

[0123] Physical and chemical properties test of layered oxide materials

[0124] 1. Physical properties test of layered oxide materials

[0125] (1) pH value test method: Add the material powder to an appropriate amount of deionized water and stir it thoroughly to dissolve or suspend it. Then, use filter paper or centrifugation to remove suspended matter or impurities to obtain a clear solution sample. Insert the combined electrode of the pH meter into the sample to be tested, wait until the pH meter reading stabilizes, and record the pH value at this time.

[0126] (2) Whether a new phase is formed after 1 day / 3 days of exposure to the environment

[0127] Perform XRD testing on the materials exposed to the environment. By comparing the XRD diffraction patterns of the materials not exposed to the humidity environment, observe whether new diffraction peaks are generated in the XRD diffraction patterns of the materials exposed to the humidity environment to determine whether impurity phases are generated in the materials: if new diffraction peaks are generated, it indicates that new phases are generated; if no new diffraction peaks are generated, it indicates that no new phases are generated.

[0128] 2. Preparation and performance testing of sodium ion batteries

[0129] (1) Preparation of sodium ion batteries

[0130] The positive electrode materials prepared in the above examples and comparative examples are used to prepare sodium ion batteries, and the preparation method is as follows:

[0131] The positive electrode material, the conductive agent Super P, and the binder PVDF were ground evenly in a mass ratio of 8:1:1, and then an appropriate amount of NMP was added to make a slurry, which was evenly coated on the pretreated aluminum foil, dried at 80°C for 1h in a blast drying oven, and then dried at 120°C for 12h in a vacuum drying oven; then cut into 14mm round positive electrode sheets with a cutting machine. A sodium metal sheet with a diameter of 14mm and a thickness of 0.2mm was used as the negative electrode, a 0.1mol / L sodium perchlorate / ethylene carbonate (EC) / dimethyl carbonate (DMC) (the volume ratio of EC to DMC was 1:1) solution was used as the electrolyte, and a Whatman GF / F glass fiber with a diameter of 16mm was used as the diaphragm. The CR2032 button battery was assembled in a glove box filled with high-purity argon.

[0132] (2) Sodium ion battery performance test

[0133] The constant current charge and discharge mode was used to perform charge and discharge tests at a current density of XC (X = 0.1, 1, 2, 5). The test items included: the first cycle charge and discharge of the material in the sodium ion battery, rate performance, and capacity retention rate after 100 cycles of 1C charge and discharge. The discharge cut-off voltage was 2.0V and the charge cut-off voltage was 4.0V.

[0134] Discharge capacity test method: Under the condition of 25℃, charge to 4.0V with XC (X=0.1, 1, 2, 5) constant current, and then discharge to 2.0V with XC (X=0.1, 1, 2, 5) constant current. The discharge capacity at this time is recorded as the XC (X=0.1, 1, 2, 5) discharge capacity.

[0135] Capacity retention rate test method for 100 cycles of 1C charge and discharge: At 25°C, charge to 4.0V at 1C constant current, and record the charge capacity at this time as the first charge capacity; then discharge to 2.0V at 1C constant current, and record the charge capacity at this time as the first discharge capacity; repeat the above charge and discharge process, and record the discharge capacity of the 100th cycle. Capacity retention rate = discharge capacity of the 100th cycle / first charge capacity*100%.

[0136] The test results of the physicochemical properties of the layered oxide materials prepared in the examples and comparative examples are shown in Table 1.

[0137] Table 1 Test item data of embodiments and comparative examples

[0138]

[0139] In the case where the main material types of Examples 1 to 7 and Comparative Examples 1 to 6 are the same, the materials obtained by the preparation method provided by the present invention in Examples 1 to 7 have extremely excellent air stability (see Example 1 for the air stability results). Figure 2 ), and the material has good rate performance and structural stability.

[0140] Comparative Example 1 did not use the double fluorination process when the material type was the same. Compared with Examples 1 to 7, it showed extremely poor air stability, poor rate performance and cycle stability.

[0141] Comparative Example 2 has the same main material as Example 1. Comparative Example 2 only uses the fluorine doping process, and the air stability is improved to a certain extent but not significantly (see the air stability results of Comparative Example 2 Figure 3 ), the rate performance and cycle performance are poorer than those of Examples 1 to 7, but are improved compared to Comparative Example 1 which does not use the double fluorination process; this further illustrates that fluorine doping has a certain effect on improving the air stability and structural stability of the material.

[0142] Comparative Example 3 only adopted the sodium fluoride coating process, and the air stability, rate performance and cycle performance of the material were improved, and the pH value of the material was significantly reduced. This shows that the sodium fluoride coating process provided by the present invention effectively reduces the residual alkali on the surface of the material, improves the stability of the material in the air, and improves the rate and cycle performance of the material.

[0143] The difference between Comparative Example 4 and Examples 1 to 7 is that a higher proportion of fluorine doping is used, and the gram capacity of the material is significantly reduced, indicating that the content of the doped fluorine element should not be too high.

[0144] The difference between Comparative Examples 5 to 6 and Examples 1 to 7 is that the reaction time of the layered oxide in the ammonium fluoride solution is different. Comparative Example 5 uses a shorter reaction time, and the improvement of the air stability of the material is not obvious, and the rate and cycle performance are also reduced compared with Examples 1 to 7; Comparative Example 6 uses a longer reaction time, and the gram capacity of the material is significantly reduced; This shows that the reaction time of the layered oxide in the ammonium fluoride solution is related to the thickness of the sodium fluoride coating layer formed, and needs to be controlled.

[0145] The test results show that the double fluorinated layered oxide solution of the present invention reduces the residual alkali on the surface of the material and improves the rate performance and cycle stability of the material on the basis of optimizing the air stability of the material.

[0146] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A layered oxide positive electrode material, characterized in that: The layered oxide cathode material includes a matrix and a coating layer provided on at least a part of the surface of the matrix; The matrix includes a fluorine-doped layered oxide; The coating layer includes sodium fluoride.

2. The layered oxide positive electrode material according to claim 1, characterized in that The chemical formula of the fluorine-doped layered oxide is Na x Ni i Fe j Mn k M m O 2-y F y , Wherein, M is at least one of Li, B, Mg, Al, K, Ca, Ti, Co, V, Cr, Cu, Zn, Zr, Nb and Sn; 0.6 < x ≤ 1, 0 < i ≤ 0.4, 0 < j ≤ 0.5, 0 < k ≤ 0.6, 0 < m ≤ 0.2, 0.03 ≤ y ≤ 0.15; and i + j + k + m = 1 is satisfied.

3. The layered oxide positive electrode material according to claim 1, characterized in that There is no residual alkali between the matrix and the coating layer; The residual alkali includes sodium carbonate and sodium hydroxide.

4. The layered oxide positive electrode material according to claim 1, characterized in that The thickness of the coating layer is 6 - 20 nm; Preferably, the thickness of the coating layer is 8 - 15 nm.

5. The method for preparing the layered oxide positive electrode material according to any one of claims 1 to 4, characterized in that: Comprising the following steps: S1, Ni i Fe j Mn k M m The (OH)2 precursor, the sodium source and the fluorine source are uniformly mixed to obtain a mixture; the mixture is first sintered and naturally cooled to obtain a fluorine-doped layered oxide; S2. Mix the fluorine-doped layered oxide with an ammonium fluoride solution, filter and dry after a chemical reaction to obtain a fluorine-doped layered oxide material preliminarily coated with sodium fluoride; Perform a second sintering on the fluorine-doped layered oxide material preliminarily coated with sodium fluoride to obtain the layered oxide cathode material.

6. The preparation method according to claim 5, characterized in that: The sodium source includes at least one of sodium carbonate, sodium hydroxide, sodium acetate, sodium oxalate, and sodium nitrate; The fluorine source includes at least one of sodium fluoride, ammonium fluoride, and ammonium bifluoride; The Ni i Fe j Mn k M m The molar ratio of the (OH)2 precursor, the sodium in the sodium source, and the fluorine in the fluorine source is 1:(1.03-1.05):(0.03-0.15).

7. The preparation method according to claim 5, characterized in that: The concentration of the ammonium fluoride solution is 0.3 - 0.8 mol / L; The solvent of the ammonium fluoride solution is at least one of methanol, tetrahydrofuran, and dimethylformamide; The mass ratio of the fluorine-doped layered oxide to the ammonium fluoride solution is 1:(10 - 20).

8. The preparation method according to claim 5, wherein In step S1, the heating rate of the first sintering is 1 - 10 °C / min, the holding temperature of the first sintering is 750 - 1100 °C, and the time of the first sintering is 8 - 20 h; In step S2, there is residual alkali on the surface of the fluorine-doped layered oxide, and the chemical reaction is the chemical reaction between the residual alkali on the surface of the fluorine-doped layered oxide and ammonium fluoride; In step S2, the temperature of the chemical reaction is 10 - 30 °C, and the time of the chemical reaction is 20 - 40 min; In step S2, the heating rate of the second sintering is 1 - 10 °C / min, the holding temperature of the second sintering is 400 - 600 °C, and the time of the second sintering is 4 - 8 h.

9. A positive electrode sheet, characterized in that: The positive electrode sheet includes the layered oxide cathode material according to any one of claims 1 - 4, and / or the layered oxide cathode material prepared by the preparation method according to any one of claims 5 - 8.

10. A sodium ion battery, characterized in that: The sodium ion battery includes the positive electrode sheet according to claim 9.

Citation Information

Cited By

  • Composite sodium electric layered oxide positive electrode material and preparation method and application thereof

    CN121726396A

  • Composite sodium electric layered oxide positive electrode material and preparation method and use thereof

    CN121726396B