By mixing the anode and cathode electrolyte of the imbalanced battery and adding valent ionic electrolyte to perform constant current electrolysis and oxidizing gas treatment, the problem of electrolyte imbalance in the prior art is solved, and efficient repair of the electrolyte and battery are achieved Increased capacity.
Patent Information
- Application Number
- CN202411093154.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-08-09
AI Technical Summary
The repair process of the imbalanced electrolyte in the prior art is complex and the effect is not ideal, and it cannot effectively solve the oxidation imbalance and reduction imbalance of the electrolyte of the all-vanadium liquid flow battery, resulting in battery capacity loss.
By mixing the anode electrolyte of the imbalanced battery and the cathode electrolyte, adding the 5-valent ion electrolyte of metal cations, obtaining RGB information to determine the pure 4-valent ion endpoint of the electrolyte, and then performing constant current electrolysis and oxidizing gas treatment, mixing A 3.5-valent ionic electrolyte is obtained, which simplifies the process and improves the quality of the electrolyte.
This method can quickly and accurately determine the repair end point of the electrolyte, reduce repair errors, and improve the utilization efficiency of the electrolyte in the unbalanced battery. The process is simple and the electrolyte quality is high, which significantly improves the electrochemical activity and reaction capacity of the battery.
Smart Images

Figure CN118943401A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to electrolyte repair, and in particular to a method for repairing an unbalanced battery electrolyte. Background Art
[0002] The single active material in the electrolyte of the all-vanadium redox flow battery (VRFB) can effectively avoid the cross-contamination of elements caused by the mutual migration of the positive and negative electrolytes of the flow battery; moreover, the all-vanadium redox flow battery has excellent safety because the electrolyte and the electrolyte reaction site (i.e., the electrode) are separated from each other, and is a highly anticipated large-scale energy storage method. However, the ion exchange membrane used in the all-vanadium redox flow battery cannot guarantee H + While passing through, it completely blocks the penetration of vanadium. Vanadium ions with different valence carry different numbers of bound water and have different diffusion rates in the proton exchange membrane, which will inevitably lead to an imbalance in the volume, concentration, and valence of the all-vanadium liquid flow battery electrolyte. Its intuitive manifestation is the battery capacity decay. The capacity recovery of the unbalanced electrolyte is one of the bottleneck technologies that affect whether the all-vanadium liquid flow battery can be applied on a large scale.
[0003] At present, the research on rebalancing of unbalanced electrolytes is mainly divided into complete rebalancing and partial rebalancing. Both complete remixing rebalancing and partial mixing rebalancing are considered from the perspective of restoring the volume and concentration of the electrolyte, and cannot solve the problems of oxidation imbalance and reduction imbalance of the electrolyte. However, in actual operation, oxidation imbalance and reduction imbalance of the electrolyte will also lead to capacity loss of the battery.
[0004] Although some repair methods are provided in the prior art, there are problems such as complex repair process and unsatisfactory repair effect. Therefore, it is urgent to provide a repair method for unbalanced electrolyte. Summary of the invention
[0005] The purpose of the present invention is to overcome the problems of complicated repair process and unsatisfactory repair effect of unbalanced electrolyte in the prior art, and to provide a method for repairing unbalanced battery electrolyte, which has good repair effect and can improve the utilization efficiency of unbalanced battery electrolyte.
[0006] In order to achieve the above object, the present invention provides a method for repairing an unbalanced battery electrolyte, comprising the following steps:
[0007] (1) mixing the anolyte and the catholyte of the unbalanced cell to obtain electrolyte I;
[0008] A pentavalent ion electrolyte of metal cations contained in the electrolyte I is configured;
[0009] (2) mixing the pentavalent ion electrolyte and the electrolyte I to obtain electrolyte II, obtaining RGB information of the electrolyte II, and using an amount of the pentavalent ion electrolyte such that the blue channel value in the RGB information of the electrolyte II is the largest, to obtain electrolyte III;
[0010] (3) dividing the electrolyte III into two parts, wherein one part of the electrolyte III is used as the cathode electrolyte, and the acid solution is used as the anode electrolyte, and constant current electrolysis is performed to obtain electrolyte IV;
[0011] (4) introducing an oxidizing gas into the electrolyte IV to oxidize the divalent metal cations contained in the electrolyte IV into trivalent cations to obtain electrolyte V; and mixing another electrolyte III with the electrolyte V in the same volume.
[0012] Preferably, in step (1), the total molar concentration of metal cations in the electrolyte I is determined to be C 总阳离子 The molar concentration of the acid radical ion is denoted as c 酸根离子 .
[0013] Preferably, in the pentavalent ion electrolyte, the molar concentration of the pentavalent cations of the metal is the same as the total molar concentration of the metal cations in the electrolyte I, and the molar concentration of the acid radical ions is the same as the molar concentration of the acid radical ions in the electrolyte I.
[0014] Preferably, the acid is sulfuric acid, the metal is vanadium metal, the pentavalent cation of the metal is a pentavalent cation of vanadium, the divalent cation of the metal is a divalent cation of vanadium, and the trivalent cation of the metal is a trivalent cation of vanadium.
[0015] Preferably, in the step (2), the process of mixing the pentavalent ion electrolyte and the electrolyte I comprises: dripping the pentavalent ion electrolyte into the electrolyte I drop by drop.
[0016] Preferably, in step (2), the mixing conditions at least include: a rotation speed of 100-800 rpm.
[0017] Preferably, in the step (2), the method for obtaining the RGB information of the electrolyte II comprises: using MATLAB software to analyze the RGB information of the electrolyte II.
[0018] Preferably, in step (3), the molar concentration of the acid radical ions in the acid solution is the same as the molar concentration of the acid radical ions in the electrolyte I.
[0019] Preferably, the conditions for constant current electrolysis include at least: a current density of 30-60 mA / cm 2 , the electrolysis time is calculated according to formula (I),
[0020] t = aznF / I Formula (I);
[0021] Among them, t is the electrolysis time, z is the number of electrons gained or lost in the reaction, F is the Faraday constant, n is the amount of tetravalent cations of the metal, I is the current, and a is the proportional coefficient, which is 1.1-1.5.
[0022] Preferably, in step (3), the volume ratio of the cathode electrolyte to the anode electrolyte is 1:1-1.5.
[0023] Preferably, in step (4), the oxidizing gas is air or oxygen.
[0024] Through the above technical scheme, the present invention mixes the anolyte and cathode electrolyte of the unbalanced battery to obtain electrolyte I, mixes electrolyte I with a 5-valent ion electrolyte containing metal cations contained in electrolyte I to obtain electrolyte II, and obtains electrolyte III when the blue channel value in the RGB information of electrolyte II is the largest. At this time, electrolyte III is a pure 4-valent ion electrolyte of metal cations. This method can quickly and accurately determine the repair end point of the 4-valent ion electrolyte of metal cations, reduce the repair error, improve the repair quality, and thus improve the utilization efficiency of the unbalanced battery electrolyte. Moreover, part of electrolyte III is treated as a 3-valent ion electrolyte of metal cations, that is, electrolyte V, and electrolyte V and another part of electrolyte III are mixed in the same volume to obtain a 3.5-valent ion electrolyte of metal cations. The process is simple and the quality of the electrolyte is high.
[0025] Other features and advantages of the present invention will be described in detail in the following detailed description. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 It is a structural schematic diagram of an RGB information testing device provided by an embodiment of the present invention;
[0027] Figure 2 This is the endpoint determination diagram for the amount of pentavalent electrolyte added in Example 1;
[0028] Figure 3 is the UV-visible spectrum detection diagram of the electrolyte III in Example 1;
[0029] Figure 4 is the UV-visible spectrum detection diagram of the 3.5-valent electrolyte obtained in Example 1;
[0030] Figure 5 It is the cyclic voltammogram of the electrolyte I in Example 1 and the repaired 3.5-valent electrolyte.
[0031] Description of Reference Numerals
[0032] 1. Shading mechanism; 2. Light source; 3. Dropper; 4. Beaker; 5. Image acquisition mechanism; 6. Image analysis mechanism. DETAILED DESCRIPTION
[0033] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0034] As mentioned above, the present invention provides a method for repairing an unbalanced battery electrolyte, comprising the following steps:
[0035] (1) mixing the anolyte and the catholyte of the unbalanced cell to obtain electrolyte I;
[0036] A pentavalent ion electrolyte of metal cations contained in the electrolyte I is configured;
[0037] (2) mixing the pentavalent ion electrolyte and the electrolyte I to obtain electrolyte II, obtaining RGB information of the electrolyte II, and using an amount of the pentavalent ion electrolyte such that the blue channel value in the RGB information of the electrolyte II is the largest, to obtain electrolyte III;
[0038] (3) dividing the electrolyte III into two parts, wherein one part of the electrolyte III is used as the cathode electrolyte, and the acid solution is used as the anode electrolyte, and constant current electrolysis is performed to obtain electrolyte IV;
[0039] (4) introducing an oxidizing gas into the electrolyte IV to oxidize the divalent metal cations contained in the electrolyte IV into trivalent cations to obtain electrolyte V; and mixing another electrolyte III with the electrolyte V in the same volume.
[0040] Chemical analysis (UV-visible spectrum detection and concentration determination) and cyclic voltammetry tests proved that the repaired electrolyte was a 3.5-valent electrolyte with good electrochemical activity, indicating that this method has a good repair effect and can improve the utilization efficiency of the unbalanced electrolyte.
[0041] The present invention mixes the anolyte and the cathode electrolyte of the unbalanced battery to obtain electrolyte I, mixes electrolyte I with a 5-valent ion electrolyte containing metal cations contained in electrolyte I to obtain electrolyte II, and obtains electrolyte III when the blue channel value in the RGB information of electrolyte II is the largest. At this time, electrolyte III is a pure 4-valent ion electrolyte of metal cations. The method can quickly and accurately determine the repair end point of the 4-valent ion electrolyte of metal cations, reduce the repair error, improve the repair quality, and thus improve the utilization efficiency of the unbalanced battery electrolyte. Moreover, part of electrolyte III is treated as a 3-valent ion electrolyte of metal cations, that is, electrolyte V, and electrolyte V and another part of electrolyte III are mixed in the same volume to obtain a 3.5-valent ion electrolyte of metal cations. The process is simple and the quality of the electrolyte is high.
[0042] According to the present invention, preferably, in the step (1), the total molar concentration of metal cations in the electrolyte I is determined to be C 总阳离子 The molar concentration of the acid radical ion is denoted as c 酸根离子 .
[0043] The total molar concentration of the metal cations in the above-mentioned electrolyte I can be measured by titration, and the reagent used in the titration can be a reagent conventionally used in the art to titrate the total molar concentration of metal cations. Taking the metal cations in the electrolyte I as trivalent vanadium ions and tetravalent vanadium ions as an example, with reference to the national standard GBT8704.5-2020, the total concentration of trivalent vanadium ions and tetravalent vanadium ions in the solution is titrated by potentiometric titration, and with reference to the industry standard T / QAS 004-2019, the sulfate concentration in the solution is titrated by gravimetric method.
[0044] According to the present invention, preferably, in the pentavalent ion electrolyte, the molar concentration of the pentavalent cations of the metal is the same as the total molar concentration of the metal cations in the electrolyte I, and the molar concentration of the acid radical ions is the same as the molar concentration of the acid radical ions in the electrolyte I. The inventors have found that under this preferred embodiment, it is possible to ensure that the metal cation concentration and the acid radical ion concentration in the electrolyte after repair are the same as the total molar concentration of the metal cations and the acid radical concentration in the unbalanced electrolyte before repair, respectively, thereby avoiding the problem of excessive deviation of the metal cation concentration and the acid radical concentration in the electrolyte due to a large number of repairs.
[0045] According to the present invention, preferably, the acid is sulfuric acid, the metal is vanadium metal, the pentavalent cation of the metal is a pentavalent cation of vanadium, the divalent cation of the metal is a divalent cation of vanadium, and the trivalent cation of the metal is a trivalent cation of vanadium. The inventors have found that under this preferred embodiment, the repair method provided by the present invention has a good repair effect on the all-vanadium redox flow battery.
[0046] In the present invention, in step (1), the process of preparing a pentavalent ion electrolyte comprises: dissolving vanadium sulfate in a sulfuric acid solution to obtain a metal tetravalent ion electrolyte, wherein the molar concentration of sulfate ions in the sulfuric acid solution is the same as the molar concentration of acid radical ions in the electrolyte I; placing the metal tetravalent ion electrolyte at the positive and negative electrodes of a flow battery, and performing constant current charging, and when the anode electrolyte is pure yellow, the anode is a pentavalent ion electrolyte.
[0047] According to the present invention, preferably, in the step (2), the process of mixing the pentavalent ion electrolyte and the electrolyte I comprises: dripping the pentavalent ion electrolyte dropwise into the electrolyte I. The inventors have found that under this preferred embodiment, the accuracy of obtaining a pure tetravalent ion electrolyte in which the electrolyte III is a metal cation can be improved, the repair error can be reduced, the repair quality can be improved, and the utilization efficiency of the unbalanced battery electrolyte can be further improved.
[0048] In the present invention, in step (2), during the mixing of the pentavalent ion electrolyte and the electrolyte I, the chemical reaction that occurs is as follows:
[0049] V 3+ +VO2 + →2VO 2+ .
[0050] According to the present invention, in order to further improve the repair quality of the unbalanced battery electrolyte, preferably, in the step (2), the mixing conditions at least include: a rotation speed of 100-800 rpm, specifically 100 rpm, 200 rpm, 300 rpm, 400 rpm, 500 rpm, 600 rpm, 700 rpm, 800 rpm, or any value between the foregoing two values.
[0051] According to the present invention, preferably, in the step (2), the method for obtaining the RGB information of the electrolyte II comprises: using MATLAB software to analyze the RGB information of the electrolyte II.
[0052] In the present invention, an RGB information testing device can be used to obtain the RGB information of the electrolyte II, such as Figure 1As shown, the RGB information measuring device includes a shading mechanism 1, a light source 2, an image acquisition mechanism 5 and an image analysis mechanism 6, the light source 2 is arranged inside the shading mechanism 1, one end of the image acquisition mechanism 5 is connected to the shading mechanism 1, and the other end is connected to the image analysis mechanism 6. The shading mechanism 1 can be a black shading box, and the inner wall of the box is white; the light source 2 can be an LED lamp, and the light source 2 is arranged on the top inner wall of the shading mechanism 1. The image acquisition mechanism 5 can adopt a conventional shooting device selected in the field, such as a camera, an optical sensor, etc. The image analysis mechanism 6 can be a computer installed with MATLAB software. The inventor found that under this preferred embodiment, the RGB information of the electrolyte II can be monitored online, and the accuracy of the RGB information measurement can be improved.
[0053] According to the present invention, the working process of the RGB information testing device includes: placing electrolyte I in a beaker 4, using a dropper 3 to drop a pentavalent ion electrolyte into electrolyte I to obtain electrolyte II, obtaining an image of electrolyte II through an image acquisition mechanism 5, storing the image in an image analysis mechanism 6, using MATLAB software to perform image processing, first cropping the image, then reducing noise, and finally extracting the RGB information of the image.
[0054] In the present invention, a conventional code for obtaining image RGB information can be used to obtain RGB information of electrolyte II, and the RGB information includes a blue channel value, a red channel value, and a green channel value. According to the present invention, in order to further reduce the deviation of the acid radical ion concentration in the repaired electrolyte, preferably, in the step (3), the molar concentration of the acid radical ions in the acid solution is the same as the molar concentration of the acid radical ions in the mixed electrolyte I.
[0055] According to the present invention, preferably, the conditions for constant current electrolysis include at least: a current density of 30-60 mA / cm 2 , specifically 30mA / cm 2 , 40mA / cm 2 , 50mA / cm 2 、60mA / cm 2 , or any value between the above two values; the electrolysis time is calculated according to formula (I);
[0056] t = aznF / I Formula (I);
[0057] Wherein, t is the electrolysis time, z is the number of electrons gained or lost in the reaction, F is the Faraday constant, n is the amount of tetravalent cations of the metal, I is the current, and a is the proportional coefficient, which is 1.1-1.5. Controlling the current density and electrolysis time within the above range can further improve the repair effect of the electrolyte.
[0058] In the present invention, it can be seen from n=cV that the electrolysis time can also be obtained according to formula (II);
[0059] t=azcVF / I Formula (II);
[0060] Wherein, c is the molar concentration of the tetravalent metal cation, and V is the volume of the electrolyte.
[0061] In the present invention, the units of the above parameters are all international standard units, the electrolysis time is s, the unit of mole number is mol, the unit of current is ampere, the unit of molar concentration is mol / L, and the unit of volume is L.
[0062] According to the present invention, preferably, in step (3), the volume ratio of the cathode electrolyte to the anode electrolyte is 1:1-1.5, specifically 1:1, 1:1.1, 1:1.2, 1:1.3, 1:1.4, 1:1.5, or any value between the two aforementioned values. The inventors have found that under this preferred embodiment, the repair effect of the electrolyte can be further improved.
[0063] According to the present invention, in order to further improve the oxidation effect of oxidizing metal divalent cations to trivalent cations, preferably, in the step (4), the oxidizing gas is air or oxygen. In order to reduce production costs, preferably, the oxidizing gas is air.
[0064] In the present invention, there is no particular limitation on the flow rate of the oxidizing gas, and the flow rate of the oxidizing gas may be 5-10 cm 3 / h.
[0065] Exemplarily, when the oxidizing gas is air, the electrolyte IV can be left to stand in the air for 24-36 hours.
[0066] According to a particularly preferred embodiment of the present invention, a method for repairing an unbalanced battery electrolyte comprises the following steps:
[0067] (1) Mixing the anolyte and the catholyte of the unbalanced cell to obtain an electrolyte I, and determining the total molar concentration of metal cations in the electrolyte I as C 总阳离子 The molar concentration of the acid radical ion is denoted as c 酸根离子 ; configuring a pentavalent ion electrolyte of the metal cations contained in the electrolyte I, in which the molar concentration of the pentavalent ion of the metal is the same as the total molar concentration of the metal cations in the electrolyte I, and the molar concentration of the acid radical ions is the same as the molar concentration of the acid radical ions in the electrolyte I;
[0068] (2) dripping the pentavalent ion electrolyte into the electrolyte I dropwise at a rotation speed of 100-800 rpm to obtain electrolyte II, acquiring RGB information of the electrolyte II, and analyzing the RGB information of the electrolyte II using MATLAB software; the amount of the pentavalent ion electrolyte is such that the blue channel value in the RGB information of the electrolyte II is the largest, thereby obtaining electrolyte III;
[0069] (3) The electrolyte III is divided into two parts, one of which is the electrolyte III as the cathode electrolyte and the acid solution as the anode electrolyte, and constant current electrolysis is performed under the condition that the volume ratio of the cathode electrolyte to the anode electrolyte is 1:1-1.5 to obtain electrolyte IV; the molar concentration of the acid radical ions in the acid solution is the same as the molar concentration of the acid radical ions in the mixed electrolyte I; the conditions of the constant current electrolysis include at least: the current density is 30-60 mA / cm 2 , the electrolysis time is calculated according to formula (I);
[0070] t = aznF / I Formula (I);
[0071] Wherein, t is the electrolysis time, z is the number of electrons gained or lost in the reaction, F is the Faraday constant, n is the amount of tetravalent cations of the metal, I is the current, and a is the proportionality coefficient, which is 1.1-1.5;
[0072] (4) introducing an oxidizing gas into the electrolyte IV to oxidize the divalent metal cations contained in the electrolyte IV into trivalent cations to obtain an electrolyte V; mixing another electrolyte III with the electrolyte V in the same volume; the oxidizing gas is air or oxygen;
[0073] The acid is sulfuric acid, the metal is vanadium metal, the pentavalent cation of the metal is a pentavalent cation of vanadium, the divalent cation of the metal is a divalent cation of vanadium, and the trivalent cation of the metal is a trivalent cation of vanadium.
[0074] The method for repairing an unbalanced battery electrolyte provided by the above particularly preferred embodiment can quickly and accurately determine the repair endpoint of a tetravalent ion electrolyte of metal cations, reduce repair errors, improve repair quality, and further improve the utilization efficiency of the unbalanced battery electrolyte.
[0075] The present invention will be described in detail below through embodiments. The RGB information measuring device comprises a shading mechanism 1, a light source 2, an image acquisition mechanism 5 and an image analysis mechanism 6, wherein the light source 2 is arranged inside the shading mechanism 1, and one end of the image acquisition mechanism 5 is connected to the shading mechanism 1 and the other end is connected to the image analysis mechanism 6. The following raw materials are commercially available unless otherwise specified.
[0076] Example 1
[0077] (1) mixing the unbalanced electrolyte to obtain 100 mL of electrolyte I, and titrating the electrolyte I to obtain a vanadium ion concentration of 1.69 mol / L and a sulfate ion concentration of 4 mol / L;
[0078] (2) A quaternary electrolyte having a vanadium ion concentration of 1.69 mol / L and a sulfate concentration of 4 mol / L was prepared, and the RGB information of the quaternary electrolyte was obtained. The RGB information was analyzed using MATLAB software to obtain a blue channel value of 204.13; the electrolyte I was placed in an RGB information test device (such as Figure 1 As shown in FIG. 1 ), a pentavalent electrolyte having a vanadium ion concentration of 1.69 mol / L and a sulfate concentration of 4 mol / L was added dropwise (0.1 mL per drop) to obtain the RGB information of electrolyte II. The blue channel value in the RGB information was analyzed using MATLAB software. When the blue channel value in the RGB information of electrolyte II was the largest, that is, it reached more than 95% of the blue channel value of the quadrivalent electrolyte, refer to FIG. Figure 2 , stop adding the pentavalent electrolyte to obtain electrolyte III;
[0079] (3) Place half of the volume of electrolyte III in the cathode chamber of the electrolytic cell, and put dilute sulfuric acid with a sulfuric acid concentration of 4 mol / L in the anode chamber of the electrolytic cell. At this time, the volume ratio of the cathode electrolyte to the anode electrolyte is 1:1, and the electrode area is 9 cm 2 , then at 40mA / cm 2 Electrolyze for 13 h at a current density of , and obtain electrolyte IV;
[0080] The electrolysis time is calculated as follows:
[0081] t=aznF / I=azcvF / I=a×1×0.07×1.695×96485 / 0.04×9=1.4×1×0.07×1.69×96485 / 0.36=44388.46s=12.33h;
[0082] (4) passing air into the electrolyte in the cathode chamber of the electrolytic cell to oxidize all the divalent vanadium ions into trivalent vanadium ions, thereby obtaining electrolyte V;
[0083] (5) Mix the electrolyte V with the other half volume of the electrolyte III in step (3) in equal volumes to obtain a 3.5-valent electrolyte.
[0084] Test Example 1
[0085] The electrolyte III obtained in step (2) of Example 1 was subjected to UV-visible spectroscopy analysis to obtain Figure 3 .Depend on Figure 3It can be seen that there is an absorption peak of tetravalent vanadium ions at around 780nm, and there is no absorption peak of trivalent vanadium ions at around 600nm and 400nm, which proves that there are tetravalent vanadium ions in the solution, but no trivalent vanadium ions; by comparing with the UV-visible light analysis curve of the diluted pentavalent electrolyte at 335nm, it is found that there is no absorption peak, so the solution does not contain pentavalent vanadium ions, but only tetravalent vanadium ions.
[0086] Test Example 2
[0087] The 3.5-valent electrolyte obtained in Example 1 was subjected to UV-visible spectroscopy analysis to obtain Figure 4 .Depend on Figure 4 It can be seen that there is an absorption peak of 4-valent vanadium ion at about 780nm, and there is an absorption peak of 3-valent vanadium ion at about 600nm and 400nm, which proves that there are 3-valent and 4-valent vanadium ions in the solution; although the ultraviolet-visible spectrum detection of 5-valent vanadium ion and 2-valent vanadium ion is relatively unstable, 3-valent vanadium ion and 5-valent vanadium ion cannot coexist in the same solution, and 4-valent vanadium ion and 2-valent vanadium ion cannot coexist. Therefore, it can be determined that there are 3-valent vanadium ions and 4-valent vanadium ions in the prepared electrolyte, and there are no 5-valent vanadium ions and 2-valent vanadium ions.
[0088] Test Example 3
[0089] The concentrations of trivalent vanadium ions and tetravalent vanadium ions in the repaired 3.5-valent electrolyte obtained in Example 1 were titrated using an automatic potentiometric titrator to obtain Table 1.
[0090] Table 1
[0091] c(trivalent vanadium ion) c(quaternary vanadium ion) c(trivalent vanadium ion):c(quaternary vanadium ion) 0.7999 0.8001 0.9997
[0092] From the results in Table 1, it can be seen that c(trivalent vanadium ion):c(quadrivalent vanadium ion)=0.9997 is in line with the national standard GB / T37204-2018 that the ratio of trivalent and quadrivalent vanadium ions in 3.5-valent electrolyte is 1±0.1, indicating that the repair method provided by the method has a good repair effect and can improve the utilization efficiency of the unbalanced battery electrolyte.
[0093] Test Example 4
[0094] Cyclic voltammetry was performed on the unbalanced electrolyte and the repaired electrolyte (the 3.5-valent electrolyte obtained in Example 1) at 0-1.7 V and a scan rate of 40 mV / s under the same three-electrode system, and the results were as follows: Figure 5 .
[0095] Depend on Figure 5It can be seen that after the electrolyte is repaired, the oxidation peak current density and reduction peak current density increase, indicating that the electrochemical activity of the electrolyte increases; the area of the redox peak increases, indicating that the electrochemical reaction capacity in the electrolyte increases; the height difference between the oxidation peak and the reduction peak is very small, and the reversibility of the electrolyte is significantly improved. Therefore, compared with the unbalanced electrolyte, the electrochemical activity, electrochemical reaction capacity and reversibility of the repaired electrolyte are significantly increased, indicating that the repair method is feasible.
[0096] Example 2
[0097] The unbalanced electrolyte was repaired according to the method of Example 1, except that the volume ratio of the cathode electrolyte to the anode electrolyte in step (3) was replaced with 1:2.
[0098] Test Example 5
[0099] The concentrations of trivalent vanadium ions and tetravalent vanadium ions in the repaired 3.5-valent electrolyte obtained in Example 3 were titrated using an automatic potentiometric titrator to obtain Table 2.
[0100] Table 2
[0101] c(trivalent vanadium ion) c(quaternary vanadium ion) c(trivalent vanadium ion):c(quaternary vanadium ion) 0.813 0.877 0.927
[0102] From the results in Table 2, it can be seen that c(trivalent vanadium ion):c(quaternary vanadium ion)=0.927 is in line with the national standard GB / T37204-2018 that the ratio of trivalent and quadrivalent vanadium ions in 3.5-valent electrolyte is 1±0.1, indicating that the repair method provided by the method has a good repair effect and can improve the utilization efficiency of the unbalanced battery electrolyte.
[0103] Comparative Example
[0104] The unbalanced electrolyte was repaired according to the method of Example 1, and the total vanadium concentration of the mixed electrolyte I was 1.6 mol / L, except that step (2) was replaced by:
[0105] (2) After the concentration of trivalent vanadium ions in the mixed electrolyte I is obtained by titration, the volume calculation formula for adding a pentavalent vanadium electrolyte having the same total vanadium concentration as the mixed electrolyte I is:
[0106] V=c 3价钒离子 ×V I / c 5价钒离子 ;
[0107] That is, a pentavalent electrolyte having a volume V is added to obtain electrolyte II.
[0108] Test Example 6
[0109] The concentrations of trivalent vanadium ions and tetravalent vanadium ions in the repaired 3.5-valent electrolyte obtained in the comparative example were titrated using an automatic potentiometric titrator to obtain Table 3.
[0110] Table 3
[0111] c(trivalent vanadium ion) c(quaternary vanadium ion) c(trivalent vanadium ion):c(quaternary vanadium ion) 0.771 0.829 0.9300
[0112] From the results in Table 3, it can be seen that c(trivalent vanadium ion):c(quaternary vanadium ion)=0.9300, which is in line with the national standard GB / T37204-2018 that the ratio of trivalent and quadrivalent vanadium ions in 3.5-valent electrolyte is 1±0.1.
[0113] It can be seen from the titration results that even if the 3.5-valent electrolyte in the comparative example meets the national standard, the degree of deviation of c (trivalent vanadium ion): c (quadrivalent vanadium ion) from 1 is large, and the degree of deviation directly affects the quality of the electrolyte. This is because, although the volume of the 5-valent electrolyte added is calculated accurately, mechanical errors (such as pipetting errors, titration errors, etc.) cannot be avoided, and by measuring the RGB information of the electrolyte II during the addition of the 5-valent electrolyte, the internal ion valence of the solution can be accurately determined, the error can be effectively reduced, and the resulting electrolyte quality is better.
[0114] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A method for repairing an unbalanced battery electrolyte, characterized in that: The steps include: (1) mixing the anolyte and the catholyte of the unbalanced cell to obtain electrolyte I; A pentavalent ion electrolyte of metal cations contained in the electrolyte I is configured; (2) mixing the pentavalent ion electrolyte and the electrolyte I to obtain electrolyte II, obtaining RGB information of the electrolyte II, and using an amount of the pentavalent ion electrolyte such that the blue channel value in the RGB information of the electrolyte II is the largest, to obtain electrolyte III; (3) dividing the electrolyte III into two parts, wherein one part of the electrolyte III is used as the cathode electrolyte, and the acid solution is used as the anode electrolyte, and constant current electrolysis is performed to obtain electrolyte IV; (4) introducing an oxidizing gas into the electrolyte IV to oxidize the divalent metal cations contained in the electrolyte IV into trivalent cations to obtain electrolyte V; and mixing another electrolyte III with the electrolyte V in the same volume.
2. The repair method according to claim 1, characterized in that: In the step (1), the total molar concentration of metal cations in the electrolyte I is determined to be C 总阳离子 The molar concentration of the acid radical ion is denoted as c 酸根离子 .
3. The repair method according to claim 2, characterized in that: In the pentavalent ion electrolyte, the molar concentration of pentavalent cations of the metal is the same as the total molar concentration of metal cations in the electrolyte I, and the molar concentration of the acid radical ions is the same as the molar concentration of the acid radical ions in the electrolyte I.
4. The repair method according to claim 3, characterized in that: The acid is sulfuric acid, the metal is vanadium metal, the pentavalent cation of the metal is a pentavalent cation of vanadium, the divalent cation of the metal is a divalent cation of vanadium, and the trivalent cation of the metal is a trivalent cation of vanadium.
5. The repair method according to any one of claims 1 to 4, characterized in that: In the step (2), the process of mixing the pentavalent ion electrolyte and the electrolyte I comprises: dripping the pentavalent ion electrolyte into the electrolyte I drop by drop; Preferably, in step (2), the mixing conditions at least include: a rotation speed of 100-800 rpm.
6. The repair method according to claim 5, characterized in that: In the step (2), the method for obtaining the RGB information of the electrolyte II includes: using MATLAB software to analyze the RGB information of the electrolyte II.
7. The repair method according to any one of claims 2 to 4, characterized in that: In the step (3), the molar concentration of the acid radical ions in the acid solution is the same as the molar concentration of the acid radical ions in the electrolyte I.
8. The repair method according to claim 7, characterized in that: The conditions of the constant current electrolysis include at least: a current density of 30-60 mA / cm 2 , the electrolysis time is calculated according to formula (I), t = aznF / I Formula (I); Among them, t is the electrolysis time, z is the number of electrons gained or lost in the reaction, F is the Faraday constant, n is the amount of tetravalent cations of the metal, I is the current, and a is the proportional coefficient, which is 1.1-1.
5.
9. The repair method according to claim 7, characterized in that: In the step (3), the volume ratio of the cathode electrolyte to the anode electrolyte is 1:1-1.
5.
10. The repair method according to any one of claims 1 to 4, characterized in that: In the step (4), the oxidizing gas is air or oxygen.
Citation Information
Patent Citations
Regeneration method for waste liquor of all-vanadium flow battery
CN102468499A
Method for reducing capacity fading of vanadium battery
CN114497665A
Preparation method of 3.5-valent sulfate acid system vanadium electrolyte
CN115882021A
Preparation method of electrolyte for vanadium redox flow battery