Electrolyte material with stable positive and negative electrode interface, solid-state battery and manufacturing method
By using the modified garnet-type LLZO and sulfide solid electrolyte and nano-NASICON in all solid lithium-ion batteries, the interface stability problem of solid electrolyte on high nickel positive electrode and silicon carbon negative electrode is solved, and the interface stability of solid electrolyte on high nickel positive electrode and silicon carbon negative electrode is achieved. High ionic conductivity and wide electrochemical windows improve the cycling and electrochemical performance of the battery, and are suitable for large-scale applications.
Patent Information
- Application Number
- CN202411121456.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-11-12
AI Technical Summary
The solid electrolytes in existing all-solid-state lithium-ion batteries have challenges to the electrochemical window of high-nickel positive electrodes, circulating volume expansion of silicon-carbon negative electrodes and poor interface contact, which seriously restrict the performance and application of the battery.
By modifying the ultra-thin PI/LiTFSI layer on the surface of the garnet-type LLZO solid electrolyte, mixing it with the sulfide solid electrolyte Li6PS5Cl, combining the nano-NASICON type electrolyte to form a double-layer clad structure, a solid electrolyte material with flexibility and rigidity was prepared. Stabilize the interface of the positive and negative electrode to suppress the interface contact difference caused by high potential oxidation and negative electrode expansion and contraction.
It achieves high ionic conductivity, wide electrochemical window and good interface stability, supports the cyclic stability of high nickel ternary positive electrode and silicon carbon negative electrode, improves the cyclic performance and electrochemical performance of the battery, and is suitable for large-scale applications.
Smart Images

Figure CN118943475A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of electrolyte materials, and more specifically, to an electrolyte material with stable positive and negative electrode interfaces, a solid-state battery, and a manufacturing method thereof. Background Art
[0002] As a core component of electric vehicles, high-energy-density secondary lithium-ion batteries have received widespread attention from the society and have broad market prospects. Compared with traditional liquid lithium batteries, solid-state lithium batteries have both high safety and high specific energy and better safety, which has attracted widespread attention in academia and industry. In terms of working principle, all-solid-state batteries are no different from traditional lithium-ion batteries. The main difference between the two is that compared with liquid electrolytes, solid electrolytes can act as a medium for ion conduction in the battery, and can also act as a diaphragm to prevent the conduction of electrons and prevent battery short circuits. They have the functions of both liquid electrolytes and diaphragms. However, the solid electrolytes in all-solid-state lithium-ion batteries in existing related technologies often face many challenges. The future development direction of all-solid-state batteries is high-nickel matching high-silicon negative electrode or lithium metal negative electrode. The large-scale application of lithium metal negative electrode is limited in the short term; high-nickel ternary positive electrode matching silicon-carbon negative electrode has a certain possibility of large-scale application in the short term; but the high potential of the high-nickel positive electrode poses a challenge to the electrochemical window of the solid electrolyte. At the same time, the silicon-carbon negative electrode has problems such as cyclic volume expansion, long-term poor solid-solid interface contact, poor charge transfer and poor cyclic stability, which seriously restrict the performance and practical application of all-solid-state lithium-ion batteries.
[0003] Solid electrolytes can be mainly divided into three categories: inorganic solid electrolytes, organic polymer solid electrolytes, and organic-inorganic composite solid electrolytes. Inorganic solid electrolytes have high ionic conductivity close to that of liquid electrolytes at room temperature, excellent mechanical strength, and good electrochemical / thermal stability; however, manufacturing difficulties, serious interfacial side reactions, high costs, and poor environmental stability limit the practical application of inorganic solid electrolytes. Sulfide solid electrolytes have the highest ionic conductivity currently available, however, most sulfide solid electrolytes are inherently unstable, releasing toxic H2S gas, accompanied by the destruction of the crystal structure and the corresponding reduction in lithium ion conductivity. Specifically, H2O molecules spontaneously attack the PS bonds in phosphorus-containing sulfides, replacing soft base S atoms with strong base O atoms, thereby reacting with hard acid P 5+ A stronger bond is formed, releasing H2S gas in the process. Another garnet-type solid electrolyte (LLZO) has a room temperature of about 10 -3 Scm-1 has a higher ionic conductivity, a wide electrochemical window [>6VvsLi / Li+], and the most stable interface for Li metal among all solid electrolytes. However, LLZO is also sensitive to the surrounding atmosphere. The reaction mechanism in ambient air can be divided into two steps: first, Li reacts with water vapor in the air.+ / H + The exchange generates LiOH·H2O intermediates, and then LiOH·H2O reacts with carbon dioxide in the air to generate a Li2CO3 surface layer. The formed Li2CO3 causes the ion conductivity to decrease and the interface resistance to increase. In addition, the sodium fast ion conductor (NASCICON) type solid electrolyte lithium aluminum titanium phosphate Li 1+x Al x Ti 2- x(PO4)3(LATP) is a type of inorganic solid electrolyte that has attracted much attention in recent years. LATP exhibits high ionic conductivity (10 -4 S / cm), and has low requirements for storage and assembly conditions. Its structural properties are very stable in air and humid environment. At the same time, due to the abundant source of raw materials, LATP is also one of the solid electrolytes with the lowest cost and the best commercial prospects. In addition, due to the high ion transfer rate of LATP solid electrolyte, it can be used not only as a solid electrolyte, but also as a positive electrode coating material; studies have found that LATP has poor stability to Li, and its capacity decays rapidly in the first week of charge and discharge cycles, and there is a "lithium eating" phenomenon, which is mainly related to the formation of a lithium-enhanced structure during the discharge process of LATP. The charge and discharge process is accompanied by irreversible changes in the structure, which affects the material capacity and cycle stability.
[0004] In short, simple sulfide, garnet (LLZO), and NASCICON solid electrolytes cannot be effectively used as solid electrolytes, and there is an urgent need to provide a solid electrolyte that can be effectively used as a solid electrolyte. Summary of the invention
[0005] The present invention first modifies an ultra-thin PI / LiTFSI layer on the surface of a garnet-type (LLZO) nano solid electrolyte to obtain PI / LiTFSI@LLZO, wherein PI is polyimide, LiTFSI is lithium bis(trifluoromethanesulfonyl imide), and PI / LiTFSI represents PI-modified LiTFSI. Then, the prepared sulfide solid electrolyte Li6PS5Cl is mixed with PI / LiTFSI@LLZO by ball milling. Then, the mixed powder is dispersed in a DMF solution containing pyromellitic anhydride and 4,4'-diaminodiphenyl ether with a nano NASICON electrolyte. The target solid electrolyte material is obtained by volatilization of the agent, calcination and high-temperature polymerization; the electrolyte material has the flexibility of sulfide electrolyte and the rigidity of LLZO and NASICON electrolytes, and has the characteristics of rigid outside and soft inside. The electrolyte has interfacial contact stability during the positive and negative electrode cycles, inhibits the high-potential oxidation of the positive electrode and the poor solid-solid interface contact during the repeated expansion and contraction of the silicon-carbon negative electrode. The solid electrolyte prepared by double nano-coating is stable in the air and has processing conditions under the dew point of the normal battery production environment, which provides ideas for accelerating the large-scale application of solid-state lithium-ion batteries.
[0006] The preparation method of the solid electrolyte material is as follows: taking a garnet-type (LLZO series) solid electrolyte dispersed in a mixed solution of pyromellitic anhydride and 4,4'-diaminodiphenyl ether, calcining at high temperature after the solvent evaporates to obtain a PI-modified PI / LLZO material, and then preparing a typical sulfide solid electrolyte Li6PS5Cl powder in an inert gas environment for use, and then a small amount of PI / LLZO and Li6PS5Cl are ball-milled and mixed and coated in an inert environment to obtain a PI / LiTFSI@LLZO@Li6PS5Cl mixed powder, and then the mixed powder is dispersed in a NASICON type nano solid electrolyte in a DMF solution containing LiTFSI (lithium bistrifluoromethanesulfonyl imide) pyromellitic anhydride and 4,4'-diaminodiphenyl ether, and the solvent is evaporated and then treated at high temperature to obtain the target solid electrolyte material powder; the solid electrolyte is prepared into an all-solid-state battery with a high-nickel ternary positive electrode and a silicon-carbon negative electrode. The electrolyte basically maintains the high ionic conductivity of the sulfide electrolyte and has excellent stability in the air. The PI ultra-thin coating composites LiTFSI and a small amount of nano-hybrid solid electrolyte coating, which has both Li ion conductivity and certain air and water isolation performance. The present invention first forms PI / LiTFSI@LLZO, which is then compounded with Li6PS5Cl to obtain PI / LiTFSI@LLZO@Li6PS5Cl, and finally coated with PI / NASICON on the outer layer to form PI / NASICON@PI / LiTFSI@LLZO@Li6PS5Cl. The @ in the present invention means surface coating.
[0007] On the one hand, the present invention provides an electrolyte material with a stable positive and negative electrode interface, with a sulfide solid electrolyte as the core, an LLZO solid electrolyte wrapped on the outside of the sulfide solid electrolyte, and a coating material coated on the outside of the LLZO solid electrolyte, wherein the coating material is PI / LiTFSI and PI / NASICON.
[0008] In another aspect, the present invention provides a method for preparing the above-mentioned electrolyte material with stable positive and negative electrode interfaces, comprising:
[0009] Prepare a first composite solid electrolyte, wherein the first composite solid electrolyte is a composite solid electrolyte PI / LiTFSI@LLZO in which a coating material is coated on the outside of a LLZO-based solid electrolyte;
[0010] preparing a second solid electrolyte, wherein the second solid electrolyte is a sulfide solid electrolyte;
[0011] Preparing a third solid electrolyte, comprising: mixing the first composite solid electrolyte and the second solid electrolyte to obtain a third solid electrolyte;
[0012] The target solid electrolyte material is prepared by adding the third solid electrolyte, lithium salt, and NASICON type nano solid electrolyte into a DMF solution containing pyromellitic dianhydride and 4,4'-diaminodiphenyl ether to obtain the target solid electrolyte material.
[0013] On the other hand, the present invention also provides a solid-state battery, comprising the above-mentioned electrolyte material with stable positive and negative electrode interfaces.
[0014] On the other hand, the present invention also provides a method for preparing the above-mentioned solid-state battery, comprising:
[0015] The composite positive electrode is prepared, comprising: mixing and grinding the electrolyte material with stable positive and negative electrode interfaces with the high-nickel ternary positive electrode material, the powder conductive agent, and the PTFE binder, rolling the powder into a film, die-cutting, and encapsulating it with aluminum foil at a pressure of 80Mpa-100Mpa for 1min-3min to obtain the composite positive electrode;
[0016] The composite negative electrode is prepared, comprising: mixing and grinding the electrolyte material with stable positive and negative electrode interfaces with the silicon-carbon negative electrode, the PTFE binder, and the powder conductive agent, rolling the powder into a film, die-cutting, and packaging with copper foil at a pressure of 60 MPa-100 MPa for 1 min-3 min to obtain the composite negative electrode;
[0017] The electrolyte membrane is prepared by using a dry membrane preparation method, the electrolyte material with stable interface between positive and negative electrodes and a poly-PTFE binder are uniformly mixed in a mortar, and finally the electrolyte membrane is prepared by multiple rolling;
[0018] And encapsulating an all-solid-state soft-pack battery, including placing a composite positive electrode and a composite negative electrode on both sides of an electrolyte membrane, pressing them, and encapsulating them with an aluminum-plastic film to form an all-solid-state soft-pack battery.
[0019] Compared with the prior art, the electrolyte material with stable positive and negative electrode interfaces and the solid-state battery provided by the present invention achieve at least the following beneficial effects:
[0020] The solid electrolyte material provided by the present invention has a high ionic conductivity at the same level as that of sulfide solid electrolytes, with a maximum of 1.91×10 -3 S / cm; it also has the high stability and wide electrochemical window of LLZO and NASCICON. The electrolyte can be used to make electrodes under the dew point of a normal lithium battery production workshop and is less affected by environmental humidity.
[0021] The all-solid-state battery based on the solid electrolyte material of the positive and negative electrode interface temperature provided by the present invention has a relatively stable positive and negative electrode interface during the cycle, can support the full battery cycle of the battery cell with high nickel ternary matching silicon carbon negative electrode, has good positive and negative electrode cycle stability, good interface contact performance, reduces the phenomenon of interface shedding caused by the volume change of the electrode during the cycle, and improves the stability of the battery cycle; at 0.1 mA cm -2 The first coulombic efficiency and the first cycle discharge capacity under the current density reached 97.8% and 201 mA / g respectively. -2 After 200 cycles of constant current charge and discharge test at a current density of 1.54 W, the discharge capacity can still be maintained at 185 mA / g, showing excellent electrical properties.
[0022] The solid electrolyte of the present invention modifies a dense and rough protective layer on the surface of the sulfide electrolyte. After the protective layer is pressed, the PI ultra-thin film squeezes the ultra-thin film at the solid-solid contact interface under high pressure, so that the PI ultra-thin film is in the particle gap and does not affect the solid-solid interface contact, and the lithium ion transmission is less affected. The use of nano-level LLZO and NASICON coating increases the conduction times between grain boundaries, but has little effect on the overall ionic conductivity. The coating of PI / LiTFSI ultra-thin coating and nano-hybrid solid electrolyte has both Li ion conduction ability and certain air and water isolation performance, which can match the current production process environment of liquid lithium-ion batteries.
[0023] The LLZO type solid electrolyte itself also has the problem of poor surface stability. First, an ultra-thin PI / LiTFSI composite layer is modified on its surface. The inner layer stabilizes the sulfide and LLZO, and then NASICON is modified on the outer layer to form a double-layer protection for the sulfide electrolyte. NASICON can maintain good chemical stability in the air in the outermost layer. This electrolyte combines the advantages of sulfide electrolyte and LLZO, NASICON, and other three electrolytes. The sulfide electrolyte particles are softer and the film-forming performance is better than LLZO and NASICON. LLZO and NASICON (poor flexibility) have better stability and combine electrical and mechanical properties.
[0024] The molecular structure of polyimide lacks polar atoms on the main chain, and it presents hydrophobic properties on the molecule, and the solid-solid non-contact surface is protected by PI; for solid batteries, the fitting of solid-solid interface contact is the most critical. The solid electrolyte of the present invention has a more stable interface contact. For the positive electrode, the non-contact surface PI protection suppresses the environmental impact of the manufacturing process, and improves the antioxidant performance under high potential, and improves the stability of the positive electrode interface contact; for the silicon-carbon negative electrode, the expansion and contraction of the battery cell during the charge and discharge process can be well buffered by the "rigid outside and soft inside" electrolyte, and after long-term expansion and contraction, it can still maintain better solid-solid interface contact, and the structural state of the electrolyte is not greatly affected. PI has high strength and toughness, and the ultra-thin film improves the structural strength of the composite electrolyte, so that it can maintain good interface contact with the active material after expansion, extrusion and contraction, and has sufficient mechanical strength to inhibit the growth of lithium dendrites.
[0025] Of course, any product implementing the present invention does not necessarily need to achieve all of the technical effects described above at the same time.
[0026] Further features and advantages of the present invention will become apparent from the following detailed description of exemplary embodiments of the present invention with reference to the attached drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] The accompanying drawings, which are incorporated in and constitute a part of the specification, illustrate embodiments of the invention and, together with the description, serve to explain the principles of the invention.
[0028] Figure 1 It is a schematic diagram of the structure of the solid electrolyte provided by the present invention;
[0029] Figure 2 It is the EIS spectrum of the solid electrolyte prepared by Example 1 to Example 3 and Comparative Example 1 to Comparative Example 2 of the present invention. DETAILED DESCRIPTION
[0030] Various exemplary embodiments of the present invention will now be described in detail with reference to the accompanying drawings. It should be noted that the relative arrangement of components and steps, numerical expressions and numerical values set forth in these embodiments do not limit the scope of the present invention unless otherwise specifically stated.
[0031] The following description of at least one exemplary embodiment is merely illustrative in nature and is in no way intended to limit the invention, its application, or uses.
[0032] Technologies, methods, and equipment known to ordinary technicians in the relevant art may not be discussed in detail, but where appropriate, the technologies, methods, and equipment should be considered as part of the specification.
[0033] In all examples shown and discussed herein, any specific values should be interpreted as merely exemplary and not limiting. Therefore, other examples of the exemplary embodiments may have different values.
[0034] It should be noted that like reference numerals and letters refer to similar items in the following figures, and therefore, once an item is defined in one figure, it need not be further discussed in subsequent figures.
[0035] Example 1
[0036] Step 1: Prepare the first composite solid electrolyte: dissolve 0.58 g of pyromellitic anhydride in 10.9 g of n-hexane solution, take 94.0 g of Li 6.65 Ga 0.15 Ln3Z 1.9 Sc 0.1 O 12 The nano solid electrolyte powder is ultrasonically dispersed in a n-hexane solution to obtain a mixed solution ①, 0.52 g of 4,4'-diaminodiphenyl ether and 0.32 g of LiTFSI (lithium bis(trifluoromethanesulfonyl imide)) are dissolved in 9.8 g of N,N-dimethylformamide (DMF) to obtain a solution ②, and then the solution ② is uniformly added to the solution ① under stirring conditions, and then the mixture solution is heat-treated at 130° C. to volatilize the solvent to obtain a mixed powder;
[0037] The mixed solution ① in the present invention is the first mixed solution, and the solution ② is the second solution.
[0038] Step 2: Transfer the mixed powder obtained in step 1 to a muffle furnace for calcination at 280°C, with a program heating rate of 5°C / min and calcination for 4 hours to obtain a composite material PI / LiTFSI@LLZO, and then ball milling is performed. The ball milling uses a 1:1 mixture of large and small balls, with a large ball diameter of 5 mm and a small ball diameter of 2 mm, a rotation speed of 250 rpm, and a time of 2 hours to obtain PI / LiTFSI@LLZO powder, which is the first composite solid electrolyte.
[0039] In this embodiment, the mass of the coating material PI / LiTFSI is 1.5% of the mass of the LLZO solid electrolyte.
[0040] Step 3: In a glove box, take appropriate amounts of Li2S, P2S5 and Li Cl powders in a molar ratio of 5:1:2 and mix them under an inert atmosphere. Add the mixture into a ball mill and use two sizes of zirconium balls to ball mill the powder. The ball milling uses a 1:2 mixture of large and small balls, with a large ball diameter of 5 mm and a small ball diameter of 2 mm, a rotation speed of 300 rpm, and a time of 1.5 h. Transfer the mixture obtained by ball milling to a tubular furnace and calcine it at 550°C for 10 h to obtain a solid electrolyte Li6PS5Cl powder, which is the second solid electrolyte.
[0041] In the entire process of preparing the Li6PS5Cl powder in step three, Ar inert gas protection is used.
[0042] Step 4: Take 5.0g of PI / LiTFSI@LLZO obtained in step 2 and 100.0g of Li6PS5Cl powder obtained in step 3 and transfer them to a ball mill, dry mix them evenly, the mixer speed is 150rpm, and the mixing time is 2h; obtain PI / LiTFSI@LLZO@Li6PS5Cl mixed powder; then take out the mixed powder, and mix PI / LiTFSI@LLZO@Li6PS5Cl: LiTFSI: Li 1.7 Al 0.3 Ti 1.7 P3O 12 : Add pyromellitic anhydride: 4,4'-diaminodiphenyl ether in a mass ratio of 10:0.05:0.12:0.04:0.036 to a DMF solution containing pyromellitic anhydride and 4,4'-diaminodiphenyl ether, and stir at 130°C to evaporate the solvent; transfer the obtained mixed powder to a muffle furnace and calcine at 250°C for 4 hours to obtain the target solid electrolyte material.
[0043] The mixed dry powder obtained here also needs to be stored in an Ar environment.
[0044] Step 5: Prepare a solid-state battery, including:
[0045] Preparation of composite positive electrode: The solid electrolyte powder obtained in step 4 is ground and mixed with high nickel ternary positive electrode material (Ni88), powder conductive agent VGCF and MWCNTs (ratio of 1:1), and PTFE binder in a mass ratio of 15:35:2:1, and then the powder is rolled into a film, die-cut, and packaged with aluminum foil at a pressure of 100M pa for 2 minutes to obtain a composite positive electrode. The thickness of the obtained composite positive electrode sheet is 140μm;
[0046] Preparation of composite negative electrode: the solid electrolyte powder obtained in step 4 is ground and mixed with silicon-carbon negative electrode, PTFE, VGCF and MWCNTs (ratio of 1:2) in a mass ratio of 20:40:3:1, and then the powder is rolled into a film, die-cut, and packaged with copper foil at a pressure of 80 MPa for 2 minutes to obtain a composite negative electrode with a thickness of 110 μm.
[0047] Preparation of electrolyte membrane: using a dry membrane preparation method, the solid electrolyte powder and poly PTFE were uniformly mixed in a mortar at a weight ratio of 99:1, and finally the electrolyte membrane with a thickness of 100 μm was prepared by multiple rolling;
[0048] The composite positive electrode and the composite negative electrode are placed on both sides of the electrolyte membrane, pressed, and packaged with an aluminum-plastic film to form an all-solid-state soft-pack battery;
[0049] Step 6: Ionic conductivity test: Take the solid electrolyte material of step 5 and press it into a disc-shaped lithium ion solid electrolyte with a diameter of 15 mm and a thickness of 1.5 mm under a pressure of 240 MPa in an environment with a moisture content of less than 30 ppm (dew point <-52 ° C). Perform EIS test at 25 ° C to calculate the lithium ion conductivity, and place it under the dew point environment for different time periods to test the change in ionic conductivity (calculate the ionic conductivity according to the formula ρ = d / (πr2×R), where ρ is the ionic conductivity, d is the sample thickness, r is the sample radius, and R is the AC impedance); The all-solid-state soft-pack battery of step 5 is subjected to electrical performance test: Cycle performance and rate performance test: The above-mentioned all-solid-state battery is placed at a constant temperature of 25 ° C and charged with a current density of 1.0 mA cm -2 The current density was cycled for 200 cycles, and the capacity retention rate at the 200th cycle was calculated.
[0050] Example 2
[0051] Step 1: Dissolve 0.46g of pyromellitic anhydride in 10.2g of n-hexane solution and 121.0g of Li7La3Zr2O 12 The nano solid electrolyte powder was ultrasonically dispersed in a n-hexane solution for 1 h to obtain a mixed solution ①, 0.44 g of 4,4'-diaminodiphenyl ether and 0.27 g of LiTFSI (lithium bistrifluoromethanesulfonyl imide) ultrasonically dispersed for 1 h were dissolved in 9.6 g of N,N-dimethylformamide (DMF) to obtain a solution ②, and then the solution ② was uniformly added to the solution ① under stirring conditions, the stirring speed was 100 rpm, the reaction time was 3 h, and then the mixture solution was heat-treated at 130° C. to volatilize the solvent to obtain a mixed powder;
[0052] Step 2: The mixed powder obtained in step 1 is transferred to a muffle furnace for calcination at 400°C, with a program heating rate of 5°C / min and calcination for 6 hours to obtain a composite material PI / LiTFSI@LLZO, and then ball milled. The ball milling uses a 1:1 mixture of large and small balls, with a large ball diameter of 5mm and a small ball diameter of 2mm, a rotation speed of 250rpm, and a time of 2 hours to obtain PI / LiTFSI@LLZO powder; the mass of the coating material PI / LiTFSI is 0.96% of the mass of the LLZO solid electrolyte;
[0053] Step 3: In a glove box, take appropriate amounts of Li2S, P2S5 and Li Cl powders in a molar ratio of 5:1:2 and mix them under an inert atmosphere. Add the mixture into a ball mill and use two sizes of zirconium balls to ball mill the powder. The ball mill uses a 1:2 mixture of large and small balls, with a large ball diameter of 5 mm and a small ball diameter of 2 mm, a rotation speed of 300 rpm, and a time of 3. Transfer the mixture obtained by ball milling to a tubular furnace and calcine at 650°C for 12 hours to obtain a solid electrolyte Li6PS5Cl powder. The preparation process of Li6PS5Cl powder is protected by Ar inert gas throughout.
[0054] Step 4: Take 4.0g of PI / LiTFSI@LLZO obtained in step 2 and 100.0g of Li6PS5Cl powder obtained in step 3 and transfer them to a ball mill, dry mix them evenly, the mixer speed is 300rpm, and the mixing time is 3h; PI / LiTFSI@LLZO@Li6PS5Cl mixed powder is obtained; then the mixed powder is taken out, and PI / LiTFSI@LLZO@Li6PS5Cl: LiTFSI: Li 1.7 Al 0.3 Ti 1.7 P3O 12 : Add pyromellitic anhydride: 4,4'-diaminodiphenyl ether in a mass ratio of 12:0.08:0.15:0.06:0.05 to a DMF solution containing pyromellitic anhydride and 4,4'-diaminodiphenyl ether, stir at 140°C to evaporate the solvent, and the stirring speed is 200 rpm; transfer the obtained mixed powder to a muffle furnace and calcine at 380°C for 5 hours to obtain the target solid electrolyte material, and the mixed dry powder obtained here also needs to be stored in an Ar environment;
[0055] Step 5: Preparation of composite positive electrode: Grind and mix the solid electrolyte powder obtained in step 4 with high nickel ternary positive electrode material (Ni88), powder conductive agent VGCF and MWCNTs (ratio of 1:1), and PTFE binder in a mass ratio of 12:35:1.5:1, then roll the powder into a film, die-cut, and package it with aluminum foil at a pressure of 80Mpa for 2 minutes to obtain a composite positive electrode. The thickness of the obtained composite positive electrode sheet is 140μm; Preparation of composite negative electrode: Grind and mix the solid electrolyte powder obtained in step 4 with silicon-carbon negative electrode, PTFE, VGCF and MWCNTs (ratio is 1:2), grind and mix in a mass ratio of 17:40:2:1, and then roll the powder into a film, die-cut, and package it with copper foil under a pressure of 80Mpa for 2 minutes to obtain a composite negative electrode with a thickness of 110μm; electrolyte membrane preparation: using a dry membrane preparation method, the above-mentioned solid electrolyte powder and polyPTFE are evenly mixed in a mortar at a weight ratio of 99:1, and finally an electrolyte membrane with a thickness of 100μm is prepared by multiple rolling; the composite positive electrode and the composite negative electrode are placed on both sides of the electrolyte membrane, pressed, and packaged into an all-solid-state soft-pack battery with an aluminum-plastic film.
[0056] Step 6: Ionic conductivity test: Take the solid electrolyte material of step 5 and press it into a disc-shaped lithium ion solid electrolyte with a diameter of 15 mm and a thickness of 1.5 mm under a pressure of 240 MPa in an environment with a moisture content of <30 ppm (dew point <-52°C). Perform EIS test at 25°C, calculate the lithium ion conductivity, and place it in the dew point environment for different time periods to test the change in ionic conductivity (calculate the ionic conductivity according to the formula ρ=d / (πr2×R), where ρ is the ionic conductivity, d is the sample thickness, r is the sample radius, and R is the AC impedance); perform electrical performance test on the all-solid-state soft-pack battery of step 5: Cycle performance and rate performance test: Place the above-mentioned all-solid-state battery at a constant temperature of 25°C, cycle it for 200 weeks at a current density of 1.0 mA cm-2, and calculate the capacity retention rate of the 200th week.
[0057] Example 3
[0058] Step 1: Dissolve 0.58g of pyromellitic anhydride in 10.9g of n-hexane solution and 73.1g of Li 6.65 Ga 0.15 Ln3Z 1.9 Sc 0.1 O 12The nano solid electrolyte powder was ultrasonically dispersed in a n-hexane solution for 1 h to obtain a mixed solution ①, 0.52 g of 4,4'-diaminodiphenyl ether and 0.32 g of LiTFSI which had been ultrasonically dispersed for 1 h were dissolved in 9.8 g of N,N-dimethylformamide (DMF) to obtain a solution ②, and then the solution ② was uniformly added to the solution ① under stirring conditions, the stirring speed was 100 rpm, the reaction time was 0.5 h, and then the mixture solution was heat treated at 150° C. to volatilize the solvent to obtain a mixed powder;
[0059] Step 2: The mixed powder obtained in step 1 is transferred to a muffle furnace for calcination at 230°C, with a program heating rate of 5°C / min, and calcined for 2h to obtain a composite material PI / LiTFSI@LLZO, and then ball milled. The ball milling uses a 1:1 mixture of large and small balls, with a large ball diameter of 5mm and a small ball diameter of 2mm, a rotation speed of 300rpm, and a time of 3h to obtain PI / LiTFSI@LLZO powder; the mass of the coating material PI / LiTFSI is 2% of the mass of the LLZO solid electrolyte;
[0060] Step 3: In a glove box, take appropriate amounts of Li2S, P2S5 and Li Cl powders in a molar ratio of 5:1:2 and mix them under an inert atmosphere. Add the mixture into a ball mill and use two sizes of zirconium balls to ball mill the powder. The ball milling uses a 1:2 mixture of large and small balls, with a large ball diameter of 5 mm and a small ball diameter of 2 mm, a rotation speed of 300 rpm, and a time of 1 h. Transfer the mixture obtained by ball milling to a tubular furnace and calcine at 450°C for 5 h to obtain a solid electrolyte Li6PS5Cl powder. The preparation process of Li6PS5Cl powder is protected by Ar inert gas throughout.
[0061] Step 4: Take 6.0g of PI / LiTFSI@LLZO obtained in step 2 and 100.0g of Li6PS5Cl powder obtained in step 3 and transfer them to a ball mill, dry mix them evenly, the mixer speed is 100rpm, and the mixing time is 1h; obtain PI / LiTFSI@LLZO@Li6PS5Cl mixed powder; then take out the mixed powder, and mix PI / LiTFSI@LLZO@Li6PS5Cl: LiTFSI: Li 1.6 Al 0.4 Ti 1.6 P3O1: pyromellitic anhydride: 4,4'-diaminodiphenyl ether are added to a DMF solution containing pyromellitic anhydride and 4,4'-diaminodiphenyl ether in a mass ratio of 9:0.03:0.1:0.02:0.02, and the solvent is volatilized by stirring at 120°C; the obtained mixed powder is transferred to a muffle furnace and calcined at 230°C for 2 hours to obtain the target solid electrolyte material. The mixed dry powder obtained here also needs to be stored in an Ar environment;
[0062] Step 5: Preparation of composite positive electrode: Grind and mix the solid electrolyte powder obtained in step 4 with high nickel ternary positive electrode material (Ni88), powder conductive agent VGCF and MWCNTs (ratio of 1:1), and PTFE binder in a mass ratio of 28:35:2:1, then roll the powder into a film, die-cut, and package it with aluminum foil at a pressure of 100Mpa for 2 minutes to obtain a composite positive electrode. The thickness of the obtained composite positive electrode sheet is 140μm; Preparation of composite negative electrode: Grind and mix the solid electrolyte powder obtained in step 4 with silicon-carbon negative electrode, PTFE, VGCF and MWCNTs (ratio is 1:2), grind and mix in a mass ratio of 23:40:3:1, and then roll the powder into a film, die-cut, and package it with copper foil under a pressure of 80Mpa. The pressing time is 2min to obtain a composite negative electrode with a thickness of 110μm. Electrolyte membrane preparation: using a dry membrane preparation method, the above-mentioned solid electrolyte powder and polyPTFE are evenly mixed in a mortar at a weight ratio of 99:1, and finally an electrolyte membrane with a thickness of 100μm is prepared by multiple rolling; the composite positive electrode and the composite negative electrode are placed on both sides of the electrolyte membrane, pressed, and packaged into an all-solid-state soft-pack battery with an aluminum-plastic film.
[0063] Step 6: Ionic conductivity test: Take the solid electrolyte material of step 5 and press it into a disc-shaped lithium ion solid electrolyte with a diameter of 15 mm and a thickness of 1.5 mm under a pressure of 240 MPa in an environment with a moisture content of <30 ppm (dew point <-52°C). Perform EIS test at 25°C, calculate the lithium ion conductivity, and place it in the dew point environment for different time periods to test the change in ionic conductivity (calculate the ionic conductivity according to the formula ρ=d / (πr2×R), where ρ is the ionic conductivity, d is the sample thickness, r is the sample radius, and R is the AC impedance); perform electrical performance test on the all-solid-state soft-pack battery of step 5: Cycle performance and rate performance test: Place the above-mentioned all-solid-state battery at a constant temperature of 25°C, cycle it for 200 weeks at a current density of 1.0 mA cm-2, and calculate the capacity retention rate of the 200th week.
[0064] Comparative Example 1
[0065] The difference between Comparative Example 1 and Example 1 is that:
[0066] Li in Comparative Example 1 6.65 Ga 0.15 Ln3Z 1.9 Sc 0.1 O 12 The solid electrolyte is not coated with PI / LITFSI and is directly used in step 3 and subsequent operations. Step 3 and the following operations are consistent with those in Example 1.
[0067] Comparative Example 2
[0068] The difference between Comparative Example 2 and Example 1 is that:
[0069] In Comparative Example 2, Li is not used. 1.7 Al 0.3 Ti 1.7 P3O 12 The remaining materials and steps are the same as those in Example 1.
[0070] Table 1 is a comparison of the performance of the solid electrolyte and solid-state battery corresponding to the examples and comparative examples
[0071]
[0072] It can be seen from Table 1 above that the solid electrolytes prepared in Examples 1-3 have better stability in the air, which is significantly better than that in Comparative Examples 1-2, and can maintain a relatively high discharge specific capacity after 200 cycles, among which Example 1 has the best performance.
[0073] Although some specific embodiments of the present invention have been described in detail by way of example, it will be appreciated by those skilled in the art that the above examples are for illustration only and are not intended to limit the scope of the present invention. It will be appreciated by those skilled in the art that the above embodiments may be modified without departing from the scope and spirit of the present invention. The scope of the present invention is defined by the appended claims.
Claims
1. An electrolyte material with stable positive and negative electrode interfaces, characterized in that: The sulfide solid electrolyte is used as the core, the sulfide solid electrolyte is wrapped with an LLZO solid electrolyte on the outside, the LLZO solid electrolyte is coated with a coating material on the outside, and the coating material is PI / LiTFSI and PI / NASICON.
2. A method for preparing an electrolyte material with a stable positive and negative electrode interface, characterized in that: include: Prepare a first composite solid electrolyte, wherein the first composite solid electrolyte is a composite solid electrolyte PI / LiTFSI@LLZO in which a coating material is coated on the outside of the LLZO-based solid electrolyte, where @ indicates that the substance PI / LiTFSI is coated on the surface of the substance LLZO particles; preparing a second solid electrolyte, wherein the second solid electrolyte is the sulfide solid electrolyte; Preparing a third solid electrolyte, comprising: mixing the first composite solid electrolyte and the second solid electrolyte to obtain a third solid electrolyte; The target solid electrolyte material is prepared by adding the third solid electrolyte, lithium salt, and NASICON type nano solid electrolyte into a DMF solution containing pyromellitic dianhydride and 4,4'-diaminodiphenyl ether to obtain the target solid electrolyte material.
3. The method for preparing an electrolyte material having a stable positive and negative electrode interface according to claim 2, The preparation of the first composite solid electrolyte comprises: Dissolve pyromellitic anhydride in a n-hexane solution, and ultrasonically disperse LLZO series nano solid electrolyte powder in the n-hexane solution for 1 h to 3 h to obtain a first mixed solution; 4,4'-diaminodiphenyl ether and LiTFSI dispersed by ultrasonication for 1 h to 3 h are dissolved in N,N-dimethylformamide to obtain a second solution; The second solution is uniformly added to the first mixed solution under stirring conditions, the stirring speed is 100rpm-200rpm, and the reaction time is 0.5h-3h; heat-treating the mixture solution to volatilize the solvent and obtain a mixed powder; The mixed powder is transferred to a muffle furnace and calcined at 230° C.-400° C. for 2-6 hours to obtain a composite material PI / LiTFSI@LLZO. The composite material PI / LiTFSI@LLZO is ball-milled to obtain PI / LiTFSI@LLZO powder, which is the first composite solid electrolyte.
4. The method for preparing an electrolyte material with stable positive and negative electrode interfaces according to claim 2, characterized in that: The mass of the coating material PI / LiTFSI is 0.8%-2% of the mass of the LLZO solid electrolyte; Alternatively, the mass ratio of the third solid electrolyte, lithium salt, NASICON type nano solid electrolyte, pyromellitic anhydride, and 4,4'-diaminodiphenyl ether is (9-12): (0.03-0.08): (0.1-0.15): (0.02-0.06): (0.02-0.05); Alternatively, the mass of the second solid electrolyte accounts for 4%-6% of the mass of the third solid electrolyte.
5. The method for preparing an electrolyte material with stable positive and negative electrode interfaces according to claim 2, characterized in that: The preparation of the second solid electrolyte comprises: Li2S, P2S5 and LiCl powders are mixed under an inert atmosphere, the mixture is added into a ball mill, and the powders are ball milled using zirconium balls of two sizes for 1-3 hours. The ball-milled mixture is transferred to a tubular furnace and calcined at 450-650°C for 5-12 hours to obtain a solid electrolyte Li6PS5Cl powder.
6. The method for preparing an electrolyte material with stable positive and negative electrode interfaces according to claim 2, characterized in that: The method for preparing the target solid electrolyte material comprises adding the third solid electrolyte, lithium salt, and NASICON type nano solid electrolyte into a DMF solution containing pyromellitic anhydride and 4,4'-diaminodiphenyl ether to obtain the target solid electrolyte material, including: The first composite solid electrolyte and the second solid electrolyte powder are transferred to a ball mill, and dry mixed evenly, the mixer speed is 100rpm-300rpm, and the mixing ball milling time is 1h-3h to obtain a third solid electrolyte mixed powder, and the third solid electrolyte mixed powder is taken out, and the third solid electrolyte, lithium salt, and NASICON type nano solid electrolyte are added to a DMF solution containing pyromellitic anhydride and 4,4'-diaminodiphenyl ether, and stirred at 120°C-140°C, and the stirring speed is 100rpm-200rpm, and the solvent is volatilized; The obtained mixed powder is transferred to a muffle furnace and calcined at 230° C.-380° C. for 2 h-5 h to obtain the target solid electrolyte material.
7. The electrolyte material with stable positive and negative electrode interfaces according to claim 1, characterized in that: The LLZO-based solid electrolyte comprises Li7La3Zr2O 12 , Li 6.2 Ga 0.3 La 2.95 R 0.05 Zr2O 12 , Li 6.65 Ga 0.15 LqCy 1.9 Sc 0.1 O 12 , Li 7.06 3Y 0.06 Zr 1.94 O 12 , Li 6.5 Ga 0.2 La 2.9 Sr 0.1 Zr2O 12 One or more of; The NASICON-type nano solid electrolyte comprises Li 1.5 Al 0.5 Ge 1.5 (PO4)3、Li 1.7 Al 0.3 Ti 1.7 Si 0.4 P 2.6 O 12 , Li 1.7 Al 0.3 Ti 1.7 P3O 12 , Li 1.6 Al 0.4 Ti 1.6 P3O 12 , Li 1.5 Al 0.4 Cr 0.1 Ge 1.5 (PO4) one or more.
8. A solid-state battery, characterized in that: The invention comprises the electrolyte material with stable positive and negative electrode interfaces as claimed in claim 1.
9. A method for preparing the solid-state battery according to claim 8, characterized in that: include: The composite positive electrode is prepared, comprising: mixing and grinding the electrolyte material with stable positive and negative electrode interfaces with the high-nickel ternary positive electrode material, the powder conductive agent, and the PTFE binder, rolling the powder into a film, die-cutting, and encapsulating it with aluminum foil at a pressure of 80Mpa-100Mpa for 1min-3min to obtain the composite positive electrode; The composite negative electrode is prepared, comprising: mixing and grinding the electrolyte material with stable positive and negative electrode interfaces with the silicon-carbon negative electrode, the PTFE binder, and the powder conductive agent, rolling the powder into a film, die-cutting, and packaging with copper foil at a pressure of 60 MPa-100 MPa for 1 min-3 min to obtain the composite negative electrode; The electrolyte membrane is prepared by using a dry membrane preparation method, the electrolyte material with stable interface between positive and negative electrodes and a poly-PTFE binder are uniformly mixed in a mortar, and finally the electrolyte membrane is prepared by multiple rolling; And encapsulating an all-solid-state soft-pack battery, comprising placing the composite positive electrode and the composite negative electrode on both sides of the electrolyte membrane, pressing them, and encapsulating them with an aluminum-plastic film to form an all-solid-state soft-pack battery.
10. The method for manufacturing a solid-state battery according to claim 9, characterized in that: The mass ratio of the positive and negative electrode interface-stabilizing electrolyte material, high-nickel ternary positive electrode material, powder conductive agent, and PTFE binder is (10-20):(30-40):(1.5-3):1; The mass ratio of the electrolyte material for stabilizing the positive and negative electrode interfaces, the silicon-carbon negative electrode, the powder conductive agent, and the PTFE binder is (15-25):(35-45):(2-4):1.
Citation Information
Patent Citations
Coated sulfide solid electrolyte material and preparation method and application thereof
CN114512710A
Core-shell structure sulfide solid electrolyte, preparation method and all-solid-state battery
CN114976222A
Ceramic filler modified high-conductivity wide-voltage window composite electrolyte material, preparation method and application
CN115064764A
Coated solid electrolyte material as well as preparation method and application thereof
CN115395087A
Modified oxide solid electrolyte material and preparation method and application thereof
CN118472356A
Cited By
Positive electrode material wrapped by mixed solid electrolyte, preparation method of positive electrode material, positive electrode plate, solid-state battery and power-related equipment
CN119786564A