Electrolyte and battery

By using 2-trifluoromethyl isocyanate and carbonate additives in lithium-ion battery electrolyte, combined with sulfur-containing additives, the problems of SEI film instability and moisture and hydrofluoric acid in natural graphite negative electrode material are solved, significantly improving the High temperature storage and cycling performance of lithium-ion batteries.

CN118943490APending Publication Date: 2024-11-12EVE ENERGY CO LTD

Patent Information

Application Number
CN202410994567.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The SEI film instability of natural graphite anode materials in existing lithium-ion batteries leads to excessive decomposition of electrolyte and loss of active lithium. The existing negative electrode film forming additives have limitations, which cannot effectively eliminate moisture and hydrofluoric acid in the electrolyte. , affects battery performance.

Method used

2-trifluoromethyl isocyanate is introduced as the first functional additive, combined with carbonate additives, optimize the density and interface stability of the SEI film, eliminate moisture and hydrofluoric acid in the electrolyte, improve the interface stability of the negative electrode, and pass Sulfur-containing additives enhance the stability of the cathode CEI film.

Benefits of technology

It significantly improves the high-temperature storage performance and high-temperature cycle performance of lithium-ion batteries, enhances the density and stability of the negative electrode SEI film, reduces interface damage during the charge and discharge cycle, and optimizes the electrochemical performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118943490A_ABST
    Figure CN118943490A_ABST
Patent Text Reader

Abstract

The invention provides an electrolyte and a battery. The electrolyte comprises a lithium salt, an organic solvent, a carbonic ester additive and a first functional additive, and the structural formula of the first functional additive is as follows: # imgabs0 #. The electrolyte can further improve the stability of a negative electrode interface and the stability of the electrolyte in the use process, reduce the side reaction of the interface, and optimize the high-temperature storage performance and the normal-temperature and high-temperature cycle performance of the battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of lithium batteries, and in particular relates to an electrolyte and a battery. Background Art

[0002] Natural graphite, which has large reserves, low commercialization costs and is environmentally friendly, is a lithium-ion battery negative electrode material with potential commercial value. However, due to the instability of the SEI film formed on the surface of natural graphite, it will not only cause excessive decomposition of the electrolyte, thereby increasing the membrane impedance, but also cause the loss of active lithium. This paper aims to improve the electrochemical performance of natural graphite negative electrode materials by screening suitable functional additives to optimize the composition of the electrolyte and regulating the structure and components of the SEI film, providing a possibility for achieving high-performance natural graphite batteries with high stability, long cycle life and commercial production.

[0003] Among the existing strategies for adjusting electrolyte components, the use of electrolyte additives can achieve twice the result with half the effort. By adding additives, the formation process of the SEI film is regulated. The optimized SEI film is thin and dense, which can improve the compatibility of the negative electrode electrolyte. There are two main types of additives for improving the stability of the SEI film, one is a reducing additive and the other is a reactive additive.

[0004] The main mechanism of action of reductive additives is to reduce the solvent before the additive, thereby inhibiting the continuous decomposition of the solvent. This type of additive can be further divided into two types. The first is a polymer additive, which undergoes an electrochemical reduction polymerization reaction in the high potential range and preferentially forms a stable SEI film on the negative electrode surface to weaken side reactions in subsequent cycles. The main characteristic of its molecule is that it contains unsaturated bonds, which can undergo reduction polymerization under potential drive, and the reduction polymerization product generated by polymerization is insoluble in the electrolyte and stably exists on the negative electrode surface, playing a protective role. The other is a reducing agent. Fluorine, borates, sulfates, nitrates and other substances contain electron-withdrawing atoms such as F, B, N, S, and can be reduced to generate LiF and LiB when used as additives. x O y ,LiS x O y and LiN x O y Salts and other compounds are adsorbed on the negative electrode to form inorganic SEI film components, which improve the mechanical stability and lithium ion transmission capacity of the SEI film.

[0005] However, the choice of electrolyte for lithium-ion batteries is very limited, and the choice of electrolyte additives in the existing electrolyte components is also very limited. The current mainstream negative electrode film-forming additives such as FEC (fluoroethylene carbonate) can improve the stability of the negative electrode SEI film to a certain extent and reduce the damage of the negative electrode SEI film, but there are certain limitations. FEC reacts with PF5 to remove F and produce HF. FEC will further produce CO2 and other gases as a side reaction. The gas increases the polarization of the battery and reduces the battery's electrical performance and high-temperature storage performance. In addition, most of the current negative electrode film-forming additives cannot eliminate the water and hydrofluoric acid in the electrolyte. The presence of water and hydrofluoric acid will have a significant deterioration effect on the stability of the negative electrode interface.

[0006] In view of this, it is still an urgent problem to develop a new type of negative electrode film-forming additive and electrolyte to improve the interface stability of graphite or silicon-carbon negative electrode and further optimize battery performance. Summary of the invention

[0007] In order to solve the problems and deficiencies in the prior art, the present invention provides an electrolyte and a battery. The electrolyte introduces a first additive (2-trifluoromethyl isocyanate), which can directly participate in the negative electrode film formation, improve the uniformity and compactness of the negative electrode SEI film, and can also eliminate moisture and hydrofluoric acid in the electrolyte, so that the negative electrode interface stability and the stability of the electrolyte during use can be further improved, the interface side reactions can be reduced, and the high temperature storage performance of the battery and the normal temperature and high temperature cycle performance can be optimized. At the same time, the additive can also work together with the carbonate additive to further optimize the compactness and uniformity of the negative electrode SEI film, so that it is not easily destroyed during the charge and discharge cycle, thereby further optimizing the charge and discharge cycle performance of the battery.

[0008] According to a first aspect of the present invention, an electrolyte is provided, comprising a lithium salt, an organic solvent, a carbonate additive, and a first functional additive; the structural formula of the first functional additive is as follows:

[0009]

[0010] In the electrolyte provided by the present invention, the first functional additive introduced is 2-trifluoromethyl isocyanate, which contains isocyanate and trifluoromethyl in its structure. First, isocyanate can react with active hydrogen, so it can eliminate moisture and hydrofluoric acid in the electrolyte, optimize the stability of the electrolyte, and further optimize the electrochemical performance of the battery; second, trifluoromethyl can effectively participate in the film formation of the negative electrode SEI, and the film-forming component has a lithium fluoride component, which can improve the interface stability of the SEI film, optimize the high-temperature storage performance of the battery, and the normal temperature and high-temperature cycle performance. It should be noted here that, generally speaking, the most commonly used lithium salt in the electrolyte is lithium hexafluorophosphate, and lithium hexafluorophosphate will inevitably carry hydrofluoric acid into the final product during its preparation process. When the hydrofluoric acid content in the lithium battery exceeds a certain concentration, it will begin to consume limited lithium ions, increase the irreversible capacity of the battery, and the lithium oxide and lithium fluoride generated at the same time are not conducive to the improvement of the electrochemical performance of the electrode, and the gas produced by the reaction will cause the pressure in the battery to increase. As the hydrofluoric acid content continues to increase, the performance of lithium batteries such as charging and discharging, and cycle efficiency will significantly decrease, or even be completely destroyed. Due to the above reasons, the hydrofluoric acid content in lithium battery electrolytes needs to be strictly controlled below 0.005%, that is, the less hydrofluoric acid content, the better. In addition, lithium hexafluorophosphate will undergo hydrolysis reaction to generate hydrofluoric acid when it comes into contact with water. At the same time, there will be a certain amount of water in the preparation process of the electrolyte, which will cause lithium hexafluorophosphate to produce more hydrofluoric acid, which is not conducive to the electrochemical performance of the battery.

[0011] At the same time, the electrolyte provided by the present invention also contains carbonate additives, which can promote the film formation of the negative electrode, and thus can work together with the first additive (2-trifluoromethyl isocyanate) to exert a certain synergistic effect, further promoting the compactness, uniformity and stability of the SEI film generated at the negative electrode, and improving the interface stability of the negative electrode. Compared with a single 2-trifluoromethyl isocyanate or carbonate additive, the combined use of the two is more conducive to the compactness and stability of the negative electrode SEI film, making the SEI film less likely to be destroyed during the charge and discharge cycle, and at the same time ensuring the rapid deintercalation of lithium ions on the negative electrode side, so it is more conducive to optimizing the electrochemical performance of the battery, especially for high-temperature storage characteristics and high-temperature cycle performance, which has a more obvious improvement.

[0012] Preferably, the mass proportion of the first functional additive in the electrolyte is 0.2-0.5%. Too little first additive is not conducive to further effectively improving the density and uniformity of the SEI film at the negative electrode interface. At the same time, because the positive and negative poles have a certain mutual influence, too little first additive will also lead to a decrease in the stability of the positive electrode interface, resulting in a decrease in the degree of optimization of the battery performance. Too much first additive, on the one hand, will limit the role of other electrolyte additives or other components of the electrolyte, resulting in a decrease in the overall performance of the electrolyte, and then the stability at the negative electrode interface or the positive electrode interface will decrease, which is not conducive to further optimization of battery performance. At the same time, too much first additive will also transition into a film, which is not conducive to the deintercalation and insertion of lithium ions, and therefore is not conducive to the cycle performance of the battery.

[0013] Preferably, the electrolyte provided by the present invention also includes a second functional additive, which is a sulfur-containing additive, and the sulfur-containing additive includes at least one of vinyl sulfate, 1,3-propane sultone, and propenyl-1,3-sultone; the mass proportion of the sulfur-containing additive in the electrolyte is 1.0-2.0%. The above-mentioned sulfur-containing additives are also mainly used to assist film formation at the negative electrode, and have high thermal stability. Too little addition is not conducive to the formation of a dense SEI film at the negative electrode, and too much addition will cause transitional film formation, which is not conducive to the deintercalation of lithium ions, resulting in decreased cycle performance. And too much addition is not conducive to its interaction with other electrolyte additives, affecting the performance of other electrolyte additives or other components of the electrolyte. Although the first additive and the second additive (sulfur-containing additive) are mainly film-formed on the negative electrode side, the introduction of these two can also further promote the stability of the positive electrode CEI film, thereby increasing the overall stability of the battery and further optimizing the electrochemical performance.

[0014] Preferably, the sulfur additive includes vinyl sulfate and 1,3-propane sultone; or, the sulfur-containing additive includes vinyl sulfate and propenyl-1,3-sultone; or, the sulfur-containing additive includes vinyl sulfate, 1,3-propane sultone and propenyl-1,3-sultone. In the combination of the above sulfur-containing additives, these combinations and the first additive will not only not have obvious adverse reactions, but also can produce certain synergistic effects when used in such a combination, especially further enhancing the interface stability and lithium conductivity of the negative electrode SEI film, and also improving the stability of the positive electrode CEI film to a certain extent, thereby further improving the normal temperature and high temperature cycle performance and storage performance of the battery.

[0015] Preferably, the carbonate additive includes at least one of vinylene carbonate and fluoroethylene carbonate; the mass proportion of the carbonate additive in the electrolyte is 0.2-0.5%. Carbonate additives such as vinylene carbonate (VC) and fluoroethylene carbonate (FEC) form a film at the negative electrode, but too little addition will not form a dense SEI film, and too much addition will lead to high impedance and high-temperature gas production. At the same time, too much addition is not conducive to its interaction with other electrolyte additives, affecting the performance of other electrolyte additives or other components of the electrolyte, which is not conducive to the comprehensive performance of the electrolyte.

[0016] Preferably, the electrolyte provided by the present invention also includes a lithium salt additive, and the lithium salt additive includes at least one of lithium bis(fluorosulfonyl)imide, lithium difluorophosphate, lithium bis(oxalatoborate), and lithium difluorobis(oxalatophosphate); the mass proportion of the lithium salt additive in the electrolyte is 1.1-2.0%. The lithium salt additive has the function of forming positive and negative electrodes, can further improve the density of the generated CEI film and SEI film, can inhibit the dissolution of positive electrode metal ions, weaken the damage of metal ions to the negative electrode SEI film, and improve the thermal stability of the film. If the amount of addition is too small, a dense SEI film cannot be formed, and if the amount of addition is too large, gas production and electrical performance will be reduced. And because other negative electrode film-forming additives such as the first functional additive (2-trifluoromethyl isocyanate) and / or the second functional additive (sulfur-containing additive) are introduced into the present invention, the negative electrode film-forming ability is greatly improved. Therefore, when a relatively high content of lithium salt additive is added at this time, the CEI film formed at the positive electrode interface can better match the SEI film formed at the negative electrode interface in terms of function. Therefore, during the charge and discharge cycle of the entire battery, the positive and negative electrode interfaces are more stable and not easily destroyed during the charge and discharge cycle, and the lithium ion insertion and extraction are more balanced, which further improves the electrochemical performance of the battery.

[0017] Preferably, the lithium salt includes lithium hexafluorophosphate, and the concentration of the lithium salt in the electrolyte is 1.0 to 1.3 mol / L.

[0018] Preferably, the organic solvent includes at least two of ethylene carbonate, dimethyl carbonate, diethyl carbonate, and ethyl methyl carbonate.

[0019] Preferably, when the organic solvent includes ethylene carbonate and ethyl methyl carbonate, calculated by volume fraction, the volume fractions of ethylene carbonate, dimethyl carbonate, diethyl carbonate and ethyl methyl carbonate in the organic solvent are 20-40%, 0-20%, 0-20% and 30-50%, respectively.

[0020] According to the second aspect of the present invention, a battery is provided, comprising the above-mentioned electrolyte. By using the electrolyte provided by the present invention, a very uniform and dense SEI film can be formed on the negative electrode side, which greatly improves the interface stability of the SEI film, and can effectively improve the instability problem caused by the continuous change of the SEI film during the charge and discharge cycle, so that the electrochemical performance of the battery is significantly improved, especially the high-temperature storage performance and high-temperature cycle performance are effectively improved. Not only that, such an electrolyte composition further improves the stability of the positive electrode CEI film, so the electrochemical performance of the battery is further improved. DETAILED DESCRIPTION

[0021] In order to enable those skilled in the art to better understand the solutions of the present invention, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only embodiments of a part of the present invention, rather than all embodiments.

[0022] Example 1

[0023] 1. Electrolyte and preparation of electrolyte

[0024] The electrolyte in this embodiment is composed of an organic solvent, a lithium salt and an additive, wherein the lithium salt is an electrolyte salt. The additives are carbonate additives, lithium salt additives, first functional additives, and second functional additives (sulfur-containing additives). The carbonate additive is fluoroethylene carbonate (FEC), and its mass fraction in the electrolyte is 0.3%. The lithium salt additive is lithium difluorophosphate (LiPO2F2), and its mass fraction in the electrolyte is 1.5%. The sulfur-containing additive is 1,3-propane sultone (PS), and its mass fraction in the electrolyte is 1.5%. The first additive is The mass fraction in the electrolyte is 0.3%. The lithium salt is lithium hexafluorophosphate (LiPF6), and its concentration in the electrolyte is 1.0 mol / L. The organic solvent is composed of ethylene carbonate, diethyl carbonate, and ethyl methyl carbonate. Taking the total volume of the organic solvent as 100%, the volume fraction of ethylene carbonate is 30%, the volume fraction of diethyl carbonate is 20%, and the volume fraction of ethyl methyl carbonate is 50%.

[0025] The preparation of the electrolyte follows the following steps: in an argon atmosphere, add the carbonate additive, lithium salt additive, first additive and sulfur-containing additive to an organic solvent, and finally add lithium hexafluorophosphate (lithium salt) and stir at low temperature to mix evenly.

[0026] 2. Preparation of batteries

[0027] The battery of this embodiment includes a positive electrode, a negative electrode, an electrolyte, and a separator.

[0028] In the preparation of the positive electrode sheet, the positive electrode active material is a nickel-cobalt-manganese ternary material (Li(Ni x Co y Mn z )O2) (where 0.5 ≤ x < 0.8, 0 < y ≤ 0.3, 0 < z ≤ 0.3 and x + y + z = 1). And the preparation method of the positive electrode sheet is as follows: Prepare a slurry by mixing the positive electrode active material (NCM523 in this embodiment), the conductive agent acetylene black, and the binder PVDF in a mass ratio of 94:3:3, coat it on an aluminum foil current collector, and dry it in vacuum to obtain the positive electrode sheet.

[0029] In the preparation of the negative electrode sheet, the negative electrode active material is graphite. And the preparation method of the negative electrode sheet is as follows: Prepare a slurry by mixing the negative electrode active material graphite, the conductive agent acetylene black, and the binders CMC and SBR in a mass percentage of 94:1:2:3, coat it on a copper foil current collector, and dry it in vacuum to obtain the negative electrode sheet

[0030] After assembling the positive and negative electrode sheets prepared above with a Celgard 2400 separator to obtain an electric core, transfer the electric core into a casing, and then inject the electrolyte prepared in this embodiment, and perform formation and constant volume to obtain the battery of this embodiment.

[0031] Example 2

[0032] 1. Electrolyte and its preparation

[0033] The difference between the electrolyte in this example and that in Example 1 is that: adjust the mass fraction of the first functional additive in the electrolyte to 0.2%, which can be obtained by adaptively adjusting the amount of the organic solvent (one or more of the organic solvents can be adjusted). The rest is the same as in Example 1.

[0034] And the preparation of the electrolyte in this example is the same as that in Example 1.

[0035] 2. Preparation of the battery

[0036] The preparation of the battery in this example is the same as that in Example 1.

[0037] Example 3

[0038] 1. Electrolyte and its preparation

[0039] The difference between the electrolyte in this example and that in Example 1 is that: adjust the mass fraction of the first functional additive in the electrolyte to 0.5%, which can be obtained by adaptively adjusting the amount of the organic solvent (one or more of the organic solvents can be adjusted). The rest is the same as in Example 1.

[0040] And the preparation of the electrolyte in this example is the same as that in Example 1.

[0041] 2. Preparation of the battery

[0042] The preparation of the battery in this example is consistent with that in Example 1.

[0043] Example 4

[0044] 1. Electrolyte and preparation of electrolyte

[0045] The electrolyte in this embodiment is different from that in Embodiment 1 in that the mass fraction of the first functional additive in the electrolyte is adjusted to 0.1%, which can be obtained by adaptively adjusting the amount of the organic solvent (one or more of the organic solvents can be adjusted). The rest is the same as in Embodiment 1.

[0046] The preparation of the electrolyte in this embodiment is consistent with that in Example 1.

[0047] 2. Preparation of batteries

[0048] The preparation of the battery in this example is consistent with that in Example 1.

[0049] Example 5

[0050] 1. Electrolyte and preparation of electrolyte

[0051] The electrolyte in this embodiment is different from that in Embodiment 1 in that the mass fraction of the first functional additive in the electrolyte is adjusted to 0.7%, which can be obtained by adaptively adjusting the amount of the organic solvent (one or more of the organic solvents can be adjusted). The rest is the same as in Embodiment 1.

[0052] The preparation of the electrolyte in this embodiment is consistent with that in Example 1.

[0053] 2. Preparation of batteries

[0054] The preparation of the battery in this example is consistent with that in Example 1.

[0055] Example 6

[0056] 1. Electrolyte and preparation of electrolyte

[0057] The electrolyte in this embodiment is different from that in Embodiment 1 in that the sulfur-containing additive is adjusted to diethyl sulfate (DTD). The rest is the same as that in Embodiment 1.

[0058] The preparation of the electrolyte in this embodiment is consistent with that in Example 1.

[0059] 2. Preparation of batteries

[0060] The preparation of the battery in this example is consistent with that in Example 1.

[0061] Example 7

[0062] 1. Electrolyte and preparation of electrolyte

[0063] The electrolyte in this embodiment is different from that in Embodiment 1 in that the sulfur-containing additives are adjusted to be vinyl sulfate (DTD) and 1,3-propane sultone (PS), and the mass fractions of DTD and PS in the electrolyte are 0.9% and 0.6%, respectively. The rest is the same as in Embodiment 1.

[0064] The preparation of the electrolyte in this embodiment is consistent with that in Example 1.

[0065] 2. Preparation of batteries

[0066] The preparation of the battery in this example is consistent with that in Example 1.

[0067] Example 8

[0068] 1. Electrolyte and preparation of electrolyte

[0069] The electrolyte in this embodiment is different from that in Embodiment 1 in that the sulfur-containing additive is adjusted to vinyl sulfate (DTD), 1,3-propane sultone (PS) and propenyl-1,3-sultone (PST), and the mass fractions of DTD, PS and PST in the electrolyte are 0.7%, 0.5% and 0.3% respectively. The rest is the same as that in Embodiment 1.

[0070] The preparation of the electrolyte in this embodiment is consistent with that in Example 1.

[0071] 2. Preparation of batteries

[0072] The preparation of the battery in this example is consistent with that in Example 1.

[0073] Example 9

[0074] 1. Electrolyte and preparation of electrolyte

[0075] The electrolyte in this embodiment is different from that in Embodiment 1 in that the mass fraction of the lithium salt additive (LiPO2F2) in the electrolyte is adjusted to 0.9%. The rest is the same as that in Embodiment 1.

[0076] The preparation of the electrolyte in this embodiment is consistent with that in Example 1.

[0077] 2. Preparation of batteries

[0078] The preparation of the battery in this example is consistent with that in Example 1.

[0079] Example 10

[0080] 1. Electrolyte and preparation of electrolyte

[0081] The electrolyte in this embodiment is different from that in Embodiment 1 in that the mass fraction of the lithium salt additive (LiPO2F2) in the electrolyte is adjusted to 2.3%. The rest is the same as that in Embodiment 1.

[0082] The preparation of the electrolyte in this embodiment is consistent with that in Example 1.

[0083] 2. Preparation of batteries

[0084] The preparation of the battery in this example is consistent with that in Example 1.

[0085] Comparative Example 1

[0086] 1. Electrolyte and preparation of electrolyte

[0087] The electrolyte in this comparative example is different from that in Example 1 in that the first functional additive is not added. The rest is the same as that in Example 1.

[0088] The preparation of the electrolyte in this comparative example is consistent with that in Example 1.

[0089] 2. Preparation of batteries

[0090] The preparation of the battery in this comparative example is consistent with that in Example 1.

[0091] Comparative Example 2

[0092] 1. Electrolyte and preparation of electrolyte

[0093] The electrolyte in this comparative example is different from that in Example 1 in that no carbonate additive is added (ie, no FEC is added). The rest is the same as in Example 1.

[0094] The preparation of the electrolyte in this comparative example is consistent with that in Example 1.

[0095] 2. Preparation of batteries

[0096] The preparation of the battery in this comparative example is consistent with that in Example 1.

[0097] Comparative Example 3

[0098] 1. Electrolyte and preparation of electrolyte

[0099] The electrolyte in this comparative example is different from that in Example 1 in that no carbonate additive (ie, no FEC) and no second additive (ie, no sulfur-containing additive PS) are added. The rest is the same as in Example 1.

[0100] The preparation of the electrolyte in this comparative example is consistent with that in Example 1.

[0101] 2. Preparation of batteries

[0102] The preparation of the battery in this comparative example is consistent with that in Example 1.

[0103] Test Case

[0104] 1. Experimental Construction Method

[0105] The batteries (lithium-ion batteries) prepared in all the above embodiments and comparative examples were subjected to electrochemical tests using a Xinwei charge and discharge test cabinet.

[0106] (1) Cycle performance test of lithium-ion batteries:

[0107] At 25 or 45°C, charge the lithium-ion battery at a constant current of 1.0C (nominal capacity) to a voltage of 4.4V, then charge at a constant voltage of 4.4V to a current ≤0.05C. After standing for 10 minutes, discharge at a constant current of 1C to 2.8V. The above is one charge and discharge cycle.

[0108] The capacity retention rate (%) of a lithium-ion battery after N cycles = (discharge capacity at the Nth cycle / initial discharge capacity) × 100%, where N is the number of cycles of the lithium-ion battery.

[0109] (2) High temperature storage performance test of lithium-ion batteries:

[0110] At 25°C, the lithium-ion battery was charged at a constant current of 1C to a voltage of 4.4V, and then charged at a constant voltage of 4.4V to a current of 0.05C. The volume of the tested lithium-ion battery was V0, and the initial capacity was C0. The lithium-ion battery was then placed in a constant temperature box at 60°C and stored for 90 days, and the volume of the tested lithium-ion battery was taken out and recorded as V1, the capacity remained C1, and the capacity recovered to C2.

[0111] The volume expansion ratio (%) of a lithium-ion battery after storage at 60°C for 90 days = (V1-V0)V0×100%.

[0112] The capacity retention rate (%) of the lithium-ion battery after storage at 60°C for 90 days = (C1 / C0)×100%, and the capacity recovery rate (%) of the lithium-ion battery after storage at 60°C for 90 days = (C2 / C0)×100%.

[0113] The batteries obtained from the above examples and comparative examples were tested as follows:

[0114] (a) High temperature storage performance test of lithium-ion batteries:

[0115] At 25°C, the lithium-ion battery was charged at a constant current of 1C to a voltage of 4.4V, and then charged at a constant voltage of 4.4V to a current of 0.05C. The volume of the tested lithium-ion battery was V0, and the initial capacity was C0. The lithium-ion battery was then placed in a constant temperature box at 60°C and stored for 90 days, and the volume of the tested lithium-ion battery was taken out and recorded as V1, the capacity remained C1, and the capacity recovered to C2.

[0116] The volume expansion rate (%) of a lithium-ion battery after storage at 60°C for 90 days = (V1-V0) / V0×100%.

[0117] The capacity retention rate (%) of the lithium-ion battery after storage at 60°C for 90 days = (C1 / C0)×100%, and the capacity recovery rate (%) of the lithium-ion battery after storage at 60°C for 90 days = (C2 / C0)×100%.

[0118] (b) High temperature storage experiment:

[0119] Carry out 5 charge and discharge cycle tests at room temperature at a charge and discharge rate of 1C, and then charge to full charge at a rate of 1C. Record the 1C capacity Q0 and battery volume V0 respectively. Store the fully charged battery at 60°C for 90 days, record the battery volume V1 and 1C discharge capacity Q1, then charge and discharge the battery at room temperature at a rate of 1C for 5 weeks, record the 1C discharge capacity Q2, and calculate the experimental data such as the battery's high temperature storage capacity retention rate, capacity recovery rate and volume change rate. The recorded results are shown in Table 1 below. The calculation formulas used are as follows: Capacity retention rate (%) = Q1 / Q0×100%; Capacity recovery rate (%) = Q2 / Q0×100%; Volume change rate (%) = (V1-V0) / V0×100%.

[0120] (c) Normal temperature cycle test:

[0121] Place the battery at 25°C, record the initial capacity as A1, the capacity after 5C / 5C cycle to 2000 weeks as A2, and calculate the capacity retention rate of the battery after 2000 weeks of high-temperature cycle by the following formula: Cycle capacity retention rate (%) = A2 / A1×100%.

[0122] (d) High temperature cycle test:

[0123] Place the battery at 45°C, record the initial capacity as A1, the capacity after 5C / 5C cycle to 2000 cycles as A2, and calculate the capacity retention rate of the battery after 2000 cycles of high-temperature cycle by the following formula: Cycle capacity retention rate (%) = A2 / A1×100%, and record the result.

[0124] 2. Experimental results

[0125] The test results of the battery performance of the above embodiments and comparative examples are shown in Table 1 below.

[0126] Table 1. Test results of relevant performance of batteries in the embodiments and comparative examples

[0127]

[0128] As can be seen from Table 1, the electrolyte provided by the present invention can form a relatively dense and uniform SEI film at the negative electrode interface, thereby effectively improving the electrochemical performance of the battery, especially the high-temperature storage characteristics and high-temperature cycle performance of the battery, with specific reference to Examples 1 to 10.

[0129] In Comparative Example 1, the first functional additive, ie, 2-trifluoromethyl isocyanate, is not added, and the CEI film formed at the positive electrode has poor stability, which ultimately leads to poor cycle and storage performance.

[0130] In Comparative Example 3, no carbonate additive is added (ie, no FEC is added), and the CEI film formed at the positive electrode has poor stability, which ultimately leads to poor cycle and storage performance.

[0131] In Comparative Example 3, no carbonate additive (ie, no FEC) and no second additive (ie, no sulfur-containing additive PS) were added, and the CEI film formed at the positive electrode had poor stability, ultimately resulting in poor cycle and storage performance.

[0132] Further comparing Example 1 with Examples 2 to 5, the mass fractions of the first functional additive in the electrolyte in Examples 4 and 5 are 0.1% and 0.7%, respectively, which are too little and too much, respectively. The stability of the CEI film formed by too little is poor, and the polarization of the CEI film formed by too much increases, and the cycle and storage performance of the battery deteriorate. And further comparing Examples 1 to 3, it can be found that when the mass fraction of the first functional additive in the electrolyte is 0.3%, the high temperature storage performance, normal temperature cycle performance and high temperature cycle performance of the battery are better.

[0133] By comparing Example 1 with Examples 6 to 8, it can be found that adjusting the type of sulfur-containing additive will also affect the performance of the battery. And after comparison, it can be found that when the sulfur-containing additive is a combination of DTD, PS and PST, the battery cycle and storage performance is better. This shows that under such a combination, the high-voltage stability of the electrolyte can be further improved, the positive and negative interface stability can be optimized, and the high-temperature storage performance, room temperature cycle performance and high-temperature cycle performance of the battery can be further optimized.

[0134] At the same time, it can be further observed that when the mass fraction of the lithium salt additive in the electrolyte is changed, the performance of the battery will also be affected. Because the lithium salt additive can participate in the film formation of the positive and negative electrodes, the appropriate addition of a certain amount of lithium salt additive can ensure the battery cycle and storage performance. Therefore, when the mass fraction of the lithium salt additive in the electrolyte is controlled within a specific range, it is more conducive to the performance of the battery.

[0135] The above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit the protection scope of the present invention. Although the present invention is described in detail with reference to the above embodiments, ordinary technicians in the relevant field should understand that the technical solutions of the present invention can be modified or equivalently replaced, but these modifications or replacements are all within the protection scope of the present invention.

Claims

1. An electrolyte, characterized in that: Including lithium salt, organic solvent, carbonate additive, and first functional additive; The structural formula of the first functional additive is as follows:

2. The electrolyte according to claim 1, wherein: The mass proportion of the first functional additive in the electrolyte is 0.2-0.5%.

3. The electrolyte according to claim 1, wherein: Also included is a second functional additive, wherein the second functional additive is a sulfur-containing additive, and the sulfur-containing additive includes at least one of vinyl sulfate, 1,3-propane sultone, and propenyl-1,3-sultone; The sulfur-containing additive accounts for 1.0-2.0% by mass in the electrolyte.

4. The electrolyte according to claim 3, wherein: The sulfur-containing additive includes the vinyl sulfate and the 1,3-propane sultone; Or, the sulfur-containing additive includes the vinyl sulfate and the propenyl-1,3-sultone; Alternatively, the sulfur-containing additive includes the vinyl sulfate, the 1,3-propane sultone, and the propenyl-1,3-sultone.

5. The electrolyte according to claim 4, wherein: The sulfur-containing additive includes vinyl sulfate, 1,3-propane sultone, and propenyl-1,3-sultone.

6. The electrolyte according to claim 1, wherein: The carbonate additive includes at least one of vinylene carbonate and fluoroethylene carbonate; The carbonate additive accounts for 0.2-0.5% by mass in the electrolyte.

7. The electrolyte according to claim 1, wherein: Also included is a lithium salt additive, wherein the lithium salt additive includes at least one of lithium bis(fluorosulfonyl)imide, lithium difluorophosphate, lithium bis(oxalatoborate), and lithium difluorobis(oxalatophosphate); The lithium salt additive accounts for 1.1-2.0% by mass in the electrolyte.

8. The electrolyte according to claim 1, wherein: The lithium salt includes lithium hexafluorophosphate, and the concentration of the lithium salt in the electrolyte is 1.0 to 1.3 mol / L.

9. The electrolyte according to claim 1, wherein: The organic solvent includes at least two of ethylene carbonate, dimethyl carbonate, diethyl carbonate, and ethyl methyl carbonate.

10. A battery, characterized in that: The electrolyte comprises the electrolyte according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Non-aqueous lithium ion battery electrolyte and lithium ion battery

    CN114865084A

  • Electrolyte and battery

    CN116706241A

  • Electrolyte additive, electrolyte containing additive and lithium ion battery

    CN117410561A

  • Electrolyte and lithium-rich manganese-based lithium secondary battery

    CN117525584A

  • Non-aqueous electrolyte containing aryl isocyanate and lithium ion battery

    CN118016995A

Cited By

  • Electrolyte and lithium ion battery

    CN121260918A