Gel electrolyte for improving wettability of pole piece and preparation method of battery
By using a gel electrolyte preparation method that improves the wettability of the electrode sheet in lithium-ion batteries, and using stabilizers to adjust the viscosity, the problem of insufficient safety and wettability of lithium-ion batteries in the process of increasing energy density is solved, and more efficient Electrochemical properties and safety.
Patent Information
- Application Number
- CN202410991950.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-11-12
AI Technical Summary
Existing lithium-ion batteries have safety problems in the process of increasing energy density, especially the poor environmental stability of all-solid electrolytes, large interface impedance, high engineering difficulty, and gel electrolytes have shortcomings in the wettability of the electrode sheet.
Using a gel electrolyte preparation method that improves the wetting of the electrode sheet, the gel electrolyte precursor is injected into the dry battery cell, and the electrolyte is allowed to fully immerse the electrode sheet, and stand under specific pressure and temperature conditions to introduce a stabilizer To delay the rise of viscosity, a dense gel electrolyte layer is formed.
It effectively improves the wetting effect of the electrolyte on the electrode sheet, delays the increase in the viscosity of the gel electrolyte, improves the safety and electrochemical performance of the battery, is suitable for existing lithium battery production equipment and processes, and is easy to scale.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of gel semi-solid batteries, and in particular to a gel electrolyte for improving the wettability of a pole piece and a preparation method of a battery. Background Art
[0002] As lithium-ion batteries continue to be used in electric vehicles, large-scale industrial and commercial energy storage, deep-sea exploration, aerospace and other fields, the energy density of lithium-ion batteries needs to be improved urgently to meet the growing demand for endurance. However, with the continuous breakthrough of the upper limit of energy density, the safety issues of lithium-ion batteries have become increasingly prominent. It has gradually become an industry consensus to use solid electrolytes to replace flammable and explosive organic liquid electrolytes to solve the safety problems of lithium-ion batteries under high energy density. However, under current technical conditions, all-solid-state electrolytes still have problems such as poor environmental stability, large interface impedance, and high engineering difficulty. The gel electrolyte, by retaining some liquid phase components, not only improves the safety characteristics, but also takes into account the electrochemical performance of the battery. At the same time, it is highly compatible with existing lithium battery production equipment and processes, and is easy to scale. This makes this technology a key research and development direction for lithium-ion iterations in the short term. Summary of the invention
[0003] Based on this, the present invention provides a gel electrolyte and a battery preparation method for improving the wettability of a pole piece in order to solve the problem of how to improve the wetting effect of the electrolyte on the pole piece.
[0004] In a first aspect, the present invention provides a method for preparing a gel electrolyte for improving the wettability of a pole piece, comprising:
[0005] Injecting a gel electrolyte precursor into the stacked dry cells and encapsulating them to obtain liquid-injected cells;
[0006] The liquid-injected battery cell is left standing at room temperature for 12 to 48 hours to allow the electrolyte to fully infiltrate the electrode;
[0007] After the electrolyte fully infiltrates the electrode, the liquid-filled battery cell is controlled to stand at a pressure of 2 to 60 psi and a temperature range of 35 to 70°C for 12 to 96 hours. When the gel electrolyte layer is completely formed, the electrolyte inside the liquid-filled battery cell is in a solidified state, that is, a gel electrolyte is formed.
[0008] The gel electrolyte precursor comprises a polymerizable monomer composition, an initiator, a lithium salt, a non-aqueous solvent, an electrolyte additive and a stabilizer;
[0009] The mass ratio of the polymerization monomer composition, initiator, lithium salt, non-aqueous solvent and electrolyte additive is 2-10:0.001-0.1:5-20:60-95:0-10;
[0010] The content of the stabilizer is 50 to 700 ppm.
[0011] The stabilizer is one or more of hydroquinone, methyl hydroquinone, tert-butylcatechol, tert-butyl hydroquinone, di-tert-butyl hydroquinone, 4-methoxyphenol, 1,1-diphenyl-2-trinitrophenylhydrazine, p-benzoquinone, anthraquinone, tetrachlorobenzoquinone, phenothiazine, 4-hydroxy-2,2,6,6-tetramethylpiperidinyl nitroxide free radical, tetramethylpiperidinyl nitroxide free radical phosphite triester, and tris(N-nitroso-N-phenylhydroxylamine)aluminum salt.
[0012] The polymerizable monomer composition consists of group A monomers and group B cross-linking monomers.
[0013] The monomers in group A are selected from one or more of difunctional propylene, acrylic acid, acrylate, acrylamide, epoxy, vinyl halide, siloxane and their derivatives.
[0014] The group B cross-linking monomers are selected from one or more of acrylates with trifunctionality or higher, polyamines, polyols, polyisocyanates, benzenesulfonic acids, glycidyl ethers and derivatives thereof.
[0015] The initiator is selected from one or more of azobisisoheptanenitrile, azobisisobutyronitrile, dibenzoyl peroxide, dicyclohexyl peroxydicarbonate, and diisobutyl peroxydicarbonate.
[0016] The lithium salt is selected from one or more of LiPF6, lithium bis(trifluoromethylsulfonyl)imide, lithium bis(fluorosulfonyl)imide, lithium bis(pentafluoroethylsulfonyl)imide, lithium bis(oxalate)borate, LiBF4, and LiClO4.
[0017] The non-aqueous solvent is one or more of linear or cyclic carbonates and fluorinated carbonates.
[0018] The second aspect of the present invention provides a method for preparing a battery with improved electrode wettability, comprising:
[0019] The gel electrolyte is placed under a pressure of 2 to 60 psi to complete pre-charging, formation, and capacity separation to obtain a battery.
[0020] Beneficial effect: The present invention introduces a stabilizer to delay the increase in viscosity of the gel electrolyte and improve the wetting effect of the electrolyte on the electrode.
[0021] It should be understood that the contents described in this section are not intended to identify the key or important features of the embodiments of the present invention, nor are they intended to limit the scope of the present invention. Other features of the present invention will become easily understood through the following description. DETAILED DESCRIPTION
[0022] The following is a description of exemplary embodiments of the present invention, including various details of the embodiments of the present invention to aid understanding, which should be considered as merely exemplary. Therefore, it should be appreciated by those of ordinary skill in the art that various changes and modifications may be made to the embodiments described herein without departing from the scope and spirit of the present invention. Likewise, for clarity and simplicity, descriptions of well-known functions and structures are omitted in the following description.
[0023] In a first aspect, the present invention provides a method for preparing a gel electrolyte for improving the wettability of a pole piece, comprising:
[0024] S1: injecting the gel electrolyte precursor into the stacked dry cells and encapsulating them to obtain liquid-injected cells;
[0025] The gel electrolyte precursor comprises a polymerizable monomer composition, an initiator, a lithium salt, a non-aqueous solvent, an electrolyte additive and a stabilizer;
[0026] Preferably, a stabilizer is introduced to delay the increase in viscosity of the gel electrolyte and improve the wetting effect of the electrolyte on the electrode.
[0027] The mass ratio of the polymerization monomer composition, initiator, lithium salt, non-aqueous solvent and electrolyte additive is 2-10:0.001-0.1:5-20:60-95:0-10;
[0028] The content of the stabilizer is 50 to 700 ppm, preferably 100 to 400 ppm.
[0029] Stabilizers can reduce viscosity by regulating the interactions between solvent molecules and between solvent and polymer chains in gel electrolytes.
[0030] The stabilizer is one or more of hydroquinone, methyl hydroquinone, tert-butylcatechol, tert-butyl hydroquinone, di-tert-butyl hydroquinone, 4-methoxyphenol, 1,1-diphenyl-2-trinitrophenylhydrazine, p-benzoquinone, anthraquinone, tetrachlorobenzoquinone, phenothiazine, 4-hydroxy-2,2,6,6-tetramethylpiperidinyl nitroxide free radical, tetramethylpiperidinyl nitroxide free radical phosphite triester, and tris(N-nitroso-N-phenylhydroxylamine)aluminum salt.
[0031] The polymerizable monomer composition consists of group A monomers and group B cross-linking monomers.
[0032] The monomers in group A are selected from one or more of difunctional propylene, acrylic acid, acrylate, acrylamide, epoxy, vinyl halide, siloxane and their derivatives.
[0033] The group B cross-linking monomers are selected from one or more of acrylates with trifunctionality or higher, polyamines, polyols, polyisocyanates, benzenesulfonic acids, glycidyl ethers and derivatives thereof.
[0034] The initiator is selected from one or more of azobisisoheptanenitrile, azobisisobutyronitrile, dibenzoyl peroxide, dicyclohexyl peroxydicarbonate, and diisobutyl peroxydicarbonate.
[0035] The lithium salt is selected from one or more of LiPF6, lithium bis(trifluoromethylsulfonyl)imide, lithium bis(fluorosulfonyl)imide, lithium bis(pentafluoroethylsulfonyl)imide, lithium bis(oxalate)borate, LiBF4, and LiClO4.
[0036] The non-aqueous solvent is one or more of linear or cyclic carbonates and fluorinated carbonates.
[0037] S2: leaving the liquid-filled battery cell at room temperature for 12 to 48 hours to allow the electrolyte to fully infiltrate the electrode;
[0038] Room temperature conditions refer to between 18°C and 25°C;
[0039] S3: After the electrolyte fully infiltrates the electrode, the liquid-filled battery cell is controlled to stand at a pressure of 2 to 60 psi and a temperature range of 35 to 70°C for 12 to 96 hours. When the gel electrolyte layer is completely formed, the electrolyte inside the liquid-filled battery cell is in a solidified state, that is, a gel electrolyte is formed.
[0040] Furthermore, the pressure range of 2 to 60 psi helps to evenly distribute the electrolyte precursor between the positive and negative electrodes, prevents the generation of bubbles, ensures good contact between the electrolyte and the electrodes, and is conducive to forming a dense gel electrolyte layer.
[0041] The temperature range of 35 to 70°C is to accelerate the chemical reaction of the gel electrolyte precursor and promote its transformation from liquid to solid or semi-solid gel. Higher temperature can speed up the reaction rate and shorten the gelation process.
[0042] The 12 to 96 hour standing time provides the electrolyte precursor with sufficient reaction time to ensure that it is completely transformed into a gel electrolyte layer and forms a stable structure.
[0043] The second aspect of the present invention provides a method for preparing a battery with improved electrode wettability, comprising:
[0044] The gel electrolyte is placed under a pressure of 2 to 60 psi to complete pre-charging, formation, and capacity separation to obtain a battery.
[0045] Example 1
[0046] Step 1: Under the condition of controlling the moisture and oxygen content in the atmosphere to be ≤10ppm, 30g of a monomer composition of methacrylate and trimethylolpropane trimethacrylate (1:2wt / wt), 1.5g of azobisisobutyronitrile initiator, 125g of lithium hexafluorophosphate lithium salt, 793.5g of a mixed solvent of ethylene carbonate (EC) and ethyl methyl carbonate (EMC) (3:7wt / wt), and 5g of an additive composition of vinylene carbonate (VC), fluoroethylene carbonate (FEC) and lithium difluorophosphate (LiDFP) (2:2:1wt / wt) were mixed to obtain a mixture A;
[0047] Step 2: Keeping the atmosphere unchanged, add 0.492 g of tetramethylpiperidinium nitroxide free radical phosphite triester (about 100 ppm) as a stabilizer to the mixture A and mix well to obtain a gel electrolyte precursor;
[0048] Step 3: Inject the gel electrolyte precursor into a 6.5Ah small soft-pack dry cell (high nickel ternary NCM811 / / silicon oxide (SiOx) / graphite (Gr) chemical system), quickly complete the packaging and place it at room temperature for 24 hours to allow the electrode to be fully infiltrated by the electrolyte, and then place the injected cell at 10psi pressure and 45°C for 48 hours to allow the gel electrolyte precursor to form a gel electrolyte layer between the positive and negative electrodes. When the gel electrolyte layer is completely formed, the electrolyte inside the injected cell is in a solidified state, that is, a gel electrolyte is formed;
[0049] Step 4: Gel electrolyte, complete pre-charging, formation, and capacity separation to obtain a battery.
[0050] The difference between Example 2 and Example 1 is that the stabilizer used in step 2 is replaced with methyl hydroquinone, and the added amount is 0.112 g (about 100 ppm).
[0051] The difference between Example 3 and Example 1 is that the monomer combination used in step 1 is replaced with 30g acrylonitrile and pentaerythritol tetraacrylate (1:2wt / wt), and 0.499g tetramethylpiperidinium nitroxide free radical phosphite triester (about 100ppm) is added in step 2.
[0052] The difference between Example 4 and Example 1 is that the amount of stabilizer added in step 2 is 0.336 g (about 300 ppm).
[0053] The difference between Example 5 and Example 1 is that the amount of the initiator used in step 1 is changed to 0.75 g.
[0054] The difference between Comparative Example 1 and Example 1 is that there is no step 2.
[0055] The difference between Comparative Example 2 and Example 1 is that the amount of stabilizer added in step 2 is 1.12 g (about 1000 ppm)
[0056] In Comparative Example 3, conventional organic liquid electrolyte was injected to obtain a battery cell under the same process conditions.
[0057] The following results were obtained by measuring the viscosity change and residual liquid amount of the electrolytes in Examples 1 to 5 and Comparative Examples 1 to 3 under the same high temperature conditions outside the battery and the discharge capacity of the battery cells obtained in Examples 1 to 5 and Comparative Examples 1 to 3.
[0058] Table 1: Experimental results of embodiments and comparative examples.
[0059]
[0060]
[0061] By comparing Example 1, Comparative Examples 1 and 3, it can be seen that the use of the gel electrolyte of the present invention can effectively alleviate the viscosity growth of the electrolyte and improve the electrode wetting effect; by comparing Examples 1 and 4, it can be found that between 12-24h, the amount of stabilizer added is large and the viscosity growth rate is slow; by comparing Examples 1 to 3, it can be seen that different polymerized monomers and stabilizer species have different effects on the stabilization effect. It can be seen from Examples 1 and 5 that the ratio of stabilizer to initiator affects the stabilization effect. Among them, "~0" means close to 0.
[0062] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions within the technical scope disclosed by the present invention should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.
Claims
1. A method for preparing a gel electrolyte for improving the wettability of a pole piece, characterized in that: include, Injecting a gel electrolyte precursor into the stacked dry cells and encapsulating them to obtain liquid-injected cells; The liquid-injected battery cell is left standing at room temperature for 12 to 48 hours to allow the electrolyte to fully infiltrate the electrode; After the electrolyte fully infiltrates the electrode, the liquid-filled battery cell is controlled to stand at a pressure of 2 to 60 psi and a temperature range of 35 to 70°C for 12 to 96 hours. When the gel electrolyte layer is completely formed, the electrolyte inside the liquid-filled battery cell is in a solidified state, that is, a gel electrolyte is formed.
2. The method for preparing a gel electrolyte for improving electrode wettability according to claim 1, characterized in that: The gel electrolyte precursor comprises a polymerizable monomer composition, an initiator, a lithium salt, a non-aqueous solvent, an electrolyte additive and a stabilizer; The mass ratio of the polymerization monomer composition, initiator, lithium salt, non-aqueous solvent and electrolyte additive is 2-10:0.001-0.1:5-20:60-95:0-10; The content of the stabilizer is 50 to 700 ppm.
3. The method for preparing a gel electrolyte for improving electrode wettability according to claim 2, characterized in that: The stabilizer is one or more of hydroquinone, methyl hydroquinone, tert-butylcatechol, tert-butyl hydroquinone, di-tert-butyl hydroquinone, 4-methoxyphenol, 1,1-diphenyl-2-trinitrophenylhydrazine, p-benzoquinone, anthraquinone, tetrachlorobenzoquinone, phenothiazine, 4-hydroxy-2,2,6,6-tetramethylpiperidinyl nitroxide free radical, tetramethylpiperidinyl nitroxide free radical phosphite triester, and tris(N-nitroso-N-phenylhydroxylamine)aluminum salt.
4. The method for preparing a gel electrolyte for improving electrode wettability according to claim 3, characterized in that: The polymerizable monomer composition consists of group A monomers and group B cross-linking monomers.
5. The method for preparing a gel electrolyte for improving electrode wettability according to claim 4, characterized in that: The monomers in group A are selected from one or more of difunctional propylene, acrylic acid, acrylate, acrylamide, epoxy, vinyl halide, siloxane and their derivatives.
6. A method for preparing a gel electrolyte for improving electrode wettability according to claim 4 or 5, characterized in that: The crosslinking monomers in group B are selected from one or more of acrylates with trifunctionality or higher, polyamines, polyols, polyisocyanates, benzenesulfonic acids, glycidyl ethers and derivatives thereof.
7. The method for preparing a gel electrolyte for improving electrode wettability according to claim 2, characterized in that: The initiator is selected from one or more of azobisisoheptanenitrile, azobisisobutyronitrile, dibenzoyl peroxide, dicyclohexyl peroxydicarbonate, and diisobutyl peroxydicarbonate.
8. A method for preparing a gel electrolyte for improving electrode wettability according to claim 2 or 7, characterized in that: The lithium salt is selected from one or more of LiPF6, lithium bis(trifluoromethylsulfonyl)imide, lithium bis(fluorosulfonyl)imide, lithium bis(pentafluoroethylsulfonyl)imide, lithium bis(oxalate)borate, LiBF4, and LiClO4.
9. The method for preparing a gel electrolyte for improving electrode wettability according to claim 8, characterized in that: The non-aqueous solvent is one or more of linear or cyclic carbonates and fluorinated carbonates.
10. A method for preparing a battery with improved electrode wettability, characterized in that: include, The gel electrolyte as claimed in any one of claims 1 to 9 is placed under a pressure of 2 to 60 psi to complete pre-charging, formation and capacity separation to obtain a battery.
Citation Information
Cited By
Pole piece, preparation method thereof, electrochemical device containing pole piece and electronic equipment
CN122348180A
Pole piece, battery containing pole piece, battery preparation method and electronic equipment
CN122348181A
Pole piece, preparation method thereof and electrochemical device containing pole piece
CN122348182A