Lithium ion battery diaphragm coating and lithium ion battery diaphragm
By using a composite coating of ceramic particles and fibers of different diameters in the lithium-ion battery separator to form a three-dimensional network structure, the problem of insufficient heat resistance of the separator is solved, and the safety and electrochemical performance of the battery are improved.
Patent Information
- Application Number
- CN202411119946.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing lithium-ion battery separators have insufficient heat resistance, which makes them prone to thermal shrinkage during charging and discharging, posing a safety hazard.
A lithium-ion battery separator coating is formed by combining ceramic particles, nano-scale short fibers, and submicron-scale long fibers. The three-dimensional network structure is formed by fiber winding and coating, which improves the heat resistance and porosity of the separator.
It enhances the heat resistance and electrochemical performance of the separator, improving the battery's safety performance and long-cycle performance.
Smart Images

Figure CN118943652A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of battery separators, and in particular to a lithium ion battery separator coating and a lithium ion battery separator. Background Art
[0002] Lithium-ion batteries are mainly composed of four major materials: positive electrode materials, negative electrode materials, electrolytes and diaphragms. Among them, the diaphragm is the key component related to the safety of lithium batteries. The performance of the diaphragm determines the interface structure and internal resistance of the battery, and directly affects the battery's capacity, cycle and safety performance. Excellent performance diaphragms play an important role in improving the overall performance of the battery. The main function of the diaphragm is to separate the positive and negative electrodes of the battery to prevent the two electrodes from contacting and short-circuiting. In addition, it also has the function of allowing electrolyte ions to pass through.
[0003] Currently, commercially available polyolefin diaphragms have poor heat resistance. During the battery charging and discharging process, the diaphragm will experience severe heat shrinkage due to the increase in the internal temperature of the battery, causing the diaphragm to easily rupture and lose its function of blocking the positive and negative electrodes, thereby making the battery operation dangerous. In order to solve the above problems, the prior art forms a ceramic coating on the surface of the diaphragm to prepare a composite diaphragm to improve the heat resistance of the diaphragm. However, the existing ceramic coating composition cannot effectively improve the problem of thermal shrinkage of the diaphragm, and there are still major safety hazards during the use of the battery. Summary of the invention
[0004] Based on the technical problems existing in the background technology, the present invention proposes a lithium-ion battery separator coating and a lithium-ion battery separator. The lithium-ion battery separator coating is formed by a composite of ceramic particles, nano-scale short fibers and submicron-scale long fibers. While improving the heat shrinkage resistance of the separator, the porosity of the separator is also increased, thereby improving the electrochemical performance of the separator when used in batteries.
[0005] The present invention provides a lithium-ion battery separator coating, comprising ceramic particles, nanometer-scale short fibers and submicrometer-scale long fibers;
[0006] Wherein, the mass ratio of the ceramic particles, the nanometer-scale short fibers and the submicron-scale long fibers is 100:1-10:5-25.
[0007] In the present invention, in the lithium-ion battery separator coating, nanometer-scale short fibers and submicron-scale long fibers of different diameters and lengths can form a length and thickness combination, thereby achieving effective entanglement and coating between fibers, and generating a synergistic effect between the fibers and the ceramic particles, realizing the construction of a three-dimensional network structure and a multi-level pore structure in the coating, so that the lithium-ion battery separator containing the coating not only has sufficient supporting strength and good heat resistance, but also improves the separator porosity, liquid absorption and electrolyte retention, and also has an improvement effect on the long cycle of the battery.
[0008] Preferably, the ceramic particles are at least one of aluminum oxide, boehmite, calcium oxide, magnesium oxide, iron oxide, silicon nitride, silicon carbide or titanium dioxide.
[0009] Preferably, the diameter of the nanometer-scale short fibers is 1-50 nm, and the length is 10-2000 nm; the diameter of the submicron-scale long fibers is 100-1000 nm, and the length is 1-100 μm.
[0010] Preferably, the nanometer-scale short fibers are nanocellulose; and the submicron-scale long fibers are at least one of aramid fibers, polyimide fibers or polyamide-imide fibers.
[0011] Preferably, the coating further comprises a binder;
[0012] Preferably, the mass ratio of the binder to the ceramic particles is 0.1-10:100.
[0013] Preferably, the binder is at least one of polyacrylate, polyacrylic acid, polyvinyl alcohol or polyamic acid lithium salt;
[0014] Preferably, the polyamic acid lithium salt is an aromatic polyamic acid lithium salt.
[0015] Preferably, the coating further comprises a dispersant;
[0016] Preferably, the mass ratio of the dispersant to the ceramic particles is 0.1-1:100.
[0017] Preferably, the dispersant is at least one of sodium carboxymethyl cellulose, polyacrylamide or sodium dodecyl sulfate.
[0018] The present invention also provides a lithium-ion battery separator, comprising a base film and the lithium-ion battery separator coating formed on the surface of the base film.
[0019] Preferably, the base film is a polyethylene porous film or a polypropylene porous film.
[0020] The present invention also provides a lithium ion battery, comprising a positive electrode, a negative electrode, an electrolyte located between the positive electrode and the negative electrode, and the lithium ion battery separator.
[0021] Compared with the prior art, the present invention has the following beneficial effects:
[0022] (1) The present invention forms entanglements between nanometer-scale short fibers and submicrometer-scale long fibers in the diaphragm coating and forms a tight wrapping between the ceramic particles, thereby improving the continuity and integrity of the coating and improving the heat resistance and high heat-resistant dimensional stability of the obtained diaphragm;
[0023] (2) The present invention forms a rich pore structure by overlapping nano-scale short fibers and submicron-scale long fibers, which not only enhances the heat resistance of the diaphragm, but also makes the diaphragm have high porosity, good air permeability and good liquid absorption, and significantly improves the long cycle effect of the battery, thereby improving the electrochemical performance and safety performance of the battery at the same time. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 This is a scanning electron microscope image of the polyimide fiber described in Example 1. DETAILED DESCRIPTION
[0025] The technical solutions of the present invention are described in detail below through specific embodiments. However, it should be clearly stated that these embodiments are for illustration only and are not to be construed as limiting the scope of the present invention.
[0026] Example 1
[0027] A lithium ion battery separator is prepared by the following method:
[0028] (1) adding 4,4'-diaminodiphenyl ether and pyromellitic acid dianhydride to N,N-dimethylformamide (DMF) at a molar ratio of 1:1, stirring and dissolving them completely, stirring and reacting for 6 hours under nitrogen protection, to obtain a polyamic acid solution with a content of 10wt%; subjecting the polyamic acid solution to electrostatic spinning, wherein the electrostatic spinning parameters include: spinning voltage of 20kV, spinning temperature of 25°C, spinning humidity of 40%, receiving roller speed of 500r / min, and receiving distance of 20cm, to obtain polyamic acid nanofibers; subjecting the polyamic acid nanofibers to thermal imidization treatment, wherein the thermal imidization parameters include: heating rate of 5°C / min, heating temperature of 300°C, and heating time of 2h, to obtain polyimide fibers (average diameter of 400nm and length of 20μm);
[0029] (2) Alumina (average particle size of 500 nm), the above-mentioned polyimide fiber, nanocellulose (average diameter of 20 nm, length of 1000 nm) and polyacrylate (BYK-381) are added to water in a mass ratio of 100:15:5:3, stirred and dispersed evenly to obtain a slurry with a content of 50 wt%; the slurry is coated on one side surface of a polyethylene diaphragm (thickness of 12 μm, porosity of 45%) by a gravure coater, and after drying in an oven at 80°C, a coating with a thickness of 4 μm is formed, thereby obtaining the lithium ion battery diaphragm.
[0030] Example 2
[0031] A lithium ion battery separator is prepared by the following method:
[0032] (1) adding 4,4'-diaminodiphenyl ether and trimellitic anhydride chloride to N,N-dimethylformamide (DMF) at a molar ratio of 1:1 and stirring to dissolve completely, then adding pyridine in an amount of 1.5 times the molar amount of 4,4'-diaminodiphenyl ether, stirring to react for 24 hours, then adding acetic anhydride in an amount of 1.1 times the molar amount of 4,4'-diaminodiphenyl ether, and stirring to react for another 24 hours to obtain a polyamide-imide solution with a content of 10 wt%; subjecting the polyamide acid solution to electrostatic spinning, wherein the electrostatic spinning parameters include: a spinning voltage of 20 kV, a spinning temperature of 25° C., a spinning humidity of 40%, a receiving roller speed of 500 r / min, and a receiving distance of 20 cm, to obtain polyamide-imide nanofibers (average diameter of 500 nm and length of 35 μm);
[0033] (2) Boehmite (average particle size of 300 nm), the above-mentioned polyamide-imide nanofibers, nanocellulose (average diameter of 20 nm, length of 1000 nm) and polyacrylate (BYK-381) are added to water in a mass ratio of 100:15:5:3, stirred and dispersed evenly to obtain a slurry with a content of 50 wt%; the slurry is coated on one side surface of a polyethylene diaphragm (thickness of 12 μm, porosity of 45%) by a gravure coater, and after drying in an oven at 80°C, a coating with a thickness of 4 μm is formed, thereby obtaining the lithium ion battery diaphragm.
[0034] Example 3
[0035] A lithium ion battery separator is prepared by the following method:
[0036] Alumina (average particle size of 500 nm), aramid fiber (aramid 1414 fiber, average diameter of 150 nm, length of 12 μm), nanocellulose (average diameter of 20 nm, length of 1000 nm) and polyacrylate (BYK-381) are added to water in a mass ratio of 100:15:5:3, stirred and dispersed evenly to obtain a slurry with a content of 50 wt%; the slurry is coated on one side surface of a polyethylene diaphragm (thickness of 12 μm, porosity of 45%) by a gravure coater, and after drying in an oven at 80°C, a coating with a thickness of 4 μm is formed, thereby obtaining the lithium ion battery diaphragm.
[0037] Example 4
[0038] A lithium ion battery separator is prepared by the following method:
[0039] (1) adding 4,4'-diaminodiphenyl ether and pyromellitic acid dianhydride to N,N-dimethylformamide (DMF) at a molar ratio of 1:1, stirring and dissolving them completely, stirring and reacting for 6 hours under nitrogen protection, to obtain a polyamic acid solution with a content of 10wt%; subjecting the polyamic acid solution to electrostatic spinning, wherein the electrostatic spinning parameters include: spinning voltage of 20kV, spinning temperature of 25°C, spinning humidity of 40%, receiving roller speed of 500r / min, and receiving distance of 20cm, to obtain polyamic acid nanofibers; subjecting the polyamic acid nanofibers to thermal imidization treatment, wherein the thermal imidization parameters include: heating rate of 5°C / min, heating temperature of 300°C, and heating time of 2h, to obtain polyimide fibers (average diameter of 400nm and length of 20μm);
[0040] (2) adding 4,4'-diaminodiphenyl ether and 3,3',4,4'-biphenyltetracarboxylic anhydride to N-methylpyrrolidone (NMP) at a molar ratio of 1:1, stirring and dissolving them completely, and stirring and reacting them for 4 hours under nitrogen protection to obtain a polyamic acid solution with a content of 30wt%; adding LiOH to deionized water and stirring and dissolving them completely to obtain a lithium hydroxide aqueous solution with a content of 1.5wt%; adding the lithium hydroxide aqueous solution to the polyamic acid solution, wherein the amount of lithium hydroxide is 5wt% of the polyamic acid, and stirring and reacting them for 6 hours to obtain an aromatic polyamic acid lithium salt solution; adding the aromatic polyamic acid lithium salt solution to acetone for precipitation, filtering, washing, and drying to obtain an aromatic polyamic acid lithium salt;
[0041] (3) Alumina (average particle size of 500 nm), the above-mentioned polyimide fiber, nanocellulose (average diameter of 20 nm, length of 1000 nm) and aromatic polyamic acid lithium salt are added into water in a mass ratio of 100:15:5:3, stirred and dispersed evenly to obtain a slurry with a content of 50 wt%; the slurry is coated on one side surface of a polyethylene diaphragm (thickness of 12 μm, porosity of 45%) by a gravure coater, and dried in an oven at 80°C to form a coating with a thickness of 4 μm, thereby obtaining the lithium ion battery diaphragm.
[0042] Comparative Example 1
[0043] A lithium ion battery separator is prepared by the following method:
[0044] (1) adding 4,4'-diaminodiphenyl ether and pyromellitic acid dianhydride to N,N-dimethylformamide (DMF) at a molar ratio of 1:1, stirring and dissolving them completely, stirring and reacting for 6 hours under nitrogen protection, to obtain a polyamic acid solution with a content of 10wt%; subjecting the polyamic acid solution to electrostatic spinning, wherein the electrostatic spinning parameters include: spinning voltage of 20kV, spinning temperature of 25°C, spinning humidity of 40%, receiving roller speed of 500r / min, and receiving distance of 20cm, to obtain polyamic acid nanofibers; subjecting the polyamic acid nanofibers to thermal imidization treatment, wherein the thermal imidization parameters include: heating rate of 5°C / min, heating temperature of 300°C, and heating time of 2h, to obtain polyimide fibers (average diameter of 400nm and length of 20μm);
[0045] (2) Alumina (average particle size of 500 nm), the above-mentioned polyimide fiber and polyacrylate (BYK-381) are added to water in a mass ratio of 100:20:3, stirred and dispersed evenly to obtain a slurry with a content of 50 wt%; the slurry is coated on one side surface of a polyethylene diaphragm (thickness of 12 μm, porosity of 45%) by a gravure coater, and after drying in an oven at 80°C, a coating with a thickness of 4 μm is formed, thereby obtaining the lithium ion battery diaphragm.
[0046] Comparative Example 2
[0047] A lithium ion battery separator is prepared by the following method:
[0048] Alumina (average particle size of 500 nm), nanocellulose (average diameter of 20 nm, length of 1000 nm) and polyacrylate (BYK-381) are added to water in a mass ratio of 100:20:3, stirred and dispersed evenly to obtain a slurry with a content of 50 wt%; the slurry is coated on one side surface of a polyethylene diaphragm (thickness of 12 μm, porosity of 45%) using a gravure coater, and after drying in an oven at 80°C, a coating with a thickness of 4 μm is formed, thereby obtaining the lithium ion battery diaphragm.
[0049] Performance Test:
[0050] The lithium-ion battery separators obtained in the above examples and comparative examples were tested for heat shrinkage, liquid absorption and battery performance, and the test results are shown in Table 1.
[0051] Thermal shrinkage rate: Cut 5cm×5cm lithium-ion battery separator samples, measure the longitudinal (MD) and transverse (TD) dimensions before baking, record them as L1 and H1 respectively, then bake the composite separator at 150℃ for 1h, measure the MD and TD dimensions again, record them as L2 and H2 respectively, the MD thermal shrinkage rate is (L1-L2) / L1×100%, and the TD thermal shrinkage rate is (H1-H2) / H1×100%;
[0052] Liquid absorption rate: Cut a 2cm×2cm lithium-ion battery separator sample and immerse it completely in the electrolyte (lithium hexafluorophosphate LiPF6 electrolyte, concentration is 1 mol / L, the molar ratio of ethylene carbonate EC, dimethyl carbonate DMC and ethyl methyl carbonate EMC is 1:1:1) for 10 minutes. After taking it out, use filter paper to absorb the liquid on the surface of the sample, and detect the weight of the lithium-ion battery separator obtained before and after immersion. The liquid absorption rate is calculated as (battery separator weight after immersion-battery separator weight before immersion) / battery separator weight after immersion;
[0053] Battery performance: The obtained lithium-ion battery separator is mixed with the positive electrode sheet (lithium cobalt oxide, conductive agent acetylene black, and polyvinylidene fluoride are mixed in N-methylpyrrolidone solvent at a mass ratio of 97:1:2 to form a positive electrode slurry, which is coated on aluminum foil and dried, and then cold pressed and striped to form a positive electrode sheet), and the negative electrode sheet (graphite, conductive carbon black Super P, styrene-butadiene rubber are mixed uniformly in deionized water in a mass ratio of 97:1:2 to form a negative electrode slurry, which is coated on a copper foil and dried before being cold pressed and slit to form a negative electrode sheet) and 1 mol / L lithium hexafluorophosphate LiPF6 electrolyte (lithium hexafluorophosphate LiPF6 is dissolved in a mixed solvent consisting of ethylene carbonate EC, dimethyl carbonate DMC and ethyl methyl carbonate EMC, and the volume ratio of the three is 1:1:1 to form an electrolyte) are assembled into a lithium-ion battery in a conventional manner, and then the battery performance test is performed, specifically, charged to 4.35V at 1C constant current and constant voltage, the battery is cut off at 0.1C, left for 10min, cycled 200 times, and the capacity retention rate of 200 times is recorded;
[0054] Table 1 Performance test results of the lithium ion battery separators described in Examples and Comparative Examples
[0055]
[0056] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A lithium ion battery separator coating, characterized in that: Including ceramic particles, nanometer-sized short fibers and submicron-sized long fibers; Wherein, the mass ratio of the ceramic particles, the nanometer-scale short fibers and the submicron-scale long fibers is 100:1-10:5-25.
2. The lithium-ion battery separator coating according to claim 1, characterized in that: The ceramic particles are at least one of aluminum oxide, boehmite, calcium oxide, magnesium oxide, iron oxide, silicon nitride, silicon carbide or titanium dioxide.
3. The lithium-ion battery separator coating according to claim 1 or 2, characterized in that: The diameter of the nanometer-scale short fibers is 1-50 nm, and the length is 10-2000 nm; the diameter of the submicron-scale long fibers is 100-1000 nm, and the length is 1-100 μm.
4. The lithium-ion battery separator coating according to any one of claims 1 to 3, characterized in that: The nanometer-scale short fibers are nanocellulose; and the submicrometer-scale long fibers are at least one of aramid fibers, polyimide fibers or polyamide-imide fibers.
5. The lithium-ion battery separator coating according to any one of claims 1 to 4, characterized in that: The coating also includes a binder; Preferably, the mass ratio of the binder to the ceramic particles is 0.1-10:
100.
6. The lithium-ion battery separator coating according to claim 5, characterized in that: The binder is at least one of polyacrylate, polyacrylic acid, polyvinyl alcohol or polyamic acid lithium salt; Preferably, the polyamic acid lithium salt is an aromatic polyamic acid lithium salt.
7. The lithium-ion battery separator coating according to any one of claims 1 to 6, characterized in that: The coating also includes a dispersant; Preferably, the mass ratio of the dispersant to the ceramic particles is 0.1-1:
100. Preferably, the dispersant is at least one of sodium carboxymethyl cellulose, polyacrylamide or sodium dodecyl sulfate.
8. A lithium ion battery separator, characterized in that: The invention comprises a base film and a lithium-ion battery separator coating according to any one of claims 1 to 7 formed on the surface of the base film.
9. The lithium-ion battery separator according to claim 8, characterized in that: The base film is a polyethylene porous film or a polypropylene porous film.
10. A lithium ion battery, characterized in that: It comprises a positive electrode, a negative electrode, an electrolyte located between the positive electrode and the negative electrode, and the lithium ion battery separator according to claim 8 or 9.
Citation Information
Patent Citations
High-stability lithium ion battery diaphragm, preparation method thereof and lithium ion battery
CN107342387A
Adhesive for silicon-carbon negative electrode and electrode material for lithium ion battery
CN113555551A
Cited By
Battery diaphragm, preparation method thereof and battery
CN120527570A