Composite diaphragm, preparation method thereof and battery

By using a composite material formed by acid-modified carbon nanotubes and polyvinylpyrrolidone in the lithium battery separator, combining binders and additives, the problem of insufficient thermal stability and wettability of the lithium battery separator is solved, and high-performance lithium is achieved Battery diaphragm.

CN118943662AActive Publication Date: 2024-11-12JIANGSU ADVANCED MATERIAL TECH CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411121357.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-15
Publication Date
2024-11-12
Estimated Expiration
2044-08-15

AI Technical Summary

Technical Problem

The existing lithium battery separators have poor thermal stability and wetting properties under hot pressing conditions, and the Al2O3 coating is incomplete, which makes it easy to absorb water, resulting in insufficient performance.

Method used

Using composite separators, including base film and coating, the coating consists of carbon nanotubes and polyvinylpyrrolidone coated carbon nanotubes. Through acid modification treatment and hydrothermal reaction, a high conductivity composite material is formed, combined with an appropriate amount of adhesive The catalyst and additive form a coating with excellent thermal stability and wettability.

Benefits of technology

The excellent heat resistance, coating bonding performance, liquid storage performance and wetting performance of the composite separator are achieved, and the overall performance and safety of lithium batteries are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118943662A_ABST
    Figure CN118943662A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of batteries, in particular to a composite diaphragm, a preparation method thereof and a battery. The composite diaphragm comprises a base membrane and a coating located on at least one side surface of the base membrane, the coating comprises a composite material and a binder, and the composite material comprises a carbon nanotube and polyvinylpyrrolidone coating the carbon nanotube. According to the composite diaphragm disclosed by the invention, the carbon nanotubes in the composite material have high conductivity and good thermal stability, and the surface-coated polyvinylpyrrolidone can improve the dispersity and wettability of the carbon nanotubes, so that the obtained composite diaphragm has excellent heat resistance, coating adhesive property, liquid storage property and wettability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of batteries, and in particular to a composite diaphragm and a preparation method thereof, and a battery. Background Art

[0002] With the rapid development of electric vehicles and mobile communication devices, the demand for lithium batteries is increasing. As an efficient and environmentally friendly energy storage device, the performance of lithium batteries directly affects the overall performance of the device. Lithium batteries are mainly composed of positive electrode materials, negative electrode materials, electrolytes and diaphragms. As a key component of lithium batteries, the diaphragm is mainly used to isolate positive and negative electrode materials to prevent short circuits, while allowing ions to pass through to complete the charging and discharging process.

[0003] Prior art CN112646303B discloses a coating slurry for lithium battery diaphragm and a preparation method thereof, wherein the slurry comprises an Al2O3-PMMA composite material, an oxidatively modified PVA and an additive, wherein the Al2O3-PMMA composite material is an Al2O3-PMMA core-shell particle with high adhesion and high wetting efficiency, wherein PMMA is used to completely encapsulate the Al2O3 particles inside to form spherical particles; potassium persulfate is used to treat the PVA solution, so that part of the PVA molecular chain is broken and a terminal carboxyl group or an aldehyde group is introduced, and a ketone group is introduced into the molecular chain. The diaphragm prepared by this method has a certain wettability, but it is difficult to control the complete coating of Al2O3, and the PMMA shell is easily broken under hot pressing conditions, and the exposed Al2O3 is easy to absorb water.

[0004] The thermal stability and wettability of existing diaphragm coatings are not ideal. Therefore, it is crucial to provide a composite diaphragm with both thermal stability and wettability.

[0005] In view of this, the present invention is proposed. Summary of the invention

[0006] An object of the present invention is to provide a composite diaphragm having excellent heat resistance, coating adhesion, liquid storage and wetting properties.

[0007] Another object of the present invention is to provide a method for preparing the composite membrane, which is simple and easy to implement, and the obtained composite membrane has good thermal stability and wettability.

[0008] Another object of the present invention is to provide a battery.

[0009] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:

[0010] A composite diaphragm comprises a base film and a coating located on at least one surface of the base film, wherein the coating comprises a composite material and a binder, and the composite material comprises carbon nanotubes and polyvinyl pyrrolidone coating the carbon nanotubes.

[0011] In some embodiments, the mass ratio of the composite material to the binder is (50-70):(20-40).

[0012] In some embodiments, the carbon nanotubes have an average diameter of 40 to 60 mm and an average length of 1 to 10 μm.

[0013] In some embodiments, in the composite material, the coverage rate of the polyvinyl pyrrolidone on the surface of the carbon nanotubes is 80% to 99%.

[0014] In some embodiments, the binder includes polymethyl methacrylate.

[0015] In some embodiments, the coating further comprises a tackifier; the mass ratio of the binder to the tackifier is (20-40):(5-10).

[0016] In some embodiments, the coating further comprises an additive, wherein the additive comprises at least one of a leveling agent, a defoaming agent and a dispersant; and the mass ratio of the composite material to the additive is (50-70):(1-5).

[0017] In some implementations, the thickness of the coating is 0.5 to 5 μm, and the porosity of the coating is 60% to 90%.

[0018] In some embodiments, the base film includes one of PE film, PP film, PI film, PET film, non-woven fabric separator, or a laminated composite of multiple thereof.

[0019] In some embodiments, the base film has a thickness of 5 to 10 μm.

[0020] In some embodiments, the porosity of the base film is 30% to 70%.

[0021] The method for preparing the composite diaphragm as described above comprises the following steps:

[0022] A slurry is coated on at least one side of the base film to form a wet film, wherein the slurry contains a composite material, a binder and a solvent, and the composite material is mainly obtained by mixing a mixed system containing acid-modified carbon nanotubes, polyvinyl pyrrolidone and water through a mixing treatment and a hydrothermal reaction; and the wet film is dried to obtain a composite diaphragm.

[0023] In some embodiments, the mass ratio of the polyvinyl pyrrolidone to the acid-modified carbon nanotubes is (200-400):(10-20).

[0024] In some embodiments, the mixed system further comprises a surfactant and a dispersant, and the mass ratio of the acid-modified carbon nanotubes, the polyvinyl pyrrolidone, the surfactant and the dispersant is (200-400):(10-20):(0.5-5):(0.5-5).

[0025] In some embodiments, the solid content of the mixed system is 20% to 30%.

[0026] In some embodiments, the rotation speed of the mixing process is 700 to 1500 rpm, and the time of the mixing process is 10 to 60 minutes.

[0027] In some embodiments, the temperature of the hydrothermal reaction is 150-200° C., and the time of the hydrothermal reaction is 6-12 hours.

[0028] In some embodiments, the method further comprises: washing and drying the material obtained after the hydrothermal reaction.

[0029] In some embodiments, the preparation method of the acid-modified carbon nanotubes includes: placing carbon nanotubes in a mixed acid of sulfuric acid and nitric acid, wherein the mass ratio of the sulfuric acid to the nitric acid is (88-92):(7-12), stirring the reaction for 2-6 hours, then performing ultrasonic treatment for 0.5-2 hours, and obtaining the acid-modified carbon nanotubes after washing and drying.

[0030] In some embodiments, the mass ratio of the composite material, the binder and the solvent is (50-70):(20-40):(70-100).

[0031] In some embodiments, the slurry further comprises a tackifier, and the mass ratio of the composite material to the tackifier is (50-70):(5-10).

[0032] In some embodiments, the slurry further comprises an additive, wherein the additive comprises at least one of a leveling agent, a defoaming agent and a dispersant; and the mass ratio of the composite material to the additive is (50-70):(1-5).

[0033] A battery comprises the composite diaphragm or the composite diaphragm prepared by the composite diaphragm preparation method.

[0034] Compared with the prior art, the present invention has the following beneficial effects:

[0035] (1) In the composite membrane of the present invention, the carbon nanotubes in the composite material have high electrical conductivity and good thermal stability, and the surface-coated polyvinyl pyrrolidone can improve the dispersibility and wettability of the carbon nanotubes, thereby making the obtained composite membrane have excellent heat resistance, coating adhesion, liquid storage and wetting properties.

[0036] (2) The preparation method of the composite membrane of the present invention is that the composite material is mainly prepared by mixing a mixed system containing acid-modified carbon nanotubes, polyvinyl pyrrolidone and water through a mixing treatment and a hydrothermal reaction. The polyvinyl pyrrolidone self-assembles to form a tubular structure, which modifies the surface of the carbon nanotubes to form a composite structure of polyvinyl pyrrolidone-coated carbon nanotubes, which has excellent thermal stability and wettability. The slurry containing the composite material, the binder and the solvent is coated on the surface of the base film, and the composite membrane can be obtained after drying. The method is simple and easy to implement, and the obtained composite membrane has good heat resistance, coating adhesion, liquid storage and wetting properties.

[0037] (3) The battery of the present invention has excellent thermal stability and good safety performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0039] Figure 1 is an infrared spectrum of the composite material in Example 1 of the present invention;

[0040] Figure 2 is a scanning electron microscope image of the composite material in Example 1 of the present invention;

[0041] Figure 3 This is a scanning electron microscope image of the pure carbon nanotubes in Example 1 of the present invention. DETAILED DESCRIPTION

[0042] The embodiments of the present invention will be described in detail below in conjunction with the examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present invention and should not be considered as limiting the scope of the present invention. If no specific conditions are specified in the examples, the conditions are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be obtained commercially.

[0043] According to one aspect of the present invention, the present invention relates to a composite diaphragm, comprising a base film and a coating located on at least one surface of the base film, wherein the coating comprises a composite material and a binder, and the composite material comprises carbon nanotubes and polyvinyl pyrrolidone (PVP) coated with carbon nanotubes (CNTs).

[0044] In the composite membrane of the present invention, the carbon nanotubes in the composite material have high electrical conductivity and good thermal stability, and the surface-coated polyvinyl pyrrolidone can improve the dispersibility and wettability of the carbon nanotubes, thereby making the obtained composite membrane have excellent thermal resistance, coating adhesion, liquid storage and wetting properties.

[0045] In some embodiments, the mass ratio of the composite material to the binder is (50-70):(20-40). In some embodiments, the mass ratio of the composite material to the binder includes but is not limited to 50:20, 55:25, 60:30, 60:40, 65:35, 70:40, etc., or any range between the two. The composite material and the binder of the present invention adopt a suitable mass ratio, thereby ensuring that the obtained composite diaphragm has better thermal stability and wettability.

[0046] In some embodiments, the average diameter of the carbon nanotubes is 40 to 60 mm, including but not limited to 40 mm, 45 mm, 50 mm, 55 mm, 60 mm, etc., or any range between the two. The average length is 1 to 10 μm, including but not limited to 1 μm, 2 μm, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm, etc., or any range between the two. The carbon nanotubes of the present invention have a suitable length and diameter, thereby ensuring the electrical conductivity, thermal stability and wettability of the composite material, so as to better improve the thermal stability and wettability of the composite membrane.

[0047] In some embodiments, in the composite material, the coverage of the polyvinyl pyrrolidone on the surface of the carbon nanotubes is 80% to 99%, including but not limited to 80%, 82%, 85%, 88%, 90%, 92%, 95% or 99%, etc., or any range between the two. The test method of coverage: select a certain area on the SEM image of the composite material, and calculate the length ratio of the polymer-covered surface and the uncovered surface. In the present invention, the appropriate coverage of polyvinyl pyrrolidone on the surface of carbon nanotubes is more conducive to ensuring the thermal stability, wettability and conductivity of the composite material.

[0048] In some embodiments, the binder includes polymethyl methacrylate (PMMA). Using PMMA as a binder can reduce process requirements and save production costs.

[0049] In some embodiments, the coating further comprises a tackifier; the tackifier comprises polyethylene oxide. The mass ratio of the binder to the tackifier is (20-40):(5-10), including but not limited to 20:5, 25:6, 30:7, 35:8, 40:10, etc., or any range value between the two. By using a tackifier in an appropriate dosage ratio, it is helpful to ensure the bonding effect of the binder.

[0050] In some embodiments, the coating further comprises an additive, wherein the additive comprises at least one of a leveling agent, a defoamer and a dispersant; the mass ratio of the composite material to the additive is (50-70):(1-5), including but not limited to 50:1, 55:2, 55:2.5, 60:3, 70:5, etc., or any range value between the two. In some embodiments, the defoamer comprises polydimethylsiloxane. The leveling agent comprises propylene glycol methyl ether acetate. The dispersant comprises an organic fluorine dispersant. In some embodiments, the mass ratio of the leveling agent, the defoamer and the dispersant is (0.8-1.2):(0.8-1.2):(0.8-1.2), for example, 0.8:1:1, 1:1:1, 1.2:1:1, etc.

[0051] In some embodiments, the base film includes one of PE film, PP film, PI film, PET film, non-woven fabric diaphragm, or a laminated composite of multiple types, such as PE / PP composite film, PI / PET composite film, PP / PE / PP composite film. In some embodiments, the thickness of the base film is 5 to 10 μm, including but not limited to 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm, etc., or any range between the two. In some embodiments, the porosity of the base film is 30% to 70%, including but not limited to 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, etc., or any range between the two.

[0052] In some embodiments, the thickness of the coating is 0.5 to 5 μm, including but not limited to 0.5 μm, 1 μm, 1.5 μm, 2 μm, 2.5 μm, 3 μm, 4 μm, 5 μm, etc., or any range between the two. The porosity of the coating is 60% to 90%, including but not limited to 60%, 65%, 70%, 75%, 80%, 85%, 90%, etc., or any range between the two. The coating of the present invention has a suitable thickness and porosity to ensure the overall performance of the coating, so that the composite diaphragm has better thermal stability and wettability.

[0053] According to another aspect of the present invention, the present invention relates to a method for preparing the composite diaphragm, comprising the following steps:

[0054] A slurry is coated on at least one side of the base film to form a wet film, wherein the slurry contains a composite material, a binder and a solvent, and the composite material is mainly obtained by mixing a mixed system containing acid-modified carbon nanotubes, polyvinyl pyrrolidone and water through a mixing treatment and a hydrothermal reaction; and the wet film is dried to obtain a composite diaphragm.

[0055] The preparation method of the composite membrane of the present invention is that the composite material is mainly prepared by mixing a mixed system containing acid-modified carbon nanotubes, polyvinyl pyrrolidone and water through a mixing treatment and a hydrothermal reaction, and the polyvinyl pyrrolidone self-assembles to easily form a tubular structure, which modifies the surface of the carbon nanotubes, and PVP is reassembled into a composite structure of PVP-coated CNTs, which has excellent thermal stability and wettability. A slurry containing the composite material, a binder and a solvent is coated on the surface of a base film, and a composite membrane can be obtained after drying. The method is simple and easy to implement, and a composite membrane with excellent heat resistance, coating adhesion, liquid storage and wetting properties can be obtained.

[0056] In some embodiments, the preparation method of the acid-modified carbon nanotubes comprises: placing the carbon nanotubes in a mixed acid of sulfuric acid and nitric acid, wherein the mass ratio of the sulfuric acid to the nitric acid is (88-92): (7-12), including but not limited to 88:7, 90:10, 92:12, etc., or any range between the two. Stirring the reaction for 2-6 hours, such as 2 hours, 3 hours, 4 hours, 5 hours, 6 hours, etc., and then ultrasonically treating for 0.5-2 hours, such as 0.5 hours, 1 hours, 1.5 hours, 2 hours, 2.5 hours, etc., washing and drying to obtain the acid-modified carbon nanotubes. Deionized water is used for washing, and the number of washing times is 5-8 times. After solid-liquid separation, drying is performed, and the drying temperature is 60-90°C and the drying time is 8-15 hours. The surface modification of carbon nanotubes is mainly because carbon nanotubes are easy to agglomerate, and the consistency of the coating used directly is very poor. After surface modification, the agglomeration amount is relatively uniform, because there are carboxyl groups on the surface, and there is a certain repulsive force when the agglomeration amount is large.

[0057] In some embodiments, the mass ratio of polyvinyl pyrrolidone to acid-modified carbon nanotubes is (200-400):(10-20), including but not limited to 200:10, 250:12, 280:15, 300:16, 350:18, 400:20, etc. The appropriate amount ratio of polyvinyl pyrrolidone to acid-modified carbon nanotubes can ensure that polyvinyl pyrrolidone forms a suitable coating on the surface of the acid-modified carbon nanotubes, so that the obtained composite material has excellent thermal stability and wettability.

[0058] In some embodiments, the mixed system further comprises a surfactant and a dispersant. The surfactant comprises sodium dodecyl sulfate, and the dispersant comprises carboxymethyl cellulose. In some embodiments, the mass ratio of the acid-modified carbon nanotubes, the polyvinyl pyrrolidone, the surfactant and the dispersant is (200-400):(10-20):(0.5-5):(0.5-5), for example, 200:10:0.5:0.5, 250:12:1:1, 300:15:2:2, 350:16:3:4, 400:20:5:5, etc. The acid-modified carbon nanotubes, polyvinyl pyrrolidone, the surfactant and the dispersant adopt an appropriate mass ratio, which is more conducive to the hydrothermal reaction.

[0059] In some embodiments, the solid content of the mixed system is 20% to 30%, including but not limited to 20%, 21%, 22%, 25%, 28% or 30%, or any range between the two.

[0060] In some embodiments, the solvent includes water, such as deionized water.

[0061] In some embodiments, the mixing process is carried out at a speed of 700 to 1500 rpm, such as 700 rpm, 800 rpm, 900 rpm, 1000 rpm, 1100 rpm, 1200 rpm, 1300 rpm, 1400 rpm or 1500 rpm, or any range of two thereof. In some embodiments, the mixing process is carried out for a time of 10 to 60 min, such as 10 min, 20 min, 30 min, 40 min, 50 min or 60 min, or any range of two thereof. Suitable mixing process conditions allow the materials to be fully mixed, which is beneficial to the subsequent hydrothermal reaction.

[0062] In some embodiments, the temperature of the hydrothermal reaction is 150-200°C, such as 150°C, 160°C, 170°C, 180°C, 190°C or 200°C, or any range between the two. The time of the hydrothermal reaction is 6-12h, such as 6h, 7h, 8h, 10h, 12h, or any range between the two. Suitable hydrothermal reaction conditions are conducive to the compounding of acid-modified carbon nanotubes and polyvinyl pyrrolidone.

[0063] In some embodiments, the method further comprises: washing and drying the material obtained after the hydrothermal reaction. The washing is carried out with water and ethanol in sequence for 5 to 8 times, and then filtering is carried out. The drying temperature is 60 to 80° C. and the drying time is 8 to 15 hours.

[0064] In some embodiments, the mass ratio of the composite material, the binder and the solvent is (50-70):(20-40):(70-100). In some embodiments, the mass ratio of the composite material, the binder and the solvent is 50:20:70, 55:25:80, 60:30:80, 70:40:100, etc.

[0065] In some embodiments, the slurry further comprises a tackifier, and the mass ratio of the binder to the tackifier is (20-40):(5-10), including but not limited to 20:5, 25:6, 30:7, 35:8, 40:10, etc., or any range between the two. The tackifier is used in an appropriate amount ratio to ensure the bonding effect of the binder.

[0066] In some embodiments, the slurry further comprises an additive, and the additive comprises at least one of a leveling agent, a defoaming agent and a dispersant; the mass ratio of the composite material to the additive is (50-70):(1-5), including but not limited to 50:1, 55:2, 55:2.5, 60:3, 70:5, etc., or any range between the two. In some embodiments, the defoaming agent comprises polydimethylsiloxane, which is helpful in suppressing foam. The leveling agent comprises propylene glycol methyl ether acetate, which helps to improve the leveling and uniformity of the slurry, improve the film-forming performance of the slurry coating, and make the coating smooth and uniform. The dispersant comprises an organic fluorine dispersant, which is beneficial for uniform dispersion of the material in the slurry. An appropriate amount of additives can effectively improve the physical and chemical properties of the slurry, and thus improve the physical and chemical properties of the coating.

[0067] In a preferred embodiment, the method for preparing the composite diaphragm comprises the following steps:

[0068] (1) placing carbon nanotubes in a mixed acid of sulfuric acid and nitric acid, wherein the mass ratio of sulfuric acid to nitric acid is (88-92):(7-12), stirring the mixture for 2-6 hours, then ultrasonically treating the mixture for 0.5-2 hours, washing the mixture 5-8 times, and drying the mixture at a temperature of 60-90° C. for 8-15 hours to obtain acid-modified carbon nanotubes.

[0069] (2) A mixed system of acid-modified carbon nanotubes, polyvinyl pyrrolidone, a surfactant, a dispersant and a solvent is mixed, wherein the mass ratio of the acid-modified carbon nanotubes, the polyvinyl pyrrolidone, the surfactant and the dispersant is (200-400):(10-20):(0.5-5):(0.5-5), the mixing speed is 700-1500 rpm, the mixing time is 10-60 min, and then the mixture is transferred to a hydrothermal reactor for mechanical energy hydrothermal reaction, the hydrothermal reaction temperature is 150-200° C., the hydrothermal reaction time is 6-12 h, and then cooled to room temperature, and then washed and dried, the washing is carried out with water and ethanol in sequence, the washing number is 5-8 times, and then filtered, and the solid material after filtration is dried at a temperature of 60-80° C. for 8-15 h to obtain a composite material.

[0070] (3) The composite material, PMMA, a thickener and additives (including a leveling agent, a defoaming agent and a dispersant) are mixed and added into deionized water. The mass ratio of the composite material, PMMA, a thickener, additives and water is (50-70):(20-40):(5-10):(1-5):(70-100). The mixture is stirred until uniformly mixed to obtain a coating slurry.

[0071] (4) The coating slurry is applied to at least one surface of the base film, and dried to obtain a composite diaphragm.

[0072] In some embodiments, the reaction of acid-modified carbon nanotubes is as follows:

[0073]

[0074] In some embodiments, the structure of the composite material is as follows:

[0075]

[0076] According to one aspect of the present invention, the present invention relates to a battery, comprising the composite diaphragm described above, or the composite diaphragm prepared by the method for preparing the composite diaphragm described above.

[0077] The battery of the present invention has more excellent cycle performance, thermal stability and good safety performance.

[0078] The following is further explained in conjunction with specific embodiments.

[0079] Example 1

[0080] A method for preparing a composite diaphragm comprises the following steps:

[0081] (1) Mix carbon nanotubes with an average diameter of 50 mm and an average length of 6 μm, a sulfuric acid solution with a mass fraction of 75%, and a nitric acid solution with a mass fraction of 60% in a mass ratio of 3:90:7, stir at 150 rpm for 5 h at room temperature, and then ultrasonically disperse for 1 h. Then wash with deionized water in small amounts and filter for 6 times, and then place the sample in a vacuum drying oven at 80°C for 12 h to obtain acid-modified carbon nanotubes.

[0082] (2) PVP (PVPK25), acid-modified carbon nanotubes, sodium dodecyl sulfate and carboxymethyl cellulose were mixed in a mass ratio of 320:15:3:3, and a certain amount of deionized water was added to obtain a solid content of 25%. The mixture was stirred at 1000 rpm for 30 min using a planetary vacuum mixer and then transferred to a hydrothermal reactor. After assembly, the mixture was placed in an oven at 165°C for 8 h and then cooled to room temperature. The mixture in the reactor was washed with water and ethanol in turn and filtered, and the process was repeated 6 times. The sample was then dried in a vacuum drying oven at 70°C for 12 h to obtain a composite material (PVP-CNTs).

[0083] (3) PVP-CNTs, PMMA, thickener (polyethylene oxide) and additives are mixed and added to deionized water. The additives are a leveling agent, a defoamer and a dispersant in a mass ratio of 1:1:1. The mass ratio of PVP-CNTs, PMMA, thickener, additive and water is 50:35:10:5:75. Stir thoroughly until the mixture is uniform to obtain a coating slurry.

[0084] (4) The coating slurry is coated on the surface of a 7 μm PE base film using a micro-gravure coating technique. The porosity of the PE base film is 41%, and the coating thickness is 2 μm. After drying, a composite lithium-ion battery separator is obtained. The thickness of the composite lithium-ion battery separator is 9 μm.

[0085] Example 2

[0086] A method for preparing a composite diaphragm, which differs from Example 1 in that:

[0087] The mass ratio of PVP-CNTs, PMMA, polyethylene oxide and additives was adjusted to 70:17:10:3.

[0088] Example 3

[0089] A method for preparing a composite diaphragm, which differs from Example 1 in that:

[0090] The mass ratio of PVP-CNTs, PMMA, polyethylene oxide and additives was adjusted to 60:30:8:2.

[0091] Example 4

[0092] A method for preparing a composite diaphragm, which differs from Example 1 in that:

[0093] In step (2), PVP (PVPK25), modified CNTs, sodium dodecyl sulfate and carboxymethyl cellulose are mixed in a mass ratio of 260:14:2.5:2.5.

[0094] Example 5

[0095] A method for preparing a composite diaphragm, which differs from Example 1 in that:

[0096] In step (2), PVP (PVPK25), modified CNTs, sodium dodecyl sulfate and carboxymethyl cellulose are mixed in a mass ratio of 380:17:3.8:4.

[0097] Example 6

[0098] A method for preparing a composite diaphragm, which differs from Example 1 in that:

[0099] In step (4), the coating slurry is coated on the surface of a 9 μm composite base membrane using a micro-gravure coating technique. The composite base membrane is a PP / PE / PP membrane with a porosity of 45%. The coating thickness is 3.5 μm. After drying, a composite lithium-ion battery separator is obtained. The thickness of the composite lithium-ion battery separator is 12.5 μm.

[0100] Example 7

[0101] A method for preparing a composite diaphragm comprises the following steps:

[0102] (1) Mix carbon nanotubes with an average diameter of 60 mm and an average length of 8 μm, a sulfuric acid solution with a mass fraction of 75%, and a nitric acid solution with a mass fraction of 60% in a mass ratio of 3:90:7, stir at 2000 rpm for 3 h at room temperature, and then ultrasonically disperse for 0.5 h. Then wash with deionized water in small amounts and filter for 8 times, and then place the sample in a vacuum drying oven at 90°C for 10 h to obtain acid-modified carbon nanotubes.

[0103] (2) PVP (PVPK30), acid-modified carbon nanotubes, sodium dodecyl sulfate and carboxymethyl cellulose were mixed in a mass ratio of 400:20:5:5, and a certain amount of deionized water was added to obtain a solid content of 30%. The mixture was stirred at 1500 rpm with a planetary vacuum mixer for 20 min, and then transferred to a hydrothermal reactor. After assembly, the mixture was placed in an oven at 200°C for 6 h, and then cooled to room temperature. The mixture in the reactor was washed with water and ethanol in turn and filtered, and the process was repeated 8 times. The sample was then dried in a vacuum drying oven at 80°C for 8 h to obtain a composite material (PVP-CNTs).

[0104] (3) PVP-CNTs, PMMA, a thickener (polyethylene oxide) and an additive are mixed and added to deionized water. The additive is a leveling agent, a defoamer and a dispersant in a mass ratio of 1:1:1. The mass ratio of PVP-CNTs, PMMA, a thickener, an additive and water is 70:40:10:5:100. Stir thoroughly until the mixture is uniformly mixed to obtain a coating slurry.

[0105] (4) The coating slurry is coated on the surface of a 7 μm PP base film using a micro-gravure coating technique. The porosity of the PP base film is 50%, and the coating thickness is 2 μm. After drying, a composite lithium-ion battery separator is obtained. The thickness of the composite lithium-ion battery separator is 9 μm.

[0106] Example 8

[0107] A method for preparing a composite diaphragm comprises the following steps:

[0108] (1) Mix carbon nanotubes with an average diameter of 40 mm and an average length of 4 μm, a sulfuric acid solution with a mass fraction of 75%, and a nitric acid solution with a mass fraction of 60% in a mass ratio of 3:90:7, stir at 1000 rpm for 6 hours at room temperature, and then ultrasonically disperse for 1.5 hours. Then wash with deionized water in small amounts and filter, repeat 6 times, and then place the sample in a vacuum drying oven at 90°C for 10 hours to obtain acid-modified carbon nanotubes.

[0109] (2) PVP (PVPK30), acid-modified carbon nanotubes, sodium dodecyl sulfate and carboxymethyl cellulose were mixed in a mass ratio of 200:10:0.5:0.5, and a certain amount of deionized water was added to obtain a solid content of 20%. The mixture was stirred at 800 rpm in a planetary vacuum mixer for 40 min, and then transferred to a hydrothermal reactor. After assembly, the mixture was placed in an oven at 150°C for 10 h and then cooled to room temperature. The mixture in the reactor was washed with water and ethanol in turn and filtered, and the process was repeated 6 times. The sample was then dried in a vacuum drying oven at 60°C for 12 h to obtain a composite material (PVP-CNTs).

[0110] (3) PVP-CNTs, PMMA, a thickener (polyethylene oxide) and an additive are mixed and added to deionized water. The additive is a leveling agent, a defoamer and a dispersant in a mass ratio of 1:1:1. The mass ratio of PVP-CNTs, PMMA, a thickener, an additive and water is 65:25:8:2:85. Stir thoroughly until the mixture is uniform to obtain a coating slurry.

[0111] (4) The coating slurry is coated on the surface of a 7 μm PET base film using a micro-gravure coating technique. The porosity of the PET base film is 55%, and the coating thickness is 2 μm. After drying, a composite lithium-ion battery separator is obtained. The thickness of the composite lithium-ion battery separator is 9 μm.

[0112] Comparative Example 1

[0113] A method for preparing a composite diaphragm, which differs from Example 1 in that:

[0114] Replace PVP-CNTs with ceramics.

[0115] Comparative Example 2

[0116] A method for preparing a composite diaphragm, which differs from Example 1 in that:

[0117] The PVP-CNTs were replaced with a mixture of ordinary PVP and CNTs.

[0118] Experimental example

[0119] 1. Graph Analysis

[0120] The infrared spectrum of the composite material in Example 1 of the present invention is as follows Figure 1 As shown in the figure, the broad and strong absorption peaks in the 3200-3600 cm region on the infrared spectrum curve are attributed to the stretching vibration peak caused by the associated hydroxyl groups. -1 and 2850cm -1 The characteristic absorption peak of the stretching vibration of the carbon-hydrogen bond of the typical methylene -CH2- appears at 1665cm -1 The carbonyl stretching vibration absorption peak of PVP appeared at 1425cm -1 The bending vibration absorption peak of methylene -CH2- appeared nearby. However, pure CNTs did not show the above characteristic peaks, thus confirming that PVP was introduced on the surface of CNTs.

[0121] The scanning electron microscope image of the composite material in Example 1 of the present invention is as follows Figure 2 The scanning electron microscope image of the pure carbon nanotubes in Example 1 is shown in Figure 3 As shown, it can be seen that the surface of the carbon nanotubes is coated with PVP.

[0122] 2. Performance test of composite diaphragm

[0123] The performance of the composite membranes obtained in each embodiment and comparative example was tested as follows:

[0124] 1. Heat resistance test

[0125] Heat resistance test is carried out according to GB / T 12027-2004 "Test method for dimensional change rate of plastic film and sheeting upon heating".

[0126] 2. Adhesion test

[0127] The adhesion test was carried out according to GB / T 2792-2014 “Test method for peel strength of adhesive tape”.

[0128] 3. Liquid storage performance test

[0129] Take a 10cm×10cm diaphragm and soak it in a lithium salt electrolyte (the mass ratio of EC, EMC and DEC is 3:5:2, LiPF6 is 1 Mol / L) at 70°C for 24 hours. Weigh the mass of the diaphragm before and after soaking. The liquid storage rate = mass after soaking / mass before soaking × 100%.

[0130] 4. Wettability test

[0131] Take a 10cm×0.5cm diaphragm, clamp both ends with clips and fix it on a steel frame at room temperature, take 2ul of electrolyte (EC:PC:DEC=1:1:1, volume ratio) and drop it on the center point, and time for 30s to record the diffusion distance of the electrolyte.

[0132] The test results are shown in Table 1.

[0133] Table 1 Performance test results of composite diaphragm

[0134]

[0135] It can be seen from Table 1 that the composite diaphragm obtained by the method of the present invention has excellent heat resistance, coating adhesion, liquid storage and wettability; wherein, the thermal shrinkage rate of TD at 130°C and 1h is less than or equal to 2.5%, and the thermal shrinkage rate of MD is less than or equal to 3%; the peel strength of the coating is greater than or equal to 60N / m, the liquid storage rate is greater than 140%, and the wettability is greater than 1cm.

[0136] The heat resistance, coating adhesion, liquid storage and wetting properties of the composite membranes of Comparative Examples 1 to 2 are relatively poor.

[0137] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein by equivalents. However, these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A composite diaphragm, characterized in that: The invention comprises a base film and a coating located on at least one side of the base film. The coating comprises a composite material and a binder. The composite material comprises carbon nanotubes and polyvinyl pyrrolidone coating the carbon nanotubes.

2. The composite diaphragm according to claim 1, characterized in that: The method comprises at least one of the following features (1) to (4): (1) The mass ratio of the composite material to the binder is (50-70):(20-40); (2) The average diameter of the carbon nanotubes is 40 to 60 mm, and the average length is 1 to 10 μm; (3) In the composite material, the coverage rate of the polyvinyl pyrrolidone on the surface of the carbon nanotubes is 80% to 99%; (4) The binder includes polymethyl methacrylate.

3. The composite diaphragm according to claim 1, characterized in that: Contains at least one of the following features (1) to (2): (1) The coating further comprises a tackifier; the mass ratio of the binder to the tackifier is (20-40):(5-10); (2) The coating further comprises an additive, wherein the additive comprises at least one of a leveling agent, a defoaming agent and a dispersant; and the mass ratio of the composite material to the additive is (50-70):(1-5).

4. The composite diaphragm according to claim 1, characterized in that: Contains at least one of the following features (1) to (4): (1) The thickness of the coating is 0.5 to 5 μm, and the porosity of the coating is 60% to 90%; (2) The base film comprises one of PE film, PP film, PI film, PET film, non-woven fabric separator, or a laminated composite of multiple thereof; (3) The thickness of the base film is 5 to 10 μm; (4) The porosity of the base film is 30% to 70%.

5. The method for preparing a composite diaphragm according to any one of claims 1 to 4, characterized in that: The following steps are involved: A slurry is coated on at least one side of the base film to form a wet film, wherein the slurry contains a composite material, a binder and a solvent, and the composite material is mainly obtained by mixing a mixed system containing acid-modified carbon nanotubes, polyvinyl pyrrolidone and water through a mixing treatment and a hydrothermal reaction; and the wet film is dried to obtain a composite diaphragm.

6. The method for preparing the composite diaphragm according to claim 5, characterized in that: Contains at least one of the following features (1) to (2): (1) The mass ratio of the polyvinyl pyrrolidone to the acid-modified carbon nanotubes is (200-400):(10-20); (2) The mixed system further comprises a surfactant and a dispersant, and the mass ratio of the acid-modified carbon nanotubes, the polyvinyl pyrrolidone, the surfactant and the dispersant is (200-400):(10-20):(0.5-5):(0.5-5).

7. The method for preparing a composite diaphragm according to claim 5, characterized in that: Contains at least one of the following features (1) to (5): (1) The solid content of the mixed system is 20% to 30%; (2) The rotation speed of the mixing process is 700 to 1500 rpm, and the time of the mixing process is 10 to 60 minutes; (3) The temperature of the hydrothermal reaction is 150 to 200° C., and the time of the hydrothermal reaction is 6 to 12 hours; (4) further comprising: washing and drying the material obtained after the hydrothermal reaction; (5) The preparation method of the acid-modified carbon nanotubes comprises: placing the carbon nanotubes in a mixed acid of sulfuric acid and nitric acid, wherein the mass ratio of the sulfuric acid to the nitric acid is (88-92):(7-12), stirring the reaction for 2-6 hours, then ultrasonically treating for 0.5-2 hours, and washing and drying to obtain the acid-modified carbon nanotubes.

8. The method for preparing a composite diaphragm according to claim 5, characterized in that: The mass ratio of the composite material, the binder and the solvent is (50-70):(20-40):(70-100).

9. The method for preparing a composite diaphragm according to claim 5, characterized in that: Contains at least one of the following features (1) to (2): (1) The slurry further comprises a tackifier, and the mass ratio of the composite material to the tackifier is (50-70):(5-10); (2) The slurry further comprises an additive, wherein the additive comprises at least one of a leveling agent, a defoaming agent and a dispersant; and the mass ratio of the composite material to the additive is (50-70):(1-5).

10. A battery, characterized in that: A composite diaphragm comprising the composite diaphragm according to any one of claims 1 to 4, or a composite diaphragm prepared by the method for preparing the composite diaphragm according to any one of claims 5 to 9.

Citation Information

Patent Citations

  • Lithium ion battery membrane with porous composite coating and preparation method thereof

    CN102769116A

  • Preparation method of conductive high-molecular composite material

    CN106751665A

  • High-safety carbon nanotube composite diaphragm and preparation process thereof

    CN112201902A

  • Preparation method of pyrrolidone modified multi-walled carbon nanotube composite epoxy powder coating

    CN113736338A

  • Modified carbon nanotube powder as well as preparation method and application thereof