Lithium ion battery diaphragm as well as preparation method and application thereof
By using photocured MOFs materials and conductive agents on the lithium-ion battery separator, the problem of manganese element dissolution in lithium manganese iron phosphate batteries is solved, the cycle life and rate performance of the battery are improved, and more efficient electrochemical performance is achieved.
Patent Information
- Application Number
- CN202411247875.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-06
- Publication Date
- 2024-11-12
AI Technical Summary
The dissolution of manganese elements in lithium manganese ferrophosphate batteries leads to the problems of short cycle life and low electron and ion conductivity, and the existing improvement methods have limited effects.
A lithium-ion battery separator is adopted, including a loaded spin coating and spray coating on the base film. The spin coating contains photocured metal organic framework materials (MOFs) and lithium supplement agents. The spray coating contains conductive agents, and through a specific preparation process Such as spin coating and electrostatic spraying, forming a composite film, inhibiting the deposition of manganese ion and dissolution of other transition metal ions.
Effectively inhibit the dissolution of manganese elements, improve the cycle life and rate performance of the battery, and improve the electrochemical performance of lithium manganese iron phosphate batteries.
Smart Images

Figure BDA0005031369490000141 
Figure BDA0005031369490000151
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium ion batteries, and in particular to a lithium ion battery separator and a preparation method and application thereof. Background Art
[0002] In recent years, with the continuous breakthroughs in the technology of the new energy market, the battery market operation has gone through several years of cycles, and the consumer demand for energy density has gradually been solved, while the demand for safety has become more and more prominent; phosphate cathodes are highly praised by consumers for their safety characteristics. Specifically, lithium iron phosphate is the most widely used cathode material, but its energy density is slightly lower, so the development of high-energy-density phosphate cathode materials is of great significance.
[0003] Lithium manganese iron phosphate battery is a new type of positive electrode material battery. It introduces manganese element on the basis of lithium iron phosphate to form a lithium manganese iron phosphate solid solution positive electrode material. With its high voltage platform, lithium manganese iron phosphate achieves an energy density that is about 20% higher than lithium iron phosphate; at the same time, with its olive tree-shaped structure, it plays a structural support role during the charging and discharging process, and has better thermodynamic and kinetic stability. Compared with traditional ternary positive electrode materials, lithium manganese iron phosphate avoids the high cost of nickel and cobalt, and also has better low-temperature electrical performance. However, lithium manganese iron phosphate positive electrode materials also have some defects, such as short cycle life caused by manganese dissolution, low electronic and ionic conductivity, etc.
[0004] The existing technology modifies the lithium iron manganese phosphate positive electrode through means such as carbon coating, ion doping, and nano-sizing to overcome the inherent defects of the lithium iron manganese phosphate positive electrode; however, the performance effect obtained by improving the positive electrode itself has certain limitations; if other functional structures in the lithium iron manganese phosphate battery can be synergistically modified to improve the defects of lithium iron manganese phosphate including manganese dissolution and short life, it will help to quickly promote the lithium iron manganese phosphate battery and improve the driving range and life.
[0005] In view of this, the present invention is proposed. Summary of the invention
[0006] The first object of the present invention is to provide a lithium-ion battery separator, which is mainly used to solve the technical defects of manganese dissolution and short battery life introduced by the positive electrode material containing manganese element (such as lithium iron manganese phosphate positive electrode) in conventional lithium-ion batteries.
[0007] The second object of the present invention is to provide a method for preparing the lithium-ion battery separator, which can meet the requirements of mass production by satisfying the structure and surface properties specified by the separator through a specific preparation process.
[0008] The third object of the present invention is to provide a lithium ion battery having the advantages of long cycle life and low manganese dissolution rate in the electrolyte.
[0009] A fourth object of the present invention is to provide an electrical device.
[0010] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:
[0011] A lithium ion battery separator, comprising a base film, and a spin coating layer and a spray coating layer sequentially loaded on at least one side of the base film;
[0012] The spin coating layer includes a MOFs material and a photocuring layer encapsulating the MOFs material; and the spray coating layer includes a lithium supplement agent and a conductive agent.
[0013] A method for preparing a lithium-ion battery separator comprises the following steps:
[0014] (1) preparing a spray coating slurry containing a lithium supplementing agent and a conductive agent, and preparing a spin coating slurry containing a MOFs material;
[0015] (2) spin coating the spin coating slurry onto the surface of the base film, and obtain a composite film loaded with the spin coating layer by embossing and ultraviolet treatment;
[0016] (3) Electrostatically spraying the spray slurry on the surface of the spin-coated layer, and then obtaining the lithium-ion battery separator through heat treatment.
[0017] A lithium ion battery comprises the lithium ion battery separator.
[0018] An electrical device comprises the lithium-ion battery.
[0019] Compared with the prior art, the present invention has the following beneficial effects:
[0020] The present invention provides a diaphragm for lithium ion batteries for replenishing lithium and inhibiting manganese dissolution, which can replenish lithium loss during the cycle process and the first charge and discharge process of the battery, and improve the cycle performance of the positive electrode of the battery containing manganese elements, such as lithium iron manganese phosphate. In the diaphragm of the present invention, a coating layer obtained by photopolymerization and curing is arranged on the surface of the base film, and a metal organic framework material (MOFs) that inhibits the deposition of manganese ions to the negative terminal is encapsulated to the surface of the diaphragm. On the one hand, the dissolution of the organic MOFs structure in the electrolyte is effectively inhibited, and the damage to the battery structure caused by the dissolution of other transition metal ions in the electrolyte is also inhibited; on the other hand, the MOFs material itself can provide a fast migration channel for lithium ion migration and improve the rate performance of the battery. DETAILED DESCRIPTION
[0021] The technical scheme of the present invention will be clearly and completely described below in conjunction with specific embodiments, but those skilled in the art will appreciate that the following described embodiments are part of embodiments of the present invention, rather than all embodiments, and are only used to illustrate the present invention, and should not be considered as limiting the scope of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work are within the scope of protection of the present invention. Those who do not specify specific conditions in the embodiments are carried out according to conventional conditions or conditions recommended by the manufacturer. Those who do not specify the manufacturer for reagents or instruments used are conventional products that can be purchased commercially. In addition, the terms "first", "second" and "third" are only used for descriptive purposes and cannot be interpreted as indicating or implying relative importance.
[0022] The first aspect of the present invention is to provide a lithium-ion battery separator. The separator comprises a base film, and a spin-coated layer and a spray-coated layer sequentially loaded on at least one side of the base film; wherein the spin-coated layer comprises an MOFs material and a photocured layer encapsulating the MOFs material; and the spray-coated layer comprises a lithium supplement agent and a conductive agent.
[0023] As a preferred embodiment, the base film includes a polyolefin film, including but not limited to a polypropylene film, a polyethylene film, an ethylene-propylene copolymer film, and the like.
[0024] As a preferred embodiment, the MOFs material includes at least one of MOF-5, MOF-74, MOF-199, MOF-177, MOF-525 or MOF-210; as a preferred embodiment, the metal base of the MOFs material includes at least one of Zr, Mg, Zn, Ni or Cu.
[0025] As a preferred embodiment, the lithium supplement includes at least one of Li2C2O4, Li2NiO2, Li5FeO4, Li2O, Li2MnO3, Li6CoO4, Li6MnO4 or Li5ReO6.
[0026] As a more preferred embodiment, the particle size of the lithium supplement is 100nm to 300nm, including but not limited to any one of 100, 120, 140, 150, 160, 180, 200, 220, 240, 250, 260, 280, 300 (nm) or a numerical range consisting of any two of them.
[0027] As a preferred embodiment, the conductive agent includes at least one of CNT, acetylene black, KB, SP, C60 or graphene.
[0028] As a more preferred embodiment, the particle size of the conductive agent is 30 nm to 60 nm, including but not limited to any one of 30, 35, 40, 45, 50, 55, 60 (nm) or a numerical range consisting of any two of them.
[0029] As a more preferred embodiment, the specific surface area of the conductive agent is 800 m 2 / g~1200m 2 / g, including but not limited to 800, 850, 900, 950, 1000, 1050, 1100, 1150, 1200 (m 2 / g) or any two of them.
[0030] As a preferred embodiment, the mass ratio of the conductive agent to the lithium supplement agent is 10% to 30%, including but not limited to any one of 10%, 12%, 14%, 15%, 16%, 18%, 20%, 22%, 24%, 25%, 26%, 28%, 30% or a ratio interval consisting of any two of them.
[0031] As a preferred implementation, the mass ratio of the spin-coated layer to the spray-coated layer is 10% to 20%.
[0032] As a preferred embodiment, the mass ratio of the MOFs material to the photocurable layer is 15% to 35%, including but not limited to any one of 15%, 20%, 25%, 30%, 35% or a numerical range consisting of any two of them.
[0033] As a preferred embodiment, the photocurable layer is obtained by photopolymerization of a thiol-containing compound, an alkenyl-containing compound and a photoinitiator. Specifically, based on the reaction of the thiol and alkenyl groups under light, the cured layer can stabilize the MOFs framework structure and inhibit the catalysis of the MOFs on the electrolyte, thereby inhibiting the side reactions in the electrolyte.
[0034] As a more preferred embodiment, the thiol-containing compound includes at least one of 1,2-ethanedithiol, a thiol-containing acrylate compound, mercaptoethanol, glutathione or mercaptopropionic acid, the olefinic compound includes at least one of methylstyrene, eugenol, 1,4-dialdehyde-2,5-divinylbenzene or methacrylate, and the photoinitiator includes dihydroxymethylpropionic acid.
[0035] As a preferred embodiment, the thickness of the lithium-ion battery separator is 20 μm to 40 μm, including but not limited to any one of 20, 22, 25, 28, 30, 32, 35, 38, 40 (μm) or a numerical range consisting of any two of them.
[0036] As a preferred embodiment, the porosity of the lithium-ion battery separator is 20% to 40%, including but not limited to any one of 20%, 22%, 25%, 28%, 30%, 32%, 35%, 38%, 40% or a numerical range consisting of any two of them.
[0037] It should be noted that the porosity test method can refer to the following physical method (i.e., based on the volume of liquid absorbed by the diaphragm), and the steps are as follows: first, weigh the diaphragm sample, and record the mass of the dry film as m1; then soak the diaphragm in n-butanol, take it out after 2 hours, and gently wipe the liquid on its surface with filter paper before weighing, and then weigh the mass of the wet film as m2, then the mass of n-butanol absorbed by the diaphragm can be obtained as m=m2-m1; then the porosity can be calculated; porosity P=m / ρV, ρ is the density of n-butanol, which is 0.8098g / cm 3 , V is the volume of the diaphragm.
[0038] As a preferred embodiment, the longitudinal heat shrinkage ratio of the lithium-ion battery separator is 1.0% to 1.3%; it is worth noting that the longitudinal direction is defined as the direction of the side parallel to the walking direction of the pole roll when the pole roll is wound.
[0039] It should be noted that the test method of the thermal shrinkage ratio can refer to the following method steps: the initial test thickness of the test diaphragm is h1; then the diaphragm is heated at 90°C for 1 hour, and then allowed to stand at room temperature to obtain a test thickness of h2; the longitudinal thermal shrinkage ratio is calculated as (h1-h2) / h1.
[0040] The second aspect of the present invention is to provide a method for preparing the lithium-ion battery separator. The method mainly includes three steps, namely, slurry preparation, spin coating preparation and spray coating preparation, and specifically includes the following steps (1) to (3).
[0041] (1) preparing a spray coating slurry containing a lithium supplement agent and a conductive agent, and preparing a spin coating slurry containing a MOFs material.
[0042] As a preferred embodiment, the solvent of the spraying slurry includes water.
[0043] As a preferred embodiment, the solid content of the spraying slurry is 20% to 60%.
[0044] As a preferred embodiment, the spin coating slurry includes the MOFs material, a thiol-containing compound, an olefinic compound and a photoinitiator.
[0045] As a more preferred embodiment, the mass ratio of the thiol-containing compound to the alkenyl-containing compound is 0.5-2.
[0046] As a more preferred embodiment, the added amount of the photoinitiator is 0.1% to 0.2% of the total mass of the thiol-containing compound and the olefinic compound.
[0047] As a more preferred embodiment, the added amount of the MOFs material is 20% to 30% of the sum of the mass of the thiol-containing compound and the olefinic compound.
[0048] As a preferred embodiment, the preparation process of the spray coating slurry and the spin coating slurry includes auxiliary means such as oscillation, stirring, centrifugation, ultrasound, heat treatment, etc. to achieve uniform mixing of the slurry.
[0049] (2) Spin coating the spin coating slurry onto the surface of the base film, and obtain a composite film loaded with the spin coating layer by embossing and ultraviolet light treatment.
[0050] As a preferred implementation, the imprinting process is performed by a nanoimprinting machine, the pressure of the imprinting process is set to 50N to 100N, and the duration of the imprinting process is 1min to 5min.
[0051] As a preferred embodiment, the illumination intensity of the ultraviolet light treatment is 20 mW / cm 2 ~50mW / cm 2 The illumination time of the ultraviolet light treatment is 2h to 3h; in some optional embodiments, the illumination intensity of the ultraviolet light treatment includes but is not limited to 20, 25, 30, 35, 40, 45, 50 (mW / cm 2 ) or any two of them.
[0052] (3) Electrostatically spraying the spray slurry on the surface of the spin-coated layer, and then obtaining a lithium-ion battery separator through heat treatment.
[0053] As a preferred implementation, the electrostatic spraying includes: a spraying voltage of 60 kV to 90 kV, a gas pressure of 0.6 MPa to 0.9 MPa, a receiving distance of 10 cm to 15 cm, and a spraying time of 5 min to 10 min.
[0054] As a preferred embodiment, the temperature of the heat treatment is 90° C. to 120° C., and the time of the heat treatment is 6 h to 10 h.
[0055] The third aspect of the present invention is to provide a lithium-ion battery. The lithium-ion battery includes the lithium-ion battery separator. It is understood that, in addition to the lithium-ion battery separator, the lithium-ion battery should include positive and negative electrodes, electrolyte, and other necessary or non-essential functional elements or packaging components.
[0056] In some preferred embodiments, the positive electrode used should use lithium manganese iron phosphate as the main positive electrode active material, or other manganese-doped positive electrode active materials; in addition, the lithium manganese iron phosphate positive electrode active material involved can be modified by means including but not limited to doping, coating, nano-crystallization, etc., and those skilled in the art can make any selection and combination on this basis. When the lithium ion battery includes the lithium ion battery separator of the present invention, whether or not other separator functional parts are used in the lithium ion battery, it can be regarded as an embodiment of the present invention.
[0057] The fourth aspect of the present invention is to provide an electric device. The electric device includes the lithium-ion battery. The electric device can be any device or apparatus that relies on electric energy to work or operate, including but not limited to new energy vehicles, building electrical equipment, industrial electrical appliances, household and agricultural electrical appliances, etc.; when including the lithium-ion battery, any electric device equipped with the lithium-ion battery can belong to an embodiment of the present invention.
[0058] Example 1
[0059] S1: Place commercially available lithium oxalate products into a nano-grinder and grind until the primary particle size is 200 nm.
[0060] S2: Take 90g of ground lithium oxalate and 10g of Ketjen black (particle size 800nm, specific surface area 100m 2 / g) and 400g of water were added to prepare a spray solution and stirred continuously to make it evenly dispersed.
[0061] S3: 100 g of 1,2-ethanedithiol, 100 g of methylstyrene, 0.2 g of dimethylolpropionic acid, and 40 g of Zr-MOF-74 material were stirred and mixed until uniform.
[0062] S4: Take a PP base film (thickness of 10 μm, porosity of 50%), place it on a silicon plate, spin-coat the solution prepared in S3 onto one side of the PP base film, and then transfer it to a nanoimprinter for alignment and imprinting, apply a pressure of 60 N, and use UV LED light at 20 mW / cm 2 The membrane was then removed after exposure to light for 3 h.
[0063] S5: Cut the diaphragm prepared in S4 and spread it flat on the receiving device of the electrostatic spraying equipment, take the solution prepared in S2, set 80 kV, 0.65 MPa (air pressure), 10 cm (spraying distance), start electrostatic spraying and continue spraying for 8 minutes, and then obtain the diaphragm precursor.
[0064] S6: Put the membrane precursor obtained in S5 into a 100° C. oven and dry it for 8 hours to obtain the composite membrane of this embodiment.
[0065] Example 2
[0066] The process is basically the same as Example 1, except that the amount of 1,2-ethanedithiol in step S3 is replaced by 65 g, and the amount of methylstyrene is replaced by 130 g.
[0067] Example 3
[0068] The process is basically the same as Example 1, except that the amount of 1,2-ethanedithiol in step S3 is replaced by 130 g, and the amount of methylstyrene is replaced by 65 g.
[0069] Example 4
[0070] The same as Example 1, except that: in step S4, the 2 Incubate under light for 2 hours.
[0071] Example 5
[0072] It is basically the same as Example 1, except that the parameters of the electrostatic spraying in step S5 are set to: 70 kV (voltage), 0.85 MPa (air pressure), and 12 cm (spraying distance).
[0073] Example 6
[0074] The method is basically the same as Example 1, except that the lithium oxalate in step S1 is replaced by Li5FeO4, the 1,2-ethanedithiol in step S3 is replaced by mercaptoethanol, and methyl styrene is replaced by 1,4-dialdehyde-2,5-divinylbenzene.
[0075] Example 7
[0076] The method is basically the same as Example 1, except that the 1,2-ethanedithiol in step S3 is replaced by mercaptopropionic acid, and methylstyrene is replaced by eugenol.
[0077] Example 8
[0078] The method is basically the same as Example 1, except that the Zr-MOF-74 material in step S3 is replaced by Ni-MOF-199.
[0079] Comparative Example 1
[0080] It is basically the same as Example 1, except that the particle size in step S1 is 1 μm.
[0081] Comparative Example 2
[0082] The same as Example 1, except that: in step S2, Ketjen black is replaced by a conductive agent sp (with a particle size of 1.5 μm and a specific surface area of 60 m 2 / g).
[0083] Comparative Example 3
[0084] The method is basically the same as Example 1, except that the mass of 1,2-ethanedithiol in step S3 is replaced by 20 g.
[0085] Comparative Example 4
[0086] The method is basically the same as Example 1, except that the mass of methyl styrene in step S3 is replaced by 500 g.
[0087] Comparative Example 5
[0088] It is basically the same as Example 1, except that the illumination time in step S4 is 24 hours.
[0089] Comparative Example 6
[0090] It is basically the same as Example 1, except that the illumination time in step S4 is 30 minutes.
[0091] Comparative Example 7
[0092] It is basically the same as Example 1, except that the air pressure in step S5 is set to 1 MPa.
[0093] Comparative Example 8
[0094] It is basically the same as Example 1, except that the air pressure in step S5 is set to 0.03 MPa.
[0095] Comparative Example 9
[0096] It is basically the same as Example 1, except that the continuous spraying time in step S5 is 1 minute.
[0097] Comparative Example 10
[0098] It is basically the same as Example 1, except that the continuous spraying time in step S5 is 30 minutes.
[0099] Comparative Example 11: The PP base film used in step S4 in Example 1.
[0100] Test example
[0101] (1) Preparation of raw materials and reagents
[0102] Prepare commercially available lithium manganese iron phosphate material and conductive carbon black (SP), and dry them under vacuum at 120°C for ≥10h. Prepare polyvinylidene fluoride (PVDF), and dry them under vacuum at 60°C for ≥4h. Prepare the battery shell in advance, put it in alcohol, ultrasonically clean it for 30min, dry it with air at 60°C overnight, and transfer it to the glove box for later use. Sandwich the diaphragms corresponding to each embodiment and comparative example between weighing paper, and use Punch out the diaphragm with a punching machine, transfer the punched diaphragm to a vacuum drying oven, bake at 60°C for more than 4h, and transfer to a glove box for use.
[0103] Preparation of 6.25% PVDF glue: Weigh 4.0000±0.0020g of PVDF powder and 60.0000±0.0020g of NMP in proportion and add them into a beaker, and stir with a mechanical stirrer at 500rpm for 3h; pour the prepared PVDF glue into a fluorinated bottle, seal it with a sealing film, and store it in a desiccator.
[0104] Preparation of 1% CMC glue solution: weigh 297.000±0.002g deionized water in a 500mL beaker, add 3.000±0.002g CMC, stir with a mechanical stirrer, gradually increase the stirring speed and finally adjust it to 800rpm; seal the beaker mouth with sealing film during the stirring process, stir for 3h until the glue solution is transparent and has no obvious particles, pour it into a reagent bottle for storage (CMC glue solution needs to be placed for more than 12h to ensure that the bubbles in the glue solution are eliminated before use).
[0105] (2) Positive electrode homogenization
[0106] The homogenization ratio is: lithium iron manganese phosphate material: PVDF: SP: dispersant = 89.5: 5: 5: 0.5. 0.0450g of D300 dispersant, 1.7877±0.0020g of PVDF glue, 2.0000±0.0020g of NMP, 0.1117±0.0005g of SP, 2.0000±0.0005g of lithium iron manganese phosphate powder, and 1 large zirconium bead (φ10mm) and 4 small zirconium beads (φ5mm) are added to a stirring tank; stirred for 7 minutes at 1000rpm and 2000rpm, and repeated 5 times with an interval of 2 minutes to obtain a slurry.
[0107] Lay a 20μm aluminum foil with a width of 11cm flat on the coating platform, and wipe it repeatedly with alcohol to ensure that the surface of the aluminum foil is clean and flat. Use a 300μm flat-head scraper to pour the slurry on a 150-mesh screen and let it flow naturally onto the aluminum foil to be coated; then take a medicine spoon and spread it evenly on the middle part of the scraper to start coating. After coating, remove the scraper and wipe it clean, transfer the coated electrode to a blast drying oven, and dry it at 100℃ for 100min and 100℃ for 720min in vacuum; take out the dried electrode and use Punch the positive electrode sheet with a punching machine and weigh its surface density to see if it is within 8.0±0.2mg / cm 2 If it is not qualified, it needs to be re-applied.
[0108] (3) Negative electrode homogenization
[0109] The homogenization ratio is: graphite: SP: CMC: SBR = 95: 1.5: 1.5: 2. Weigh 10.0000 ± 0.0020g of graphite powder and 0.1580 ± 0.0020g of SP and add them to the mixing tank, stir at 800rpm for 3min, and crush the undispersed SP particles with a spatula; add 8.0000 ± 0.5000g of CMC glue to the mixing tank, stir at 800rpm for 3min, then stir at 2000rpm for 2min, repeat 5 times until the slurry becomes a paste; add the remaining 7.7900 ± 0.5000g of CMC glue to the mixing tank, stir at 2000rpm for 2min, repeat 5 times; then add 0.4390 ± 0.0050g of SBR emulsion and stir at 2000rpm for 3min.
[0110] Lay the matte surface of 8μm copper foil flat on the coating platform, and wipe it repeatedly with alcohol to ensure that the copper foil surface is clean and flat; use a 120μm fixed scraper and two layers of 6μm copper foil on both sides (coating area height 132μm), pour the slurry on the middle part of the scraper and start coating. After coating, remove the scraper and wipe it clean, transfer the coated electrode to a blast drying oven, and dry it at 70±5℃ for 15min. Take out the dried electrode and use Punch out three pole pieces and determine whether their surface density is within 4.5±0.5mg / cm 2 If the surface of the electrode is smooth, even, flat and has no burrs on the edge, select the electrode; if it is unqualified, adjust the scraper scale and re-apply.
[0111] (4) Assembly
[0112] The stacking order of assembled batteries is: negative electrode shell → nickel foam → stainless steel gasket → electrolyte → negative electrode plate → diaphragm → electrolyte → positive electrode plate → positive electrode shell.
[0113] The steps and requirements for assembling the battery include the following: transfer the electrode to the glove box, and place the positive and negative electrode shells of the button battery on dust-free paper for standby use; place the negative electrode shells in a row, add nickel foam and stainless steel gaskets (convex side facing up) in turn, and use a 5mL dropper to add 3 drops of electrolyte, with the negative electrode current collector close to the gasket, and the diaphragm in the middle (note to separate the weighing paper from the diaphragm); then use a 5mL dropper to add 15 drops of electrolyte, put in the positive electrode to ensure that the active material side faces down and that the electrode is completely soaked; buckle the positive electrode shell with insulated tweezers, transfer the battery to the sealing machine, and apply 850kg pressure to seal; remove the packaged battery from the sealing machine, and wipe the residual electrolyte on the battery and the sealing machine with dust-free paper; transfer the battery out of the glove box, wipe it with alcohol, and put it in a ziplock bag for standby use; use a voltage internal resistance meter to test the open circuit voltage of the battery, and select a battery with an open circuit voltage of about 0.2V for testing.
[0114] (5) Electrical performance test
[0115] The button cells corresponding to the above-prepared embodiments and comparative examples were tested (nominal capacity 150 mAh / g); the ratio of the discharge gram capacity under 1C and 0.1C conditions was recorded; then the charge and discharge cycle was performed, charging to 4.3V at 0.1C, and then discharging to 3.0V at 0.1C, and the cycle was performed for 50 cycles, and the cycle capacity retention rate was recorded; the battery after 50 cycles was disassembled to obtain the negative electrode sheet, and its Mn element content was tested. The results of the above electrical performance tests are recorded in the following Table 1.
[0116] Table 1
[0117]
[0118]
[0119] As can be seen from Table 1, the batteries prepared according to the embodiments of the present invention have good performance in capacity and effectively prevent the manganese element from dissolving into the negative electrode, and have good electrical performance compared to Comparative Example 11 (conventional PP film).
[0120] Further comparison of the data measured in the embodiment of the present invention and other comparative examples shows that: 1) Comparative Example 1 uses a large-particle lithium oxalate lithium supplement, and the large particles will cause lithium ions to be blocked, thereby reducing the rate performance. 2) Comparative Example 2 uses a conductive agent with a low specific surface area, which is not tightly combined with lithium oxalate, resulting in an increase in the lithium desorption potential and a decrease in capacity. 3) In Comparative Example 3, the amount of thiol material used is too low, resulting in an incomplete encapsulation structure, which in turn causes the MOFs structure to dissolve, thereby resulting in a decrease in the ability to inhibit Mn dissolution. 4) In Comparative Example 4, when the amount of olefinic material used is too large, the cross-linked structure obtained by photopolymerization is too large, resulting in the MOFs structure being over-encapsulated, which in turn causes the Mn ions to be unable to migrate into the framework structure, thereby reducing performance. 5) When the illumination time in Comparative Example 5 is too long, the mechanical strength of the composite diaphragm is too rigid and cannot be attached to the positive electrode sheet, thereby reducing the rate performance. 6) In Comparative Example 6, the illumination time is too short, resulting in an incomplete encapsulation layer of the MOFs obtained by photopolymerization, and manganese dissolves, resulting in reduced performance. 7) In Comparative Example 7, the air pressure during the electrostatic spraying process was too high, which damaged the base membrane and interfered with the battery performance. 8) In Comparative Example 8, the spray pressure during the electrostatic spraying process was too low, resulting in the coating containing MOFs not being tightly bonded to the base membrane, resulting in poor performance. 9) In Comparative Example 9, the spraying time during the electrostatic spraying process was too short, resulting in an uneven spraying area, which in turn resulted in a decrease in lithium replenishment capacity. 10) In Comparative Example 10, the spraying time during the electrostatic spraying process was too long, resulting in the risk of the sprayed layer and the membrane falling off, and also hindering the transmission of lithium ions, resulting in a decrease in capacity.
[0121] Although the present invention has been illustrated and described with specific embodiments, it should be appreciated that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Those skilled in the art should understand that the technical solutions described in the above embodiments may be modified, or some or all of the technical features thereof may be replaced by equivalents without departing from the spirit and scope of the present invention. However, these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention. Therefore, this means that all such replacements and modifications within the scope of the present invention are included in the appended claims.
Claims
1. A lithium ion battery separator, characterized in that: The diaphragm includes a base film, and a spin coating layer and a spray coating layer sequentially loaded on at least one side of the base film; The spin coating layer includes a MOFs material and a photocurable layer encapsulating the MOFs material; The spray layer includes a lithium supplement agent and a conductive agent.
2. The lithium-ion battery separator according to claim 1, characterized in that The MOFs material includes at least one of MOF-5, MOF-74, MOF-199, MOF-177, MOF-525 or MOF-210; The metal base of the MOFs material includes at least one of Zr, Mg, Zn, Ni or Cu.
3. The lithium ion battery separator according to claim 1, characterized in that: The lithium supplement includes at least one of Li2C2O4, Li2NiO2, Li5FeO4, Li2O, Li2MnO3, Li6CoO4, Li6MnO4 or Li5ReO6; And / or, the conductive agent includes at least one of CNT, acetylene black, KB, SP, C60 or graphene; Preferably, the particle size of the lithium supplement agent is 100nm to 300nm, and the particle size of the conductive agent is 30nm to 60nm; Preferably, the specific surface area of the conductive agent is 800 m 2 / g~1200m 2 / g.
4. The lithium-ion battery separator according to claim 1, characterized in that The photocurable layer is obtained by photopolymerization reaction of a mercapto-containing compound, an olefin-containing compound and a photoinitiator; Preferably, the thiol-containing compound includes at least one of 1,2-ethanedithiol, thiol-containing acrylate compounds, mercaptoethanol, glutathione or mercaptopropionic acid; Preferably, the alkenyl-containing compound comprises at least one of methylstyrene, eugenol, 1,4-dialdehyde-2,5-divinylbenzene or methacrylate; Preferably, the photoinitiator comprises dimethylolpropionic acid.
5. The lithium ion battery separator according to claim 1, characterized in that: The thickness of the lithium ion battery separator is 20 μm to 40 μm; And / or, the porosity of the lithium-ion battery separator is 20% to 40%.
6. The method for preparing a lithium ion battery separator according to any one of claims 1 to 5, characterized in that: The preparation method comprises the following steps: (1) preparing a spray coating slurry containing a lithium supplementing agent and a conductive agent, and preparing a spin coating slurry containing a MOFs material; (2) spin coating the spin coating slurry onto the surface of the base film, and obtain a composite film loaded with the spin coating layer by embossing and ultraviolet treatment; (3) Electrostatically spraying the spray slurry on the surface of the spin-coated layer, and then obtaining a lithium-ion battery separator through heat treatment.
7. The method for preparing a lithium ion battery separator according to claim 6, characterized in that: The spin coating slurry comprises the MOFs material, a thiol-containing compound, an olefin-containing compound and a photoinitiator; Preferably, the mass ratio of the thiol group in the thiol-containing compound to the alkenyl group in the alkenyl-containing compound is 0.5 to 2; Preferably, the added amount of the MOFs material is 20% to 30% of the sum of the mass of the thiol-containing compound and the olefinic compound.
8. The method for preparing a lithium ion battery separator according to claim 6, characterized in that: The illumination intensity of the ultraviolet light treatment is 20 mW / cm 2 ~50mW / cm 2 The illumination time of the ultraviolet light treatment is 2h to 3h; And / or, the electrostatic spraying includes: a spraying voltage of 60 kV to 90 kV, a gas pressure of 0.6 MPa to 0.9 MPa, a receiving distance of 10 cm to 15 cm, and a spraying time of 5 min to 10 min.
9. A lithium ion battery, characterized in that: The invention comprises the lithium ion battery separator as claimed in any one of claims 1 to 5.
10. An electrical device, characterized in that: Comprising the lithium ion battery as claimed in claim 9.
Citation Information
Patent Citations
Polymer-coated MOF (Metal Organic Framework) particles as well as preparation method and application thereof
CN117402380A
Lithium supplement composite diaphragm, preparation method thereof and battery
CN118431672A
Cited By
Secondary battery and electric device
CN122338225A
A secondary battery and an electric device
CN122338225B