Pearlescent colorful glazed tile with three-dimensional positioning effect and preparation method of pearlescent colorful glazed tile

By adding a positioning dry grain layer with concave and convex effect at the bottom of the pearlescent fuse glaze layer, the problem of the existing pearlescent fuse glaze tiles is not strong, and a stronger gloss effect and a lower production energy consumption are achieved.

CN118930328AActive Publication Date: 2024-11-12FOSHAN DONGPENG CERAMIC +3

Patent Information

Application Number
CN202411034384.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-12
Estimated Expiration
2044-07-31

AI Technical Summary

Technical Problem

The pearlescent effect of existing pearlescent fuse glazed tiles is not strong, resulting in limited application, and a flat decorative layer is not conducive to the presentation of pearlescent effect.

Method used

A layer of positioning dry grain layer with concave and convex effect is added to the bottom of the pearlescent fuse glaze layer, so that the pearlescent fuse glaze layer can produce thickness deviations on the top of the glaze tiles, thereby achieving the pearlescent color effect.

Benefits of technology

By generating mica vitreous and cerium oxide with layered structure, the refractive, reflection and interference of light are enhanced, the pearl gloss effect of pearlite fuses is improved, and the production energy consumption is reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118930328A_ABST
    Figure CN118930328A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of architectural ceramics, and discloses a pearlescent colorful glazed tile with a stereotactic effect and a preparation method thereof.The preparation method comprises the steps that firstly, a frit with a pearlescent effect is prepared from white metal oxide cerium oxide with a high refractive index and layered vitreous fluoroaluminosilicate which is generated through a wrapping formula and has a low optical refractive index; meanwhile, the positioning dry particle layer with the concave-convex effect is additionally arranged at the bottom of the pearly lustrous frit glaze layer, so that the pearly lustrous frit glaze layer can generate thickness deviation at the top of the glazed tile, namely, the pearly lustrous frit glaze layer is thinner in the convex area of the positioning dry particle layer and thicker in the concave area of the positioning dry particle layer; the thickness deviation is beneficial to promoting the pearlescent frit with the carrier of the layered structure to generate stronger reflection, refraction and interference under the illumination condition, so that the pearlescent magical color effect on the surface of the glazed tile is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of building ceramics, and in particular to a pearlescent colorful glazed tile with a three-dimensional positioning effect and a preparation method thereof. Background Art

[0002] With the continuous progress of society and the continuous improvement of people's living standards, people will have different ideas when choosing ceramic products. In real life, people pay more attention to the functionality and practicality of ceramic products. Based on market demand, ceramic production has also developed rapidly, and ceramic production technology has become more and more mature. The preparation of glazes in the firing process of ceramics is also extremely important. Ceramic industry players have also paid attention to the development of functional and practical glazes. The same body will produce different effects due to different glazes. Different hand touch and visual perception of the glaze will also affect the choice of consumers.

[0003] Glaze is a layer of glass covering the surface of ceramic body. It has similar physical and chemical properties to glass, with dense texture, impermeable to water and air, and resistant to acid and alkali erosion. It is usually made of natural mineral raw materials and certain chemical raw materials, which melt at high temperature to form a shiny glass layer. Glazes come in various weights, and the glaze with pearlescent effect is called pearlescent glaze, which can produce a pearl-like appearance on the glaze surface, making the tile look more upscale and elegant, and can increase the decorative effect of the interior space.

[0004] Pearlescent frit is a frit with pearlescent effect. When the glaze with pearlescent frit is applied to the surface of the body and fired at high temperature, the surface of the tile can present a pearlescent effect with pearl luster, which not only meets the market demand for the aesthetic appearance of tile products, but also provides new ideas and directions for technological innovation and product upgrading in the ceramic industry, avoids the homogenization of tile products, and improves the added value of tile products. However, due to the selection of raw materials and differences in preparation processes, the existing pearlescent frit has the technical problem that the glaze of the produced tiles has a weak pearlescent effect, which limits its application. In addition, in order to control the production cost of tiles, the hierarchical structure of the existing pearlescent glazed tiles generally includes a body layer, a base glaze layer, an inkjet printing layer and a pearlescent glaze layer, and each glaze layer is a flat decorative layer. The flat surface of the decorative layer is not conducive to the presentation of the pearlescent effect in the pearlescent glaze layer, resulting in poor pearlescent effect of the existing pearlescent glazed tiles. Summary of the invention

[0005] The purpose of the present invention is to propose a pearlescent fantasy glazed tile with a three-dimensional positioning effect and a preparation method, and to add a positioning dry particle layer with a concave-convex effect at the bottom of the pearlescent frit glaze layer, so that the pearlescent frit glaze layer can produce a thickness deviation at the top of the glazed tile, thereby achieving the pearlescent fantasy effect of the glazed tile, so as to overcome the shortcomings of the prior art.

[0006] To achieve this object, the present invention adopts the following technical solutions:

[0007] A method for preparing a pearlescent colorful glazed tile with a three-dimensional positioning effect comprises the following steps:

[0008] A. preparing a ceramic blank, pressing the ceramic blank, and drying it to obtain a blank layer;

[0009] B. applying a base glaze on the top of the green body layer to obtain a base glaze layer;

[0010] C. Printing positioning glue on the top of the base glaze layer according to a preset pattern, and then spreading positioning dry particles on the top of the base glaze layer, and adsorbing and recovering the positioning dry particles that are not adhered by the positioning glue to obtain a positioning dry particle layer;

[0011] D. applying pearlescent frit glaze on the top of the positioning dry particle layer to obtain a pearlescent frit glaze layer;

[0012] E. After drying, put it into the kiln for firing, and after polishing, the pearlescent colorful glazed tiles with three-dimensional positioning effect are obtained;

[0013] In step D, the raw materials of the pearlescent frit glaze include pearlescent frit, and calculated by weight, the pearlescent frit includes the following raw materials: 30-40 parts of perlite, 10-15 parts of calcined alumina, 8-15 parts of potassium hexafluoroaluminate, 2-8 parts of zinc oxide, 5-15 parts of calcite, 5-15 parts of potassium feldspar, 3-8 parts of calcium fluoride, 1-5 parts of zirconium oxide, 5-12 parts of cerium oxide and 5-10 parts of lead carbonate.

[0014] Preferably, in step D, the temperature curve of the pearlescent melt is:

[0015] It takes 1.5 to 3 hours to rise from room temperature to 500°C;

[0016] It takes 1.5 to 2.5 hours to increase the temperature from 500°C to 1100°C;

[0017] From 1100℃ to 1550℃, it takes 0.2~0.4h;

[0018] 1550℃, keep warm for 0.1~0.2h;

[0019] It takes 0.05 to 0.1 h to reduce the temperature from 1550°C to 1450°C.

[0020] 1450℃, keep warm for 0.2~0.4h.

[0021] Preferably, the particle sizes of the perlite, the potassium hexafluoroaluminate, and the cerium oxide are all through a 325-mesh sieve, and the particle size of the zirconium oxide is through a 250-mesh sieve.

[0022] Preferably, in step D, the pearlescent frit glaze comprises the following raw materials, calculated by weight: 4-6 parts of kaolin and 94-96 parts of pearlescent frit, and according to weight percentage, the pearlescent frit glaze passes through a 325-mesh sieve with a sieve residue of 0.2-0.4%.

[0023] Preferably, in step D, the pearlescent frit glaze is applied by spraying, and the specific gravity of the pearlescent frit glaze is 1.28-1.32.

[0024] Preferably, in step C, the particle size distribution of the positioned dry particles is as follows according to mass percentage: 40% residue on a 120-140 mesh sieve, 20% residue on a 100-120 mesh sieve and 40% residue on a 80-100 mesh sieve.

[0025] Preferably, in step C, the positioning dry particles include the following raw materials, calculated by weight: 10-15 parts of quartz, 10-15 parts of calcined alumina, 5-10 parts of corundum, 30-40 parts of potassium feldspar, 5-15 parts of sodium feldspar, 2-5 parts of calcined talc, 10-15 parts of magnesium carbonate, 8-15 parts of wollastonite and 1-5 parts of zinc oxide.

[0026] Preferably, the weight of the positioning dry particles is 58-62 g / 350 mm 2 .

[0027] Preferably, in step D, the pearlescent frit comprises the following raw materials, calculated by weight: 36 parts of perlite, 13 parts of calcined alumina, 10 parts of potassium hexafluoroaluminate, 4 parts of zinc oxide, 10 parts of calcite, 10 parts of potassium feldspar, 5 parts of calcium fluoride, 2 parts of zirconium oxide, 7 parts of cerium oxide and 8 parts of lead carbonate;

[0028] In step C, the positioning dry particles include the following raw materials, calculated by weight: 13 parts of quartz, 8 parts of calcined alumina, 7 parts of corundum, 35 parts of potassium feldspar, 10 parts of sodium feldspar, 3 parts of calcined talc, 12 parts of magnesium carbonate, 10 parts of wollastonite and 2 parts of zinc oxide.

[0029] A pearlescent colorful glazed tile with a three-dimensional positioning effect is prepared using the method for preparing the pearlescent colorful glazed tile with a three-dimensional positioning effect.

[0030] The technical solution provided by the present invention may include the following beneficial effects:

[0031] 1. Perlite is used as a carrier of a layered structure, and potassium, silicon, aluminum and fluorine are introduced into the frit formula. The proportion of the above four key elements in the formula system is limited by the amount of raw materials added, so that the raw material formula of the pearlescent frit generates a mica glass body with a layered structure after the reaction. Since the generated mica glass body has the transparency of the glass phase, and the cerium oxide wrapped on its surface is white, and the above-mentioned transparency and white color characteristics are attached to the carrier with a layered structure, when the incident light is incident on the above-mentioned special carrier, it can form a strong pearlescent reflection, bringing a kind of aesthetic enjoyment to consumers.

[0032] 2. Potassium hexafluoroaluminate in the raw material of the frit can reduce the melting point of calcined alumina, so that the formula system can produce mica components at a lower calcination temperature, thereby reducing the energy consumption of frit production. The added zinc oxide and lead carbonate can be used as strong fluxing flux and crystal nucleation agent to reduce the crystallization activation energy and crystallization peak temperature, which is beneficial to the crystallization of cerium oxide and zirconium oxide, thereby further improving the pearl luster of the frit. The lead oxide after high-temperature decomposition of lead carbonate can also generate lead silicate compounds with silicon oxide in the formula system, while ensuring the fluxing performance, preventing the dissolution of a large amount of added lead.

[0033] 3. A positioning dry particle layer with a concave-convex effect is added to the bottom of the pearlescent frit glaze layer, so that the pearlescent frit glaze layer can produce a thickness deviation on the top of the glazed tile, that is, the pearlescent frit glaze layer is thinner in the protruding area of ​​the positioning dry particle layer, and thicker in the concave area of ​​the positioning dry particle layer. The above thickness deviation is conducive to promoting the pearlescent frit with a layered structure carrier to produce stronger reflection, refraction and interference under light conditions, thereby enhancing the pearlescent fantasy effect on the surface of the glazed tile. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 is a SEM image of the pearlescent frit of the present invention.

[0035] Figure 2 It is a schematic diagram of the brick surface effect of Example 1 of the present invention. DETAILED DESCRIPTION

[0036] A method for preparing a pearlescent colorful glazed tile with a three-dimensional positioning effect comprises the following steps:

[0037] A. preparing a ceramic blank, pressing the ceramic blank, and drying it to obtain a blank layer;

[0038] B. applying a base glaze on the top of the green body layer to obtain a base glaze layer;

[0039] C. Printing positioning glue on the top of the base glaze layer according to a preset pattern, and then spreading positioning dry particles on the top of the base glaze layer, and adsorbing and recovering the positioning dry particles that are not adhered by the positioning glue to obtain a positioning dry particle layer;

[0040] D. applying pearlescent frit glaze on the top of the positioning dry particle layer to obtain a pearlescent frit glaze layer;

[0041] E. After drying, put it into the kiln for firing, and after polishing, the pearlescent colorful glazed tiles with three-dimensional positioning effect are obtained;

[0042] In step D, the raw materials of the pearlescent frit glaze include pearlescent frit, and calculated by weight, the pearlescent frit includes the following raw materials: 30-40 parts of perlite, 10-15 parts of calcined alumina, 8-15 parts of potassium hexafluoroaluminate, 2-8 parts of zinc oxide, 5-15 parts of calcite, 5-15 parts of potassium feldspar, 3-8 parts of calcium fluoride, 1-5 parts of zirconium oxide, 5-12 parts of cerium oxide and 5-10 parts of lead carbonate.

[0043] In order to solve the technical problem that the pearlescent effect of the existing pearlescent frit is not strong, the technical scheme first proposes a pearlescent frit with a layered carrier structure, which is formed by wrapping the layered glassy fluoroaluminosilicate (hereinafter referred to as "mica glass") generated by the formula and having a low optical refractive index (refractive index of 1.54) with white metal oxide cerium oxide having a high refractive index (refractive index of 2.44), so as to generate a frit with a pearlescent effect; when the incident light irradiates the surface of the frit, complex refraction, reflection and interference phenomena can occur, thereby presenting a strong pearl luster. In addition, since the metal oxide wrapped on the outer surface of the mica particles is cerium oxide, and the cerium oxide crystal is a face-centered cubic crystal structure, the crystal plane parallel to the glaze surface has a low interfacial energy, so it shows strong anisotropy during the growth process, has good specular reflection characteristics for visible light, thereby forming a strong specular reflection, and the cubic zirconia crystal can form a good scattering effect on the incident light, so that the pearlescent effect of the frit is effectively enhanced. Furthermore, the raw material of the frit also contains zirconium oxide, which can generate cubic zirconium oxide crystals with a refractive index of 2.14, and assist the cerium oxide crystals to further enhance the pearlescent effect of the frit.

[0044] like Figure 1 The figure shows the SEM image of the pearlescent frit prepared by the present scheme. The gray part in the figure is cerium oxide, the black part is mica glass, and the white particles are cubic zirconia crystals. It can be seen that the essence of the pearlescent frit is cerium oxide wrapped in mica glass, and zirconium oxide crystals are present on the surface of cerium oxide.

[0045] Specifically, the technical solution uses perlite as a carrier of a layered structure, and introduces potassium, silicon, aluminum and fluorine elements into the frit formula, and limits the proportion of the above four key elements in the formula system by the amount of raw materials added, so that the raw material formula of the pearlescent frit generates a mica glass body with a layered structure after the reaction. Since the generated mica glass body has the transparency of the glass phase, and the cerium oxide wrapped on its surface is white, and the above-mentioned transparency and white color characteristics are attached to the carrier with a layered structure, when the incident light is incident on the above-mentioned special carrier, it can form a strong pearlescent reflection, bringing a kind of aesthetic enjoyment to consumers.

[0046] Furthermore, potassium hexafluoroaluminate in the raw material of the frit can reduce the melting point of calcined alumina, so that the formula system can produce mica components at a lower calcination temperature, thereby reducing the energy consumption of frit production; the added zinc oxide and lead carbonate can be used as strong fluxing flux and crystal nucleation agent, reducing the crystallization activation energy and crystallization peak temperature, which is beneficial to the crystallization of cerium oxide and zirconium oxide, thereby further improving the pearl luster of the frit. In addition, the lead oxide after high-temperature decomposition of lead carbonate can also generate lead silicate compounds with silicon oxide in the formula system, while ensuring the fluxing performance, preventing the dissolution of a large amount of added lead.

[0047] Furthermore, in order to make the glazed tiles present a pearlescent color effect, the present solution also adds a positioning dry particle layer with a concave-convex effect at the bottom of the pearlescent frit glaze layer, so that the pearlescent frit glaze layer can produce a thickness deviation on the top of the glazed tile, that is, the pearlescent frit glaze layer is thinner in the protruding area of ​​the positioning dry particle layer, and thicker in the recessed area of ​​the positioning dry particle layer. The above-mentioned thickness deviation is conducive to promoting the pearlescent frit with a layered structure carrier to produce stronger reflection, refraction and interference under light conditions, thereby enhancing the pearlescent color effect on the surface of the glazed tile.

[0048] Further, in step D, the temperature curve of the pearlescent melt is:

[0049] It takes 1.5 to 3 hours to rise from room temperature to 500°C;

[0050] It takes 1.5 to 2.5 hours to increase the temperature from 500°C to 1100°C;

[0051] From 1100℃ to 1550℃, it takes 0.2~0.4h;

[0052] 1550℃, keep warm for 0.1~0.2h;

[0053] It takes 0.05 to 0.1 h to reduce the temperature from 1550°C to 1450°C.

[0054] 1450℃, keep warm for 0.2~0.4h.

[0055] In a preferred embodiment of the present technical solution, by optimizing the temperature curve of the frit during high-temperature firing, it is beneficial to ensure that the pearlescent effect of the frit is further enhanced.

[0056] Specifically, the frit needs to be kept at 1550° for 0.1 to 0.2 hours during the high-temperature firing process. If the holding time is too long, the glass generated in the formula system will increase significantly, thereby covering the generated layered structure and easily weakening the overall pearlescent luster of the frit; if the holding time is too short, the amount of mica glass synthesized is small, making it difficult to obtain a strong pearlescent effect.

[0057] More specifically, it takes 0.05 to 0.1 h for the temperature of the frit to drop from 1550°C to 1450°C during the high-temperature firing process. If the cooling time is too short, the mica glass is not completely wrapped by the cerium oxide, which can easily weaken the overall pearl luster of the frit; if the cooling time is too long, the long-term cooling will easily lead to a decrease in the viscosity of the frit, which is not conducive to the cerium oxide crystals wrapping the mica glass, and the pearl luster will also deteriorate.

[0058] Preferably, in step D, the temperature curve of the pearlescent melt is:

[0059] It takes 2h to rise from room temperature to 500℃;

[0060] It takes 2h to increase the temperature from 500℃ to 1100℃;

[0061] From 1100℃ to 1550℃, it takes 0.3h;

[0062] 1550℃, keep warm for 0.1h;

[0063] It takes 0.05h to reduce the temperature from 1550℃ to 1450℃;

[0064] 1450℃, keep warm for 0.3h.

[0065] As a better embodiment of the above embodiment, this solution further optimizes the temperature curve of the pearlescent frit, which is conducive to achieving the best pearlescent effect of the frit.

[0066] To further illustrate, the particle sizes of the perlite, the potassium hexafluoroaluminate, and the cerium oxide all pass through a 325-mesh sieve, and the particle size of the zirconium oxide passes through a 250-mesh sieve.

[0067] The present solution also optimizes the particle sizes of perlite, potassium hexafluoroaluminate, cerium oxide and zirconium oxide, so as to make the glossiness of the pearlescent frit uniform, thereby avoiding the phenomenon of uneven flash points in the pearlescent glaze using the above-mentioned pearlescent frit.

[0068] Further, in step D, the pearlescent frit glaze includes the following raw materials, calculated by weight: 4-6 parts of kaolin and 94-96 parts of pearlescent frit, and according to weight percentage, the pearlescent frit glaze passes through a 325-mesh sieve with a sieve residue of 0.2-0.4%.

[0069] In order to effectively improve the suspension of pearlescent frit glaze containing pearlescent frit and avoid the frit from forming precipitation in the glaze slurry, this scheme also adds kaolin to the pearlescent frit glaze, which can effectively improve the suspension and water retention of the glaze slurry and improve the operability when applying the glaze.

[0070] To further illustrate, in step D, the pearlescent frit glaze is applied by spraying, and the specific gravity of the pearlescent frit glaze is 1.28-1.32.

[0071] In one embodiment of the present technical solution, the specific gravity of the pearlescent frit glaze used for spraying glaze is controlled. On the one hand, the solid content of the sprayed glaze can be increased while the spray gun is able to achieve atomization. On the other hand, the thickness deviation can be better formed at the top of the positioning dry particle layer to achieve an ideal pearlescent fantasy effect.

[0072] Preferably, the specific gravity of the pearlescent frit glaze is 1.3.

[0073] Further, in step C, the particle size distribution of the positioned dry particles is as follows according to mass percentage: 40% of the residue on a 120-140 mesh sieve, 20% of the residue on a 100-120 mesh sieve, and 40% of the residue on a 80-100 mesh sieve.

[0074] In another embodiment of the present technical solution, by optimizing the particle grading of the positioning dry particles, it has the following advantages: first, it is conducive to improving the fluidity of the positioning dry particles, and improving the convenience and stability of their application; second, it is conducive to increasing the calcination temperature of the positioning dry particles, thereby reducing the melting boundary, enhancing the three-dimensional concave-convex effect of the positioning dry particles, and further enhancing the pearlescent fantasy effect of the pearlescent frit glaze layer.

[0075] It should be noted that the positioning dry particles in this solution refer to small particles with a certain particle size distribution formed after the positioning molten block is crushed into particles of a certain fineness by a crusher.

[0076] Further, in step C, the positioning dry particles include the following raw materials, calculated by weight: 10-15 parts of quartz, 10-15 parts of calcined alumina, 5-10 parts of corundum, 30-40 parts of potassium feldspar, 5-15 parts of sodium feldspar, 2-5 parts of calcined talc, 10-15 parts of magnesium carbonate, 8-15 parts of wollastonite and 1-5 parts of zinc oxide.

[0077] In order to make the pearlescent frit glaze layer produce a stable thickness deviation, this solution needs to reduce the high temperature viscosity of the positioning dry particles to ensure the concave and convex effect formed on its surface. To this end, this solution also optimizes the raw material formula of the positioning dry particles so that the positioning dry particles after firing use corundum and cordierite as the main crystal phase, so that the positioning dry particles are not easy to melt flat during the firing process of the glazed tile, and maintain the positioning state during the laying of the material.

[0078] Further, the weight of the positioning dry particles is 58-62 g / 350 mm 2 .

[0079] In the actual production of pearlescent iridescent glazed tiles, the concave-convex effect of the positioning dry particle layer can be controlled by adjusting the gram weight of the positioning dry particles (i.e., the amount of positioning dry particles used in step D), thereby adjusting the pearlescent iridescent effect of the pearlescent frit glaze layer.

[0080] It should be noted that the gram weight of the positioned dry particles in this solution refers to the weight of the positioned dry particles in a 350mm*350mm tray.

[0081] Preferably, the weight of the positioning dry particles is 60g / 350mm 2 .

[0082] Further, in step D, the pearlite frit includes the following raw materials, calculated by weight: 36 parts of perlite, 13 parts of calcined alumina, 10 parts of potassium hexafluoroaluminate, 4 parts of zinc oxide, 10 parts of calcite, 10 parts of potassium feldspar, 5 parts of calcium fluoride, 2 parts of zirconium oxide, 7 parts of cerium oxide and 8 parts of lead carbonate;

[0083] In step C, the positioning dry particles include the following raw materials, calculated by weight: 13 parts of quartz, 8 parts of calcined alumina, 7 parts of corundum, 35 parts of potassium feldspar, 10 parts of sodium feldspar, 3 parts of calcined talc, 12 parts of magnesium carbonate, 10 parts of wollastonite and 2 parts of zinc oxide.

[0084] This scheme also provides an optimal ratio of pearlescent frit and positioning dry particles, which is conducive to achieving the best surface gloss and static friction coefficient of pearlescent fantasy glazed tiles and the strongest pearlescent fantasy effect.

[0085] A pearlescent colorful glazed tile with a three-dimensional positioning effect is prepared using the method for preparing the pearlescent colorful glazed tile with a three-dimensional positioning effect.

[0086] This solution overcomes the shortcomings of the prior art by adding a positioning dry particle layer with a concave-convex effect at the bottom of the pearlescent frit glaze layer, so that the pearlescent frit glaze layer can produce a thickness deviation on the top of the glazed tile, thereby achieving a pearlescent color effect of the glazed tile.

[0087] The technical solution of the present invention is further illustrated below through specific implementation methods.

[0088] Example 1

[0089] A. Prepare a ceramic green body, press the ceramic green body, and dry it to obtain a green body layer; wherein the green body layer is prepared from conventional green body raw materials in the ceramic field, and the chemical composition of the green body layer includes SiO2 67.85%, Al2O3 17.23%, Fe2O3 1.42%, TiO2 0.23%, CaO 1.18%, MgO 1.65%, K2O 1.85%, Na2O2.05% and ignition loss 4.3% in terms of mass percentage.

[0090] B. Applying a base glaze on the top of the green body layer to obtain a base glaze layer; wherein the base glaze layer is formed by firing a conventional base glaze in the ceramic field, and the chemical composition of the base glaze layer includes, by mass percentage, 16.73% Al2O3, 50.48% SiO2, 8.04% CaO, 5.79% MgO, 7.01% BaO, 4.85% ZnO, 3.9% K2O and 3.03% Na2O.

[0091] C. Printing positioning glue on the top of the base glaze layer according to a preset pattern, then spreading positioning dry particles on the top of the base glaze layer, and adsorbing and recovering the positioning dry particles not adhered by the positioning glue to obtain a positioning dry particle layer; wherein, the positioning dry particles include the following raw materials, calculated by weight: 13 parts of quartz, 8 parts of calcined alumina, 7 parts of corundum, 35 parts of potassium feldspar, 10 parts of sodium feldspar, 3 parts of calcined talc, 12 parts of magnesium carbonate, 10 parts of wollastonite and 2 parts of zinc oxide, and the weight of the positioning dry particles is 60g / 350mm 2 .

[0092] D. Spraying pearlescent frit glaze on the top of the positioning dry particle layer to obtain a pearlescent frit glaze layer; wherein, calculated by weight, the raw materials of the pearlescent frit glaze include 5 parts of kaolin and 95 parts of pearlescent frit, and according to weight percentage, the pearlescent frit glaze passes through a 325 mesh sieve, with a sieve residue of 0.2-0.4%, and a specific gravity of 1.3; calculated by weight, the pearlescent frit includes the following raw materials: 36 parts of perlite passing through a 325 mesh sieve, 13 parts of calcined alumina, 10 parts of potassium hexafluoroaluminate passing through a 325 mesh sieve, 4 parts of zinc oxide, 10 parts of calcite, 10 parts of potassium feldspar, 5 parts of calcium fluoride, 2 parts of zirconium oxide passing through a 250 mesh sieve, 7 parts of cerium oxide passing through a 325 mesh sieve, and 8 parts of lead carbonate. In addition, the temperature curve of the pearlescent frit is:

[0093] It takes 2h to rise from room temperature to 500℃;

[0094] It takes 2h to increase the temperature from 500℃ to 1100℃;

[0095] From 1100℃ to 1550℃, it takes 0.3h;

[0096] 1550℃, keep warm for 0.1h;

[0097] It takes 0.05h to reduce the temperature from 1550℃ to 1450℃;

[0098] 1450℃, keep warm for 0.3h.

[0099] E. After drying, the tiles are put into kiln for firing. After polishing, the tiles with pearlescent colorful glaze and three-dimensional positioning effect are obtained. The schematic diagram of the tile surface effect is as follows: Figure 2 shown.

[0100] Example 2

[0101] A. Prepare a ceramic green body, press the ceramic green body, and dry it to obtain a green body layer; wherein the green body layer is prepared from conventional green body raw materials in the ceramic field, and the chemical composition of the green body layer includes SiO2 67.85%, Al2O3 17.23%, Fe2O3 1.42%, TiO2 0.23%, CaO 1.18%, MgO 1.65%, K2O 1.85%, Na2O2.05% and ignition loss 4.3% in terms of mass percentage.

[0102] B. Applying a base glaze on the top of the green body layer to obtain a base glaze layer; wherein the base glaze layer is formed by firing a conventional base glaze in the ceramic field, and the chemical composition of the base glaze layer includes, by mass percentage, 16.73% Al2O3, 50.48% SiO2, 8.04% CaO, 5.79% MgO, 7.01% BaO, 4.85% ZnO, 3.9% K2O and 3.03% Na2O.

[0103] C. Printing positioning glue on the top of the base glaze layer according to a preset pattern, then spreading positioning dry particles on the top of the base glaze layer, and adsorbing and recovering the positioning dry particles that are not adhered by the positioning glue to obtain a positioning dry particle layer; wherein, the positioning dry particles include the following raw materials, calculated by weight: 15 parts of quartz, 15 parts of calcined alumina, 5 parts of corundum, 40 parts of potassium feldspar, 5 parts of sodium feldspar, 5 parts of burned talc, 10 parts of magnesium carbonate, 15 parts of wollastonite and 5 parts of zinc oxide, and the weight of the positioning dry particles is 58g / 350mm 2 .

[0104] D. Spraying pearlescent frit glaze on the top of the positioning dry particle layer to obtain a pearlescent frit glaze layer; wherein, calculated by weight, the raw materials of the pearlescent frit glaze include 5 parts of kaolin and 95 parts of pearlescent frit, and according to weight percentage, the pearlescent frit glaze passes through a 325 mesh sieve, the residue is 0.2-0.4%, and the specific gravity is 1.3; calculated by weight, the pearlescent frit includes the following raw materials: 30 parts of perlite passing through a 325 mesh sieve, 10 parts of calcined alumina, 8 parts of potassium hexafluoroaluminate passing through a 325 mesh sieve, 2 parts of zinc oxide, 5 parts of calcite, 5 parts of potassium feldspar, 3 parts of calcium fluoride, 1 part of zirconium oxide passing through a 250 mesh sieve, 5 parts of cerium oxide passing through a 325 mesh sieve, and 5 parts of lead carbonate. In addition, the temperature curve of the pearlescent frit is:

[0105] It takes 1.5h to rise from room temperature to 500℃;

[0106] It takes 2.5 hours to increase the temperature from 500°C to 1100°C;

[0107] From 1100℃ to 1550℃, it takes 0.4h;

[0108] 1550℃, keep warm for 0.1h;

[0109] It takes 0.1h to reduce the temperature from 1550℃ to 1450℃;

[0110] 1450℃, keep warm for 0.4h.

[0111] E. After drying, it is put into the kiln for firing, and after polishing, a pearlescent colorful glazed tile with a three-dimensional positioning effect is obtained.

[0112] Example 3

[0113] A. Prepare a ceramic green body, press the ceramic green body, and dry it to obtain a green body layer; wherein the green body layer is prepared from conventional green body raw materials in the ceramic field, and the chemical composition of the green body layer includes SiO2 67.85%, Al2O3 17.23%, Fe2O3 1.42%, TiO2 0.23%, CaO 1.18%, MgO 1.65%, K2O 1.85%, Na2O2.05% and ignition loss 4.3% in terms of mass percentage.

[0114] B. Applying a base glaze on the top of the green body layer to obtain a base glaze layer; wherein the base glaze layer is formed by firing a conventional base glaze in the ceramic field, and the chemical composition of the base glaze layer includes, by mass percentage, 16.73% Al2O3, 50.48% SiO2, 8.04% CaO, 5.79% MgO, 7.01% BaO, 4.85% ZnO, 3.9% K2O and 3.03% Na2O.

[0115] C. Printing positioning glue on the top of the base glaze layer according to a preset pattern, and then spreading positioning dry particles on the top of the base glaze layer, and adsorbing and recovering the positioning dry particles that are not adhered by the positioning glue to obtain a positioning dry particle layer; wherein, the positioning dry particles include the following raw materials, calculated by weight: 10 parts of quartz, 10 parts of calcined alumina, 10 parts of corundum, 30 parts of potassium feldspar, 15 parts of sodium feldspar, 2 parts of calcined talc, 15 parts of magnesium carbonate, 8 parts of wollastonite and 1 part of zinc oxide, and the weight of the positioning dry particles is 62g / 350mm 2 .

[0116] D. Spraying pearlescent frit glaze on the top of the positioning dry particle layer to obtain a pearlescent frit glaze layer; wherein, calculated by weight, the raw materials of the pearlescent frit glaze include 5 parts of kaolin and 95 parts of pearlescent frit, and according to weight percentage, the pearlescent frit glaze passes through a 325 mesh sieve, the residue is 0.2-0.4%, and the specific gravity is 1.3; calculated by weight, the pearlescent frit includes the following raw materials: 40 parts of perlite passing through a 325 mesh sieve, 15 parts of calcined alumina, 15 parts of potassium hexafluoroaluminate passing through a 325 mesh sieve, 8 parts of zinc oxide, 15 parts of calcite, 15 parts of potassium feldspar, 8 parts of calcium fluoride, 5 parts of zirconium oxide passing through a 250 mesh sieve, 12 parts of cerium oxide passing through a 325 mesh sieve, and 10 parts of lead carbonate. In addition, the temperature curve of the pearlescent frit is:

[0117] It takes 3h to rise from room temperature to 500℃;

[0118] It takes 1.5h to increase the temperature from 500℃ to 1100℃;

[0119] From 1100℃ to 1550℃, it takes 0.2h;

[0120] 1550℃, keep warm for 0.2h;

[0121] It takes 0.05h to reduce the temperature from 1550℃ to 1450℃;

[0122] 1450℃, keep warm for 0.2h.

[0123] E. After drying, it is put into the kiln for firing, and after polishing, a pearlescent colorful glazed tile with a three-dimensional positioning effect is obtained.

[0124] Comparative Example

[0125] a. preparing a ceramic green body, pressing the ceramic green body, and drying it to obtain a green body layer; wherein the green body layer is prepared from conventional green body raw materials in the ceramic field, and the chemical composition of the green body layer includes, by mass percentage, SiO2 67.85%, Al2O3 17.23%, Fe2O3 1.42%, TiO2 0.23%, CaO 1.18%, MgO 1.65%, K2O 1.85%, Na2O2.05% and a loss on ignition of 4.3%.

[0126] b. Applying a bottom glaze on the top of the green body layer to obtain a bottom glaze layer; wherein the bottom glaze layer is formed by firing a conventional bottom glaze in the ceramic field, and the chemical composition of the bottom glaze layer includes Al2O3 16.73%, SiO2 50.48%, CaO8.04%, MgO 5.79%, BaO 7.01%, ZnO 4.85%, K2O 3.9% and Na2O3.03% in terms of mass percentage.

[0127] c. Spraying pearlescent frit glaze on the top of the base glaze layer to obtain a pearlescent frit glaze layer; wherein, calculated by weight, the raw materials of the pearlescent frit glaze include 5 parts of kaolin and 95 parts of pearlescent frit, and according to weight percentage, the pearlescent frit glaze passes through a 325 mesh sieve, with a sieve residue of 0.2-0.4%, and a specific gravity of 1.3; calculated by weight, the pearlescent frit includes the following raw materials: 30 parts of perlite passing through a 325 mesh sieve, 10 parts of calcined alumina, 8 parts of potassium hexafluoroaluminate passing through a 325 mesh sieve, 2 parts of zinc oxide, 5 parts of calcite, 5 parts of potassium feldspar, 3 parts of calcium fluoride, 1 part of zirconium oxide passing through a 250 mesh sieve, 5 parts of cerium oxide passing through a 325 mesh sieve, and 5 parts of lead carbonate. In addition, the temperature curve of the pearlescent frit is:

[0128] It takes 1.5h to rise from room temperature to 500℃;

[0129] It takes 2.5 hours to increase the temperature from 500°C to 1100°C;

[0130] From 1100℃ to 1550℃, it takes 0.4h;

[0131] 1550℃, keep warm for 0.1h;

[0132] It takes 0.1h to reduce the temperature from 1550℃ to 1450℃;

[0133] 1450℃, keep warm for 0.4h.

[0134] d. After drying, put it into the kiln for firing, and after polishing, you can get glazed tiles.

[0135] The glazed tiles prepared in Examples 1-3 and the comparative example were subjected to conventional glossiness tests and static friction coefficient tests in the field of architectural ceramics. The results are shown in Table 1 below:

[0136] Table 1 Performance test results of glazed tiles of Examples 1-3 and Comparative Examples

[0137]

[0138] The pearlescent iridescent glazed tiles proposed in this scheme add a positioning dry particle layer with a concave-convex effect at the bottom of the pearlescent frit glaze layer, so that the pearlescent frit glaze layer can produce a thickness deviation on the top of the glazed tiles, thereby achieving the pearlescent iridescent effect of the glazed tiles; at the same time, the positioning dry particle layer with a concave-convex effect can also give the glazed tiles a certain anti-slip performance.

[0139] The technical principle of the present invention is described above in conjunction with specific embodiments. These descriptions are only for explaining the principle of the present invention and cannot be interpreted as limiting the scope of protection of the present invention in any way. Based on the explanations herein, those skilled in the art can associate other specific implementations of the present invention without paying creative labor, and these methods will fall within the scope of protection of the present invention.

Claims

1. A method for preparing pearlescent colorful glazed tiles with a three-dimensional positioning effect, characterized in that: The following steps are involved: A. preparing a ceramic blank, pressing the ceramic blank, and drying it to obtain a blank layer; B. applying a base glaze on the top of the green body layer to obtain a base glaze layer; C. Printing positioning glue on the top of the base glaze layer according to a preset pattern, and then spreading positioning dry particles on the top of the base glaze layer, and adsorbing and recovering the positioning dry particles that are not adhered by the positioning glue to obtain a positioning dry particle layer; D. applying pearlescent frit glaze on the top of the positioning dry particle layer to obtain a pearlescent frit glaze layer; E. After drying, put it into the kiln for firing, and after polishing, the pearlescent colorful glazed tiles with three-dimensional positioning effect are obtained; In step D, the raw materials of the pearlescent frit glaze include pearlescent frit, and calculated by weight, the pearlescent frit includes the following raw materials: 30-40 parts of perlite, 10-15 parts of calcined alumina, 8-15 parts of potassium hexafluoroaluminate, 2-8 parts of zinc oxide, 5-15 parts of calcite, 5-15 parts of potassium feldspar, 3-8 parts of calcium fluoride, 1-5 parts of zirconium oxide, 5-12 parts of cerium oxide and 5-10 parts of lead carbonate.

2. The method for preparing a pearlescent colorful glazed tile with a three-dimensional positioning effect according to claim 1, characterized in that: In step D, the temperature curve of the pearlescent melt is: It takes 1.5 to 3 hours to rise from room temperature to 500°C; It takes 1.5 to 2.5 hours to increase the temperature from 500°C to 1100°C; From 1100℃ to 1550℃, it takes 0.2~0.4h; 1550℃, keep warm for 0.1~0.2h; It takes 0.05 to 0.1 h to reduce the temperature from 1550°C to 1450°C. 1450℃, keep warm for 0.2~0.4h.

3. The method for preparing a pearlescent colorful glazed tile with a three-dimensional positioning effect according to claim 1, characterized in that: The particle sizes of the perlite, the potassium hexafluoroaluminate, and the cerium oxide all pass through a 325-mesh sieve, and the particle size of the zirconium oxide passes through a 250-mesh sieve.

4. The method for preparing a pearlescent colorful glazed tile with a three-dimensional positioning effect according to claim 1, characterized in that: In step D, the pearlescent frit glaze comprises the following raw materials, calculated by weight: 4-6 parts of kaolin and 94-96 parts of pearlescent frit, and according to weight percentage, the pearlescent frit glaze passes through a 325-mesh sieve with a sieve residue of 0.2-0.4%.

5. The method for preparing a pearlescent colorful glazed tile with a three-dimensional positioning effect according to claim 1, characterized in that: In step D, the pearlescent frit glaze is applied by spraying, and the specific gravity of the pearlescent frit glaze is 1.28-1.

32.

6. The method for preparing a pearlescent colorful glazed tile with a three-dimensional positioning effect according to claim 1, characterized in that: In step C, the particle size distribution of the positioned dry particles is as follows according to mass percentage: 40% of the residue on a 120-140 mesh sieve, 20% of the residue on a 100-120 mesh sieve, and 40% of the residue on a 80-100 mesh sieve.

7. The method for preparing a pearlescent colorful glazed tile with a three-dimensional positioning effect according to claim 1, characterized in that: In step C, the positioning dry particles include the following raw materials, calculated by weight: 10 to 15 parts of quartz, 10 to 15 parts of calcined alumina, 5 to 10 parts of corundum, 30 to 40 parts of potassium feldspar, 5 to 15 parts of sodium feldspar, 2 to 5 parts of calcined talc, 10 to 15 parts of magnesium carbonate, 8 to 15 parts of wollastonite and 1 to 5 parts of zinc oxide.

8. The method for preparing a pearlescent colorful glazed tile with a three-dimensional positioning effect according to claim 1, characterized in that: The weight of the positioning dry particles is 58-62 g / 350 mm 2 .

9. The method for preparing a pearlescent colorful glazed tile with a three-dimensional positioning effect according to claim 7, characterized in that: In step D, the pearlite frit includes the following raw materials, calculated by weight: 36 parts of perlite, 13 parts of calcined alumina, 10 parts of potassium hexafluoroaluminate, 4 parts of zinc oxide, 10 parts of calcite, 10 parts of potassium feldspar, 5 parts of calcium fluoride, 2 parts of zirconium oxide, 7 parts of cerium oxide and 8 parts of lead carbonate; In step C, the positioning dry particles include the following raw materials, calculated by weight: 13 parts of quartz, 8 parts of calcined alumina, 7 parts of corundum, 35 parts of potassium feldspar, 10 parts of sodium feldspar, 3 parts of calcined talc, 12 parts of magnesium carbonate, 10 parts of wollastonite and 2 parts of zinc oxide.

10. A pearlescent colorful glazed tile with a three-dimensional positioning effect, characterized in that: The pearlescent colorful glazed tile with a three-dimensional positioning effect is prepared using the preparation method of any one of claims 1 to 9.

Citation Information

Patent Citations

  • Metallic luster glaze and preparation method thereof

    CN106587624A

  • Ceramic frit, ceramic dry granular glaze and ceramic tile

    CN114477765A

  • Glazed rock plate with embossing effect and preparation method thereof

    CN118084508A

  • Digital positioning matte dry granular glaze marble tile and preparation method thereof

    CN118164787A

  • Pigment compositions with improved sparking effect

    US20110237683A1

Cited By

  • Silver foil dry granular glaze, ceramic tile with silver foil decorative effect and preparation method of ceramic tile

    CN119569338A