Lithium ion battery tab structure and riveting process of lithium ion battery tab structure and rivet

By adopting multi-layered polar ear structure and ultrasonic welding technology in lithium battery manufacturing, the tight fit and precise riveting of the extreme ears are achieved, solving the problems of bending and hole drilling in traditional riveting methods, and improving the battery Performance and safety reduce production costs and improve efficiency.

CN118943670APending Publication Date: 2024-11-12PHYLION BATTERY (CHUZHOU) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410982140.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-22
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The punching and riveting method of the pole ear in traditional lithium battery manufacturing can easily lead to problems such as bending, leaking hole punching, and biasing rivets, which affects battery performance and safety, and is low in production efficiency and high cost, making it difficult to adapt to large-scale production.

Method used

The polar ear structure with a multi-layered arrangement is fully fitted by ultrasonic welding, and then drilled and riveted to ensure the close connection of the riveted ends. Use appropriate riveted holes and rivets to improve riveting accuracy and firmness.

Benefits of technology

It reduces the internal resistance of the battery, improves battery performance and safety, reduces the generation of bad products, improves production efficiency and reduces costs, is suitable for large-scale production, and simplifies the rework process and improves the overall performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118943670A_ABST
    Figure CN118943670A_ABST
Patent Text Reader

Abstract

The invention discloses a lithium ion battery tab structure and a riveting process of the lithium ion battery tab structure and a rivet, and the riveting process comprises the following steps: S1, preparing a battery cell which is provided with the tab structure, and the tab structure comprises a plurality of tabs which are stacked; s2, the tabs are put into an ultrasonic welding machine for ultrasonic welding, and the multiple stacked tabs are attached together through ultrasonic welding; s3, punching holes in the attached tabs by using a punching machine; and S4, riveting the tab and the rivet by using riveting equipment. Due to the introduction of the ultrasonic welding process, the tabs are completely attached together through ultrasonic welding, so that the tabs are connected more firmly, battery scrapping caused by connection problems is reduced, the one-time yield of the batteries is improved, the production cost is reduced, meanwhile, the production efficiency is also improved, and large-scale production is facilitated.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of lithium battery manufacturing, and in particular to a lithium ion battery pole ear structure and a riveting process thereof with a rivet. Background Art

[0002] Lithium-ion batteries are widely used in various portable electronic devices, electric vehicles and other fields due to their high energy density, long cycle life and environmental protection. In the manufacturing process of lithium-ion batteries, battery connection technology is a very critical link, which directly affects the performance and safety of the battery. Among them, the connection method of the tabs has an important impact on the performance of the battery. The traditional tab connection method is mainly through punching and riveting. Although this method is simple and fast, it is prone to problems such as tab bending, missing punching, and rivet penetration. This will not only affect the performance of the battery, but may also cause battery safety problems.

[0003] To solve these problems, the existing solution is to directly perform punching and riveting after short circuit testing. Although this method is simple and easy to implement, due to factors such as the material and shape of the tab, the punching and riveting process may cause problems such as tab bending, missing holes, and rivet deviation. In addition, this method may also cause the internal resistance of the battery to be too high, thereby affecting the performance of the battery.

[0004] Therefore, there are some problems and shortcomings in the existing riveting process for lithium battery manufacturing. First, the method of drilling and riveting directly after short circuit measurement may cause problems such as bending of the pole ears, missing holes, and rivet penetration, which will not only affect the performance of the battery, but also may cause battery safety problems. Secondly, this method may cause the internal resistance of the battery to be too high, thereby affecting the performance of the battery. Finally, this method has low production efficiency and high cost, which is not conducive to large-scale production. Therefore, how to improve the riveting process for lithium battery manufacturing, improve battery performance and safety, reduce production costs, and improve production efficiency is a problem that needs to be solved urgently in the current lithium battery manufacturing field. Summary of the invention

[0005] In order to overcome the above disadvantages, one of the purposes of the present invention is to provide a lithium-ion battery tab structure that can reduce the internal resistance of the battery and improve the performance of the battery.

[0006] In order to achieve the above purpose, the technical solution adopted by the present invention is: a lithium-ion battery tab structure, including a tab family connected to a battery cell, the tab family including a plurality of tabs arranged in layers, the tabs being used to connect the battery cell and the rivet, and each tab having an end away from the battery cell and the tab adjacent thereto being bonded together to form a riveted end. Since the tabs are completely bonded together, there will be no defects such as tab bending, missing holes, and rivet penetration during subsequent punching, thereby reducing the internal resistance of the battery and improving the performance of the battery.

[0007] After the tabs are fully fitted, the normal punching and riveting processes will be more precise during the later stages because the tabs are fully fitted, and there will be no adverse effects caused by loose tabs.

[0008] Furthermore, the tabs at the riveted ends are tightly fitted together to form a whole.

[0009] Furthermore, a riveting hole is provided on the riveting end, the riveting hole is used for riveting with a rivet, and the diameter of the riveting hole is matched with the diameter of the rivet.

[0010] Further, the diameter of the rivet hole is 5-10 mm. Exemplarily, the diameter of the rivet hole is 5 mm, 6 mm, 7 mm, 8 mm, 9 mm, 10 mm or a range consisting of any two thereof.

[0011] Furthermore, the material of the tab is aluminum foil, with a thickness of 0.05-0.15 mm and a width of 50 mm. For example, the thickness is 0.05 mm, 0.10 mm, 0.15 mm or a range consisting of any two of them.

[0012] Another object of the present invention is to provide a riveting process for a lithium-ion battery tab and a rivet, comprising the following steps:

[0013] S1. Prepare a battery cell, wherein the battery cell has a tab structure as described above, and the tab structure includes a plurality of tabs stacked in layers;

[0014] S2, placing the tabs in an ultrasonic welding machine for ultrasonic welding, so that the tabs stacked together are bonded together by ultrasonic welding;

[0015] S3, punching holes on the fitted tabs with a punching machine;

[0016] S4. Use riveting equipment to rivet the tabs and rivets.

[0017] Furthermore, S1 also includes the following steps: placing the tab in a short circuit tester for testing, recording the test results, and ensuring that the electrical performance of the tab is normal;

[0018] Furthermore, S4 also includes the following steps: performing a short-circuit test on the riveted tab again, and after the test is completed, recording the test result to ensure that the electrical performance of the tab is normal.

[0019] Furthermore, in the short circuit test, the test voltage is 5V, the current is 1A, and the test time is 3 seconds.

[0020] Further, in S2, the ultrasonic frequency is 20 kHz, the welding pressure is 0.5-1.5 MPa, and the welding time is 1-5 seconds. For example, the welding pressure is 0.5 MPa, 1.0 MPa, 1.5 MPa, and the welding time is 1 second, 2 seconds, 3 seconds, 4 seconds, and 5 seconds.

[0021] Further, in S4, the diameter of the rivet is 5-10mm, the riveting height of the positive pole tab is 10.45-10.65mm, and the riveting height of the negative pole tab is 10.35-10.45mm. Exemplarily, the diameter of the rivet is 5mm, 6mm, 7mm, 8mm, 9mm, 10mm, or a range consisting of any two thereof, the riveting height of the positive pole tab is 10.45mm, 10.50mm, 10.55mm, 10.60mm, 10.65mm, or a range consisting of any two thereof, and the riveting height of the negative pole tab is 10.35mm, 10.40mm, 10.45mm, or a range consisting of any two thereof.

[0022] The beneficial effects of the present invention are:

[0023] 1) Reduce internal resistance: Since the tabs are completely fitted together, there will be no defects such as tab bending, missing holes, and rivet deviation during subsequent punching, thereby reducing the internal resistance of the battery and improving the performance of the battery.

[0024] 2) Reduce the occurrence of defects: After the tabs are fully fitted, the normal punching and riveting processes will be more precise during the later stages because the tabs are fully fitted, and there will be no defects caused by loose tabs.

[0025] 3) Improve production efficiency and reduce costs: The original riveting process will produce poor battery cells due to loose tabs, easy tab bending, missing holes, and rivet penetration during the manufacturing process. Due to the introduction of ultrasonic welding technology, the tabs are completely fitted together by ultrasonic welding, making the connection of the tabs more secure, thereby reducing battery scrapping caused by connection problems, improving the primary yield of the battery, reducing production costs, and also improving production efficiency, which is conducive to large-scale production.

[0026] 4) Improve production capacity: Due to the introduction of ultrasonic welding technology, the connection of the tabs is more secure (the original riveting process makes the tabs loosely stressed in a single layer, and after ultrasonic welding, the tabs are riveted together and evenly stressed), thereby reducing battery scrapping due to connection problems, improving the battery's first-time yield, and thus increasing production capacity.

[0027] 5) Facilitates repair: When repairing a battery with poor welding, the battery needs to be disassembled: break the shell - disassemble the cover - re-rivet; when disassembling the cover, the original riveted tabs are loose and easy to break (the endurance of the single tab is too low), causing the battery to be scrapped and wasted. During the secondary riveting, the aperture and the rivet cannot be 100% tightly matched (external force will cause the single or multiple tabs to deform), resulting in high contact internal resistance of the battery and reduced overall battery performance. The tabs are also easy to break and damage due to looseness, resulting in scrapping. By adding an ultrasonic welding process before punching, the tabs can be perfectly fitted together. When the battery is repaired after welding, the tabs are fitted together when the cover plate is disassembled, which makes it less likely to cause single-layer or multi-layer damage to the tabs (due to uniform force and increased endurance). It is also easier to rivet and rivet in the re-riveting process, avoiding tab damage, rivet deviation and other defects. There is no shape change caused by external force on the aperture (the tabs are fitted together to increase endurance), and they are perfectly matched with the rivets to reduce the contact internal resistance and improve the overall performance of the battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] The drawings constituting a part of this application are used to provide a further understanding of the present invention. The illustrative embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute improper limitations on the present invention.

[0029] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the following briefly introduces the drawings required for use in the description of the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.

[0030] Figure 1 It is a schematic diagram of the traditional tab structure;

[0031] Figure 2 It is a side view of the structure of the pole ear of the present invention;

[0032] Figure 3 This is a front view of the structure of the pole ear of the present invention;

[0033] Figure 4 It is a comparison diagram of the traditional pole ear structure and the pole ear structure of the present invention, wherein Figure a is a diagram of the traditional pole ear structure and the state before rivet riveting, and Figure b is a diagram of the pole ear structure of the present invention and the state before rivet riveting.

[0034] Among them: 1. Battery cell; 2. Tab family; 3. Tab; 4. Riveted end; 5. Riveted hole. DETAILED DESCRIPTION

[0035] In order to make the above-mentioned purpose, features and advantages of the present invention more obvious and easy to understand, the specific embodiments of the present invention are described in detail below. In the following description, many specific details are set forth to facilitate a full understanding of the present invention. However, the present invention can be implemented in many other ways different from those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present invention, so the present invention is not limited by the specific embodiments disclosed below.

[0036] Except as shown in the operating examples or otherwise indicated, all numbers used in the specification and claims to indicate the amount of ingredients, physicochemical properties, etc. are understood to be adjusted by the term "about" in all cases. Therefore, unless otherwise indicated, the numerical parameters listed in the above specification and the attached claims are approximate values, and those skilled in the art can use the teachings disclosed herein to seek to obtain the desired properties and appropriately change these approximate values. The use of numerical ranges expressed as endpoints includes all numbers within the range and any range within the range, for example, 1 to 5 includes 1, 1.1, 1.3, 1.5, 2, 2.75, 3, 3.80, 4 and 5, etc.

[0037] The applicant found that the traditional connection method of the pole ear 3 is mainly through punching and riveting. Although this method is simple and fast, it is prone to problems such as bending of the pole ear 3, missing punching, and rivet penetration, which will not only affect the performance of the battery, but may also cause battery safety problems.

[0038] See attached Figure 2 As shown, an embodiment of the present invention provides a lithium-ion battery tab structure, including a tab group 2 connected to a battery cell 1, the tab group 2 including a plurality of tabs 3 stacked, the tabs 3 used to connect the battery cell 1 and the rivet, and one end of each tab 3 away from the battery cell 1 is fitted together with the tab 3 adjacent thereto to form a riveted end 4. The tabs 3 located at the riveted end 4 can be tightly fitted to form a whole without external pressure.

[0039] The main method of connecting the tabs is through punching and riveting. Figure 1 As shown, the end of the conventional pole lug 3 away from the battery cell 1 is also an independent sheet structure. Since the pole lug 3 is relatively thin, the pole lug 3 is prone to bending, missing holes, and rivet penetration deviation during the process of punching each pole lug 3. The present application arranges the pole lugs 3 to be fitted with each other before punching to form a whole, thereby increasing the thickness of the pole lug 3 at the riveted end 4 during punching and overcoming the problem of the pole lug 3 being easily bent. Since only one hole needs to be punched on the pole lug 3 at the riveted end 4, the problems of missing holes and rivet penetration deviation during the punching of the pole lug 3 are overcome, thereby improving the performance of the battery and improving the safety of the battery.

[0040] See attached Figure 3 As shown, in some embodiments, a riveting hole 5 is provided on the riveting end 4, and the riveting hole 5 is used for riveting with a rivet, and the diameter of the riveting hole 5 is adapted to the diameter of the rivet, the aperture of the riveting hole 5 is 5-10mm, the diameter of the rivet is 5-10mm, the riveting height of the positive electrode tab 3 is 10.45-10.65mm, and the riveting height of the negative electrode tab 3 is 10.35-10.45mm.

[0041] In some embodiments, the tab 3 is made of aluminum foil with a thickness of 0.05-0.15 mm and a width of 50 mm.

[0042] An embodiment of the present invention provides a riveting process for a lithium-ion battery tab and a rivet to solve the above problem, which specifically includes the following steps:

[0043] S1, preparing a cleaned and dried lithium battery cell 1, wherein the cell 1 has the above-mentioned tab structure, and the tab structure includes a plurality of stacked tabs 3;

[0044] The material of the tab is aluminum foil with a thickness of 0.1mm and a width of 50mm. Put the tab into the short circuit tester, set the test voltage to 5V, the current to 1A, and the test time to 3 seconds. After the test is completed, record the test results to ensure that the electrical performance of the tab is normal.

[0045] S2. Place the tabs 3 in an ultrasonic welding machine for ultrasonic welding. Through ultrasonic welding, several stacked tabs 3 are bonded together to form riveted ends 4. Ultrasonic welding is a process that uses high-frequency vibration waves to transmit to the surfaces of two objects to be welded, and under pressure, the surfaces of the two objects are rubbed against each other to form a fusion between molecular layers. By adding the ultrasonic welding process, this process can make the tabs 3 fit together completely, avoiding the problems of tab 3 bending, missing holes, and rivet penetration that may occur in the subsequent punching process.

[0046] In some embodiments, in the welding process, the ultrasonic frequency is 20 kHz, the welding pressure is 0.5-1.5 MPa, and the welding time is 1-5 seconds. Preferably, the ultrasonic welding pressure is 1 MPa, and the welding time is 2 seconds.

[0047] S3, punching holes on the fitted tab 3 with a punching machine; the diameter of the holes punched by the punching machine on the tab 3 is 5-10 mm.

[0048] S4. Use riveting equipment to rivet the tab 3 and the rivet. The diameter of the rivet is 5-10mm, the riveting height of the positive tab 3 is 10.45-10.65mm, and the riveting height of the negative tab 3 is 10.35-10.45mm. Perform a short-circuit test on the riveted tab again, with a test voltage of 5V, a current of 1A, and a test time of 3 seconds. After the test is completed, record the test results to ensure that the electrical performance of the tab is normal.

[0049] Through the above steps, the internal resistance of the battery can be effectively reduced and the performance of the battery can be improved. At the same time, since the production of defective products is reduced, the production efficiency is greatly improved, the production cost is reduced, and it is suitable for large-scale production.

[0050] Example

[0051] The following examples describe the disclosure of the present invention in more detail, and these examples are intended for illustrative purposes only, as various modifications and variations within the scope of the disclosure of the present invention will be apparent to those skilled in the art. Unless otherwise stated, all parts, percentages, and ratios reported in the following examples are by weight, and all reagents used in the examples are commercially available or synthesized according to conventional methods and can be used directly without further processing, and the instruments used in the examples are commercially available.

[0052] Example 1

[0053] A riveting process for a lithium-ion battery tab and a rivet, specifically comprising the following steps:

[0054] S1. Prepare a cleaned and dried lithium battery cell, wherein the cell has a tab structure as described above, and the tab structure comprises a plurality of tabs stacked in layers;

[0055] The material of the tab is aluminum foil with a thickness of 0.1mm and a width of 50mm. Put the tab into the short circuit tester, set the test voltage to 5V, the current to 1A, and the test time to 3 seconds. After the test is completed, record the test results to ensure that the electrical performance of the tab is normal.

[0056] S2. Place the tab into an ultrasonic welding machine for ultrasonic welding. In the welding process, the ultrasonic frequency is 20 kHz, the welding pressure is 1 MPa, and the welding time is 2 seconds.

[0057] S3. Use a punching machine to punch holes on the fitted tabs; the diameter of the holes punched by the punching machine on the tabs is 8 mm.

[0058] S4. Use riveting equipment to rivet the tabs and rivets. The diameter of the rivet is 8mm, the riveting height of the positive tab is 10.45mm, and the riveting height of the negative tab is 10.35mm. Perform a short-circuit test on the riveted tabs again, with a test voltage of 5V, a current of 1A, and a test time of 3 seconds. After the test is completed, record the test results to ensure that the electrical performance of the tabs is normal.

[0059] Example 2

[0060] A riveting process for a lithium-ion battery tab and a rivet, specifically comprising the following steps:

[0061] S1. Prepare a cleaned and dried lithium battery cell, wherein the cell has a tab structure as described above, and the tab structure comprises a plurality of tabs stacked in layers;

[0062] The material of the tab is aluminum foil with a thickness of 0.05mm and a width of 50mm. Put the tab into the short circuit tester, set the test voltage to 5V, the current to 1A, and the test time to 3 seconds. After the test is completed, record the test results to ensure that the electrical performance of the tab is normal.

[0063] S2. Place the tab into an ultrasonic welding machine for ultrasonic welding. In the welding process, the ultrasonic frequency is 20 kHz, the welding pressure is 0.5 MPa, and the welding time is 5 seconds.

[0064] S3. Use a punching machine to punch holes on the fitted tabs; the diameter of the holes punched by the punching machine on the tabs is 5 mm.

[0065] S4. Use riveting equipment to rivet the tabs and rivets. The diameter of the rivet is 5mm, the riveting height of the positive tab is 10.65mm, and the riveting height of the negative tab is 10.45mm. Perform a short-circuit test on the riveted tabs again, with a test voltage of 5V, a current of 1A, and a test time of 3 seconds. After the test is completed, record the test results to ensure that the electrical performance of the tabs is normal.

[0066] Example 3

[0067] A riveting process for a lithium-ion battery tab and a rivet, specifically comprising the following steps:

[0068] S1. Prepare a cleaned and dried lithium battery cell, wherein the cell has a tab structure as described above, and the tab structure comprises a plurality of tabs stacked in layers;

[0069] The material of the tab is aluminum foil with a thickness of 0.05mm and a width of 50mm. Put the tab into the short circuit tester, set the test voltage to 5V, the current to 1A, and the test time to 3 seconds. After the test is completed, record the test results to ensure that the electrical performance of the tab is normal.

[0070] S2. Place the tab into an ultrasonic welding machine for ultrasonic welding. In the welding process, the ultrasonic frequency is 20 kHz, the welding pressure is 1.5 MPa, and the welding time is 1 second.

[0071] S3. Use a punching machine to punch holes on the fitted tabs; the diameter of the holes punched by the punching machine on the tabs is 10 mm.

[0072] S4. Use riveting equipment to rivet the tabs and rivets. The diameter of the rivet is 10mm, the riveting height of the positive tab is 10.65mm, and the riveting height of the negative tab is 10.45mm. Perform a short-circuit test on the riveted tabs again, with a test voltage of 5V, a current of 1A, and a test time of 3 seconds. After the test is completed, record the test results to ensure that the electrical performance of the tabs is normal.

[0073] Comparative Example 1

[0074] The riveting process of Comparative Example 1 is basically the same as that of Example 1, the main difference being that ultrasonic welding is not performed on the tab, and the end of the tab away from the battery cell is loose. The specific process steps are as follows:

[0075] A riveting process for a lithium-ion battery tab and a rivet, specifically comprising the following steps:

[0076] S1. Prepare a cleaned and dried lithium battery cell, wherein the cell has a tab structure as described above, and the tab structure comprises a plurality of tabs stacked in layers;

[0077] The material of the tab is aluminum foil with a thickness of 0.1mm and a width of 50mm. Put the tab into the short circuit tester, set the test voltage to 5V, the current to 1A, and the test time to 3 seconds. After the test is completed, record the test results to ensure that the electrical performance of the tab is normal.

[0078] S2. Use a punching machine to punch holes on the fitted tabs; the diameter of the holes punched by the punching machine on the tabs is 8 mm.

[0079] S3. Use riveting equipment to rivet the tabs and rivets. The diameter of the rivet is 8mm, the riveting height of the positive tab is 10.45mm, and the riveting height of the negative tab is 10.35mm. Perform a short-circuit test on the riveted tabs again, with a test voltage of 5V, a current of 1A, and a test time of 3 seconds. After the test is completed, record the test results to ensure that the electrical performance of the tabs is normal.

[0080] Comparative Example 2

[0081] The riveting process of Comparative Example 2 is basically the same as that of Example 2, the main difference being that the pole ear is not ultrasonically welded, and the pole ear is loose at the end away from the battery cell. The specific process steps are as follows:

[0082] A riveting process for a lithium-ion battery tab and a rivet, specifically comprising the following steps:

[0083] S1. Prepare a cleaned and dried lithium battery cell, wherein the cell has a tab structure as described above, and the tab structure comprises a plurality of tabs stacked in layers;

[0084] The material of the tab is aluminum foil with a thickness of 0.05mm and a width of 50mm. Put the tab into the short circuit tester, set the test voltage to 5V, the current to 1A, and the test time to 3 seconds. After the test is completed, record the test results to ensure that the electrical performance of the tab is normal.

[0085] S2. Use a punching machine to punch holes on the fitted tabs; the diameter of the holes punched by the punching machine on the tabs is 10 mm.

[0086] S3. Use riveting equipment to rivet the tabs and rivets. The diameter of the rivet is 10mm, the riveting height of the positive tab is 10.65mm, and the riveting height of the negative tab is 10.45mm. Perform a short-circuit test on the riveted tabs again, with a test voltage of 5V, a current of 1A, and a test time of 3 seconds. After the test is completed, record the test results to ensure that the electrical performance of the tabs is normal.

[0087] Experimental Examples

[0088] The internal resistance test of the lithium-ion batteries prepared by the riveting process of Example 1-2 and Comparative Example 1-2 was carried out. The test process was as follows: using a pulse short-circuit tester, the test voltage was 150V, the pressing pressure of the battery core was 0.6±0.1Mpa, the test voltage drop VD1: 10%, VD2: 20%, and the test time was 200ms

[0089] The test results are as follows:

[0090] Internal resistance(Ωm) Example 1 0.03 Example 2 0.06 Comparative Example 1 0.08 Comparative Example 2 0.15

[0091] Since the tabs in Example 1 and Example 2 are completely fitted together, there will be no defects such as tab bending, missing holes, and rivet deviation during subsequent punching, thereby reducing the internal resistance of the battery and improving the performance of the battery.

[0092] This technical solution can be widely used in application fields such as lithium battery manufacturing, battery connection technology and mechanical riveting technology.

[0093] First, by adding ultrasonic welding process after short circuit testing, this technical solution can effectively improve the problems in the riveting process of lithium battery manufacturing, such as bending of the tabs, missing holes, and rivet deviation, thereby improving the performance and safety of the battery. This has important practical value for the lithium battery manufacturing industry.

[0094] Secondly, this technical solution can also reduce the internal resistance of the battery and improve the performance of the battery, which has important promotion value in the field of battery connection technology. Because the battery with low internal resistance can provide higher power output and meet higher power demand, it has important application value for electric vehicles and other equipment that require high power output.

[0095] Finally, this technical solution can also improve production efficiency and reduce production costs, which has important economic value for the field of mechanical riveting technology, because efficient production can increase production capacity, reduce the consumption of manpower and material resources, thereby reducing production costs and improving the competitiveness of enterprises.

[0096] In general, this technical solution has broad application prospects and huge market demand. It is of great significance in promoting the development of lithium battery manufacturing technology, improving battery performance and safety, reducing production costs, and improving production efficiency.

[0097] The above implementation modes are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with this technology to understand the content of the present invention and implement it, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.

Claims

1. A lithium-ion battery tab structure, characterized in that: The invention comprises a pole lug group (2) connected to a battery cell (1), wherein the pole lug group (2) comprises a plurality of pole lugs (3) arranged in a stacked manner, wherein the pole lugs (3) are used to connect the battery cell (1) and a rivet, and an end of each pole lug (3) away from the battery cell (1) is affixed with an adjacent pole lug (3) to form a riveted end (4).

2. The lithium-ion battery tab structure according to claim 1, characterized in that: The pole lugs (3) located at the riveted ends (4) are tightly fitted to form a whole.

3. The lithium-ion battery tab structure according to claim 1, characterized in that: A rivet hole (5) is provided on the rivet end (4), the rivet hole (5) is used for riveting with a rivet, and the diameter of the rivet hole (5) is matched to the diameter of the rivet.

4. The lithium-ion battery tab structure according to claim 3, characterized in that: The diameter of the riveting hole (5) is 5-10 mm.

5. The lithium-ion battery tab structure according to claim 1, characterized in that: The material of the pole ear (3) is aluminum foil, with a thickness of 0.05-0.15 mm and a width of 50 mm.

6. A riveting process for a lithium-ion battery tab and a rivet, characterized in that: The steps include: S1. Prepare a battery cell (1), wherein the battery cell (1) has a tab structure according to any one of claims 1 to 5, wherein the tab structure comprises a plurality of tabs (3) stacked in layers; S2, placing the electrode tab (3) into an ultrasonic welding machine for ultrasonic welding, so that a plurality of stacked electrode tabs (3) are bonded together by ultrasonic welding; S3, punching holes on the fitted tabs (3) using a punching machine; S4. Use riveting equipment to rivet the tab (3) and the rivet.

7. The riveting process for lithium-ion battery tabs and rivets according to claim 6, characterized in that: S1 also includes the following steps: placing the tab (3) in a short-circuit tester for testing, recording the test results, and ensuring that the electrical performance of the tab (3) is normal; S4 also includes the following steps: performing a short-circuit test on the riveted pole lug (3) again, and after the test is completed, recording the test result to ensure that the electrical performance of the pole lug (3) is normal.

8. The riveting process for lithium-ion battery tabs and rivets according to claim 7, characterized in that: In the short circuit test, the test voltage is 5V, the current is 1A, and the test time is 3 seconds.

9. The riveting process for lithium-ion battery tabs and rivets according to claim 6, characterized in that: In S2, the ultrasonic frequency is 20 kHz, the welding pressure is 0.5 to 1.5 MPa, and the welding time is 1 to 5 seconds.

10. The riveting process for lithium-ion battery tabs and rivets according to claim 6, characterized in that: In S4, the diameter of the rivet is 5-10 mm, the riveting height of the positive electrode tab (3) is 10.45-10.65 mm, and the riveting height of the negative electrode tab (3) is 10.35-10.45 mm.