High-frequency hole-conditioning agent for copper deposition process of printed circuit board and use method of high-frequency hole-conditioning agent
By using a specific proportion of emulsifiers, organic solvents, penetrants, surfactants, cationic agents and cruders in the whole pore agent, the problem of poor plating quality at low concentrations of palladium is solved, and efficient plating formation and Cost savings, the coating backlight level reaches 10.0.
Patent Information
- Application Number
- CN202411298654.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-18
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
It is difficult for existing pore whole agents to form high-quality plating under low concentration palladium conditions, resulting in high production costs and poor plating quality.
Using a high frequency pore-integrating agent, including emulsifiers, organic solvents, penetrants, surfactants, cationic agents, cruders and detergents, ensures the cleanliness of the pore walls and the time of impregnation by a specific proportion combination and impregnation temperature and time. Cation adsorption to form a high-quality coating.
Under low concentration palladium conditions, high-quality plating is achieved, reducing the cost of metal palladium, and the backlight level of the plating reaches 10.0, significantly improving the whole hole effect.
Smart Images

Figure CN118946038A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of circuit board processing, and in particular relates to a high-frequency pore-smoothing agent used in a copper deposition process of a printed circuit board and a use method thereof. Background Art
[0002] Circuit board, also called PCB board, is an indispensable component for electronic products to achieve circuit interconnection. Hole metallization process is the core process of printed circuit board manufacturing. It mainly uses chemical copper plating and electroplating copper to plate a conductive layer on the hole wall of the insulated PCB board to make the interlayer wires interconnected. Chemical copper plating is the core process of hole metallization. It is to reduce Cu 2+ Reducing to single element Cu makes the PCB insulation hole wall conductive with the inner and outer copper surfaces, providing a good carrier for electroplating copper thickening; the performance of the chemical copper plating process will directly affect the quality of the final electronic and electrical products.
[0003] The process flow of hole metallization of PCB board is as follows: loading → bulking → secondary countercurrent water washing → desmearing → washing → neutralization / reduction → washing → hole filling → washing → micro-etching and roughening → washing → pre-preg → activation → washing → acceleration → washing → copper deposition → washing → unloading.
[0004] The functions of the hole-forming process are: first, cleaning the circuit board surface; second, since potassium permanganate is used to remove the slag, the plate hole presents a negative charge, and the active palladium also carries a negative charge. Like charges repel each other, so the hole-forming makes the PCB board hole present a positive charge after the slag is removed, which is convenient for the subsequent adsorption of the negatively charged active palladium; the temperature can promote the cationic surfactant in the hole-forming agent to adhere to the PCB board hole, so that the palladium activator in the PCB board hole has a higher effective adsorption amount. However, the existing hole-forming agent requires a high concentration of metal palladium, and the high concentration of palladium is expensive, and low concentration of metal palladium cannot be used, which greatly increases the production cost. Therefore, a hole-forming agent that can be used for low concentration palladium and has good electroplating quality is urgently needed. Summary of the invention
[0005] One of the purposes of the present invention is to provide a high-frequency pore-forming agent for a copper plating process of a printed circuit board in view of the deficiencies of the prior art, which can form a coating by pore-forming under the condition of low palladium concentration and has good coating quality.
[0006] In order to achieve the above object, the present invention adopts the following technical solutions:
[0007] A high-frequency pore-smoothing agent for a printed circuit board copper deposition process comprises the following raw materials in parts by weight:
[0008] 3-8 parts of emulsifier; 15-25 parts of organic solvent; 2-5 parts of penetrant; 0.4-0.8 parts of surfactant; 0.04-0.08 parts of cationic agent; 1.0-2.5 parts of roughening agent; 0.5-1.5 parts of detergent; 57.12-78.06 parts of deionized water.
[0009] Wherein, the emulsifier is one or more of monoethanolamine, alkylphenol polyoxyethylene ether, and fatty alcohol polyoxyethylene ether.
[0010] Wherein, the organic solvent includes one or more of methanol, ethanol, ethylene glycol, diethylenetriamine, and ethylene glycol monomethyl ether.
[0011] Wherein, the penetrant is one or more of sodium chloride, sodium dodecylbenzene sulfonate, and sodium dodecyl sulfate.
[0012] Wherein, the surfactant is one or both of Triton and sodium glycocholate.
[0013] Wherein, the cationic agent is one or more of cocamidopropyl betaine, sodium lauryl sulfate and sodium lauryl sulfate.
[0014] Wherein, the roughening agent is one or more of cyclohexylthiophthalimide, octadecyltrimethylammonium chloride, and sodium dodecylbenzenesulfonate.
[0015] Wherein, the cleaning agent is one or more of sodium hydroxide, potassium hydroxide, and sodium dodecylbenzene sulfonate.
[0016] Another object of the present invention is to provide a method for using a pore-forming agent to address the deficiencies of the prior art, which can form a coating by pore-forming under low palladium concentration conditions and has good coating quality.
[0017] In order to achieve the above object, the present invention adopts the following technical solutions:
[0018] A method for using a pore-leveling agent comprises immersing a PCB sheet in the pore-leveling agent according to any one of claims 1 to 8 for 1 to 15 minutes at a temperature of 30 to 60 degrees Celsius.
[0019] Otherwise, the temperature is 40-50 degrees Celsius, and the immersion time is 4-6 minutes.
[0020] Compared with the prior art, the beneficial effect of the present invention is that due to the pore-forming agent of the present invention, the pores can be formed into a plating layer under the condition of low palladium concentration, and the plating layer has good quality. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1This is a test result diagram of the coating prepared by the pore-forming agent of Example 1 of the present invention at a palladium concentration of 30 μg / mL at level 10.0.
[0022] Figure 2 This is a test result diagram of the coating prepared by the pore-forming agent of Example 1 of the present invention at a palladium concentration of 20 μg / mL at level 9.5.
[0023] Figure 3 This is a test result diagram of the coating prepared by the pore-forming agent of Example 2 of the present invention at a palladium concentration of 30 μg / mL at level 9.5.
[0024] Figure 4 This is a test result diagram of the coating prepared by the pore-forming agent of Example 2 of the present invention at a palladium concentration of 20 μg / mL at level 9.0.
[0025] Figure 5 This is a test result chart of the coating prepared by the pore-forming agent of Comparative Example 1 of the present invention at a palladium concentration of 30 μg / mL at level 9.0. DETAILED DESCRIPTION
[0026] A high-frequency pore-smoothing agent for a copper plating process of a printed circuit board, comprising the following raw materials in parts by weight:
[0027] 3-8 parts of emulsifier; 15-25 parts of organic solvent; 2-5 parts of penetrant; 0.4-0.8 parts of surfactant; 0.04-0.08 parts of cationic agent; 1.0-2.5 parts of roughening agent; 0.5-1.5 parts of detergent; 57.12-78.06 parts of deionized water.
[0028] The weight proportion of the emulsifier can be 3 parts, 4 parts, 5 parts, 6 parts, 7 parts, 8 parts; the weight proportion of the organic solvent can be 15 parts, 18 parts, 20 parts, 22 parts, 23 parts, 25 parts; the weight proportion of the penetrant can be 2 parts, 3 parts, 4 parts, 5 parts; the weight proportion of the cationic agent can be 0.04 parts, 0.05 parts, 0.06 parts, 0.07 parts, 0.08 parts; the weight proportion of the penetrant can be 2 parts, 3 parts, 4 parts, 5 parts; the weight proportion of the surfactant can be 0.4 parts, 0.5 parts, 0.6 parts, 0.7 parts, 0.8 ... cationic agent can be 0.04 parts, 0.05 parts, 0.06 parts, 0.07 parts, 0.08 parts; the weight proportion of the cationic agent can be 0.04 parts, 0.05 parts, 0.06 parts, 0.07 parts, 0.08 parts; the weight proportion of the cationic agent can be 0.04 parts, 0.05 parts, 0.06 parts, 0.07 parts, 0.08 parts; the weight proportion of the cationic agent can be 0. The weight proportions of the sub-agent can be 0.04 parts, 0.05 parts, 0.06 parts, 0.07 parts, and 0.08 parts; the weight proportions of the roughening agent can be 1.0 parts, 1.2 parts, 1.5 parts, 1.8 parts, 2.0 parts, 2.4 parts, and 2.5 parts; the weight proportions of the cleaning agent can be 0.5 parts, 0.7 parts, 0.9 parts, 1.0 parts, 1.2 parts, 1.4 parts, and 1.5 parts; the weight proportions of deionized water can be 57.12 parts, 59 parts, 60 parts, 61 parts, 64 parts, 68 parts, 70 parts, 73 parts, 75 parts, 76 parts, and 78.06 parts.
[0029] The high-frequency hole-smoothing agent of the present invention includes an emulsifier, a penetrant, a surfactant and a detergent, which can synergistically clean the circuit board so that both the board surface and the hole wall can be cleaned without residual pollution, thereby ensuring smooth hole-smoothing. Preferably, the mass ratio of the emulsifier, the penetrant, the surfactant and the detergent is 5:3:0.6:0.8.
[0030] The high-frequency pore-scaling agent of the present invention uses a special cationic agent to make the hole wall (microscopic) of the printed circuit board more uniformly coarsened, adhere more densely and evenly to the hole wall surface, and the hole wall presents a stronger positive charge. In the subsequent process, in the solution with a lower (reduced) palladium concentration, it can also effectively adsorb metal palladium, improve the density and reaction rate of the subsequent chemical copper layer deposition, protect the quality of the copper deposition product, and thus reduce the cost of metal palladium.
[0031] The emulsifier is one or more of monoethanolamine, alkylphenol polyoxyethylene ether, and fatty alcohol polyoxyethylene ether. The emulsifier can emulsify the oil stains on the surface and hole wall of the fluffy board and the sweat stains secreted by the human body, so that the larger volume of stains is decomposed into a large number of small stains for later cleaning.
[0032] The organic solvent includes one or more of methanol, ethanol, ethylene glycol, diethylenetriamine, and ethylene glycol monomethyl ether. The organic solvent can dissolve the above-mentioned raw material components to form a uniform liquid, so that the performance of the pore-scaling agent is stable. The organic solvent can effectively dissolve the organic pollutants remaining on the cleaning plate surface and the hole wall.
[0033] The penetrant is one or more of sodium chloride, sodium dodecylbenzene sulfonate, and sodium dodecyl sulfate. The penetrant can enhance the permeability and hydrophilicity of the panel surface and the hole wall, so that the pore-forming agent can be cleaned and emulsified at every place on the panel and the hole wall surface.
[0034] Wherein, the surfactant is one or both of Triton and sodium glycocholate. Surfactants can reduce the surface tension of the drug solution.
[0035] Wherein, the cationic agent is one or more of cocamidopropyl betaine, sodium dodecyl sulfate, and sodium lauryl sulfate. The cationic agent has positively charged cations, so that the plate surface, especially the surface of the pore wall resin and other materials, uniformly adsorbs the cations, which is beneficial to the subsequent adsorption of negatively charged metal palladium. Preferably, the cationic agent is a mixture of cocamidopropyl betaine, sodium dodecyl sulfate, and sodium lauryl sulfate in a mass ratio of 1:1.5:2.
[0036] The roughening agent is one or more of cyclohexylthiophthalimide, octadecyltrimethylammonium chloride, and sodium dodecylbenzenesulfonate. The roughening agent of the present invention is more active than other roughening agents, and can accelerate the (microscopic) biting and roughening of the material of the plate hole wall, promote the adsorption of characteristic cations, make the hole wall surface more positively charged, and facilitate the subsequent effective adsorption of metal palladium (negatively charged).
[0037] Wherein, the cleaning agent is one or more of sodium hydroxide, potassium hydroxide, sodium dodecylbenzene sulfonate. The cleaning agent can clean the oil stains on the plate surface and the hole wall.
[0038] A method for using a pore-leveling agent, comprising: dipping a PCB sheet in the pore-leveling agent of any one of claims 1 to 8 for 1 to 15 minutes at a temperature of 30 to 60° C. Specifically, the temperature may be 30° C., 35° C., 38° C., 40° C., 45° C., 48° C., 50° C., 54° C., 56° C., or 60° C., and the dipping time may be 1 minute, 2 minutes, 4 minutes, 8 minutes, 10 minutes, 12 minutes, or 15 minutes.
[0039] Otherwise, the temperature is 40-50 degrees Celsius, and the immersion time is 4-6 minutes.
[0040] Example 1
[0041] A high-frequency pore-smoothing agent for a copper plating process of a printed circuit board comprises the following raw materials in parts by weight: 6 parts of an emulsifier; 20 parts of an organic solvent; 3.5 parts of a penetrant; 0.6 parts of a surfactant; 0.06 parts of a cationic agent; 2 parts of a roughening agent; 1 part of a detergent; and 66.84 parts of deionized water.
[0042] Among them, the emulsifier is alkylphenol polyoxyethylene ether; the organic solvent is ethylene glycol; the penetrant is sodium chloride; the surfactant is Triton; the cationic agent is cocamidopropyl betaine; the roughening agent is cyclohexylthiophthalimide; and the cleaning agent is sodium hydroxide.
[0043] The high-frequency pore-forming agent of Example 1 was used to form pores at palladium concentrations of 20 μg / mL and 30 μg / mL, and then tested.
[0044] Example 2
[0045] A high-frequency pore-smoothing agent for a copper plating process of a printed circuit board comprises the following raw materials in parts by weight: 3 parts of an emulsifier; 15 parts of an organic solvent; 2 parts of a penetrant; 0.4 parts of a surfactant; 0.04 parts of a cationic agent; 1 part of a roughening agent; 0.5 parts of a detergent; and 78.06 parts of deionized water.
[0046] The emulsifier is alkylphenol polyoxyethylene ether; the organic solvent is ethanol; the surfactant is sodium glycocholate; the cationic agent is sodium dodecyl sulfate; and the roughening agent is octadecyltrimethylammonium chloride.
[0047] The high-frequency pore-forming agent of Example 2 was used to form pores at palladium concentrations of 20 μg / mL and 30 μg / mL, and then tested.
[0048] Example 3
[0049] The difference from Example 1 is that the mass ratio of emulsifier, penetrant, surfactant and detergent is 6:2:0.4:0.7
[0050] The rest is the same as Example 1 and will not be described again here.
[0051] Example 4
[0052] The difference from Example 1 is that the mass ratio of the emulsifier, the penetrant, the surfactant and the detergent is 7:4:0.5:0.9.
[0053] The rest is the same as Example 1 and will not be described again here.
[0054] Example 5
[0055] The difference from Example 1 is that the mass ratio of the emulsifier, the penetrant, the surfactant and the detergent is 5:3:0.6:0.8.
[0056] The rest is the same as Example 1 and will not be described again here.
[0057] Example 6
[0058] The difference from Example 1 is that the cationic agent is a mixture of cocamidopropyl betaine and sodium lauryl sulfate in a mass ratio of 1:1.5.
[0059] The rest is the same as Example 1 and will not be described again here.
[0060] Example 7
[0061] The difference from Example 1 is that the cationic agent is a mixture of cocamidopropyl betaine, sodium lauryl sulfate and sodium lauryl sulfate in a mass ratio of 2:1.5:1.
[0062] The rest is the same as Example 1 and will not be described again here.
[0063] Example 8
[0064] The difference from Example 1 is that the cationic agent is a mixture of cocamidopropyl betaine, sodium lauryl sulfate and sodium lauryl sulfate in a mass ratio of 1:3:5.
[0065] The rest is the same as Example 1 and will not be described again here.
[0066] Example 9
[0067] The difference from Example 1 is that the roughening agent is octadecyltrimethylammonium chloride.
[0068] The rest is the same as Example 1 and will not be described again here.
[0069] Example 10
[0070] The difference from Example 1 is that the roughening agent is sodium dodecylbenzene sulfonate.
[0071] The rest is the same as Example 1 and will not be described again here.
[0072] Comparative Example 1
[0073] The difference from Example 1 is that no emulsifier is added.
[0074] The rest is the same as Example 1 and will not be described again here.
[0075] Comparative Example 2
[0076] The difference from Example 1 is that no penetrant is added.
[0077] The rest is the same as Example 1 and will not be described again here.
[0078] Comparative Example 3
[0079] The difference from Example 1 is that no surfactant is added.
[0080] The rest is the same as Example 1 and will not be described again here.
[0081] Comparative Example 4 is a commercially available alkaline pore-forming agent, and the plating is performed under the condition of a palladium concentration of 30 μg / mL. The rest is the same as Example 1 and will not be repeated here.
[0082] Comparative Example 5 is a commercially available alkaline pore-forming agent, and the plating is performed under the condition of a palladium concentration of 50 μg / mL. The rest is the same as Example 1 and will not be repeated here.
[0083] The prepared samples were evaluated for the backlight effect of through-hole plating. The backlight level of the sample after plating was used to evaluate whether it could evenly cover the entire through-hole substrate surface, thereby reflecting the treatment effect of the whole-hole agent and the regeneration effect of the whole-hole agent. The backlight level standard was divided into 0~10 levels with reference to the national test standard. The through-hole area of each example sample was removed, and the through-hole section was observed at 100 times in the transmission mode of the metallographic microscope. The number and form of the light-transmitting points in the section were compared with the backlight level diagram to obtain the level determination result. According to the backlight level determination, the activation effect and performance of the whole-hole agent can be determined. The higher the backlight level, the more complete the coverage of the catalytic particles in the whole-hole agent, and the better the activation effect; the lower the backlight level, the more light leakage, which indicates that the catalytic effect of the whole-hole agent is poor or the catalytic performance is reduced, thereby indicating the performance and stability of the whole-hole agent and the whole-hole agent after regeneration. Preferably, the backlight determination standard is greater than level 9.0 and the copper layer reliability thermal shock test is qualified without a break in the copper layer.
[0084] Table 1
[0085] project Palladium concentration (μg / mL) <![CDATA[Palladium adsorption amount on hole wall (μg / cm 2 )]]> Backlight level Appearance Example 1 20 0.87 9.5 No stratification Example 2 20 0.85 9.0 No stratification Example 3 30 0.85 9.0 No stratification Example 4 30 0.84 9.0 No stratification Example 5 30 0.86 9.0 No stratification Example 6 30 0.83 9.0 No stratification Example 7 30 0.84 9.0 No stratification Example 8 30 0.86 9.0 No stratification Example 9 30 0.84 9.0 No stratification Example 10 30 0.83 9.0 No stratification Example 1 30 0.96 10.0 No stratification Example 2 30 0.94 9.5 No stratification Comparative Example 1 40 0.83 9.5 No stratification Comparative Example 2 30 0.75 8.0 Copper layer has voids Comparative Example 3 20 0.54 6.0 Copper layer has voids Comparative Example 4 30 0.74 8.0 Copper layer has voids Comparative Example 5 50 0.76 8.0 Copper layer has voids
[0086] It can be concluded from the above table and from comparative examples 4 and 5 that although the alkaline pore-forming agent on the market can form a coating without stratification, its backlight rating is only 8.0. Figure 5 As shown, the coating has cracks and the copper layer has voids. At the same time, the palladium concentration for coating needs to be 30-50 μg / mL, so the cost is high. However, the pore-forming agents of Examples 1 and 2 of the present invention can form a coating when the palladium concentration is 30 μg / mL, and the backlight level of the coating is as high as 10.0 and 9.5, which has a good pore-forming effect. Figures 1 to 4 As shown, the pore-forming agents of Examples 1 and 2 of the present invention can still form a coating at a low palladium concentration of 20 μg / mL, and the backlight levels of the coating are 9.5 and 9.0 respectively, and the judgment results are qualified. Compared with the pore-forming agents in the prior art, the pore-forming agent of the present invention can form a coating at a lower concentration, and can save more than 25% of the cost of metal palladium.
[0087] By comparing Examples 1 and 3 to 5, it can be concluded that when the mass ratio of the emulsifier, the penetrant, the surfactant and the detergent is 5:3:0.6:0.8, it has a better adsorption and pore-forming effect, a larger amount of palladium is adsorbed, the thickness of the coating is better, and the coating effect is better.
[0088] By comparison of Examples 1 and 6 to 8, it can be concluded that when the cationic agent is a mixture of cocamidopropyl betaine, sodium lauryl sulfate and sodium lauryl sulfate in a mass ratio of 1:3:5, the prepared pore-forming agent has a better pore-forming effect, adsorbs more palladium, and forms a better plating effect.
[0089] By comparing Examples 1, 9, and 10, it can be concluded that when cyclohexylthiophthalimide is used as the roughening agent, the amount of palladium adsorbed on the pore wall is greater than that on octadecyltrimethylammonium chloride and sodium dodecylbenzenesulfonate. This is because when the roughening agent is cyclohexylthiophthalimide, it has better biting and roughening ability, and can form deeper holes on the circuit board. Therefore, the thickness of the coating formed by adsorption is thicker, and the coating effect is better.
[0090] By comparing Example 1 and Comparative Examples 1 to 3, it can be concluded that when one of the raw material components of the present invention is missing, the cleaning degree of the board surface or the hole wall is insufficient. Therefore, there will be voids during plating, and a dense plating layer cannot be formed. The plating effect is poor, the palladium adsorption amount is small, and the backlight level is low.
[0091] According to the disclosure and teaching of the above description, those skilled in the art to which the present invention belongs can also change and modify the above embodiment. Therefore, the present invention is not limited to the above specific embodiment, and any obvious improvement, replacement or modification made by those skilled in the art on the basis of the present invention belongs to the protection scope of the present invention. In addition, although some specific terms are used in this specification, these terms are only for the convenience of description and do not constitute any limitation to the present invention.
Claims
1. A high-frequency pore-forming agent for copper plating process of printed circuit boards, characterized in that: The invention comprises the following raw materials in parts by weight: 3-8 parts of emulsifier; 15-25 parts of organic solvent; 2-5 parts of penetrant; 0.4-0.8 parts of surfactant; 0.04-0.08 parts of cationic agent; 1.0-2.5 parts of roughening agent; 0.5-1.5 parts of detergent; 57.12-78.06 parts of deionized water.
2. The high-frequency pore-smoothing agent for copper plating process of printed circuit boards according to claim 1, characterized in that: The emulsifier is one or more of monoethanolamine, alkylphenol polyoxyethylene ether, and fatty alcohol polyoxyethylene ether.
3. The high-frequency pore-smoothing agent for copper plating process of printed circuit boards according to claim 1, characterized in that: The organic solvent includes one or more of methanol, ethanol, ethylene glycol, diethylenetriamine, and ethylene glycol monomethyl ether.
4. The high-frequency pore-smoothing agent for copper plating process of printed circuit boards according to claim 1, characterized in that: The penetrant is one or more of sodium chloride, sodium dodecylbenzene sulfonate, and sodium dodecyl sulfate.
5. The high-frequency pore-smoothing agent for copper plating process of printed circuit boards according to claim 1, characterized in that: The surfactant is one or both of Triton and sodium glycocholate.
6. The high-frequency pore-smoothing agent for copper plating process of printed circuit boards according to claim 1, characterized in that: The cationic agent is one or more of cocamidopropyl betaine, sodium lauryl sulfate and sodium lauryl sulfate.
7. The high-frequency pore-smoothing agent for copper plating process of printed circuit boards according to claim 1, characterized in that: The roughening agent is one or more of cyclohexylthiophthalimide, octadecyltrimethylammonium chloride, and sodium dodecylbenzenesulfonate.
8. The high-frequency pore-smoothing agent for copper plating process of printed circuit boards according to claim 1, characterized in that: The cleaning agent is one or more of sodium hydroxide, potassium hydroxide, and sodium dodecylbenzene sulfonate.
9. A method for using a pore-regulating agent, characterized in that: At a temperature of 30 to 60 degrees Celsius, the PCB board is immersed in the pore-forming agent according to any one of claims 1 to 8 for 1 to 15 minutes.
10. The method for using the pore-regulating agent according to claim 9, characterized in that: The temperature is 40-50 degrees Celsius, and the immersion time is 4-6 minutes.