Hollow CoFe-coated HCNFs microwave absorbing material and preparation method and application thereof
By constructing a method for preparing hollow CoFe@HCNFs microwave absorbing materials, the problems of MOFs derivative nanoparticle aggregation and poor microwave absorption performance of one-dimensional carbon fiber structures were solved. This method achieved strong absorption capacity and wide absorption bandwidth microwave absorption effect with low filling amount, and significantly improved reflection loss value and bandwidth.
Patent Information
- Application Number
- CN202410999854.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-11-12
AI Technical Summary
In the existing technology, MOFs derivatives have problems such as nanoparticle aggregation and poor microwave absorption performance. Moreover, the microwave absorbing materials with one-dimensional carbon fiber structure have a narrow effective absorption bandwidth and a high filling rate, which makes it difficult to meet the requirements of microwave absorbing materials for strong absorption capacity and wide absorption bandwidth.
ZIF67@CoFe-PBA cubes were prepared by ion exchange, and ZIF67@CoFe-PBA/PAN PS fibers were formed by electrospinning. Subsequently, pre-oxidation and carbonization were carried out to form hollow CoFe@HCNFs composite materials. Sulfurized hollow CoFe@HCNFs microwave absorbing materials were prepared by hydrothermal reaction. The hollow structure of one-dimensional fibers and the core-shell structure of MOF precursors were constructed to enhance the attenuation ability of electromagnetic waves and reduce the filling amount of composite materials.
At extremely low filler content, hollow CoFe@HCNFs microwave absorbing material exhibits excellent microwave absorption performance and a wide absorption bandwidth, with a reflection loss of -54.7dB and a maximum effective absorption bandwidth of 8.0GHz. Moreover, the raw materials are inexpensive and readily available, and the preparation method is simple.
Smart Images

Figure HDA0004961258360000011 
Figure HDA0004961258360000012 
Figure HDA0004961258360000021
Abstract
Description
Technical Field
[0001] The invention belongs to the field of microwave absorption, and in particular relates to a hollow CoFe@HCNFs microwave absorption material and a preparation method and application thereof. Background Art
[0002] With the rapid advancement of 5G mobile technology, people are in an era where information exchange and communication are becoming increasingly convenient. This technological innovation has certainly brought significant improvements to people's quality of life, but the problem of electromagnetic wave pollution brought about by 5G technology has also become increasingly prominent. If people are exposed to a complex electromagnetic environment for a long time, it may cause various adverse effects on the human body. In addition, electromagnetic waves may also interfere with precision electronic equipment and systems, affecting the normal operation of electronic instruments. Therefore, in order to effectively solve the problem of electromagnetic wave pollution, it is necessary to further design and develop microwave absorbing materials with strong loss capacity, wide absorption bandwidth and lightweight characteristics.
[0003] Magnetic carbon-based composites derived from metal-organic framework (MOFs) materials can give full play to the synergistic advantages of magnetic loss and dielectric loss, and therefore become a hot research material. However, MOFs derivatives in powder form have the problem of nanoparticle agglomeration, and the effect of adjusting the absorbing performance by controlling their own components is not obvious. In addition, the one-dimensional carbon fiber structure has a good improvement effect on the impedance matching and attenuation characteristics of the absorbing material, but the single carbon fiber exhibits poor absorbing performance due to its high dielectric constant. By effectively compounding MOFs derivatives with one-dimensional carbon fibers, a fiber composite absorbing material with the advantages of both carbon fiber matrix and MOFs derivatives can be obtained. However, most studies rarely regulate the microstructure of carbon fiber and MOFs at the same time, and there are still problems with narrow effective absorption bandwidth and high filling rate of absorbing materials. Therefore, it is necessary to design a magnetic carbon fiber composite absorbing material derived from MOFs to meet the requirements of strong absorption capacity and wide effective absorption bandwidth of microwave absorbing materials under the new situation. Summary of the invention
[0004] In view of the problems existing in the prior art, the present invention provides a hollow CoFe@HCNFs microwave absorbing material and a preparation method and application thereof. The composite material prepared by the method exhibits excellent microwave absorption performance and a wide absorption bandwidth at an extremely low filling amount.
[0005] The present invention is achieved through the following technical solutions:
[0006] The present invention provides a method for preparing a hollow CoFe@HCNFs microwave absorbing material, comprising the following steps:
[0007] S1, ZIF67 cubes were reacted with K3[Fe(CN6)] by ion exchange method to obtain ZIF67@CoFe-PBA cubes;
[0008] S2, ZIF67@CoFe-PBA cubes were mixed with polyacrylonitrile powder and polystyrene in a solvent and electrospun to obtain ZIF67@CoFe-PBA / PAN PS fibers;
[0009] S3, pre-oxidation and carbonization of ZIF67@CoFe-PBA / PAN PS fibers to obtain hollow CoFe@HCNFs composites.
[0010] Preferably, in S1, the preparation method of the ZIF67 cube is: dissolving Co(NO3)2·6H2O and hexadecyltrimethylammonium bromide in water to obtain solution A; dissolving 2-methylimidazole in water to form solution B; adding solution A to solution B, stirring to react, and washing the obtained product to obtain ZIF67 cubes.
[0011] Preferably, S1 is specifically as follows: dispersing ZIF67 cubes in anhydrous ethanol to obtain solution C; dissolving K3[Fe(CN6)] in water to form solution D; pouring solution D into solution C, stirring, and washing the obtained product to obtain ZIF67@CoFe-PBA cubes.
[0012] Preferably, in S2, the positive voltage used for electrospinning is 10-20 kV.
[0013] Preferably, in S3, the pre-oxidation temperature is 200-280° C., and the time is 1-3 h; the carbonization temperature is 600-900° C., and the time is 1-6 h.
[0014] Preferably, the method further comprises: S4, mixing thioacetamide and the hollow CoFe@HCNFs composite material in water, and performing a hydrothermal reaction to obtain a sulfurized hollow CoFe@HCNFs microwave absorbing material.
[0015] Furthermore, in S4, the temperature of the hydrothermal reaction is 100-200° C., and the time is 4-12 h.
[0016] Furthermore, in S4, the mass ratio of the hollow CoFe@HCNFs composite material to thioacetamide is 1:(0-15).
[0017] The present invention provides a hollow CoFe@HCNFs microwave absorbing material obtained by the preparation method as described above.
[0018] The present invention provides application of the hollow CoFe@HCNFs microwave absorbing material in electromagnetic wave absorption.
[0019] Compared with the prior art, the present invention has the following beneficial effects:
[0020] The present invention enhances the attenuation ability of electromagnetic waves and reduces the filling amount of composite materials by constructing the hollow structure of one-dimensional fiber and the core-shell structure of MOF precursor. First, the ZIF67@CoFe-PBA cube prepared by ion exchange method has a core-shell structure with ZIF67 as the core and CoFe-PBA as the shell, and the cube size is uniform and has good dispersibility; after high-temperature carbonization, ZIF67@CoFe-PBA forms a cube of core-shell structure CoFe@C, and the gap between the core and the shell is larger. Co7Fe3 alloy exists in the material, and the formation of Co7Fe3 alloy significantly increases the conductive loss energy of the material. Secondly, ZIF67@CoFe-PBA cubes are mixed with polyacrylonitrile powder and PS to prepare fibers. Due to the pyrolysis of PS during high-temperature carbonization, the one-dimensional fiber forms a hollow structure. The construction of the hollow porous structure not only enhances the multiple reflection and scattering ability of electromagnetic waves, but also adjusts the dielectric constant, thereby optimizing impedance matching, which is conducive to enhancing the absorption of electromagnetic waves and significantly reducing the filling amount of composite materials. The raw materials of the microwave absorbing material of the invention are cheap and easily available, the preparation method is simple, the equipment is easy to operate, the yield of the fiber composite material is high, and the microwave absorbing material of the invention is a potential microwave absorbing material.
[0021] Furthermore, after the hollow CoFe@HCNFs composite material is vulcanized, metal sulfide is formed, the types of components are increased, and a rich heterogeneous interface is constructed, which is beneficial to improving the interface polarization and dissipating electromagnetic waves. The electromagnetic wave absorption performance of the sample is tested by a vector network analyzer. The results show that when the filling ratio of the composite material is only 5wt% and the addition amount of thioacetamide is 75mg, the vulcanized hollow CoFe@HCNFs microwave absorption material obtains a minimum reflection loss value of -54.7dB and a maximum effective absorption bandwidth of 8.0GHz. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0023] Figure 1are SEM images of the materials of the present invention; (a) is a SEM image of the CoFe@HCNFs fiber prepared in Example 2 of the present invention; (b) is a SEM image of the S-CoFe@HCNFs-75 fiber prepared in Example 5; (c) is a SEM image of the S-CoFe@HCNFs-225 fiber prepared in Example 8;
[0024] Figure 2 This is the XRD pattern of the sulfided hollow CoFe@HCNFs microwave absorbing material prepared in Example 5 of the present invention;
[0025] Figure 3 The reflection loss value of the hollow CoFe@HCNFs microwave absorbing material prepared in Example 2 of the present invention when the filling amount is 5wt%;
[0026] Figure 4 The reflection loss value of the CoFe@CNFs microwave absorbing material prepared in Comparative Example 1 of the present invention when the filling amount is 5wt%;
[0027] Figure 5 This is a SEM image of the CoFe@CNFs microwave absorbing material prepared in Comparative Example 1 of the present invention;
[0028] Figure 6 The reflection loss value of the sulfided hollow CoFe@HCNFs microwave absorbing material prepared in Example 5 of the present invention when the filling amount is 5wt%;
[0029] Figure 7 This is a real part diagram of the dielectric loss of the sulfided hollow CoFe@HCNFs microwave absorbing material prepared in Example 5 of the present invention;
[0030] Figure 8 This is the imaginary part diagram of the dielectric loss of the sulfided hollow CoFe@HCNFs microwave absorbing material prepared in Example 5 of the present invention;
[0031] Fig. 9 This is the dielectric loss tangent diagram of the sulfided hollow CoFe@HCNFs microwave absorbing material prepared in Example 5 of the present invention;
[0032] Fig.10 This is a real part diagram of magnetic loss of the sulfided hollow CoFe@HCNFs microwave absorbing material prepared in Example 5 of the present invention;
[0033] Fig.11 This is the imaginary part diagram of magnetic loss of the sulfided hollow CoFe@HCNFs microwave absorbing material prepared in Example 5 of the present invention;
[0034] Fig.12 This is the magnetic loss tangent diagram of the sulfurized hollow CoFe@HCNFs microwave absorbing material prepared in Example 5 of the present invention. DETAILED DESCRIPTION
[0035] The following describes the embodiments of the present invention through specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention.
[0036] It should be noted that the process equipment or devices not specifically specified in the following embodiments are all conventional equipment or devices in the art.
[0037] It should be noted that the terms "include" and "have" and any variations thereof are intended to cover non-exclusive inclusions. For example, a process, method, system, product or device that includes a series of steps or units is not necessarily limited to those steps or units clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices. Moreover, unless otherwise specified, the numbering of each method step is only a convenient tool for identifying each method step, and is not intended to limit the order of arrangement of each method step or to define the scope of the present invention. Changes or adjustments in their relative relationships should also be regarded as the scope of the present invention without substantially changing the technical content.
[0038] The method for preparing the hollow CoFe@HCNFs microwave absorbing material of the present invention comprises the following steps:
[0039] (1) Dissolving Co(NO3)2·6H2O and cetyltrimethylammonium bromide (CTAB) in deionized water to obtain solution A; dissolving 2-methylimidazole in deionized water to form solution B;
[0040] (2) pouring solution A obtained in step (1) into solution B, stirring magnetically, washing and centrifuging to obtain purple precipitate ZIF67 cubes after sufficient reaction;
[0041] (3) dispersing the purple precipitate ZIF67 cubes obtained in step (2) in anhydrous ethanol to obtain solution C; dissolving K3[Fe(CN6)] in deionized water to form solution D;
[0042] (4) Pour solution D obtained in step (3) into solution C, stir magnetically, wash the product, and centrifuge to obtain blue precipitate ZIF67@CoFe-PBA cubes;
[0043] (5) dispersing the blue precipitate ZIF67@CoFe-PBA cubes obtained in step (4) in N,N-dimethylformamide (DMF), and then adding polyacrylonitrile powder (PAN) and polystyrene (PS), and continuing to stir to obtain solution E; transferring solution E to a syringe, installing it on an electrospinning device for electrospinning to obtain a ZIF67@CoFe-PBA / PAN PS fiber membrane material;
[0044] (6) pre-oxidizing the fiber membrane material obtained in step (5), and then carbonizing it at a high temperature to obtain a hollow CoFe@HCNFs composite material;
[0045] (7) dissolving thioacetamide in deionized water to form a solution F; placing the magnetic carbon-based fiber composite material obtained in step (6) into the solution F for a hydrothermal reaction, and obtaining a product of a sulfurized hollow CoFe@HCNFs microwave absorbing material (S-CoFe@HCNFs).
[0046] In step (2) of the present invention, stirring is carried out at room temperature for 0.5 to 5 hours; in step (4), stirring is carried out at room temperature for 1 to 4 hours.
[0047] In step (5) of the present invention, the positive voltage is 10 to 20 kV, and the receiving distance between the tip of the syringe needle and the receiver is 10 to 20 cm.
[0048] In step (6) of the present invention, the fiber pretreatment temperature is 200-280°C for 1-3h; the inert atmosphere is argon, the carbonization temperature is 600-900°C, the heating rate is 2-5°C / min, and the carbonization time is 1-6h.
[0049] In step (7) of the present invention, the mass ratio of the hollow CoFe@HCNFs composite material to thioacetamide is 1:(0-15); the hydrothermal reaction temperature is 100-200° C., and the reaction time is 4-12 hours.
[0050] The hollow CoFe@HCNFs microwave absorbing material or the sulfided hollow CoFe@HCNFs microwave absorbing material obtained by the preparation method of the present invention can be used in electromagnetic wave absorption.
[0051] Embodiment 1:
[0052] A method for preparing a hollow CoFe@HCNFs microwave absorbing material comprises the following steps:
[0053] (1) 0.29 g of Co(NO3)2·6H2O and 20 mg of hexadecyltrimethylammonium bromide (CTAB) were dissolved in 10 mL of deionized water to obtain solution A; 4.52 g of 2-methylimidazole was dissolved in 80 mL of deionized water to form solution B;
[0054] (2) pouring solution A obtained in step (1) into solution B, stirring at room temperature for 0.5 h, washing and centrifuging to obtain ZIF67 cubes after sufficient reaction;
[0055] (3) Disperse 22 mg of ZIF67 cubes obtained in step (2) in 15 mL of anhydrous ethanol to obtain solution C; dissolve 50 mg of K3[Fe(CN6)] in 5 mL of deionized water to form solution D;
[0056] (4) Pour the solution D obtained in step (3) into the solution C and stir at room temperature for 4 h. Wash and centrifuge the product to obtain core-shell ZIF67@CoFe-PBA cubes.
[0057] (5) 0.6 g of ZIF67@CoFe-PBA cubes obtained in step (4) were dispersed in 5 mL of N,N-dimethylformamide (DMF), and then 0.3 g of polyacrylonitrile powder (PAN) and 0.1 g of polystyrene (PS) were added and stirred to obtain solution E; solution E was transferred to a syringe and installed on an electrospinning device to electrospin ZIF67@CoFe-PBA / PAN PS fibers; specific parameter settings were used during the electrospinning process, specifically: the positive voltage was set to 10 kV, the receiving distance was controlled at 10 cm, the needle model was No. 20, and the propulsion rate was set to 0.8 mL / h;
[0058] (6) The fiber material obtained in step (5) was first pre-oxidized at 280°C for 3 hours, then transferred to a tubular furnace for carbonization at a heating rate of 2°C / min, and gradually heated to 600°C for carbonization for 6 hours under an argon atmosphere. After cooling to room temperature, a hollow CoFe@HCNFs composite material was obtained.
[0059] Embodiment 2:
[0060] A method for preparing a hollow CoFe@HCNFs microwave absorbing material comprises the following steps:
[0061] (1) 0.29 g of Co(NO3)2·6H2O and 20 mg of hexadecyltrimethylammonium bromide (CTAB) were dissolved in 10 mL of deionized water to obtain solution A; 4.52 g of 2-methylimidazole was dissolved in 80 mL of deionized water to form solution B;
[0062] (2) pouring solution A obtained in step (1) into solution B, stirring at room temperature for 3 h, washing and centrifuging to obtain ZIF67 cubes after sufficient reaction;
[0063] (3) Disperse 22 mg of ZIF67 cubes obtained in step (2) in 15 mL of anhydrous ethanol to obtain solution C; dissolve 50 mg of K3[Fe(CN6)] in 5 mL of deionized water to form solution D;
[0064] (4) Pour the solution D obtained in step (3) into the solution C and stir at room temperature for 2 h. Wash and centrifuge the product to obtain core-shell ZIF67@CoFe-PBA cubes.
[0065] (5) 0.6 g of ZIF67@CoFe-PBA cubes obtained in step (4) were dispersed in 5 mL of N,N-dimethylformamide (DMF), and then 0.3 g of polyacrylonitrile powder (PAN) and 0.1 g of polystyrene (PS) were added and stirred to obtain solution E; solution E was transferred to a syringe and installed on an electrospinning device to electrospin ZIF67@CoFe-PBA / PAN PS fibers; specific parameter settings were used during the electrospinning process, specifically: the positive voltage was set to 15 kV, the receiving distance was controlled at 15 cm, the needle model was No. 20, and the propulsion rate was set to 0.8 mL / h;
[0066] (6) The fiber material obtained in step (5) was first pre-oxidized at 200°C for 2 h, then transferred to a tubular furnace for carbonization at a heating rate of 3°C / min, and gradually heated to 700°C for carbonization for 2 h under an argon atmosphere. After cooling to room temperature, a hollow CoFe@HCNFs composite material was obtained.
[0067] Embodiment 3:
[0068] A method for preparing a hollow CoFe@HCNFs microwave absorbing material comprises the following steps:
[0069] (1) 0.29 g of Co(NO3)2·6H2O and 20 mg of hexadecyltrimethylammonium bromide (CTAB) were dissolved in 10 mL of deionized water to obtain solution A; 4.52 g of 2-methylimidazole was dissolved in 80 mL of deionized water to form solution B;
[0070] (2) pouring solution A obtained in step (1) into solution B, stirring at room temperature for 5 h, washing and centrifuging to obtain ZIF67 cubes after sufficient reaction;
[0071] (3) Disperse 22 mg of ZIF67 cubes obtained in step (2) in 15 mL of anhydrous ethanol to obtain solution C; dissolve 50 mg of K3[Fe(CN6)] in 5 mL of deionized water to form solution D;
[0072] (4) Pour the solution D obtained in step (3) into the solution C and stir at room temperature for 1 h. Wash and centrifuge the product to obtain core-shell ZIF67@CoFe-PBA cubes.
[0073] (5) 0.6 g of ZIF67@CoFe-PBA cubes obtained in step (4) were dispersed in 5 mL of N,N-dimethylformamide (DMF), and then 0.3 g of polyacrylonitrile powder (PAN) and 0.1 g of polystyrene (PS) were added and stirred to obtain solution E; solution E was transferred to a syringe and installed on an electrospinning device to electrospin ZIF67@CoFe-PBA / PAN PS fibers; specific parameter settings were used during the electrospinning process, specifically: the positive voltage was set to 20 kV, the receiving distance was controlled at 20 cm, the needle model was No. 20, and the propulsion rate was set to 0.8 mL / h;
[0074] (6) The fiber material obtained in step (5) was first pre-oxidized at 250°C for 1 h, then transferred to a tubular furnace for carbonization at a heating rate of 5°C / min, and gradually heated to 900°C for carbonization for 1 h under an argon atmosphere. After cooling to room temperature, a hollow CoFe@HCNFs composite material was obtained.
[0075] Embodiment 4:
[0076] A method for preparing a sulfided hollow CoFe@HCNFs microwave absorbing material comprises the following steps:
[0077] (1) 0.29 g of Co(NO3)2·6H2O and 20 mg of hexadecyltrimethylammonium bromide (CTAB) were dissolved in 10 mL of deionized water to obtain solution A; 4.52 g of 2-methylimidazole was dissolved in 80 mL of deionized water to form solution B;
[0078] (2) pouring solution A obtained in step (1) into solution B, stirring at room temperature for 0.5 h, washing and centrifuging to obtain ZIF67 cubes after sufficient reaction;
[0079] (3) Disperse 22 mg of ZIF67 cubes obtained in step (2) in 15 mL of anhydrous ethanol to obtain solution C; dissolve 50 mg of K3[Fe(CN6)] in 5 mL of deionized water to form solution D;
[0080] (4) Pour the solution D obtained in step (3) into the solution C and stir at room temperature for 4 h. Wash and centrifuge the product to obtain core-shell ZIF67@CoFe-PBA cubes.
[0081] (5) 0.6 g of ZIF67@CoFe-PBA cubes obtained in step (4) were dispersed in 5 mL of N,N-dimethylformamide (DMF), and then 0.3 g of polyacrylonitrile powder (PAN) and 0.1 g of polystyrene (PS) were added and stirred to obtain solution E; solution E was transferred to a syringe and installed on an electrospinning device to electrospin ZIF67@CoFe-PBA / PAN PS fibers; specific parameter settings were used during the electrospinning process, specifically: the positive voltage was set to 10 kV, the receiving distance was controlled at 10 cm, the needle model was No. 20, and the propulsion rate was set to 0.8 mL / h;
[0082] (6) The fiber material obtained in step (5) was first pre-oxidized at 280° C. for 3 h, then transferred to a tubular furnace for carbonization at a heating rate of 2° C. / min, gradually heated to 600° C. for carbonization for 6 h under an argon atmosphere, and cooled to room temperature to obtain a hollow CoFe@HCNFs composite material;
[0083] (7) Dissolve 75 mg of thioacetamide in 40 mL of deionized water to form a solution F; place a 15 mg piece of hollow CoFe@HCNFs composite material obtained in step (6) into solution F for hydrothermal reaction at a temperature of 100 ° C. for 12 h. After cooling to room temperature, wash and obtain a sulfurized hollow CoFe@HCNFs microwave absorbing material (S-CoFe@HCNFs-75).
[0084] Embodiment 5:
[0085] A method for preparing a sulfided hollow CoFe@HCNFs microwave absorbing material comprises the following steps:
[0086] (1) 0.29 g of Co(NO3)2·6H2O and 20 mg of hexadecyltrimethylammonium bromide (CTAB) were dissolved in 10 mL of deionized water to obtain solution A; 4.52 g of 2-methylimidazole was dissolved in 80 mL of deionized water to form solution B;
[0087] (2) pouring solution A obtained in step (1) into solution B, stirring at room temperature for 3 h, washing and centrifuging to obtain ZIF67 cubes after sufficient reaction;
[0088] (3) Disperse 22 mg of ZIF67 cubes obtained in step (2) in 15 mL of anhydrous ethanol to obtain solution C; dissolve 50 mg of K3[Fe(CN6)] in 5 mL of deionized water to form solution D;
[0089] (4) Pour the solution D obtained in step (3) into the solution C and stir at room temperature for 2 h. Wash and centrifuge the product to obtain core-shell ZIF67@CoFe-PBA cubes.
[0090] (5) 0.6 g of ZIF67@CoFe-PBA cubes obtained in step (4) were dispersed in 5 mL of N,N-dimethylformamide (DMF), and then 0.3 g of polyacrylonitrile powder (PAN) and 0.1 g of polystyrene (PS) were added and stirred to obtain solution E; solution E was transferred to a syringe and installed on an electrospinning device to electrospin ZIF67@CoFe-PBA / PAN PS fibers; specific parameter settings were used during the electrospinning process, specifically: the positive voltage was set to 15 kV, the receiving distance was controlled at 15 cm, the needle model was No. 20, and the propulsion rate was set to 0.8 mL / h;
[0091] (6) The fiber material obtained in step (5) was pre-oxidized at 200° C. for 2 h, and then transferred to a tubular furnace for carbonization at a heating rate of 3° C. / min. The fiber material was gradually heated to 700° C. for carbonization for 2 h under an argon atmosphere, and then cooled to room temperature to obtain a hollow CoFe@HCNFs composite material;
[0092] (7) Dissolve 75 mg of thioacetamide in 40 mL of deionized water to form a solution F; place a 15 mg piece of hollow CoFe@HCNFs composite material obtained in step (6) into solution F for hydrothermal reaction at a temperature of 150° C. for 8 h. After cooling to room temperature, wash to obtain a sulfurized hollow CoFe@HCNFs microwave absorbing material (S-CoFe@HCNFs-75).
[0093] Embodiment 6:
[0094] A method for preparing a sulfided hollow CoFe@HCNFs microwave absorbing material comprises the following steps:
[0095] (1) 0.29 g of Co(NO3)2·6H2O and 20 mg of hexadecyltrimethylammonium bromide (CTAB) were dissolved in 10 mL of deionized water to obtain solution A; 4.52 g of 2-methylimidazole was dissolved in 80 mL of deionized water to form solution B;
[0096] (2) pouring solution A obtained in step (1) into solution B, stirring at room temperature for 5 h, washing and centrifuging to obtain ZIF67 cubes after sufficient reaction;
[0097] (3) Disperse 22 mg of ZIF67 cubes obtained in step (2) in 15 mL of anhydrous ethanol to obtain solution C; dissolve 50 mg of K3[Fe(CN6)] in 5 mL of deionized water to form solution D;
[0098] (4) Pour the solution D obtained in step (3) into the solution C and stir at room temperature for 1 h. Wash and centrifuge the product to obtain core-shell ZIF67@CoFe-PBA cubes.
[0099] (5) 0.6 g of ZIF67@CoFe-PBA cubes obtained in step (4) were dispersed in 5 mL of N,N-dimethylformamide (DMF), and then 0.3 g of polyacrylonitrile powder (PAN) and 0.1 g of polystyrene (PS) were added and stirred to obtain solution E; solution E was transferred to a syringe and installed on an electrospinning device to electrospin ZIF67@CoFe-PBA / PAN PS fibers; specific parameter settings were used during the electrospinning process, specifically: the positive voltage was set to 20 kV, the receiving distance was controlled at 20 cm, the needle model was No. 20, and the propulsion rate was set to 0.8 mL / h;
[0100] (6) The fiber material obtained in step (5) was first pre-oxidized at 250° C. for 1 h, then transferred to a tubular furnace for carbonization at a heating rate of 5° C. / min, gradually heated to 900° C. for carbonization for 1 h under an argon atmosphere, and cooled to room temperature to obtain a hollow CoFe@HCNFs composite material;
[0101] (7) Dissolve 75 mg of thioacetamide in 40 mL of deionized water to form a solution F; place a 15 mg piece of hollow CoFe@HCNFs composite material obtained in step (6) into solution F for hydrothermal reaction at a temperature of 200 ° C. for 4 h. After cooling to room temperature, wash and obtain a sulfurized hollow CoFe@HCNFs microwave absorbing material (S-CoFe@HCNFs-225).
[0102] Embodiment 7:
[0103] A method for preparing a sulfided hollow CoFe@HCNFs microwave absorbing material comprises the following steps:
[0104] (1) 0.29 g of Co(NO3)2·6H2O and 20 mg of hexadecyltrimethylammonium bromide (CTAB) were dissolved in 10 mL of deionized water to obtain solution A; 4.52 g of 2-methylimidazole was dissolved in 80 mL of deionized water to form solution B;
[0105] (2) pouring solution A obtained in step (1) into solution B, stirring at room temperature for 0.5 h, washing and centrifuging to obtain ZIF67 cubes after sufficient reaction;
[0106] (3) Disperse 22 mg of ZIF67 cubes obtained in step (2) in 15 mL of anhydrous ethanol to obtain solution C; dissolve 50 mg of K3[Fe(CN6)] in 5 mL of deionized water to form solution D;
[0107] (4) Pour the solution D obtained in step (3) into the solution C and stir at room temperature for 4 h. Wash and centrifuge the product to obtain core-shell ZIF67@CoFe-PBA cubes.
[0108] (5) 0.6 g of ZIF67@CoFe-PBA cubes obtained in step (4) were dispersed in 5 mL of N,N-dimethylformamide (DMF), and then 0.3 g of polyacrylonitrile powder (PAN) and 0.1 g of polystyrene (PS) were added and stirred to obtain solution E; solution E was transferred to a syringe and installed on an electrospinning device to electrospin ZIF67@CoFe-PBA / PAN PS fibers; specific parameter settings were used during the electrospinning process, specifically: the positive voltage was set to 10 kV, the receiving distance was controlled at 10 cm, the needle model was No. 20, and the propulsion rate was set to 0.8 mL / h;
[0109] (6) The fiber material obtained in step (5) was first pre-oxidized at 280° C. for 3 h, then transferred to a tubular furnace for carbonization at a heating rate of 2° C. / min, gradually heated to 600° C. for carbonization for 6 h under an argon atmosphere, and cooled to room temperature to obtain a hollow CoFe@HCNFs composite material;
[0110] (7) Dissolve 225 mg of thioacetamide in 40 mL of deionized water to form a solution F; place a 15 mg piece of hollow CoFe@HCNFs composite material obtained in step (6) into solution F for hydrothermal reaction at a temperature of 100 ° C. for 12 h. After cooling to room temperature, wash and obtain a sulfurized hollow CoFe@HCNFs microwave absorbing material (S-CoFe@HCNFs-225).
[0111] Embodiment 8:
[0112] A method for preparing a sulfided hollow CoFe@HCNFs microwave absorbing material comprises the following steps:
[0113] (1) 0.29 g of Co(NO3)2·6H2O and 20 mg of hexadecyltrimethylammonium bromide (CTAB) were dissolved in 10 mL of deionized water to obtain solution A; 4.52 g of 2-methylimidazole was dissolved in 80 mL of deionized water to form solution B;
[0114] (2) pouring solution A obtained in step (1) into solution B, stirring at room temperature for 3 h, washing and centrifuging to obtain ZIF67 cubes after sufficient reaction;
[0115] (3) Disperse 22 mg of ZIF67 cubes obtained in step (2) in 15 mL of anhydrous ethanol to obtain solution C; dissolve 50 mg of K3[Fe(CN6)] in 5 mL of deionized water to form solution D;
[0116] (4) Pour the solution D obtained in step (3) into the solution C and stir at room temperature for 2 h. Wash and centrifuge the product to obtain core-shell ZIF67@CoFe-PBA cubes.
[0117] (5) 0.6 g of ZIF67@CoFe-PBA cubes obtained in step (4) were dispersed in 5 mL of N,N-dimethylformamide (DMF), and then 0.3 g of polyacrylonitrile powder (PAN) and 0.1 g of polystyrene (PS) were added and stirred to obtain solution E; solution E was transferred to a syringe and installed on an electrospinning device to electrospin ZIF67@CoFe-PBA / PAN PS fibers; specific parameter settings were used during the electrospinning process, specifically: the positive voltage was set to 15 kV, the receiving distance was controlled at 15 cm, the needle model was No. 20, and the propulsion rate was set to 0.8 mL / h;
[0118] (6) The fiber material obtained in step (5) was pre-oxidized at 200° C. for 2 h, and then transferred to a tubular furnace for carbonization at a heating rate of 3° C. / min. The fiber material was gradually heated to 700° C. for carbonization for 2 h under an argon atmosphere, and then cooled to room temperature to obtain a hollow CoFe@HCNFs composite material;
[0119] (7) Dissolve 225 mg of thioacetamide in 40 mL of deionized water to form a solution F; place a 15 mg piece of hollow CoFe@HCNFs composite material obtained in step (6) into solution F for hydrothermal reaction at a temperature of 150° C. for 8 h. After cooling to room temperature, wash to obtain a sulfurized hollow CoFe@HCNFs microwave absorbing material (S-CoFe@HCNFs-225).
[0120] Embodiment 9:
[0121] A method for preparing a sulfided hollow CoFe@HCNFs microwave absorbing material comprises the following steps:
[0122] (1) 0.29 g of Co(NO3)2·6H2O and 20 mg of hexadecyltrimethylammonium bromide (CTAB) were dissolved in 10 mL of deionized water to obtain solution A; 4.52 g of 2-methylimidazole was dissolved in 80 mL of deionized water to form solution B;
[0123] (2) pouring solution A obtained in step (1) into solution B, stirring at room temperature for 5 h, washing and centrifuging to obtain ZIF67 cubes after sufficient reaction;
[0124] (3) Disperse 22 mg of ZIF67 cubes obtained in step (2) in 15 mL of anhydrous ethanol to obtain solution C; dissolve 50 mg of K3[Fe(CN6)] in 5 mL of deionized water to form solution D;
[0125] (4) Pour the solution D obtained in step (3) into the solution C and stir at room temperature for 1 h. Wash and centrifuge the product to obtain core-shell ZIF67@CoFe-PBA cubes.
[0126] (5) 0.6 g of ZIF67@CoFe-PBA cubes obtained in step (4) were dispersed in 5 mL of N,N-dimethylformamide (DMF), and then 0.3 g of polyacrylonitrile powder (PAN) and 0.1 g of polystyrene (PS) were added and stirred to obtain solution E; solution E was transferred to a syringe and installed on an electrospinning device to electrospin ZIF67@CoFe-PBA / PAN PS fibers; specific parameter settings were used during the electrospinning process, specifically: the positive voltage was set to 20 kV, the receiving distance was controlled at 20 cm, the needle model was No. 20, and the propulsion rate was set to 0.8 mL / h;
[0127] (6) The fiber material obtained in step (5) was first pre-oxidized at 250° C. for 1 h, then transferred to a tubular furnace for carbonization at a heating rate of 5° C. / min, gradually heated to 900° C. for carbonization for 1 h under an argon atmosphere, and cooled to room temperature to obtain a hollow CoFe@HCNFs composite material;
[0128] (7) Dissolve 225 mg of thioacetamide in 40 mL of deionized water to form a solution F; place a 15 mg piece of hollow CoFe@HCNFs composite material obtained in step (6) into solution F for hydrothermal reaction at a temperature of 200 ° C. for 4 h. After cooling to room temperature, wash and obtain a sulfurized hollow CoFe@HCNFs microwave absorbing material (S-CoFe@HCNFs-225).
[0129] Comparative Example 1:
[0130] A method for preparing a CoFe@CNFs microwave absorbing material comprises the following steps:
[0131] (1) 0.29 g of Co(NO3)2·6H2O and 20 mg of hexadecyltrimethylammonium bromide (CTAB) were dissolved in 10 mL of deionized water to obtain solution A; 4.52 g of 2-methylimidazole was dissolved in 80 mL of deionized water to form solution B;
[0132] (2) pouring solution A obtained in step (1) into solution B, stirring at room temperature for 5 h, washing and centrifuging to obtain ZIF67 cubes after sufficient reaction;
[0133] (3) Disperse 22 mg of ZIF67 cubes obtained in step (2) in 15 mL of anhydrous ethanol to obtain solution C; dissolve 50 mg of K3[Fe(CN6)] in 5 mL of deionized water to form solution D;
[0134] (4) Pour the solution D obtained in step (3) into the solution C and stir at room temperature for 1 h. Wash and centrifuge the product to obtain core-shell ZIF67@CoFe-PBA cubes.
[0135] (5) 0.6 g of ZIF67@CoFe-PBA cubes obtained in step (4) were dispersed in 5 mL of N,N-dimethylformamide (DMF), and then 0.3 g of polyacrylonitrile powder (PAN) was added and stirred to obtain solution E; solution E was transferred to a syringe and installed on an electrospinning device to electrospin ZIF67@CoFe-PBA / PAN fibers; specific parameter settings were used during the electrospinning process, specifically: the positive voltage was set to 20 kV, the receiving distance was controlled at 20 cm, the needle model was No. 20, and the propulsion rate was set to 0.8 mL / h;
[0136] (6) The fiber material obtained in step (5) was pre-oxidized at 200°C for 2 h, and then transferred to a tubular furnace for carbonization at a heating rate of 3°C / min. It was gradually heated to 700°C for carbonization for 2 h under an argon atmosphere, and then cooled to room temperature to obtain a CoFe@CNFs composite material.
[0137] Figure 1 The SEM images of the hollow CoFe@HCNFs microwave absorbing materials prepared in Examples 2, 5 and 8 are shown, where (a) is Example 2, (b) and (c) are Example 5, and (d) is Example 8. It can be seen from the figure that the core-shell CoFe@C cubes are densely and evenly distributed on the one-dimensional carbon fiber. Figure 1 In (c), it can be observed that the carbon fibers show a unique hollow structure, which is caused by the complete decomposition of polystyrene.
[0138] Figure 2 The XRD spectrum of the sulfided hollow CoFe@HCNFs microwave absorbing material prepared in the embodiment with the best performance (Example 5) is shown, indicating the presence of Co7Fe3 alloy and Co3S4 particles in the material.
[0139] Figure 3 This is a reflection loss diagram of the hollow CoFe@HCNFs microwave absorbing material prepared in Example 2 of the present invention when the filling amount is 5wt%. When the matching thickness is 3.2mm, the reflection loss value of the hollow CoFe@HCNFs microwave absorbing material is -21.9dB, and the maximum effective absorption bandwidth of 6.0GHz is achieved when the thickness is 2.5mm.
[0140] Figure 4 The reflection loss diagram of the CoFe@CNFs microwave absorbing material prepared in Comparative Example 1 of the present invention when the filling amount is 5wt%. The CoFe@CNFs microwave absorbing material achieved a reflection loss value of -17.6dB and a maximum effective absorption bandwidth of 6.0GHz. The only difference between Comparative Example 1 and Example 2 is that no PS is added, so the fiber in the obtained microwave absorbing material is a non-hollow structure ( Figure 5 ). By comparing Example 2 with Comparative Example 1, it can be seen that the reflection loss of the microwave absorbing material of Comparative Example 1 is weaker than that of Example 2, indicating that the hollow structure can enhance the multiple reflection and scattering capabilities of electromagnetic waves, which is conducive to enhancing the absorption of electromagnetic waves.
[0141] Figure 6The reflection loss diagram of the vulcanized hollow CoFe@HCNFs microwave absorbing material prepared by the embodiment with the best performance of the present invention (Example 5) when the filling amount is 5wt%. When the matching thickness is 3.2mm, the vulcanized hollow CoFe@HCNFs microwave absorbing material has a reflection loss value of -54.7dB, and a maximum effective absorption bandwidth of 8.0GHz is achieved at a thickness of 2.5mm, showing excellent microwave absorption performance. The only difference between Example 5 and Example 2 is the addition of the final vulcanization step. By comparing Example 5 and Example 2, it can be seen that the reflection loss of the microwave absorbing material of Example 5 is significantly stronger than that of Example 2, indicating that vulcanization increases the types of components and constructs a rich heterogeneous interface, which is beneficial to improving the interface polarization and dissipating electromagnetic waves.
[0142] Figure 7 The real part of the dielectric loss of the sulfided hollow CoFe@HCNFs microwave absorbing material prepared in the embodiment with the best performance of the present invention (Example 5) is shown in Figure 2. In the range of 2-18 GHz, the real part of the dielectric loss decreases from 9.9 to 3.7, showing an overall downward trend.
[0143] Figure 8 The imaginary part of the dielectric loss of the sulfided hollow CoFe@HCNFs microwave absorbing material prepared in the embodiment with the best performance of the present invention (Example 5) shows that the curve fluctuates to a certain extent in the high frequency band, indicating that there is a synergistic effect of multiple polarization mechanisms in this frequency band.
[0144] Fig. 9 The dielectric loss tangent diagram of the sulfided hollow CoFe@HCNFs microwave absorbing material prepared in the embodiment with the best performance (Example 5) of the present invention shows that the sulfided hollow CoFe@HCNFs microwave absorbing material exhibits good dielectric loss capability.
[0145] Fig.10 The real part of the magnetic loss of the sulfided hollow CoFe@HCNFs microwave absorbing material prepared in the embodiment with the best performance of the present invention (Example 5) is about 1.07 in the low frequency band and about 1.48 in the high frequency band.
[0146] Fig.11 The imaginary part of the magnetic loss of the sulfided hollow CoFe@HCNFs microwave absorbing material prepared in the embodiment with the best performance of the present invention (Example 5) can be seen that the magnetic loss capacity gradually decreases with the increase of frequency.
[0147] Fig.12 The magnetic loss tangent diagram of the sulfided hollow CoFe@HCNFs microwave absorbing material prepared in the embodiment with the best performance (Example 5) of the present invention has an overall trend similar to that of the magnetic loss imaginary part diagram.
[0148] The reason why the sulfided hollow CoFe@HCNFs microwave absorbing material prepared by the present invention exhibits excellent absorbing performance is that: first, the conductive network formed by the 3D fiber structure and the formation of the Co7Fe3 alloy significantly increase the conductive loss energy of the material, and the construction of the hollow porous structure of the 1D fiber not only enhances the multiple reflection and scattering capabilities of electromagnetic waves, but also adjusts the dielectric constant, thereby optimizing impedance matching. It is worth noting that the overall density of the material is also reduced. Secondly, a very rich heterogeneous interface is provided between Co3S4, Co7Fe3 alloy, carbon component and paraffin (the medium used in the test), resulting in enhanced interface polarization.
[0149] The contents of the present invention can be further clearly understood through the above-given embodiments, but they are not intended to limit the present invention.
Claims
1. A method for preparing a hollow CoFe@HCNFs microwave absorbing material, characterized in that: The following steps are involved: S1, ZIF67 cubes were reacted with K3[Fe(CN6)] by ion exchange method to obtain ZIF67@CoFe-PBA cubes; S2, ZIF67@CoFe-PBA cubes were mixed with polyacrylonitrile powder and polystyrene in a solvent and electrospun to obtain ZIF67@CoFe-PBA / PAN PS fibers; S3, pre-oxidation and carbonization of ZIF67@CoFe-PBA / PAN PS fibers to obtain hollow CoFe@HCNFs composites.
2. The method for preparing the sulfided hollow CoFe@HCNFs microwave absorbing material according to claim 1, characterized in that: In S1, the ZIF67 cube is prepared by: dissolving Co(NO3)2·6H2O and hexadecyltrimethylammonium bromide in water to obtain solution A; dissolving 2-methylimidazole in water to form solution B; Solution A was added to solution B, and the reaction was stirred. The resulting product was washed to obtain ZIF67 cubes.
3. The method for preparing the sulfided hollow CoFe@HCNFs microwave absorbing material according to claim 1, characterized in that: S1 is specifically as follows: ZIF67 cubes are dispersed in anhydrous ethanol to obtain solution C; K3[Fe(CN6)] is dissolved in water to form solution D; solution D is poured into solution C, stirred, and the obtained product is washed to obtain ZIF67@CoFe-PBA cubes.
4. The method for preparing the sulfided hollow CoFe@HCNFs microwave absorbing material according to claim 1, characterized in that: In S2, the positive voltage used for electrospinning is 10 to 20 kV.
5. The method for preparing the sulfided hollow CoFe@HCNFs microwave absorbing material according to claim 1, characterized in that: In S3, the pre-oxidation temperature is 200-280°C, and the time is 1-3 hours; the carbonization temperature is 600-900°C, and the time is 1-6 hours.
6. The method for preparing the sulfided hollow CoFe@HCNFs microwave absorbing material according to claim 1, characterized in that: Also includes: S4, mixing thioacetamide and the hollow CoFe@HCNFs composite material in water, performing a hydrothermal reaction, and obtaining a sulfurized hollow CoFe@HCNFs microwave absorbing material.
7. The method for preparing the sulfided hollow CoFe@HCNFs microwave absorbing material according to claim 6, characterized in that: In S4, the temperature of the hydrothermal reaction is 100-200°C and the time is 4-12 hours.
8. The method for preparing the sulfided hollow CoFe@HCNFs microwave absorbing material according to claim 6, characterized in that: In S4, the mass ratio of the hollow CoFe@HCNFs composite material to thioacetamide is 1:(0-15).
9. A hollow CoFe@HCNFs microwave absorbing material obtained by the preparation method according to any one of claims 1 to 8.
10. Use of the hollow CoFe@HCNFs microwave absorbing material according to claim 9 in electromagnetic wave absorption.