A kind of reduced-shrinkage phosphate-based water reducer and preparation method thereof
By introducing small molecule alcohols with hydrophobic modified polyether segments and ester bond grafts into the water reducer, the problem of insufficient adaptability of existing reduced-reduced polycarboxylic acid water reducer is solved, and low dosage and high amount are achieved The water reduction rate and good slump retention performance significantly reduce the dry shrinkage of concrete and improve the mechanical properties and adaptability of concrete.
Patent Information
- Application Number
- CN202311220986.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-09-21
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2043-09-21
AI Technical Summary
The existing reduction-type polycarboxylic acid water reducing agent has adaptability problems with cement, machined sand and mineral blends in actual projects. The mud content in sand and gravel has a significant impact on its performance, which limits its application. scope.
By introducing small molecule alcohols grafted with hydrophobic modified polyether segments and ester bonds, a reduced-reducing phosphate-based water reducer was prepared to reduce the surface tension of the pore solution and achieve a unified effect of water reduction and reduction.
The reduced-shrinkage phosphate-based water reducing agent has low dosage, high water reduction rate and good slump retention performance. It can effectively reduce the drying and shrinkage of concrete, improve the mechanical properties of concrete, and show good bubble stabilization and adaptability.
Smart Images

Figure BDA0004460578420000021 
Figure BDA0004460578420000022 
Figure BDA0004460578420000031
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of concrete admixtures in building materials, and in particular to a reduced-shrinkage phosphate-based water reducer and a preparation method thereof. Background Art
[0002] How to reduce or prevent concrete from cracking or fissures due to drying shrinkage is a research topic of great interest to concrete workers in various countries. In order to reduce the shrinkage of concrete and control the strength reduction caused by internal defects of concrete, researchers have developed concrete expansion agents and shrinkage reducers. Among them, concrete expansion agents are an important way to solve the shrinkage of concrete and have been widely used in shrinkage compensating concrete, self-stressed concrete and shrinkage-free self-flowing grouting materials. However, since many expansion agents may cause alkali-aggregate reaction in concrete, shrinkage reducers that can both reduce concrete shrinkage and avoid alkali-aggregate reaction have become a key research direction. Shrinkage reducers can significantly reduce the early shrinkage of concrete, mainly by reducing the surface tension in the pore solution and reducing the shrinkage stress generated when the capillaries lose water.
[0003] Some shrinkage reducers reported in the early period were mainly small-molecule alcohols, ethers, and alcohol amines. These shrinkage reducers have high dosages and do not reduce water. Directly adding them into concrete shrinkage reducers will have an adverse effect on concrete strength, increase the cost of concrete, and be detrimental to the construction of large-volume concrete. Therefore, it is necessary to study shrinkage-reducing water reducers. Polycarboxylate water reducers have become the first choice for shrinkage-reducing water reducers due to their unique advantages of molecular structure and designable performance.
[0004] Patent CN116023599A introduces a shrinkage-reducing polycarboxylic acid water-reducing agent and a preparation method thereof, which is prepared by free copolymerization of a multi-block structure polyether monomer, a hyperbranched functional monomer, a vinyl polyoxyethylene ether macromonomer, and an unsaturated acid, and has good dispersibility, collapse retention, and shrinkage-reducing properties.
[0005] Patent CN115043608B introduces a shrinkage-reducing water-reducing agent for building concrete and its preparation method, which is compounded by polyglycerol-modified polycarboxylic acid water-reducing agent, anti-segregation agent and modified polycarboxylic acid slump-retaining agent, wherein the polyglycerol-modified polycarboxylic acid water-reducing agent with shrinkage-reducing function is obtained by introducing polyglycerol into the esterification product of maleic anhydride and ethylene glycol monoethyl ether after modification and then grafting it onto the polycarboxylic acid main chain as a whole. The prepared shrinkage-reducing water-reducing agent can reduce the surface tension of the solution, effectively reduce the drying shrinkage of concrete, and further improve the mechanical properties of the concrete. In addition, it also has good foam stabilization performance, so that the concrete has good workability.
[0006] However, in actual engineering use, the above shrinkage-reducing polycarboxylate water-reducing agents often have compatibility problems with cement, machine-made sand, and mineral admixtures (fly ash, mineral powder, etc.). The mud content in sand and gravel also has a significant impact on the performance of polycarboxylate water-reducing agents, which greatly restricts the application of shrinkage-reducing polycarboxylate water-reducing agents. Therefore, it is necessary to develop a more adaptable shrinkage-reducing water-reducing agent to meet actual needs. Summary of the invention
[0007] In view of this, the object of the present invention is to provide a shrinkage-reducing phosphate-based water reducer and a preparation method thereof, wherein the water reducer improves the surface tension of the pore solution by introducing a hydrophobically modified polyether segment and an ester-grafted small molecule alcohol shrinkage reducer, and finally obtains a shrinkage-reducing phosphate-based water reducer with both shrinkage and water reduction properties.
[0008] Based on the above objectives, in a first aspect, the present invention provides a shrinkage-reducing phosphate-based water reducer, which comprises the following components: a hydrophobically modified polyether monomer A, a polyether phosphate ester monomer B, an esterified small monomer C, an aldehyde monomer D and an acid catalyst E.
[0009] As a further embodiment of the present invention, the hydrophobically modified polyether monomer A is a hydrophobically modified polyether monomer, and its structural formula is shown in (I):
[0010]
[0011] Wherein R1 is H or an alkyl group of 1 to 3 carbon atoms; n is the average added mole number of propylene oxide, and n is an integer of 1 to 6; m is the average added mole number of ethylene oxide, and m is an integer of 10 to 100; and the condition of mn≥7 is satisfied.
[0012] As a further embodiment of the present invention, the polyether phosphate monomer B is a polyether phosphate monomer having a structural formula as follows:
[0013] (II) as shown:
[0014]
[0015] wherein r is the average number of added moles of ethylene oxide, and r is an integer of 4 to 8.
[0016] As a further embodiment of the present invention, the structural formula of the esterified small monomer C is shown in (III):
[0017]
[0018] Wherein R2 is a C1-C8 alkyl group; p is the average number of added moles of propylene oxide, and p is 0, 1 or 2; q is the average number of added moles of ethylene oxide, and q is an integer of 2-6.
[0019] As a further embodiment of the present invention, the structural formula of the aldehyde monomer D is R3CHO.
[0020] As a further embodiment of the present invention, the aldehyde monomer D is selected from any one of formaldehyde, paraformaldehyde and acetaldehyde;
[0021] The acid catalyst E is selected from any one of concentrated sulfuric acid, benzenesulfonic acid, methanesulfonic acid, p-toluenesulfonic acid, and ethylsulfonic acid, or a combination of two of them in any proportion.
[0022] In a second aspect, the present invention provides a method for preparing a shrinkage-reducing phosphate-based water reducer, comprising the following steps:
[0023] Place hydrophobically modified polyether monomer A, polyether phosphate monomer B, and esterified small monomer C in a reaction container under nitrogen protection;
[0024] Heat to 80-90℃, stir evenly after melting;
[0025] Then, the temperature is raised to 120-140°C, and the acid catalyst E and aldehyde monomer D are added, and refluxed at normal pressure for 4-8 hours;
[0026] After the reaction is completed, the temperature is slowly lowered to 70°C, liquid alkali is used for neutralization, and water is added for dilution to obtain a reduced-shrinkage phosphate-based water reducer.
[0027] As a further embodiment of the present invention, the acid catalyst E is used in an amount of 0.5-3% of the total mass of the hydrophobically modified polyether monomer A, the polyether phosphate monomer B, the esterified small monomer C and the aldehyde monomer D.
[0028] As a further embodiment of the present invention, the hydrophobically modified polyether monomer A, polyether phosphate monomer B, esterified small monomer C, and aldehyde monomer D are condensed in a molar ratio of a:b:c:d, wherein the molar ratio of a:b:c is 1:1-4:1-1.5; and the molar ratio of (a+b+c):d is 1.05-1.4:1.
[0029] As a further embodiment of the present invention, the weight average molecular weight of the shrinkage-reducing phosphate-based water reducer ranges from 10,000 to 100,000, the pH value of the shrinkage-reducing phosphate-based water reducer ranges from 5.0 to 6.0, and the solid content ranges from 30 to 50%.
[0030] Compared with the prior art, the present invention provides a reduced-shrinkage phosphate-based water reducer and a preparation method thereof, which has the following beneficial effects:
[0031] (1) The present invention provides a shrinkage-reducing phosphate-based water reducer and a preparation method thereof. The prepared shrinkage-reducing phosphate-based water reducer has low dosage, high water reduction rate, good collapse retention performance, excellent shrinkage reduction effect, and realizes the unity of water reduction and shrinkage reduction.
[0032] (2) The present invention introduces a hydrophobically modified polyether segment and a small molecule alcohol connected by an ester bond into the structure of the phosphate-based water reducer to reduce the surface tension of the pore solution and the concentration of alkaline ions, thereby achieving the shrinkage reduction function.
[0033] These and other aspects of the present application will be more concise and understandable in the following description of the embodiments. It should be understood that the above general description and the following detailed description are only exemplary and explanatory and cannot limit the present application. DETAILED DESCRIPTION
[0034] The present invention is described in detail below by examples, which are merely illustrative and do not limit the scope of application of the present invention. According to the disclosure herein, those skilled in the art can change the reagents, catalysts and reaction process conditions within the scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.
[0035] The present invention is achieved through the following technical solutions:
[0036] The present invention provides a method for preparing a shrinkage-reducing phosphate-based water reducer, which is prepared by polycondensation reaction of a hydrophobically modified polyether monomer A, a polyether phosphate monomer B, an esterified small monomer C, and an aldehyde monomer D;
[0037] The monomer A described in the present invention is a phenol polyether monomer, which is obtained by sequentially adding phenol or phenoxyethanol to propylene oxide and ethylene oxide, and can be prepared according to the method described in the public literature or patents;
[0038] The monomer B is a modified phenol polyether containing a phosphoric acid group, which is prepared by modifying the phenol polyether through a phosphorylation reaction, and can be prepared according to the method described in the public literature or patent;
[0039] The esterified small monomer C is benzoate, which is prepared by the esterification reaction of benzoic acid and a small molecule alcohol, and can be prepared according to the method described in the public literature or patent;
[0040] The aldehyde monomer D is selected from any one of formaldehyde, paraformaldehyde and acetaldehyde;
[0041] The weight average molecular weight of the shrinkage-reducing phosphate-based water reducer of the present invention is in the range of 10,000 to 100,000. If the weight average molecular weight is too large or too small, the water reduction and slump retention performances will be deteriorated.
[0042] The shrinkage-reducing phosphate-based water reducer of the present invention can be used alone or in combination with aminosulfonic acid-based water reducers, polycarboxylic acid water reducers, etc. on the market. It can also be added with air entraining agents, retarders, early strength agents, thickening and water-retaining agents, retarders and defoamers for compounding.
[0043] The invention provides a method for preparing a shrinkage-reducing phosphoric acid-based water reducer, which is prepared by polycondensation reaction of hydrophobically modified polyether monomer A, polyether phosphate monomer B, esterified small monomer C and aldehyde monomer D. The specific steps are: placing the hydrophobically modified polyether monomer A, polyether phosphate monomer B and esterified small monomer C in a reaction container under nitrogen protection, heating to 80-90 DEG C, stirring evenly after melting, then heating to 120-140 DEG C, adding acid catalyst E and aldehyde monomer D, reflux at normal pressure for 4-8 hours, slowly cooling to 70 DEG C after the reaction is completed, neutralizing with liquid alkali, and diluting with water to obtain the shrinkage-reducing phosphoric acid-based water reducer, wherein the pH value of the water reducer is 5.0-6.0 and the solid content is 30-50%.
[0044] The raw materials used in the examples are listed in Table 1, as follows:
[0045] Table 1 Compound codes in the synthetic examples
[0046]
[0047] The information of the reduced-type phosphate-based water reducer in the embodiment is listed in Table 2, as follows:
[0048] Table 2 Information table of reduced phosphate-based water reducer
[0049]
[0050] Example 1
[0051] 1 mol of hydrophobically modified polyether monomer A-1, 1 mol of polyether phosphate monomer B-3 and 1 mol of esterified small monomer C-1 were placed in a reaction vessel under nitrogen protection, heated to 80°C, stirred evenly after melting, then heated to 120°C, acid catalyst E-1 (3% of the total mass of monomers A, B, C and D) and 2.857 mol of aldehyde monomer D-1 were added, refluxed at normal pressure for 8 hours, and after the reaction was completed, the temperature was slowly lowered to 70°C, neutralized with liquid alkali, diluted with water to obtain a reduced-shrinkage phosphate-based water reducer PSRA-1, with a measured pH value of 5.0 and a solid content of 30%.
[0052] Example 2
[0053] 1 mol of hydrophobically modified polyether monomer A-2, 2 mol of polyether phosphate monomer B-1, and 1.1 mol of esterified small monomer C-3 are placed in a reaction vessel under nitrogen protection, heated to 85°C, stirred evenly after melting, then heated to 130°C, acid catalyst E-2 (2.5% of the total mass of monomers A, B, C, and D) and 2.929 mol of aldehyde monomer D-1 are added, refluxed at normal pressure for 6 hours, and after the reaction is completed, slowly cooled to 70°C, neutralized with liquid alkali, diluted with water to obtain a reduced-shrinkage phosphate-based water reducer PSRA-2, with a measured pH value of 5.3 and a solid content of 35%.
[0054] Example 3
[0055] 1 mol of hydrophobically modified polyether monomer A-3, 3 mol of polyether phosphate monomer B-3, and 1.3 mol of esterified small monomer C-2 are placed in a reaction vessel under nitrogen protection, heated to 90°C, stirred evenly after melting, then heated to 140°C, and acid catalyst E-3 (1% of the total mass of monomers A, B, C, and D) and 4.077 mol of aldehyde monomer D-2 are added. Reflux at normal pressure for 4 hours. After the reaction is completed, the temperature is slowly lowered to 70°C, neutralized with liquid alkali, and diluted with water to obtain a reduced-shrinkage phosphate-based water reducer PSRA-3. The pH value is measured to be 6.0 and the solid content is 40%.
[0056] Example 4
[0057] 1 mol of hydrophobically modified polyether monomer A-4, 4 mol of polyether phosphate monomer B-2, and 1.5 mol of esterified small monomer C-1 are placed in a reaction vessel under nitrogen protection, heated to 90°C, stirred evenly after melting, then heated to 125°C, acid catalyst E-4 (0.5% of the total mass of monomers A, B, C, and D) and 5.2 mol of aldehyde monomer D-3 are added, refluxed at normal pressure for 5 hours, and after the reaction is completed, slowly cooled to 70°C, neutralized with liquid alkali, diluted with water, and a reduced-shrinkage phosphate-based water reducer PSRA-4 is obtained. The pH value is measured to be 5.5 and the solid content is 45%.
[0058] Example 5
[0059] 1 mol of hydrophobically modified polyether monomer A-1, 1 mol of polyether phosphate monomer B-2, and 1.2 mol of esterified small monomer C-1 are placed in a reaction vessel under nitrogen protection, heated to 80°C, stirred evenly after melting, then heated to 125°C, acid catalyst E-5 (2% of the total mass of monomers A, B, C, and D) and 3.047 mol of aldehyde monomer D-1 are added, refluxed at normal pressure for 7 hours, and after the reaction is completed, slowly cooled to 70°C, neutralized with liquid alkali, diluted with water to obtain a reduced-shrinkage phosphate-based water reducer PSRA-5, with a measured pH value of 5.8 and a solid content of 50%.
[0060] Example 6
[0061] 1 mol of hydrophobically modified polyether monomer A-1, 3.5 mol of polyether phosphate monomer B-2, and 1 mol of esterified small monomer C-3 are placed in a reaction vessel under nitrogen protection, heated to 80°C, stirred evenly after melting, then heated to 135°C, acid catalyst E-1 (2.5% of the total mass of monomers A, B, C, and D) and 4.583 mol of aldehyde monomer D-3 are added, refluxed at normal pressure for 4.5 hours, and after the reaction is completed, slowly cooled to 70°C, neutralized with liquid alkali, and diluted with water to obtain a reduced-shrinkage phosphate-based water reducer PSRA-6, with a measured pH value of 5.1 and a solid content of 45%.
[0062] Example 7
[0063] 1 mol of hydrophobically modified polyether monomer A-1, 4 mol of polyether phosphate monomer B-1, and 1.4 mol of esterified small monomer C-3 are placed in a reaction vessel under nitrogen protection, heated to 85°C, stirred evenly after melting, then heated to 120°C, and acid catalyst E-1 (2% of the total mass of monomers A, B, C, and D) and 4.571 mol of aldehyde monomer D-1 are added, refluxed at normal pressure for 5 hours, and after the reaction is completed, slowly cooled to 70°C, neutralized with liquid alkali, and diluted with water to obtain a reduced-shrinkage phosphate-based water reducer PSRA-7, with a measured pH value of 5.6 and a solid content of 40%.
[0064] Example 8
[0065] 1 mol of hydrophobically modified polyether monomer A-4, 2.5 mol of polyether phosphate monomer B-1, and 1 mol of esterified small monomer C-3 are placed in a reaction vessel under nitrogen protection, heated to 90°C, stirred evenly after melting, then heated to 135°C, acid catalyst E-2 (1.5% of the total mass of monomers A, B, C, and D) and 3.462 mol of aldehyde monomer D-1 are added, refluxed at normal pressure for 7 hours, and after the reaction is completed, slowly cooled to 70°C, neutralized with liquid alkali, and diluted with water to obtain a reduced-shrinkage phosphate-based water reducer PSRA-8, with a measured pH value of 5.4 and a solid content of 40%.
[0066] Example 9
[0067] 1 mol of hydrophobically modified polyether monomer A-2, 3 mol of polyether phosphate monomer B-1, and 1.25 mol of esterified small monomer C-1 were placed in a reaction vessel under nitrogen protection, heated to 80°C, stirred evenly after melting, then heated to 130°C, and acid catalyst E-4 (2% of the total mass of monomers A, B, C, and D) and 4.773 mol of aldehyde monomer D-2 were added, refluxed at normal pressure for 6 hours, and after the reaction was completed, the temperature was slowly lowered to 70°C, neutralized with liquid alkali, and diluted with water to obtain a reduced-shrinkage phosphate-based water reducer PSRA-9, with a measured pH value of 6 and a solid content of 40%.
[0068] Comparative Example 1
[0069] The monomer A-1 in Example 1 for synthesizing the shrinkage-reducing phosphate-based water reducer was replaced with phenol polyether (R1=H, n=0, m=100), and the other reaction conditions remained unchanged to obtain the water reducer PC-1.
[0070] Comparative Example 2
[0071] The monomer C-1 in Example 4 for synthesizing the shrinkage-reducing phosphate-based water reducer was removed, and the other reaction conditions remained unchanged to obtain the water reducer PC-2.
[0072] Comparative Example 3
[0073] The conventional commercially available polycarboxylate water-reducing agent PCA is denoted as PC-3.
[0074] Comparative Example 4
[0075] The commercially available BHY-2A concrete shrinkage-reducing water reducer is denoted as PC-4.
[0076] Application Example 1
[0077] The effects of the reduced-shrinkage phosphate-based water reducer prepared in the examples and the comparative water reducer on the fluidity of fresh cement paste and its loss over time were evaluated. The cement paste fluidity test was carried out in accordance with the GB / T8077-2000 standard, with a fixed water-cement ratio of 0.29. The experimental results are shown in Table 3.
[0078] Table 3 Effect of different water reducing agents on the fluidity of fresh cement paste and its loss over time
[0079]
[0080]
[0081] Conch cement, Onoda cement and Helin cement were used to carry out the pure paste test respectively. It can be seen from the data in Table 3 that the comparative examples PC-3 and PC-4 have unstable fluidity in different cements under the condition of 0.11% dosage, and the retention performance is not as good as that of the reduced-shrinkage phosphate-based water reducer PSRA-1~9. In Onoda cement, the initial fluidity of PC-3 is 232mm, and the pure paste fluidity of 60min becomes 167mm, which is a great loss; in Helin cement, the initial fluidity of PC-3 is 215mm, and the pure paste fluidity of 60min becomes 153mm, which is a great loss. The reduced-shrinkage phosphate-based water reducer PSRA-1~9 and the comparative example PC-1 / 2 prepared by the present invention have good dispersibility and retention performance under the condition of 0.11% dosage, have good adaptability to the three cements, and show low sensitivity.
[0082] Application Example 2
[0083] The effects of the shrinkage-reducing phosphate-based water reducer prepared in the embodiment and the comparative water reducer on the performance and shrinkage properties of fresh concrete were evaluated. The cement used was Onoda 52.5PII Portland cement, the sand was medium sand with a fineness modulus Mx=2.6, and the gravel was continuously graded crushed stone with a particle size of 5-20 mm. The cement dosage in the concrete mix ratio was 360Kg / m3, the sand ratio was 36-40%, and the water consumption was the minimum water consumption when the slump was (210±10) mm, including the water contained in the admixture and sand and gravel materials. According to GB / 8076-2008 "Concrete Admixtures", the slump and expansion of the concrete were tested; according to GBT / 50082-2009 "Standard for Test Methods for Long-term Performance and Durability of Ordinary Concrete", the shrinkage of the concrete was tested, and the experimental results are shown in Table 4.
[0084] Table 4 Effects of different water reducing agents on the properties and shrinkage of fresh concrete
[0085]
[0086]
[0087] As can be seen from Table 4, the comparative example PC-1 lacks the modified hydrophobic polyether segment. Compared with the example PSRA-1, the concrete water reduction and slump retention performances are basically the same, and the 28-day drying shrinkage reduction rate is significantly reduced, indicating that the modified hydrophobic segment has a significant shrinkage reduction effect; the comparative example PC-2 lacks the ester-grafted small molecule alcohols. Compared with the example PSRA-4, the concrete water reduction and slump retention performances are basically the same, and the 28-day drying shrinkage reduction rate is significantly reduced, indicating that the small molecule alcohol in the esterified small monomer structure will fall off into the paste pore solution under the alkaline environment of the cement paste to play a shrinkage reduction role; the concrete retention performance of the example PC-3 is poor, and the 28-day drying shrinkage rate is much lower than the shrinkage-reducing phosphate-based water reducer prepared by the present invention; the concrete retention performance of the example PC-4 is also poor, and the 28-day drying shrinkage rate is also lower than the shrinkage-reducing phosphate-based water reducer prepared by the present invention. It can be clearly seen that the introduction of modified hydrophobic polyether segments and ester-grafted small molecule alcohols can significantly improve the shrinkage reduction performance of the water reducer. At the same time, the shrinkage-reducing phosphate-based water reducer prepared by the present invention exhibits better retention performance and cement adaptability than the carboxylic acid group in the polycarboxylic acid water reducer due to the presence of the phosphate group.
[0088] A person skilled in the art should understand that the discussion of any of the above embodiments is only exemplary and is not intended to imply that the scope of the disclosure of the embodiments of the present invention (including the claims) is limited to these examples; under the concept of the embodiments of the present invention, the technical features in the above embodiments or different embodiments can also be combined, and there are many other changes in different aspects of the embodiments of the present invention as above, which are not provided in detail for the sake of simplicity. Therefore, any omissions, modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the embodiments of the present invention should be included in the protection scope of the embodiments of the present invention.
Claims
1. A reduced-shrinkage phosphate-based water reducer, characterized in that: The water reducing agent comprises the following components: a hydrophobically modified polyether monomer A, a polyether phosphate monomer B, an esterified small monomer C, an aldehyde monomer D and an acid catalyst E. The hydrophobically modified polyether monomer A is a hydrophobically modified polyether monomer, and its structural formula is shown in (I): Wherein R1 is H or an alkyl group of 1 to 3 carbon atoms; n is the average number of added moles of propylene oxide, and n is an integer of 1 to 6; m is the average number of added moles of ethylene oxide, and m is an integer of 10 to 100; and the condition of mn≥7 is satisfied, and the polyether phosphate monomer B is a polyether phosphate monomer, and its structural formula is shown in (II): Wherein r is the average number of moles of ethylene oxide added, and r is an integer from 4 to 8, The structural formula of the esterified small monomer C is shown in (III): wherein R2 is a C1-C8 alkyl group; p is the average number of added moles of propylene oxide, and p is 0, 1 or 2; q is the average number of added moles of ethylene oxide, and q is an integer of 2 to 6; The hydrophobically modified polyether monomer A, polyether phosphate monomer B, esterified small monomer C, and aldehyde monomer D are polycondensed according to the molar ratio of a:b:c:d, wherein the molar ratio of a:b:c is 1:1-4:1-1.5; the molar ratio of (a+b+c):d is 1.05-1.4:
1.
2. A shrinkage-reducing phosphate-based water reducer according to claim 1, characterized in that: The aldehyde monomer D is selected from any one of formaldehyde, paraformaldehyde and acetaldehyde; The acid catalyst E is selected from any one of concentrated sulfuric acid, benzenesulfonic acid, methanesulfonic acid, p-toluenesulfonic acid, and ethylsulfonic acid, or a combination of two of them in any proportion.
3. A method for preparing a reduced-shrinkage phosphate-based water reducer, characterized in that: The following steps are involved: Place hydrophobically modified polyether monomer A, polyether phosphate monomer B, and esterified small monomer C in a reaction container under nitrogen protection; Heat to 80-90℃, stir evenly after melting; Then, the temperature is raised to 120-140°C, and the acid catalyst E and aldehyde monomer D are added, and refluxed at normal pressure for 4-8 hours; After the reaction is completed, the temperature is slowly lowered to 70°C, liquid alkali is used for neutralization, and water is added for dilution to obtain a reduced-shrinkage phosphate-based water reducer; Wherein, the hydrophobically modified polyether monomer A is a hydrophobically modified polyether monomer, and its structural formula is shown in (I): Wherein R1 is H or an alkyl group of 1 to 3 carbon atoms; n is the average number of added moles of propylene oxide, and n is an integer of 1 to 6; m is the average number of added moles of ethylene oxide, and m is an integer of 10 to 100; and the condition of mn≥7 is satisfied, and the polyether phosphate monomer B is a polyether phosphate monomer, and its structural formula is shown in (II): Wherein r is the average number of moles of ethylene oxide added, and r is an integer from 4 to 8, The structural formula of the esterified small monomer C is shown in (III): wherein R2 is a C1-C8 alkyl group; p is the average number of added moles of propylene oxide, and p is 0, 1 or 2; q is the average number of added moles of ethylene oxide, and q is an integer of 2 to 6; The hydrophobically modified polyether monomer A, polyether phosphate monomer B, esterified small monomer C, and aldehyde monomer D are polycondensed according to the molar ratio of a:b:c:d, wherein the molar ratio of a:b:c is 1:1-4:1-1.5; the molar ratio of (a+b+c):d is 1.05-1.4:
1.
4. The method for preparing the reduced-shrinkage phosphate-based water reducer according to claim 3, characterized in that: The amount of the acid catalyst E used is 0.5-3% of the total mass of the hydrophobically modified polyether monomer A, the polyether phosphate monomer B, the esterified small monomer C and the aldehyde monomer D.
5. The method for preparing the reduced-shrinkage phosphate-based water reducer according to claim 3, characterized in that The weight average molecular weight of the shrinkage-reducing phosphate-based water reducer ranges from 10,000 to 100,000, the pH value of the shrinkage-reducing phosphate-based water reducer is 5.0-6.0, and the solid content is 30-50%.