Laminated solar cell module, preparation method thereof and photovoltaic system
Patent Information
- Application Number
- CN202411023849.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-29
- Publication Date
- 2024-11-12
AI Technical Summary
[0004]本申请提供一种叠层太阳能电池组件及其制备方法和光伏系统,以解决或缓解上面提出的一项或更多项技术问题
[0009] In the first aspect of this application, through stacked cell design, a top cell is introduced on the front side of the silicon substrate. The top cell itself has several functional layers. The existence of each functional layer hinders the Na + Diffusion to the front side of the silicon substrate; in addition, TaO is introduced on the back side of the silicon substrate x layer, TaO x The layer can provide additional free electrons, which can effectively promote the collection and transmission of electrons and suppress carrier recombination at the interface. + The diffusion also acts as a barrier. The first aspect of this application can inhibit Na + The risk of migration from the transparent glass layer to the surface of the silicon substrate creates a PID effect, reducing corrosion of the silicon substrate.
Smart Images

Figure CN118946177A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of solar cells, and in particular to a laminated solar cell assembly and a preparation method thereof and a photovoltaic system. Background Art
[0002] Further reducing the levelized cost of energy (LCE) of photovoltaic (PV) and improving the reliability and durability of photovoltaic modules have become research trends. In the field of crystalline silicon photovoltaics, various external stress sources such as high temperature and humidity may cause catastrophic failure of photovoltaic equipment. Among them, potential induced degradation (PID) is one of the stressors with the greatest negative impact. PID is caused by the high system voltage generated by the series connection of system-level photovoltaic modules. For silicon solar cells, PID manifests itself in different forms. The first form is that there is a potential difference between the battery and the aluminum module frame (or, a potential difference is generated between the battery and the ground), which will drive the Na + The formation of an electrical shunt path (PID-s (shunt)) on the silicon substrate from the transparent glass layer through the laminate and the device pn junction will lead to a loss of fill factor (FF). The second form is PID polarization, which is caused by the accumulation of metal ions in the module transparent glass layer passivation / anti-reflection coating stack. It is reported that PID polarization exists in a variety of silicon solar cell architectures, including p-type bifacial passivated emitter rear contact (bifacial p-PERC), n-type passivated emitter, rear fully diffused (n-PERT) and n-type integrated back contact (IBC) solar cells. The third form is corrosion PID (PID-c (corrosion)), which has two factors: 1. A large amount of charge accumulates in the cell to form an electric field opposite to the passivation field, which deteriorates the passivation effect on the cell surface; 2. The corrosion effect caused by the electrochemical reaction of the dielectric layer, transparent conductive oxide film or metal contact. Corrosion PID is a physical damage and belongs to the irreversible PID effect in solar cells. The open circuit voltage, short circuit current and power reduction caused by PID-c are irreversible.
[0003] It should be noted that the above content is not necessarily prior art, nor is it intended to limit the scope of patent protection of this application. Summary of the invention
[0004] The present application provides a laminated solar cell module and a preparation method thereof and a photovoltaic system to solve or alleviate one or more technical problems raised above.
[0005] The first aspect of the present application provides a laminated solar cell assembly, comprising:
[0006] Transparent glass layer, top cell, bottom cell, backplane, and frame;
[0007] The bottom cell comprises a crystalline silicon cell, the crystalline silicon cell comprises a silicon substrate, and the back side of the silicon substrate is provided with TaO x layer;
[0008] The top cell and the bottom cell are stacked and encapsulated as a whole in a space surrounded by the back plate, the transparent glass layer and the frame. Sealant is filled between the top cell, the bottom cell and the back plate, between the top cell, the bottom cell and the transparent glass layer, and between the top cell, the bottom cell and the frame.
[0009] In the first aspect of the present application, a top cell is introduced on the front side of the silicon substrate through a stacked cell design. The top cell itself has several functional layers. The existence of each functional layer hinders the Na + Diffusion to the front of the silicon substrate; in addition, TaO is introduced to the back of the silicon substrate x layer, TaO x The layer can provide additional free electrons, which can effectively promote the collection and transmission of electrons and inhibit the carrier recombination at the interface. + The diffusion of Na can also play a blocking role. In the first aspect of the present application, it can inhibit + The risk of PID effect generated by migration from the transparent glass layer to the surface of the silicon substrate is reduced, thereby reducing corrosion to the silicon substrate.
[0010] A second aspect of the present application provides a method for preparing a laminated solar cell assembly, comprising the following operations:
[0011] Provides top cell, sealant, backsheet, and clear glass layers;
[0012] The bottom cell is provided in the following manner: TaO is deposited on the back side of the silicon substrate x layer, in the TaO x Depositing a gate line layer on a side away from the silicon substrate;
[0013] Laminating the top cell and the bottom cell to obtain a cell sheet;
[0014] The battery cell or the battery string including the battery cell, the sealant, the back plate and the transparent glass layer are laminated, and then a frame is installed to assemble into a laminated solar cell module.
[0015] The laminated solar cell module prepared in the embodiment of the second aspect of the present application has excellent anti-PID performance while having the advantages of the laminated cell itself. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] In the accompanying drawings, unless otherwise specified, the same reference numerals throughout the multiple drawings represent the same or similar parts or elements. These drawings are not necessarily drawn to scale. It should be understood that these drawings only depict some embodiments disclosed in the present application and should not be regarded as limiting the scope of the present application.
[0017] Figure 1 is a schematic structural diagram of a stacked heterojunction solar cell provided by some embodiments;
[0018] Figure 2 It is a schematic diagram of the structure of the stacked heterojunction solar cell provided in Example 1.
[0019] Description of reference numerals:
[0020] 1-transparent glass layer; 2-frame; 3-sealant; 4-top cell; 5-bottom cell; 6-backplane; 4-1-nickel oxide hole transport layer; 4-2-perovskite active layer, 4-3-SnO2 layer; 4-4-electron transport layer; 4-5-ITO layer; 4-6-AlO b Layer: 4-7-SiN c layer; 4-8-Ag / Al electrode; 5-1-silicon substrate; 5-2-TaO x layer; 5-3-Mg layer; 5-4-gate line layer. DETAILED DESCRIPTION
[0021] Embodiments of the present application are described in detail below, and examples of the embodiments are shown in the accompanying drawings. In the accompanying drawings, for clarity, the sizes of layers, regions, elements and their relative sizes may be exaggerated. Wherein the same or similar reference numerals throughout represent the same or similar elements or elements with the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present application, and cannot be understood as limitations on the present application. It should be noted that, in the absence of conflict, the embodiments in the present application and the features in the embodiments can be combined with each other.
[0022] It should be understood that when an element or layer is referred to as "on ...", "adjacent to ...", "connected to" or "coupled to" other elements or layers, it can be directly on, adjacent to, connected to or coupled to other elements or layers, or there can be intervening elements or layers. On the contrary, when an element is referred to as "directly on ...", "directly adjacent to ...", "directly connected to" or "directly coupled to" other elements or layers, there is no intervening element or layer. It should be understood that although the terms first, second, third, etc. can be used to describe various elements, components, regions, layers and / or parts, these elements, components, regions, layers and / or parts should not be limited by these terms. These terms are only used to distinguish one element, component, region, layer or part from another element, component, region, layer or part. Therefore, without departing from the teachings of the present disclosure, the first element, component, region, layer or part discussed below can be represented as the second element, component, region, layer or part. And when the second element, component, region, layer or part is discussed, it does not mean that the present disclosure necessarily has the first element, component, region, layer or part.
[0023] In this application, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements, unless otherwise clearly defined. For ordinary technicians in this field, the specific meanings of the above terms in this application can be understood according to specific circumstances.
[0024] It should be noted that the terms "first", "second", etc. in the specification and claims of the present application and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the terms used in this way can be interchangeable where appropriate, so that the embodiments of the present application described herein can be implemented in an order other than those illustrated or described herein, for example. In addition, the terms "including" and "having" and any of their variations are intended to cover non-exclusive inclusions, for example, a process, method, system, product or device that includes a series of steps or units is not necessarily limited to those steps or units that are clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices.
[0025] Most current PID studies are based on single-junction photovoltaic cells, which have an edge-sealed encapsulated transparent glass layer / transparent glass layer micromodule, where the front of the perovskite device and the transparent glass layer of the module are filled with nitrogen and / or air, rather than through a laminate (e.g., thermoplastic polyurethane (TPU) or ethyl acetate (EVA)). Currently, there is no research on the PID effect in stacked perovskite / silicon tandem devices, which have achieved a photovoltaic conversion efficiency (PCE) of 31.3%.
[0026] Accordingly, the present invention provides a laminated solar cell module and a preparation method thereof and a photovoltaic system to improve the anti-PID performance of the laminated solar cell module.
[0027] Hereinafter, exemplary embodiments according to the present application will be described in more detail with reference to the accompanying drawings. It should be noted that these exemplary embodiments can be implemented in many different forms and should not be construed as being limited to the embodiments described herein.
[0028] An embodiment of a first aspect of the present application provides a laminated solar cell module.
[0029] In some embodiments, Figure 1 As shown, the laminated solar cell module comprises:
[0030] Transparent glass layer 11, top cell 4, bottom cell 5, back plate 6 and frame 22;
[0031] The top cell 4 and the bottom cell 5 are stacked, and the top cell 4 and the bottom cell 5 are encapsulated as a whole in a space surrounded by the back plate 6, the transparent glass layer 1 and the frame 2, and sealant is filled between the top cell and the bottom cell and the back plate 6, between the top cell and the bottom cell and the transparent glass layer 1, and between the top cell and the bottom cell and the frame 2;
[0032] The bottom cell 5 comprises a crystalline silicon cell, and the crystalline silicon cell comprises a silicon substrate, and the back of the silicon substrate is provided with TaO x layer.
[0033] In the first aspect of the present application, a top battery 4 is introduced on the front side of the silicon substrate through a stacked battery design. The top battery 4 itself has several functional layers. The existence of each functional layer hinders the Na + Diffusion to the front of the silicon substrate; in addition, TaO is introduced to the back of the silicon substrate x layer, TaO x The layer can provide additional free electrons, which can effectively promote the collection and transmission of electrons and inhibit the carrier recombination at the interface. +The risk of PID effect generated by migration from the transparent glass layer 1 to the surface of the silicon substrate is reduced, thereby reducing the corrosion of the silicon substrate.
[0034] It is worth noting that TaO x The layer is a high-quality silicon contact electron selective layer, which has the characteristics of small conduction band offset and large valence band offset (~2.9eV). The small conduction band offset allows electrons from the silicon conduction band to flow through the TaO x layer, and the valence band offset is large, which can block the holes in the silicon valence band from flowing to TaO x The TaO layer prevents holes from flowing to the metal cathode. x The layer can effectively passivate silicon surface defects and has high thermal and chemical stability at different pH levels.
[0035] It is understandable that the silicon substrate has different forms in different crystalline silicon solar cells. For example, when the bottom cell is a heterojunction cell, the silicon substrate is: an intrinsic amorphous silicon film and a P-type amorphous silicon film are sequentially deposited on the front of the N-type crystalline silicon to form a pn junction; an intrinsic amorphous silicon film and an n-type amorphous silicon film are sequentially deposited on the back of the N-type crystalline silicon to form a back surface field. When the bottom cell is a PERC cell, the silicon substrate is: phosphorus is doped on the front of the P-type silicon wafer, and then the front and back sides are passivated respectively. When the bottom cell is a TOPCon cell, the silicon substrate is: an ultra-thin silicon oxide layer is prepared on the back of the N-type silicon substrate cell and a doped polysilicon thin layer is deposited to form a passivation contact structure.
[0036] The embodiments of the present application do not limit the transparent glass layer, backplane, grid line layer and frame. For example, the transparent glass layer can be made of solar ultra-white original glass or solar coated (semi) tempered glass. The backplane can be a backplane with model BEC-301D (HRB) purchased from Hangzhou Foster Applied Materials Co., Ltd. or a backplane with model PV331C purchased from Hubei Huitian New Materials Co., Ltd. The frame can be an aluminum alloy frame purchased from Yongzhen Technology (Chuzhou) Co., Ltd.; the grid line layer can be made of Ag / Al paste.
[0037] For stacked cells, the top cell (top cell) uses a wide bandgap absorption layer to effectively convert short-wavelength spectra to minimize light loss, while the bottom cell (bottom cell) uses a narrow bandgap absorption layer to capture near-infrared photons to maximize current density. When the device is illuminated by light, the wide-bandgap top cell absorbs short-wavelength photons with energy higher than its bandgap, generating a high open-circuit voltage (VOC), while the narrow-bandgap bottom cell absorbs long-wavelength photons, which can reduce photothermal loss and improve photoelectric conversion efficiency. Generally, the top cell may be a perovskite cell and the bottom cell may be a crystalline silicon solar cell. In some embodiments, the top cell may be a perovskite cell. Thus, a perovskite cell is introduced as a top cell on the front side of the silicon substrate. The top cell has several functional layers, and the presence of each functional layer hinders the Na + Diffusion to the front side of the silicon substrate; at the same time, the internal ion migration of the perovskite layer of the top cell causes the establishment of a built-in electric field, which + It plays a charge shielding role. In some embodiments, the bottom cell can be a crystalline silicon cell, for example, a PERC cell, a heterojunction cell, a tunnel oxide passivation contact solar cell (TOPCon cell), etc. Preferably, the bottom cell can be a heterojunction cell, and the photovoltaic conversion efficiency (PCE) of the stacked cell of the stacked perovskite / heterojunction cell is as high as 31.3%.
[0038] Regarding the structure of the stacked solar cell module, those skilled in the art can select according to their needs, for example, a four-terminal (4-T) stacked solar cell module and a two-terminal (2-T) stacked solar cell module, which is not limited in the embodiments of the present application.
[0039] In some embodiments, in the laminated solar cell assembly, the TaO x The resistivity of the layer is 0.4Ω / cm 2 ~1Ω / cm 2 , for example, 0.4Ω / cm 2 , 0.5Ω / cm 2 , 0.6Ω / cm 2 , 0.8Ω / cm 2 , 1Ω / cm 2 Etc. Therefore, it is more conducive to the transmission of electrons. The resistivity test method is to test according to the non-contact eddy current method in the standard GB / T 6616-2009.
[0040] In some embodiments, in the laminated solar cell assembly, the TaO x The thickness of the layer is 5 nm to 15 nm, for example, 5 nm, 6 nm, 7 nm, 8 nm, 10 nm, 12 nm, 14 nm, 15 nm, etc. Thus, TaO xIn addition to providing additional free electrons, the conductivity and light transmittance of the TaO layer are significantly optimized, which effectively promotes the collection and transmission of electrons and inhibits the carrier recombination at the interface. If the thickness is greater than 15nm, it will cause difficulty in electron transmission and fail to increase the current. If the thickness is less than 5nm, the TaO x The resistivity of the layer is large, which is not conducive to current collection.
[0041] In some embodiments, in the laminated solar cell assembly, the TaO x A passivation layer is provided on a side of the layer away from the silicon substrate, and the passivation layer is away from the TaO x A gate line layer is provided on one side of the layer; the passivation layer includes SiN a Therefore, it has excellent passivation performance.
[0042] Preferably, the SiN a The thickness of the layer is 85 nm to 90 nm, for example, 85 nm, 86 nm, 87 nm, 88 nm, 90 nm, etc. Thus, the appearance of the battery cell is uniform without color difference.
[0043] Preferably, the SiN a The refractive index of the layer is 2.00 to 2.05, for example, 2.00, 2.05, etc. Thus, the refractive index of the passivation film layer is moderate, which is beneficial to the absorption of light and the transmission inside the cell, and the passivation effect is excellent. The refractive index of the present application is measured using the photovoltaic laser ellipsometer system XE2000 / 3000 launched by Shanghai Xike Company, using a He-Ne laser, and the extracted laser wavelength is 632.8nm.
[0044] In some embodiments, in the laminated solar cell module, the SiN a A Mg electrode layer is provided between the gate line layer and the gate line layer, thereby further increasing the electron transmission rate through the Mg electrode layer with a low work function.
[0045] In some embodiments, in the laminated solar cell assembly, the sealant includes at least one of thermoplastic polyurethane, ethylene-vinyl acetate copolymer, and polyolefin elastomer, thereby playing the role of sealing protection, anti-ultraviolet aging and improving photoelectric conversion efficiency.
[0046] The second aspect of the present application provides a method for preparing a laminated solar cell assembly, comprising the following operations:
[0047] Providing a top cell 4, a sealant 3, a back sheet 6 and a transparent glass layer 1;
[0048] The bottom cell 5 is provided in the following manner: TaO is deposited on the back side of the silicon substrate x Layer 5-2, in the TaO xThe SiN layer 5-2 is deposited on the side away from the silicon substrate 5-1. a layer, in SiN a layer away from the TaO x A gate line layer 5-4 is deposited on one side of the layer 5-2;
[0049] Laminating the top battery 4 and the bottom battery 5 to obtain a battery cell;
[0050] The battery cells or the battery string including the battery cells, the sealant 3, the back plate 6 and the transparent glass layer 1 are stacked, and then the frame 2 is installed to assemble into a laminated solar cell module.
[0051] The laminated solar cell module prepared in the embodiment of the second aspect of the present application has excellent anti-PID performance while having the advantages of the laminated cell itself.
[0052] Optionally, TaO is deposited on the back side of the silicon substrate. x The specific operations of the layer are:
[0053] Ta(OEt)5 was used as a precursor, O3 and H2O were used as co-reactants, and TaO was deposited on the back of the silicon substrate by atomic force deposition. x Thus, the more uniform and dense TaO x Further, TaO is deposited by atomic force deposition. x The operation of the layer includes: the reaction temperature is 220℃~250℃, for example, 220℃, 230℃, 240℃, 250℃, etc.; the film forming rate is For example, etc.; preheating time 800s~900s, for example, 800s, 850s, 900s, etc.; precursor purge 10s~20s, for example, 10s, 15s, 20s, etc.; H2O and O3 mixture purge 10s~15s, for example, 10s, 12s, 14s, 15s, etc.
[0054] Alternatively, plasma enhanced chemical vapor deposition is used to deposit TaO x SiN is deposited on the layer a Thus, a more uniform and dense SiN a layer.
[0055] The third aspect of the present application provides a photovoltaic system, including the laminated solar cell assembly in any of the above embodiments. The advantages of the laminated solar cell assembly are also possessed by the photovoltaic system, which will not be repeated here. The above photovoltaic system has a wide range of applications, not only limited to photovoltaic power stations, such as ground power stations, rooftop power stations and water power stations, but also includes various equipment and devices that use solar energy to generate electricity, such as user solar power supplies, solar street lights, solar cars and solar buildings. Of course, it can be understood that the application scenarios of the photovoltaic system are not limited to this, that is, the photovoltaic system can be used in all fields where solar energy is required for power generation. Taking the photovoltaic power generation system network as an example, the photovoltaic system may include a photovoltaic array, a junction box and an inverter. The photovoltaic array may be an array combination of multiple laminated solar cell assemblies. For example, multiple laminated solar cell assemblies can form multiple photovoltaic arrays. The photovoltaic array is connected to the junction box. The junction box can converge the current generated by the photovoltaic array. The converged current flows through the inverter to convert it into the alternating current required by the mains power grid and then connected to the mains network to realize solar power supply.
[0056] The following will conduct performance tests on the structure of the laminated solar cell assembly provided in the embodiments of the present application and related comparative examples.
[0057] Example 1
[0058] See the schematic diagram of the structure of the stacked solar cell module. Figure 2 ,as follows:
[0059] The top cell includes a 10nm nickel oxide hole transport layer 4-1, a 100μm FA 0.85 Cs 0.15 PbI3 perovskite active layer 4-2, 200nm SnO2 layer 4-3, 5nm LiF layer, 40nm C60 layer and 7nm BCP layer composed of electron transport layer 4-4, 200nm ITO layer 4-5, 80nm AlO b Layers 4-6 and 40nm SiN c The anti-reflection layer is composed of layer 4-7, and the Ag / Al electrode 4-8 is arranged on the surface, and the lower side of the Ag / Al electrode 4-8 is in contact with the ITO layer 4-5;
[0060] The bottom cell includes a silicon substrate 5-1, which is a 200 μm n-type crystalline silicon substrate on which a 40 nm p-type amorphous silicon film, a 100 nm n-type amorphous silicon film, a 5 nm SiO d Amorphous layer, a 100nm P-type amorphous silicon film is deposited on the back of the n-type crystalline silicon; a 5nm TaO x Layer 5-2, 15nm Mg layer 5-3, 20nm Ag gate line layer 5-4;
[0061] Among them, TaO x The resistivity of the layer is 0.4Ω / cm 2 ;
[0062] The top cell 4 and the bottom cell 5 are stacked together, and the periphery of the two are sealed with a sealant 3. The top is laminated with a transparent glass layer 1, the bottom is laminated with a back plate 6, and the sides are encapsulated with a frame 5.
[0063] The transparent glass layer 1 is purchased from Anhui Jiuzhou Industrial Co., Ltd., a solar ultra-clear original glass, with a size of 2378 mm × 1297 mm × 2.0 mm;
[0064] Sealant 3 was purchased from Yancheng Baijia Niandai Film Technology Co., Ltd., model B601 HP, weight 450G / m 2 ;
[0065] The back plate 6 was purchased from Hubei Huitian New Materials Co., Ltd., model PV331C;
[0066] The frame 5 is an aluminum alloy frame purchased from Yongzhen Technology (Chuzhou) Co., Ltd., with a size of 2382mm×1134mm×30mm.
[0067] Embodiment 2 to Embodiment 5
[0068] The other conditions are the same as those in Example 1, except that the TaO x The thicknesses of the layers are 8 nm, 15 nm, 2 nm, and 20 nm, respectively.
[0069] Comparative Example 1
[0070] The other conditions are the same as those in Example 1, except that the bottom cell does not have TaO x layer.
[0071] Comparative Example 2
[0072] The other conditions are the same as those in Example 1, except that the TaO x layer is replaced by a TiO2 layer.
[0073] The laminated solar cell modules of the embodiment and the comparative example were subjected to PID test, and the PID test conditions were as follows: IEC TS62804-1, the modules were tested at -1500V for 96 hours at 85°C and 85%RH, wherein the module frame was grounded and the positive and negative terminals of the junction box were short-circuited, and the results are shown in Table 1.
[0074] Table 1
[0075]
[0076] Note:0max - Maximum power before battery-induced degradation; P max -The maximum power after battery induced decay; GAP is (P max- P 0max ) / P max ×100%.
[0077] It can be seen from Table 1 that the anti-PID performance of Examples 1 to 5 is better than that of Comparative Examples 1 to 2. Specifically, the GAP of Examples 1 to 5 is smaller than that of Comparative Examples 1 and 2, indicating that due to the TaO x The presence of the layer improves the anti-PID performance of the laminated solar cell module. Furthermore, the performance of Examples 1 to 3 is better. In the range of 5nm to 15nm, TaO x The thicker the layer, the better the electron transfer and the higher the current. x The anti-PID performance is the worst. Comparative Example 2 uses a 5nm TiO2 layer, a TiO2 layer and a TaO x The TaO layer belongs to the transition metal oxide. Both can be used as carrier selection contact layers in high-quality MIS passivation heterojunction structures. They have a wide range of work functions, good semiconductor properties, high light transmittance, and provide excellent passivation effects on silicon surfaces. x Can provide free electrons, therefore, has better anti-PID performance.
[0078] It should be noted that the terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise", "axial", "radial", "circumferential", etc. are only for the convenience of describing the present application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present application. The orientation words "inside" and "outside" refer to the inside and outside relative to the outline of each component itself. For example, if the device in the accompanying drawings is inverted, the device described as "above other devices or structures" or "above other devices or structures" will be positioned as "below other devices or structures" or "below other devices or structures". Therefore, the exemplary term "above..." can include both "above..." and "below..." orientations. The device can also be positioned in other different ways (rotated 90 degrees or in other orientations), and the spatial relative descriptions used here are interpreted accordingly.
[0079] It should also be noted that "one embodiment", "another embodiment", "embodiment", etc. mentioned in this application refer to the specific features, structures or characteristics described in conjunction with the embodiment included in at least one embodiment generally described in this application. The same expression appearing in multiple places in the specification does not necessarily refer to the same embodiment. Further, when a specific feature, structure or characteristic is described in conjunction with any embodiment, it is claimed that the realization of such feature, structure or characteristic in conjunction with other embodiments also falls within the scope of this application.
[0080] In the above embodiments, the description of each embodiment has its own emphasis. For parts that are not described in detail in a certain embodiment, reference can be made to the relevant descriptions of other embodiments.
[0081] It should also be noted that the above are only preferred embodiments of the present application, and the patent protection scope of the present application is not limited thereto. Any equivalent structure or equivalent process transformation made using the contents of the present application specification and drawings, or directly or indirectly used in other related technical fields, are also included in the patent protection scope of the present application.
Claims
1. A laminated solar cell module, characterized in that: include: Transparent glass layer, top cell, bottom cell, backplane, frame and sealant; The bottom cell comprises a crystalline silicon cell, the crystalline silicon cell comprises a silicon substrate, and the back side of the silicon substrate is provided with TaO x layer; The top cell and the bottom cell are stacked, and the top cell and the bottom cell are integrally encapsulated in a space surrounded by the back plate, the transparent glass layer and the frame. The sealant is filled between the top cell and the bottom cell and the back plate, between the top cell and the bottom cell and the transparent glass layer, and between the top cell and the bottom cell and the frame.
2. The laminated solar cell assembly according to claim 1, characterized in that: The TaO x The resistivity of the layer is 0.4Ω / cm 2 ~1Ω / cm 2 ; and / or The TaO x The thickness of the layer is 5 nm to 15 nm.
3. The laminated solar cell assembly according to claim 1, characterized in that: The TaO x A passivation layer is provided on a side of the layer away from the silicon substrate, and the passivation layer is away from the TaO x A gate line layer is provided on one side of the layer; The passivation layer includes SiN a layer.
4. The laminated solar cell assembly according to claim 3, characterized in that: The SiN a The thickness of the layer is 85nm to 90nm; and / or The SiN a The refractive index of the layer is 2.00 to 2.
05.
5. The laminated solar cell assembly according to claim 4, characterized in that: The SiN a A Mg electrode layer is provided between the gate line layer.
6. The laminated solar cell assembly according to claim 1, characterized in that: The sealant includes at least one of thermoplastic polyurethane, ethylene-vinyl acetate copolymer, and polyolefin elastomer.
7. The laminated solar cell module according to claim 1, characterized in that: The top cell comprises a perovskite cell; and / or The bottom cell comprises one of an emitter back passivation cell, a heterojunction cell, and a tunnel oxide layer passivation contact solar cell.
8. The laminated solar cell assembly according to claim 1, characterized in that: The structure of the laminated solar cell assembly is a two-terminal laminated solar cell assembly or a four-terminal laminated solar cell assembly.
9. A method for preparing a laminated solar cell module, characterized in that: The following operations are included: Provides top cell, sealant, backsheet, and clear glass layers; The bottom cell is provided in the following manner: TaO is deposited on the back side of the silicon substrate x layer, in the TaO x Depositing a gate line layer on a side away from the silicon substrate; Laminating the top cell and the bottom cell to obtain a cell sheet; The battery cell or the battery string including the battery cell, the sealant, the back plate and the transparent glass layer are laminated, and then a frame is installed to assemble into a laminated solar cell module.
10. The method for preparing a laminated solar cell assembly according to claim 9, characterized in that: Deposition of TaO on the back side of silicon substrate x Layer operations include: Ta(OEt)5 was used as a precursor, H2O and O3 were used as co-reactants, and TaO was deposited on the back of the silicon substrate by atomic force deposition. x layer; and / or Plasma enhanced chemical vapor deposition on TaO x SiN is deposited on the layer a layer.
11. The method for preparing a laminated solar cell assembly according to claim 10, characterized in that: TaO was deposited by atomic force deposition x Layer operations include: The reaction temperature is 220℃~250℃, and the film forming rate is The preheating time is 800s to 900s, the precursor purge is 10s to 20s, and the mixture of H2O and O3 is purge for 10s to 15s.
12. A photovoltaic system, characterized in that: The photovoltaic system comprises the laminated solar cell module according to any one of claims 1 to 8 or the laminated solar cell module prepared by the preparation method according to any one of claims 9 to 11.