Filter material for air filter and method for producing same
By using a binder resin and water repellent that does not contain fluorine and silicone as the main components, filter materials for air filters that do not contain PFAS and silicone compounds are manufactured, and the physical property balance difficulties in the prior art are solved. and the problem of material limitations, achieving efficient air filtration effect.
Patent Information
- Application Number
- CN202380029831.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-04-04
- Filing Date
- 2023-03-16
- Publication Date
- 2024-11-12
AI Technical Summary
When the existing filters use filter materials to capture submicron or micron unit particles, it is difficult to obtain a physical balance of PF value, water repellency and strength, and contain PFAS and silicone compounds with high decomposition and bioaccumulation, which limits them. use.
Adhesive resin and water repellent that are free of fluorine and silicon as the main components, and control the mass ratio of solid content between the adhesive resin and the water repellent through the wet non-woven fabric manufacturing method, and optimize the adhesive The combination of the mixture resin and the water repellent forms a filter material for an air filter that does not contain PFAS and siloxane compounds.
The physical balance of PF value, water repellency and strength is achieved, and the capture efficiency and pressure loss of the air filter are improved, and the use limitations of PFAS and siloxane compounds are avoided.
Smart Images

Figure BDA0005056619000000011 
Figure BDA0005056619000000101 
Figure BDA0005056619000000111
Abstract
Description
Technical Field
[0001] The present invention relates to a filter material for an air filter, which is used for air filters arranged in semiconductors, liquid crystals, clean rooms suitable for the food industry, building air conditioners or air purifiers, etc. Background Art
[0002] In order to capture and remove submicron or micron particles in the air, an air filter with air filter material is usually used. Air filters are classified into coarse dust filters, medium and high performance filters, HEPA, ULPA, etc. according to the particle size that can be captured and its capture efficiency. The later the filter, the smaller the particle size can be captured and the higher the capture efficiency.
[0003] Air filter filter materials are required to have the required particle capture efficiency and low pressure loss to avoid increasing the air supply energy. As an index of capture efficiency and pressure loss, there is a PF value shown in the number 1. The higher the value, the higher the capture efficiency of the filter material and the lower the pressure loss, the better it is.
[0004] [Number 1]
[0005]
[0006] Here, transmittance [%] = 100 - capture efficiency [%]
[0007] Furthermore, the filter material for an air filter is required to have sufficient strength so as not to be damaged or cracked during processing or ventilation use.
[0008] Furthermore, as a physical property required of the filter material for the air filter, there is water repellency. By having sufficient water repellency, the following problem can be prevented: when condensation or high humidity air passes through due to temperature changes, the pores of the filter material are blocked by water droplets. In addition, near the sea, the deliquescence phenomenon in which the sea salt particles captured by the filter material are liquefied and flow out due to the moisture in the air can be prevented. On the other hand, if the water repellency is low, there is a problem of infiltration of the sealant or hot melt adhesive used when processing the filter material into an air filter unit.
[0009] In order to impart water repellency to a filter material, a method of attaching a fluorine-based water repellent and / or a silicone-based water repellent is widely used (for example, refer to Patent Document 1 or Patent Document 2).
[0010] Examples of filter materials using water repellents other than fluorine-based and silicone-based ones include a method using synthetic paraffin (for example, see Patent Document 3) and a method using an alkyl ketene dimer (for example, see Patent Document 4).
[0011] Prior art literature
[0012] Patent Literature
[0013] Patent Document 1: Japanese Patent Laid-Open No. 2-175997
[0014] Patent Document 2: Japanese Patent Laid-Open No. 9-225226
[0015] Patent Document 3: WO97 / 04851
[0016] Patent Document 4: WO02 / 016005 Summary of the invention
[0017] [Problems to be solved by the invention]
[0018] However, in the technology disclosed in Patent Document 1 or Patent Document 2, since the perfluoroalkyl compounds (hereinafter referred to as PFAS) constituting the fluorine-based water repellent are difficult to decompose and have high bioaccumulation, there is a trend to restrict their use worldwide. In addition, the siloxane compounds constituting the silicone-based water repellent and the cyclic siloxanes as their condensates have the following problems: they adhere to the surface of the semiconductor substrate or the glass substrate, resulting in a decrease in product yield or repulsion. Furthermore, cyclic siloxanes are also difficult to decompose and have high bioaccumulation like PFAS, so there is a trend to restrict their use.
[0019] Furthermore, in the techniques disclosed in Patent Document 3 or Patent Document 4, it is difficult to achieve a balance in physical properties among the PF value, strength, and water repellency of the filter material in either method.
[0020] As described above, a filter material for air filters that does not contain PFAS and siloxane compounds is required, but in the prior art, it is difficult to obtain a filter material with a good balance of PF value, water repellency and strength. Therefore, the subject of the present invention is to provide a filter material for air filters that does not contain PFAS and siloxane compounds and has a good balance of PF value, water repellency and strength.
[0021] [Technical means to solve the problem]
[0022] The present inventors have conducted intensive research to solve the above-mentioned problems, and as a result, found that the above-mentioned problems can be solved by using a binder resin and a water repellent agent having an acrylic polymer containing no fluorine and silicon in the molecule as a main component, thereby completing the present invention. That is, the filter material for an air filter of the present invention comprises a wet nonwoven fabric, and the filter material for an air filter is characterized in that it contains a binder resin and a water repellent agent, and the water repellent agent has an acrylic polymer containing no fluorine and silicon in the molecule as a main component.
[0023] In the filter material for an air filter of the present invention, regarding the solid content mass ratio of the binder resin to the water repellent, the water repellent is preferably 5 to 90 parts by mass relative to 100 parts by mass of the binder resin, more preferably 30 to 90 parts by mass, further preferably 40 to 90 parts by mass, further preferably 40 to 70 parts by mass. By achieving this ratio, a filter material having a good balance of physical properties of PF value, water repellency and strength can be obtained.
[0024] The filter material for an air filter of the present invention is preferably such that the wet nonwoven fabric contains glass fibers. According to this configuration, a filter material for an air filter having a higher PF value can be obtained.
[0025] In the filter material for an air filter of the present invention, it is preferable that the binder resin is an acrylic binder resin.
[0026] In the filter material for an air filter of the present invention, it is preferable that the water repellent agent is a cationic water repellent agent.
[0027] The filter material for an air filter of the present invention preferably has a total solid content of the binder resin and the water repellent in the filter material of 3 to 12% by mass relative to the entire filter material. By achieving this ratio, a filter material having a particularly good balance of PF value and strength can be obtained.
[0028] The filter material for an air filter of the present invention preferably does not contain a cross-linking agent, and has a structure in which the fibers of the wet-laid nonwoven fabric are bonded to each other by the binder resin.
[0029] In the filter material for an air filter of the present invention, it is preferable that the water repellent agent has a structure attached to fibers of the wet-laid nonwoven fabric.
[0030] The filter material for an air filter of the present invention preferably has a structure in which the binder resin and the water repellent agent are cross-linked without the intermediary of a cross-linking agent.
[0031] The manufacturing method of the filter material for air filter of the present invention is characterized by having the following steps: using a wet papermaking method to make a sheet of fiber slurry to form a wet sheet; impregnating the wet sheet in an aqueous dispersion, the aqueous dispersion containing a binder resin and a water repellent having an acrylic polymer that does not contain fluorine and silicon in the molecule as a main component; and heating the wet sheet impregnated in the aqueous dispersion to dry it to obtain a dry sheet. Using this manufacturing method, a filter material for air filter that does not contain PFAS and siloxane compounds and has a good balance of physical properties of PF value, water repellency and strength can be obtained.
[0032] In the method for producing the filter material for an air filter of the present invention, it is preferred that the fiber slurry contains glass fibers. In this production method, a filter material for an air filter having a higher PF value can be obtained.
[0033] In the method for producing a filter material for an air filter of the present invention, it is preferred that the binder resin is an acrylic binder resin, the aqueous dispersion does not contain a crosslinking agent, the binder resin bonds the fibers of the dry sheet to each other, and the water repellent is attached to the fibers of the dry sheet.
[0034] [Effects of the invention]
[0035] According to the present invention, it is possible to obtain a filter material for an air filter that does not contain PFAS and siloxane compounds and has a good balance in physical properties such as PF value, water repellency and strength. DETAILED DESCRIPTION
[0036] Next, the present invention will be described in detail by showing the embodiments, but the present invention is not to be construed as being limitative of these descriptions. The embodiments can be modified in various ways as long as the effects of the present invention are exhibited.
[0037] The binder resin of the present embodiment makes the fibers of the nonwoven fabric bonded to each other, and is used to give the required strength to the air filter filter material. That is, the air filter filter material of the present embodiment preferably does not contain a cross-linking agent such as a polyisocyanate compound, and has a structure in which the fibers of the wet nonwoven fabric are bonded to each other by the binder resin. Regarding the composition of the binder resin, for example, it is selected from polyacrylate resin, polymethacrylate resin, polystyrene resin, polyvinyl acetate resin, polyurethane resin, polyvinyl alcohol, etc. It is preferably an acrylic binder resin such as a polyacrylate resin and a polymethacrylate resin.
[0038] The water repellent of the present embodiment is attached to the fibers of the non-woven fabric and is used to impart the desired water repellency to the filter material for the air filter. The main component of the water repellent is composed of an acrylic polymer (hereinafter sometimes referred to as an acrylic polymer) that does not contain fluorine and silicon in the molecule. The water repellent contains more than 50% by mass of the acrylic polymer, preferably more than 80% by mass, and more preferably more than 90% by mass. Acrylic polymer refers to a polymer obtained by polymerizing acrylate or methacrylate as the main raw material monomer. Acrylic polymer is synthesized by containing more than 50% by mass of the raw material monomer, preferably more than 80% by mass, and more preferably more than 90% by mass. As an example of such a water repellent, there can be cited: Unidyne XF series (manufactured by Daikin Industries, Ltd.) containing acrylic polymers, etc., which can be selected from these commercially available products. The water repellent may also contain a trace amount of silicone of about 50 to 150 ppm as an additive.
[0039] The water repellent is preferably a cationic water repellent. By being cationic, the water repellency is further improved. In particular, when the wet nonwoven fabric contains glass fibers, it is easy to improve the fixation of the water repellent to the glass fibers, so the water repellent is easy to remain in the filter material. Therefore, it is easy to improve the water repellency.
[0040] When both the binder resin and the water repellent are acrylic resin compounds, the binder resin in this embodiment is preferably an acrylic resin compound in which the carbon number of the ester part of the acrylic acid ester or methacrylic acid ester as the raw material monomer of the polyacrylate is mainly 8 or less (preferably 80% by mass or more, more preferably 90% by mass or more in the acrylic acid ester or methacrylic acid ester). If the carbon number of the ester part exceeds 8, there is a concern that it is difficult to obtain bonding strength.
[0041] In addition, the water repellent in the present embodiment is preferably an acrylic resin compound in which the carbon number of the ester part of the acrylic acid ester or methacrylic acid ester as the raw material monomer of the polyacrylate is mainly more than 8 (in the acrylic acid ester or methacrylic acid ester, preferably 80% by mass or more, more preferably 90% by mass or more). In the water repellent here, the ester part is preferably a hydrocarbon group. The hydrocarbon group can be linear or branched, can be a saturated hydrocarbon or an unsaturated hydrocarbon, and can have an alicyclic or aromatic ring. Among these, linear is preferred, and linear alkyl is more preferred. The carbon number of the ester part is preferably 9 or more, and more preferably 12 or more. If the carbon number is 8 or less, there is a concern that sufficient water repellency cannot be exerted as a water repellent treatment agent.
[0042] In the present embodiment, regarding the solid content mass ratio of the binder resin and the water repellent (binder resin / water repellent), when the binder resin is set to 100 parts by mass, the water repellent is preferably 5 to 90 parts by mass, and the water repellent is more preferably 30 to 90 parts by mass, further preferably 40 to 90 parts by mass, and further preferably 40 to 70 parts by mass. By becoming this ratio, a filter material with a good balance of physical properties of PF value, water repellency and strength can be obtained. If the mass ratio of the water repellent is less than 30 parts by mass, there is a concern that sufficient water repellency cannot be obtained. On the other hand, if the mass ratio of the water repellent is higher than 90 parts by mass, there is a concern that sufficient strength cannot be obtained, and there is also a concern that a sufficient PF value cannot be obtained.
[0043] In this embodiment, the total solid content of the binder resin and the water repellent in the filter material is preferably 3 to 12% by mass relative to the entire filter material. More preferably, it is 4 to 10% by mass. If the total content of these components is less than 3% by mass, there is a concern that sufficient water repellency and strength cannot be obtained. On the other hand, if the total content is higher than 12% by mass, there is a concern that a sufficient PF value cannot be obtained.
[0044] In the filter material for an air filter of the present embodiment, the water repellency is preferably 300 mm water column height or more, more preferably 508 mm water column height or more.
[0045] In the filter material for an air filter of the present embodiment, the tensile strength of a single component of the filter material is preferably 0.30 kN / m or more, and more preferably 0.40 kN / m or more.
[0046] In this embodiment, the components of the binder resin and the water repellent are mixed to prepare an aqueous dispersion, and the aqueous dispersion is impregnated into a wet nonwoven fabric in a wet state, and then the wet nonwoven fabric is dried and cross-linked by heating. As for the heating method at this time, if it is a papermaking machine, a multi-drum dryer, a Yankee dryer, a hot air dryer, etc. are used, and if it is a hand copying device, a rotary dryer, a circulating dryer, etc. are used. The heating temperature is 80 to 180°C, and more preferably 100 to 160°C.
[0047] In the present embodiment, additives such as a defoaming agent may be appropriately added to the aqueous dispersion used for impregnation within a range that does not impair the effects of the present invention.
[0048] The wet nonwoven fabric of the present embodiment preferably includes glass fibers. Since glass fibers have high rigidity, the gaps required for air to pass through can be sufficiently maintained in the filter material, thereby obtaining a high PF value. As glass fibers, glass wool fibers, chopped glass fibers, etc. can be used.
[0049] In the present embodiment, the average fiber diameter of the glass fiber is not particularly limited, and is preferably 0.1 to 10 μm, and more preferably 0.2 to 7 μm. By being within this range, a filter material with a good balance between pressure loss and capture efficiency, i.e., a high PF value, is obtained. In addition, two or more glass fibers with different average fiber diameters may be included. In order to obtain a further high capture efficiency, it is preferred that at least a portion of the glass fibers be glass fibers with a fiber diameter of less than 1 μm.
[0050] In the present embodiment, fibers other than glass fibers may be used as fibers constituting the wet nonwoven fabric. Examples of these fibers include natural fibers such as wood pulp; regenerated fibers such as rayon fibers; and synthetic fibers such as polyolefin fibers, polyurethane fibers, and vinylon fibers. The amount of these fibers blended is preferably set within a range that does not hinder the effect of increasing the PF value of the glass fibers. For example, it is less than 30% by mass of the entire fiber, more preferably less than 20% by mass, and further preferably less than 10% by mass.
[0051] In the manufacturing step of the air filter material of the present embodiment, the raw material fiber is dispersed in water to obtain a raw material slurry, which is made into a sheet material by a wet papermaking method to obtain a wet sheet material. When a large amount of glass fiber is used as the raw material fiber, the water used for dispersion and papermaking is preferably acidic, and more preferably has a pH value of 2 to 4. By dispersing and papermaking in an acidic state, the glass fibers are easily bonded to each other, and the strength can be improved.
[0052] (Example)
[0053] The present invention is described below with reference to specific examples, but the present invention is not limited to these descriptions. In addition, the "parts" in the examples represent the solid content mass ratio of the fibers in the raw material slurry or the solid content mass ratio of the components in the impregnation liquid, with the total amount of all fibers in the raw material slurry being 100 parts and the binder resin in the impregnation liquid being 100 parts. In addition, the "%" in the examples represents the solid content mass ratio of the components in the filter material.
[0054] <Example 1>
[0055] 60 parts of glass wool (B-06-F, manufactured by Unifrax Co.) with an average fiber diameter of 0.65 μm, 30 parts of glass wool (B-26-R, manufactured by Unifrax Co.) with an average fiber diameter of 2.44 μm, and 10 parts of chopped glass fibers (EC-6-6-SP, manufactured by Unifrax Co.) with an average fiber diameter of 6 μm and a cut length of 6 mm were dissociated using a table dissociator and acidic water with a pH of 3.0 to obtain a raw material slurry. Subsequently, the raw material slurry was made into paper to obtain a wet nonwoven fabric. Furthermore, 100 parts of an acrylic binder resin (VONCOATAN-1190S, manufactured by DIC Corporation) and 20 parts of a cationic acrylic water repellent (Unidyne XF-4001, manufactured by Daikin Industries, Ltd.) containing an acrylic polymer containing no fluorine or silicon in its molecule as a main component, and water were mixed to prepare an impregnation solution, and the prepared impregnation solution was impregnated into the wet nonwoven fabric, and the nonwoven fabric was dried using a rotary dryer at 130° C. (drying time: 2 minutes), and then heated using a dryer at 160° C. for 2 minutes to obtain a nonwoven fabric with a basis weight of 70 g / m 2 The content of the impregnated component in the filter material was 5.1%.
[0056] <Example 2>
[0057] A 70 g / m3 impregnation solution was prepared by mixing 100 parts of an acrylic binder resin (VONCOATAN-1190S, manufactured by DIC Corporation), 30 parts of a cationic acrylic water repellent (Unidyne XF-4001, manufactured by Daikin Industries, Ltd.) containing an acrylic polymer containing no fluorine or silicon in its molecule as a main component, and water. 2 The content of the impregnated component in the filter material was 5.2%.
[0058] <Example 3>
[0059] A 70 g / m3 impregnation solution was prepared in the same manner as in Example 1 except that 100 parts of an acrylic binder resin (VONCOATAN-1190S, manufactured by DIC Corporation) and 40 parts of a cationic acrylic water repellent (Unidyne XF-4001, manufactured by Daikin Industries, Ltd.) containing an acrylic polymer containing no fluorine or silicon in its molecule as a main component and water were mixed. 2 The content of the impregnated component in the filter material was 5.1%.
[0060] <Example 4>
[0061] A 70 g / m2 impregnation liquid was obtained in the same manner as in Example 1 except that 100 parts of an acrylic binder resin (VONCOATAN-1190S, manufactured by DIC Corporation) and 50 parts of a cationic acrylic water repellent (Unidyne XF-4001, manufactured by Daikin Industries, Ltd.) containing an acrylic polymer not containing fluorine and silicon in its molecule as a main component and water were mixed. 2 The content of the impregnated component in the filter material was 5.4%.
[0062] <Example 5>
[0063] A 70 g / m3 impregnation solution was prepared by mixing 100 parts of an acrylic binder resin (VONCOATAN-1190S, manufactured by DIC Corporation), 70 parts of a cationic acrylic water repellent (Unidyne XF-4001, manufactured by Daikin Industries, Ltd.) containing an acrylic polymer not containing fluorine or silicon in its molecule as a main component, and water. 2 The content of the impregnated component in the filter material was 5.3%.
[0064] <Example 6>
[0065] A 70 g / m2 impregnation liquid was obtained in the same manner as in Example 1 except that 100 parts of an acrylic binder resin (VONCOATAN-1190S, manufactured by DIC Corporation) and 90 parts of a cationic acrylic water repellent (Unidyne XF-4001, manufactured by Daikin Industries, Ltd.) containing an acrylic polymer containing no fluorine or silicon in its molecule as a main component and water were mixed. 2 The content of the impregnated component in the filter material was 5.2%.
[0066] <Example 7>
[0067] A 70 g / m2 impregnation liquid was prepared in the same manner as in Example 1 except that 100 parts of an acrylic binder resin (VONCOATAN-1190S, manufactured by DIC Corporation) and 100 parts of a cationic acrylic water repellent (Unidyne XF-4001, manufactured by Daikin Industries, Ltd.) containing an acrylic polymer not containing fluorine or silicon in its molecule as a main component and water were mixed. 2 The content of the impregnated component in the filter material was 5.2%.
[0068] <Example 8>
[0069] A 70 g / m3 impregnation solution was prepared in the same manner as in Example 1 except that 100 parts of an acrylic binder resin (VONCOATAN-1190S, manufactured by DIC Corporation) and 40 parts of a cationic acrylic water repellent (Unidyne XF-4001, manufactured by Daikin Industries, Ltd.) containing an acrylic polymer containing no fluorine or silicon in its molecule as a main component and water were mixed. 2 Since the conditions for impregnating the wet paper with the impregnation liquid were adjusted, the content of the impregnation component in the filter material was 3.0%.
[0070] <Example 9>
[0071] A 70 g / m3 impregnation solution was prepared in the same manner as in Example 1 except that 100 parts of an acrylic binder resin (VONCOATAN-1190S, manufactured by DIC Corporation) and 40 parts of a cationic acrylic water repellent (Unidyne XF-4001, manufactured by Daikin Industries, Ltd.) containing an acrylic polymer containing no fluorine or silicon in its molecule as a main component and water were mixed. 2 Since the conditions for impregnating the wet paper with the impregnation liquid were adjusted, the content of the impregnation component in the filter material was 12.1%.
[0072] <Example 10>
[0073] A 70 g / m2 impregnation solution was prepared in the same manner as in Example 1 except that 100 parts of an acrylic binder resin (VONCOATAN-1190S, manufactured by DIC Corporation) and 5 parts of a cationic acrylic water repellent (Unidyne XF-4001, manufactured by Daikin Industries, Ltd.) containing an acrylic polymer containing no fluorine or silicon in its molecule as a main component and water were mixed. 2 The content of the impregnated component in the filter material was 5.2%.
[0074] <Example 11>
[0075] A 70 g / m2 impregnation solution was prepared by mixing 100 parts of an acrylic binder resin (VONCOATAN-1190S, manufactured by DIC Corporation), 10 parts of a cationic acrylic water repellent (Unidyne XF-4001, manufactured by Daikin Industries, Ltd.) containing an acrylic polymer not containing fluorine or silicon in its molecule as a main component, and water. 2 The content of the impregnated component in the filter material was 5.2%.
[0076] <Comparative Example 1>
[0077] Except that the impregnation step was omitted, a 70 g / m 2 Filter material for air filters.
[0078] <Comparative Example 2>
[0079] A 70 g / m2 impregnation liquid was obtained in the same manner as in Example 1 except that 100 parts of an acrylic binder resin (VONCOATAN-1190S, manufactured by DIC Corporation) and water were mixed. 2 The content of the impregnated component in the filter material was 5.4%.
[0080] <Comparative Example 3>
[0081] A 70 g / m2 impregnation liquid was obtained in the same manner as in Example 1 except that 100 parts of an acrylic binder resin (VONCOATAN-1190S, manufactured by DIC Corporation) and 20 parts of an alkyl ketene dimer (SE2380, manufactured by Seikyo PMC Corporation) were mixed with water. 2 The content of the impregnated component in the filter material was 5.3%.
[0082] <Comparative Example 4>
[0083] A 70 g / m2 impregnation liquid was obtained in the same manner as in Example 1 except that 100 parts of an acrylic binder resin (VONCOATAN-1190S, manufactured by DIC Corporation) and 20 parts of a paraffin-based water repellent (Petrox P-200, manufactured by Meisei Chemical Industries, Ltd.) were mixed with water. 2 The content of the impregnated component in the filter material was 5.4%.
[0084] <Comparative Example 5>
[0085] A 70 g / m2 impregnation liquid was obtained in the same manner as in Example 1 except that 100 parts of an acrylic binder resin (VONCOATAN-1190S, manufactured by DIC Corporation) and 20 parts of a fluorine-based water repellent (AsahiGuard AG-E300, manufactured by AGC Corporation) were mixed with water. 2 The content of the impregnated component in the filter material was 5.4%.
[0086] <Comparative Example 6>
[0087] In addition to using an impregnating solution prepared by mixing 100 parts of a cationic acrylic water-repellent agent (Unidyne XF-4001, manufactured by Daikin Industries, Ltd.) having an acrylic polymer without fluorine and silicon in the molecule as a main component and water, a filter material for an air filter having a basis weight of 70 g / m 2 was obtained in the same manner as in Example 1. In addition, the content rate of the impregnating component in the filter material was 2.5%.
[0088] The following method was used to evaluate the filter materials for air filters obtained in the examples and comparative examples.
[0089] <Pressure loss>
[0090] The pressure loss was measured as the differential pressure when air was passed through the filter material for an air filter having an effective area of 100 cm 2 at a face velocity of 5.3 cm / sec using a manometer (Manostar Gauge WO81, manufactured by Yamamoto Electric Co., Ltd.).
[0091] <Transmittance>
[0092] Using a laser particle counter (KC-22B, manufactured by RION Co., Ltd.), the number of PAO particles upstream and downstream was measured when air containing polydisperse polyalphaolefin (PAO) particles generated by a Laskin nozzle was passed through the filter material for an air filter having an effective area of 100 cm 2 at a face velocity of 5.3 cm / sec, and the transmittance was calculated based on the ratio of the number of particles upstream and downstream. The target particle sizes were set to 0.10 to 0.15 μm and 0.30 μm.
[0093] <PF value>
[0094] The PF value was calculated using the formula shown in Equation (1) based on the values of the pressure loss and particle transmittance. The target particle sizes were set to 0.10 to 0.15 μm and 0.30 μm.
[0095] <Tensile strength>
[0096] The tensile strength was measured using an automatic stereoplotter AGX-S (manufactured by Shimadzu Corporation) under the conditions of a test width of 1 inch, a test length of 100 mm, and a tensile speed of 15 mm / min.
[0097] <Water repellency>
[0098] The water repellency was measured in accordance with MIL-STD-282.
[0099] The evaluation results of the filter materials for air filters carried out by the above method are shown in Tables 1 to 2.
[0100] [Table 1]
[0101]
[0102] [Table 2]
[0103]
[0104] In Examples 1 to 11, the PF value at 0.10 to 0.15 μm is 8.80 or more, and the PF value at 0.30 μm is 12.47 or more. In Examples 1 to 9, the water repellency value is 290 mm water column height or more. In Example 11, the water repellency value is 200 mm water column height or more.
[0105] By comparing Examples 1 to 11 with Comparative Example 2, it was confirmed that water repellency was imparted by using a water repellent, and Example 10 showed a water repellency value of 100 mm water column height or more, which was the practical lower limit, Example 11 showed a water repellency value (200 mm water column height) higher than that of Example 10 and better than the practical lower limit, Example 1 showed a water repellency value (290 mm water column height or more) with no practical problems, Examples 2 and 8 showed practically preferred water repellency values (300 mm water column height or more), and Examples 3 to 7 and 9 satisfied a practically more preferred water repellency value (508 mm water column height or more).
[0106] By comparing Examples 1 to 11 with Comparative Examples 1 and 6, it was confirmed that tensile strength was imparted by using an adhesive resin, and that Example 7 showed a tensile strength value (0.27 kN / m or more) that was not a problem in practical use, and Example 6 showed a tensile strength value (0.30 kN / m or more) that was preferred in practical use. Examples 1 to 5 and Examples 8 to 11 satisfied a tensile strength value (0.40 kN / m or more) that was further preferred in practical use.
[0107] Comparison of Examples 1 to 7 with Comparative Examples 3 and 4 confirms that: according to the present invention, a filter material having a good balance of PF value and water repellency can be obtained compared with the case of using other non-fluorine-based water repellent agents. That is, in Examples 1 to 7, the PF value of 0.10 to 0.15 μm is 9.55 or more, the PF value of 0.30 μm satisfies 12.99 or more, and the water repellency value satisfies a water column height of 290 mm or more, and a filter material having a good balance of physical properties can be obtained.
Claims
1. A filter material for an air filter, comprising a wet nonwoven fabric, The filter material for an air filter is characterized by containing a binder resin and a water repellent. The water repellent agent has an acrylic polymer containing no fluorine or silicon in its molecule as a main component.
2. The filter material for an air filter according to claim 1, characterized in that: Regarding the solid content mass ratio of the binder resin to the water repellent agent, the water repellent agent is 5 to 90 parts by mass based on 100 parts by mass of the binder resin.
3. The filter material for an air filter according to claim 1, characterized in that: Regarding the solid content mass ratio of the binder resin to the water repellent agent, the water repellent agent is 30 to 90 parts by mass based on 100 parts by mass of the binder resin.
4. The filter material for an air filter according to claim 1, characterized in that: Regarding the solid content mass ratio of the binder resin to the water repellent agent, the water repellent agent is 40 to 90 parts by mass relative to 100 parts by mass of the binder resin.
5. The filter material for an air filter according to claim 1, characterized in that: Regarding the solid content mass ratio of the binder resin to the water repellent agent, the water repellent agent is 40 to 70 parts by mass relative to 100 parts by mass of the binder resin.
6. The filter material for an air filter according to claim 1, characterized in that: The wet-laid nonwoven fabric contains glass fibers.
7. The filter material for an air filter according to claim 1, characterized in that: The binder resin is an acrylic binder resin.
8. The filter material for an air filter according to claim 1, characterized in that: The water repellent is a cationic water repellent.
9. The filter material for an air filter according to claim 1, characterized in that: The total solid content mass content of the binder resin and the water repellent agent in the filter material is 3 to 12% by mass with respect to the entire filter material.
10. The filter material for an air filter according to claim 1, characterized in that: A cross-linking agent is not contained, and the binder resin bonds the fibers of the wet nonwoven fabric to each other.
11. The filter material for an air filter according to claim 1, characterized in that: The water-repellent agent is attached to fibers of the wet nonwoven fabric.
12. The filter material for an air filter according to claim 1, characterized in that: The binder resin and the water repellent agent are cross-linked without the aid of a cross-linking agent.
13. A method for manufacturing a filter material for an air filter, characterized in that The steps are as follows: The wet papermaking method is used to make a sheet of fiber slurry to form a wet sheet; The wet sheet is immersed in an aqueous dispersion containing a binder resin and a water repellent having an acrylic polymer containing no fluorine or silicon in its molecule as a main component; and The wet sheet impregnated with the aqueous dispersion is heated and dried to obtain a dry sheet.
14. The method for producing a filter material for an air filter according to claim 13, wherein: The slurry of fibers comprises glass fibers.
15. The method for producing a filter material for an air filter according to claim 13, wherein: The binder resin is an acrylic binder resin, The aqueous dispersion does not contain a crosslinking agent, The binder resin bonds the fibers of the dry sheet to each other, and The water repellent is attached to fibers of the drying sheet.
Citation Information
Patent Citations
Aqueous emulsion surface treatment agent
CN105745272A
Water-based surface treatment agent
CN105765025A
Filter material for air filter and its production
JP1997225226A
Filter medium for air filter and its manufacturing method
JP2004154672A
Filtering medium for air filter and its manufacturing method
JP2008194584A