Novel composite material and method for manufacturing composite material
By coating the surface of cellulose nanofibers with copper compounds, forming a coating layer and adjusting the thickness of the coating layer, the problems of poor oxidation and antibacterial effects of copper particles are solved, and the oxidation resistance and antibacterial properties of the composite material are achieved.
Patent Information
- Application Number
- CN202380030778.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-28
- Filing Date
- 2023-03-27
- Publication Date
- 2024-11-12
AI Technical Summary
In the prior art, copper particles are prone to oxidation, resulting in a decrease in conductivity and antibacterial effects, and the antiviral and antibacterial effects of metal-containing oxidized cellulose nanofibers are not ideal.
By coating the surface of the cellulose nanofibers with copper compounds, a cladding layer is formed to reduce the oxidation of copper, and the thickness and cladding ratio of the cladding layer are adjusted by impregnating the copper particle dispersion liquid to ensure the conductivity and antibacteriality of the composite material .
The oxidation resistance and antibacterial properties of copper are achieved, ensuring that the composite material can still show conductivity without sintering, and improving the antibacterial and odor-proof effect.
Smart Images

Figure BDA0005061739550000111 
Figure BDA0005061739550000141
Abstract
Description
Technical Field
[0001] The invention relates to a novel composite material, a method for preparing the composite material, and a spray, a sanitary material, a filter and a coating agent containing the composite material. Background Art
[0002] Copper has various functions such as electrical conductivity, thermal conductivity, and antibacterial properties. However, copper is easily oxidized, and cannot exhibit the above functions after oxidation. Therefore, when using copper, it is desired to improve oxidation resistance. For example, Patent Document 1 discloses surface-coated copper particles having copper particles and a specific organic film, wherein the organic film is formed on the surface of the copper particles. For surface-coated copper particles, the copper particles have excellent oxidation resistance, and the resulting sintered body has excellent electrical conductivity. In addition, Patent Document 2 describes metal-containing oxidized cellulose nanofibers containing metals other than sodium in the form of salts, and the metal-containing oxidized cellulose nanofibers have a high antibacterial effect.
[0003] Prior art literature
[0004] Patent Literature
[0005] Patent document 1: Japanese Patent Application Publication No. 2019-214748.
[0006] Patent document 2: International Publication No. 2019 / 107195. Summary of the invention
[0007] The composite material of the present invention comprises: a core material composed of cellulose nanofibers; and a covering layer composed of copper covering the core material. DETAILED DESCRIPTION
[0008] The surface-coated copper fine particles described in Patent Document 1 have excellent electrical conductivity when sintered, but if not sintered, the organic film on the surface increases the electrical resistance, so that desired electrical conductivity cannot be obtained.
[0009] The metal-containing oxidized cellulose nanofibers described in Patent Document 2 have a low metal ion concentration, and therefore have low antiviral and antibacterial effects. In addition, the deodorizing effect is difficult to utilize for a long period of time, and there is room for improvement.
[0010] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a novel composite material capable of reducing oxidation of copper and exhibiting functions of copper such as antibacterial property and electrical conductivity, and a method for producing the composite material.
[0011] Hereinafter, the present invention will be described in detail with reference to one embodiment.
[0012] [Composite Materials]
[0013] The composite material of the present invention comprises: a core material composed of cellulose nanofibers; and a coating layer composed of copper coating the core material.
[0014] The composite material of the present invention can exhibit functions of copper such as antibacterial property and electrical conductivity by covering a core material composed of cellulose nanofibers with a covering layer composed of copper to reduce oxidation of copper.
[0015] The core material constituting the composite material is composed of cellulose nanofibers, which are fibrous materials having a fiber diameter of 500 nm or less and are produced by defibrillating plant fibers to the nanoscale.
[0016] The average fiber diameter of the cellulose nanofibers is not particularly limited, and from the viewpoint of maintaining transparency, may be 3 nm to 100 nm, 3 nm to 80 nm, 4 nm to 60 nm, or 4 nm to 40 nm.
[0017] The average fiber length of the cellulose nanofibers is not particularly limited, but may be 0.5 μm to 100 μm, 0.5 μm to 50 μm, or 0.5 μm to 5 μm, from the viewpoint of handleability.
[0018] The average fiber diameter and average fiber length of the cellulose nanofibers are obtained by averaging the fiber diameter and fiber length obtained by observing each fiber using an atomic force microscope (AFM).
[0019] The average aspect ratio of the cellulose nanofibers may be 10 or more, or 50 or more. The upper limit of the average aspect ratio is not particularly limited, but is usually 1000 or less. The average aspect ratio can be calculated by the following formula (1).
[0020] Aspect ratio = average fiber length / average fiber diameter (1)
[0021] The raw material of the cellulose nanofiber is not particularly limited, and examples thereof include wood, bamboo, hemp plants, jute, kenaf, farm waste, cloth, conifer unbleached kraft pulp (NUKP), conifer bleached kraft pulp (NBKP), broadleaf unbleached kraft pulp (LUKP), broadleaf bleached kraft pulp (LBKP), conifer unbleached sulfite pulp (NUSP), conifer bleached sulfite pulp (NBSP), thermomechanical pulp (TMP), recycled pulp, waste paper, etc. The fiber raw material may be used alone or in combination of two or more.
[0022] Cellulose nanofibers may be subjected to modification treatment. Specific examples of modification treatment include esterification such as acetylation, phosphorylation, carbamateization, carbamide, etherification, carboxymethylation, TEMPO (2,2,6,6-tetramethylpiperidin-1-oxyl free radical) oxidation, and periodic acid oxidation. Cellulose nanofibers may be subjected to only one of these modification treatments, or may be subjected to two or more.
[0023] Commercially available cellulose nanofibers may be used, such as ELLEX-☆ (registered trademark) (manufactured by Daio Paper Co., Ltd.), ELLEX-S (manufactured by Daio Paper Co., Ltd.), and Cellenpia (registered trademark) (manufactured by Nippon Paper Industries, Ltd.).
[0024] The coating layer covering the core material is composed of copper. The copper forming the coating layer may also be derived from copper compounds such as copper halide, copper carboxylate, and cuprous oxide. Examples of copper halide include copper iodide, copper bromide, and copper chloride. Examples of copper carboxylate include copper oxalate and copper acetate.
[0025] From the viewpoint of productivity, the copper compound may be a copper halide or copper chloride.
[0026] The thickness of the coating layer can be 1 nm or more and 150 nm or less, 2 nm or more and 120 nm or less, or 3 nm or more and 100 nm or less. When the thickness of the coating layer is 1 nm or more, the functions of copper such as antibacterial property and electrical conductivity can be further exerted, and when the thickness of the coating layer is 150 nm or less, the oxidation of copper can be reduced.
[0027] The composite material is cut using a focused ion beam (FIB) to produce a cross-sectional slice, which is photographed using a transmission electron microscope (TEM), and the thickness of the coating layer can be calculated as an average value of 100,000 to 500,000 points. Specifically, the thickness can be measured by the method described in the Examples.
[0028] In addition, when the composite material of the present invention has a plating layer described later, the total thickness of the coating layer composed of copper and the plating layer is included in the range of the thickness of the coating layer.
[0029] The covering layer may cover the entire surface of the core material or only a part of it.
[0030] The coating layer may have a coverage ratio of 0.5% to 99% or less, 1% to 99% or more, 5% to 99% or more, or 10% to 99% or more relative to the core material. When the coating layer has a coverage ratio of 0.5% or more, the functions of copper such as antibacterial property and electrical conductivity can be further exerted, and when the coating layer has a coverage ratio of 99% or less, oxidation of copper can be reduced.
[0031] The coverage of the coating layer can be measured by a thermal decomposition method using an electric furnace or a differential thermal-thermogravimetric simultaneous measurement device (TG / DTA). Specifically, it can be measured by the method described in the Examples.
[0032] From the viewpoint of further exerting the functions of copper such as antibacterial property and electrical conductivity, the composite material of the present invention may also have a plating layer covering the coating layer. Examples of the metal constituting the plating layer include copper, nickel, chromium, cobalt, tin, and the like.
[0033] The thickness of the plating layer may be 0.01 μm or more and 0.50 μm or less, 0.01 μm or more and 0.20 μm or less, or 0.01 μm or more and 0.10 μm or less. When the thickness of the plating layer is 0.01 μm or more, the functions of copper such as antibacterial property and electrical conductivity can be further exerted, and when the thickness of the plating layer is 0.50 μm or less, transparency can be maintained.
[0034] The thickness of the plating layer can be measured by a fluorescent X-ray analyzer or FIB-TEM (Focused Ion Beam-Transmission Electron Microscope).
[0035] [Method for producing composite material]
[0036] The method for producing the composite material of the present invention is a method of immersing cellulose nanofibers in a copper particle dispersion.
[0037] The copper particle dispersion is obtained by mixing a copper compound, a reducing compound, a water-soluble chloride, and a reducing sugar in a dispersion medium.
[0038] The copper compound is not particularly limited as long as it is a compound containing a copper atom. As the copper compound, for example, copper halide, copper carboxylate, cuprous oxide, etc. can be mentioned. As copper halide, copper iodide, copper bromide, copper chloride, etc. can be mentioned. As copper carboxylate, copper oxalate, copper acetate, etc. can be mentioned. From the viewpoint of manufacturability, the copper compound can be a copper halide or copper chloride. The copper compound can be used alone or in combination of two or more.
[0039] The reducing compound is not particularly limited as long as it has a reducing power to reduce the copper compound and free the metallic copper. Examples of the reducing compound include sodium compounds such as sodium borohydride, sodium sulfite, sodium bisulfite, sodium thiosulfate, and sodium hypophosphite; hydrazine compounds such as hydrazine, hydrazine derivatives, hydrazine hydrochloride, and hydrazine sulfate; and organic acids such as oxalic acid and formic acid. From the perspective of adjusting the thickness of the coating layer to the desired thickness, the reducing compound may be a sodium compound or sodium borohydride. The reducing compound may be used alone or in combination of two or more.
[0040] From the viewpoint of adjusting the thickness of the coating layer to a desired thickness, the amount of the reducing compound may be 1 mol to 50 mol, 2 mol to 40 mol, or 2 mol to 30 mol per mol of the copper compound.
[0041] The water-soluble chloride is used as a colloid stabilizer. Examples of the water-soluble chloride include sodium chloride, potassium chloride, and magnesium chloride. The water-soluble chloride may also be sodium chloride. The water-soluble chloride may be used alone or in combination of two or more.
[0042] From the viewpoint of stability of the copper particle dispersion, the amount of the water-soluble chloride may be 2 mol to 80 mol, 2 mol to 60 mol, or 2 mol to 40 mol per mol of the copper compound.
[0043] Reducing sugars are used as reducing aids. Examples of reducing sugars include sucrose, galactose, and fructose. The reducing sugar may also be sucrose. The reducing sugars may be used alone or in combination of two or more.
[0044] From the viewpoint of the reducing property of the copper compound, the amount of the reducing sugar may be 0.5 mol to 10 mol, 1 mol to 5 mol, or 1 mol to 2 mol per mol of the copper compound.
[0045] Examples of the dispersion medium include water and alcohols, and examples of the alcohol include methanol, ethanol, propanol, and butanol.
[0046] The dispersion medium may be used in any amount as long as the copper particles can be dispersed.
[0047] A copper compound, a reducing compound, a water-soluble chloride and a reducing sugar are added to a dispersion medium and stirred manually or with a stirrer to prepare a copper particle dispersion. The order of mixing the above compounds is not particularly limited, and the copper compound, the water-soluble chloride and the reducing sugar may be added to the dispersion medium and the reducing compound may be added while stirring.
[0048] From the viewpoint of adjusting the thickness of the coating layer to the desired thickness, the rate of addition of the reducing compound may be 0.1 g / min to 5.0 g / min, 0.1 g / min to 3.0 g / min, or 0.1 g / min to 2.0 g / min.
[0049] Based on the total amount (100% by mass) of the dispersion, the solid content concentration of the copper particle dispersion can be 1% by mass or more and 80% by mass or less, 5% by mass or more and 50% by mass or less, or 10% by mass or more and 40% by mass or less. When the solid content concentration is 1% by mass or more, the coating rate of the coating layer can be prepared to a desired range, and when the solid content concentration is 80% by mass or less, the dispersibility of the copper particles is ensured.
[0050] In addition, in this invention, "solid content concentration" means the content (concentration) of the component other than a dispersion medium.
[0051] The agitator used in the dispersion treatment for obtaining the copper particle dispersion can use various known agitators. For example, a high-speed stirring and mixing device such as a disperser and a homogenizer; a kneading machine such as a roll mill, a kneader, an extruder; a high-pressure disperser such as a high-pressure homogenizer; a medium-type disperser such as a paint shaker and a bead mill; a mixing and stirring device such as an anchor-shaped impeller, etc. These devices can also be used in combination.
[0052] The average particle size of the copper particles contained in the copper particle dispersion can be 1 nm or more and 150 nm or less, 2 nm or more and 130 nm or less, or 3 nm or more and 120 nm or less. When the average particle size of the copper particles is 1 nm or more, antibacterial properties can be exhibited, and when the average particle size of the copper particles is 150 nm or less, the obtained composite material can further exert the functions of copper such as antibacterial properties and electrical conductivity.
[0053] The average particle size of the copper particles can be measured by a field emission scanning electron microscope (FE-SEM). Specifically, it can be measured using the method described in Examples.
[0054] The shape of the copper particles is not particularly limited, and examples thereof include spherical, plate-like, flaky, scaly, dendritic, rod-like, and linear shapes.
[0055] Then, the cellulose nanofibers are immersed in the copper particle dispersion, thereby obtaining a composite material having a core material composed of the cellulose nanofibers and a coating layer composed of copper coating the core material.
[0056] There is no particular limitation on the conditions for immersing the cellulose nanofibers in the copper particle dispersion, and the immersion temperature may be 5°C to 60°C for 0.1 hour to 6 hours, 5°C to 40°C for 0.1 hour to 3 hours, or 10°C to 40°C for 0.5 hour to 2 hours. By immersing the cellulose nanofibers in the copper particle dispersion under the above conditions, the coating rate of the coating layer can be prepared to be within the desired range.
[0057] Furthermore, by appropriately adjusting the amount of cellulose nanofibers immersed in the copper particle dispersion, the coverage rate of the coating layer can be adjusted to a desired range.
[0058] From the viewpoint of the adsorptivity of copper particles, the cellulose nanofibers may be immersed in an aqueous solution of a cationic surfactant having a quaternary amine group before being immersed in the copper particle dispersion. As the cationic surfactant having a quaternary amine group, for example, trimethyl stearyl ammonium chloride, dicocoyl dimethyl ammonium chloride, etc. may be cited. The cationic surfactant having a quaternary amine group may also be trimethyl stearyl ammonium chloride.
[0059] The composite material obtained in this way can be washed with water or alcohol. Examples of the alcohol used for washing include methanol, ethanol, propanol, and the like.
[0060] The coating layer of the composite material may also be plated to form a coating layer on the surface of the coating layer. The plating process uses electroless plating. Electroless plating is, for example, a method of causing an electroless plating solution to contact the coating layer of the composite material, so that the metal contained in the electroless plating solution is precipitated and a coating layer consisting of a metal film is formed. The electroless plating solution used in the electroless plating process can use a known electroless plating solution without particular limitation.
[0061] Alternatively, the coating layer may be subjected to electroless plating and then electrolytic plating to form a plated layer. The electrolytic plating treatment can be performed using a known method and is not particularly limited.
[0062] [Dispersion liquid]
[0063] The composite material of the present invention can also be used in a dispersion in which the composite material is dispersed. Examples of the dispersion medium for dispersing the composite material include water, organic solvents, and resins.
[0064] Examples of the organic solvent used as the dispersion medium include ethanol, terpineol, carbitol acetate, etc. The organic solvent may be used alone or in combination of two or more.
[0065] Examples of the resin used for the dispersion medium include silicone resins, epoxy resins, acrylic resins, etc. The resins may be used alone or in combination of two or more.
[0066] The composite material is added to a dispersion medium and stirred sufficiently by hand or with a stirrer to prepare a dispersion liquid.
[0067] The solid content concentration of the dispersion liquid may be 0.1% to 50% by mass, 0.1% to 40% by mass, or 0.1% to 20% by mass, based on the total amount of the dispersion liquid (100% by mass). When the solid content concentration is 0.1% to 40% by mass, the antibacterial property can be exhibited, and when the solid content concentration is 50% to 50% by mass, the dispersibility in the dispersion medium can be ensured.
[0068] [use]
[0069] The composite material of the present invention reduces copper oxidation and can exhibit copper functions such as antibacterial property and electrical conductivity. Therefore, the composite material of the present invention and the dispersion containing the composite material can be suitably used as sprays containing them; sanitary materials such as masks, diapers, and sanitary products; transparent conductive materials for liquid crystal displays, touch screens, solar cells, etc.; filters for air conditioners, air purifiers, etc.; and coating agents for antifouling and anti-damage purposes.
[0070] Example
[0071] Next, the present invention will be specifically described by way of examples, but the present invention is not limited to these examples at all.
[0072] (Production Example 1)
[0073] 10 g of sucrose was added to a reactor containing 1 L of an aqueous solution containing 20 mmol of copper chloride (CuCl2) and 0.1 mol of sodium chloride (NaCl), and sodium borohydride (NaBH4) was added dropwise at a rate of 1 g / min while stirring to obtain a copper nanocolloid liquid containing copper particles with an average particle size of 5 nm and a solid content concentration of 1% by mass.
[0074] Cellulose nanofibers (trade name: ELLEX-☆ (registered trademark), manufactured by Daio Paper Co., Ltd., average fiber diameter 5 nm, average fiber length 1 μm) washed with a 1M sodium hydroxide (NaOH) aqueous solution in advance were immersed in a 1% trimethylstearyl ammonium chloride aqueous solution, and then immersed in the above copper nanocolloid solution at a temperature of 25° C. for 1 hour, and then washed with ethanol to obtain a composite material 1. The cross section of the obtained composite material 1 was observed using a field emission scanning electron microscope (FE-SEM) (JSM-7401F, manufactured by JEOL Ltd.), and it was confirmed that a copper layer (coating layer) of approximately uniform thickness was formed on the entire surface of the cellulose nanofibers in the composite material 1.
[0075] It should be noted that the coverage rate of the coating layer of the composite material 1 is 99%, and the thickness of the coating layer is 5 nm.
[0076] (Production Example 2)
[0077] 10g of sucrose was added to a reactor containing 1L of an aqueous solution containing 30mmol of copper chloride (CuCl2) and 0.1mol of sodium chloride (NaCl), and sodium borohydride (NaBH4) was added dropwise at a rate of 2g / min while stirring to obtain a copper nano colloidal liquid containing copper particles with an average particle size of 20nm. 1L of water was added to the obtained copper nano colloidal liquid for dilution to prepare a copper nano colloidal liquid with a solid content concentration of 2% by mass.
[0078] Cellulose nanofibers (trade name: ELLEX-☆ (registered trademark), manufactured by Daio Paper Industries, Ltd., with an average fiber diameter of 5 nm and an average fiber length of 1 μm) that had been previously washed with a 1M sodium hydroxide (NaOH) aqueous solution were immersed in a 1% trimethylstearyl ammonium chloride aqueous solution, and then immersed in the above-mentioned copper nanocolloid solution at a temperature of 25°C for 1 hour, and then washed with ethanol to obtain a composite material 2 having a copper layer (coating layer) formed on the surface of the cellulose nanofibers.
[0079] It should be noted that the coverage rate of the coating layer of the composite material 2 is 50%, and the thickness of the coating layer is 20 nm.
[0080] (Production Example 3)
[0081] Sucrose 10g is added to a reactor containing 1L of an aqueous solution containing copper chloride (CuCl2) 50mmol and sodium chloride (NaCl) 0.1mol, and sodium borohydride (NaBH4) is dripped into the reactor at a speed of 2.5g / min while stirring to obtain a copper nano colloidal liquid containing copper particles with an average particle size of 50nm. Water 4L is added to the obtained copper nano colloidal liquid and diluted to make a copper nano colloidal liquid with a solid content concentration of 5% by mass.
[0082] Cellulose nanofibers (trade name: ELLEX-☆ (registered trademark), manufactured by Daio Paper Industries, Ltd., with an average fiber diameter of 5 nm and an average fiber length of 1 μm) that had been previously washed with a 1M sodium hydroxide (NaOH) aqueous solution were immersed in a 1% trimethylstearyl ammonium chloride aqueous solution, and then immersed in the above-mentioned copper nanocolloid solution at a temperature of 25°C for 1 hour, and then washed with ethanol to obtain a composite material 3 having a copper layer (coating layer) formed on the surface of the cellulose nanofibers.
[0083] It should be noted that the coverage rate of the coating layer of the composite material 3 is 20%, and the thickness of the coating layer is 50 nm.
[0084] (Production Example 4)
[0085] The same method as in Manufacturing Example 1 was used, except that cellulose nanofibers with an average fiber diameter of 20 nm and an average fiber length of 1 μm and trade name: ELLEX-S, manufactured by Daio Paper Co., Ltd., were used to obtain a composite material 4' having a copper layer (coating layer) formed on the surface of the cellulose nanofibers. The obtained composite material 4' was immersed in an electroless plating solution (OPC-700 electroless copper MK, manufactured by Okuno Pharmaceutical Co., Ltd.) and subjected to electroless copper plating treatment to obtain a composite material 4 having a copper plating layer formed on the surface of the coating layer.
[0086] It should be noted that the coverage rate of the coating layer of the composite material 4 was 99%, and the total thickness of the copper layer (5 nm) and the copper plating layer (75 nm) was 80 nm.
[0087] (Production Example 5)
[0088] Sucrose 10g is added to a reactor containing 1L of an aqueous solution containing cupric chloride (CuCl2) 20mmol and sodium chloride (NaCl) 0.1mol, and sodium borohydride (NaBH4) is dripped into the reactor at a speed of 1g / min while stirring to obtain a copper nano colloidal liquid containing copper particles of an average particle size of 5nm. Water 9L is added to the obtained copper nano colloidal liquid and diluted to make a copper nano colloidal liquid with a solid content concentration of 0.1% by mass.
[0089] Cellulose nanofibers (trade name: ELLEX-☆ (registered trademark), manufactured by Daio Paper Industries, Ltd., with an average fiber diameter of 5 nm and an average fiber length of 1 μm) that had been previously washed with a 1 M sodium hydroxide (NaOH) aqueous solution were immersed in a 1% trimethylstearyl ammonium chloride aqueous solution, and then immersed in the above-mentioned copper nanocolloid solution at a temperature of 25°C for 0.5 hour and then washed with ethanol to obtain a composite material 5 having a copper layer (coating layer) formed on the surface of the cellulose nanofibers.
[0090] It should be noted that the coverage rate of the coating layer of the composite material 5 is 10%, and the thickness of the coating layer is 5 nm.
[0091] (Production Example 6)
[0092] 2L of 15M sodium hydroxide (NaOH), 100mL of 0.2M copper (II) nitrate (Cu(NO3)2), 30mL of ethylenediamine (EDA) and 2.5mL of 35% by mass hydrazine aqueous solution were added to the reaction flask and stirred and mixed for 20 seconds. The solution was heated to 80°C and stirred at 200 rpm for 60 minutes. After the reaction, the reaction solution was washed with a 3% by mass hydrazine aqueous solution to obtain copper nanowires.
[0093] 〔Evaluation Item〕
[0094] (Average particle size of copper particles)
[0095] The dispersion medium was evaporated from the copper nano-colloid liquid obtained in Production Examples 1 to 5 to obtain copper particles.
[0096] The average particle size of the copper particles was calculated as an average value of 100 copper particles from an image of the copper particles captured using a field emission scanning electron microscope (FE-SEM) (JSM-7401F, manufactured by JEOL Ltd.).
[0097] (Shape of copper (particles))
[0098] The dispersion medium was evaporated from the copper nano-colloid liquid obtained in Production Examples 1 to 5 to obtain copper particles.
[0099] The shape of the copper (particles) was confirmed by taking an image of the copper particles or the copper nanowires obtained in Production Example 6 using a field emission scanning electron microscope (FE-SEM) (JSM-7401F, manufactured by JEOL Ltd.).
[0100] (Covering rate of coating layer or ratio of copper contained in copper nanowire)
[0101] For the obtained composite material or copper nanowire, a differential thermal-thermogravimetric simultaneous measurement device (TG / DTA) (TG209F1Libra, manufactured by NETZSCH, Germany) was used to heat 10 mg of the sample from 25°C to 600°C at a heating rate of 10°C / min in an argon environment, and the mass of the sample after holding for 60 minutes was measured. The coating rate of the coating layer in the composite material is calculated as the ratio of the mass of the sample after the measurement to the mass of the sample before the measurement. In addition, the ratio of copper contained in the copper nanowire is calculated based on the ratio of the mass of the sample after the measurement to the mass of the sample before the measurement.
[0102] (Thickness of coating layer or diameter of copper nanowire)
[0103] The composite material or copper nanowire obtained was cut using a focused ion beam (FIB) to make a cross-sectional slice, and the cross-section was photographed using a transmission electron microscope (TEM) at a magnification of 500,000 times, and the thickness of the coating layer of the composite material and the diameter of the copper nanowire were calculated by measuring the average value of 500,000 points. It should be noted that in Table 1, the thickness of the coating layer of the composite material 4 obtained in Preparation Example 4 is the total thickness of the copper layer and the copper plating layer.
[0104] [Table 1]
[0105]
[0106] (Examples 1 to 5, Comparative Examples 1 and 2)
[0107] The components of the types and blending amounts described in Table 2 were mixed to prepare a dispersion.
[0108] The details of the components described in Table 2 used for preparing the dispersion are as follows.
[0109] Composite material 1: the composite material produced in Production Example 1.
[0110] Composite material 2: the composite material produced in Production Example 2.
[0111] Composite material 3: the composite material produced in Production Example 3.
[0112] Composite material 4: the composite material produced in Production Example 4.
[0113] Composite material 5: the composite material produced in Production Example 5.
[0114] Copper nanowire: the copper nanowire produced in Production Example 6.
[0115] Cellulose nanofiber (CNF): ELLEX-☆ (registered trademark), manufactured by Daio Paper Industries, Ltd., with an average fiber diameter of 5 nm and an average fiber length of 1 μm.
[0116] Ethanol (dispersion medium): manufactured by Tokyo Chemical Industry Co., Ltd.
[0117] 〔Evaluation Item〕
[0118] (Degree of oxidation)
[0119] For composite materials or copper nanowires, X-ray diffraction (XRD) is used to quantify the content using the RIR (reference intensity ratio) method based on the integrated intensity ratio of the strongest line peaks of each component of Cu, CuO, and Cu2O. The degree of oxidation is calculated using the following formula (1) and evaluated according to the following evaluation criteria.
[0120] Mathematical formula 1
[0121] Oxidation degree (%) = ([CuO] + [Cu2O]) / ([Cu] + [CuO] + [Cu2O]) × 100 (1)
[0122] It should be noted that in formula (1), [Cu] represents the content (mass %) of copper (Cu) in the composite material or copper nanowires, [CuO] represents the content (mass %) of copper (II) oxide in the composite material or copper nanowires, and [Cu2O] represents the content (mass %) of copper (I) oxide in the composite material or copper nanowires.
[0123] [Evaluation criteria]
[0124] A: The degree of oxidation is less than 1%.
[0125] B: The degree of oxidation is 1% or more and less than 3%.
[0126] C: The degree of oxidation is 3% or more.
[0127] (Antiviral)
[0128] The antiviral effect of the antiviral product (antiviral processed glass) obtained by applying the dispersion on glass and drying was evaluated. The virus infectivity titer was 2×10 4 100mL of influenza A virus solution with a PFU / mL was added to the surface of an antiviral processed glass with a size of 5cm×5cm and allowed to stand at 25°C for 2 hours. Then, the virus solution on the surface of the antiviral processed glass was recovered, the number of plaques in the recovered solution was determined, and the virus infectivity titer was measured. In addition, the virus infectivity titer of the influenza A virus solution before standing for 2 hours was also measured. The antiviral effect is determined by these virus infectivity titers. The case where the virus infectivity titer after standing for 2 hours is below the detection limit is set to "++", the case where the antiviral activity value after standing for 2 hours calculated according to the following formula is reduced by more than 1 is set to "+", and the case where the virus infectivity titer after standing for 2 hours is "++" and the antiviral activity value after standing for 2 hours is other than "+" is set to "-".
[0129] Antiviral activity value = log(Vb)-log(Vc)
[0130] Wherein, log(Vb) is the common logarithm value of the virus infectivity titer of the influenza A virus solution before standing for 2 hours, and log(Vc) is the common logarithm value of the virus infectivity titer of the influenza A virus solution after standing for 2 hours on the antiviral processed glass surface.
[0131] (Antibacterial and deodorizing effect)
[0132] The dispersion was applied to a sterilized standard cotton cloth, and the antibacterial and deodorizing effects were evaluated. It should be noted that the meanings of the evaluation indicators in Table 2 are as follows.
[0133] (Antibacterial test)
[0134] The antibacterial test method is carried out in accordance with JISL-1902:2008 quantitative test (bacterial liquid absorption method). A sample prepared by adding 0.9 mL of the dispersion to 0.4 g of sterilized standard cotton cloth is used as the test sample. The test strain uses Escherichia coli or Staphylococcus aureus. After culturing at room temperature (25°C) for 24 hours, an antibacterial activity value of 2.2 or more (bacterial reduction rate = 99.4% or more) is used as the judgment value of the effect.
[0135] (Deodorization test)
[0136] The test cotton cloth to which 3 L of test gas (ammonia gas) and 1 mL of dispersion liquid were added was put into a 5 L Tedlar air bag, and the gas concentration after 2 hours was reduced by 90% or more from the initial concentration (=100 ppm) as the judgment value.
[0137] [Judgment criteria]
[0138] Based on the above measurement results, evaluation was performed according to the following criteria.
[0139] A: In the antibacterial test, the antibacterial activity value was 2.4 or more, and in the deodorization test, the gas concentration was reduced by 96% or more, and a high antibacterial and deodorizing effect was confirmed.
[0140] B: In the antibacterial test, the antibacterial activity value was 2.2 or more and less than 2.4, and in the deodorization test, the gas concentration was reduced by 90% or more and less than 96%, and the antibacterial and deodorizing effect was confirmed.
[0141] C: In the antibacterial test, the antibacterial activity value was less than 2.2, or the reduction in gas concentration in the deodorization test was less than 90%, and the antibacterial effect or deodorizing effect could not be confirmed.
[0142] (Conductivity (surface resistivity))
[0143] The surface resistivity of the composite material, copper nanowire or CNF was measured by a four-probe method using "Loresta HP MCP-T410" manufactured by Mitsubishi Chemical Analytech Co., Ltd. and evaluated according to the following evaluation criteria.
[0144] [Evaluation criteria]
[0145] A: Surface resistivity is less than 50Ω / sq.
[0146] B: The surface resistivity is 50 Ω / sq. or more and less than 100 Ω / sq.
[0147] C: Surface resistivity is 100Ω / sq. or more.
[0148] (Transmittance)
[0149] The dispersion was applied to a glass substrate, and the total light transmittance of the dispersion was measured. The total light transmittance was measured using a turbidimeter "NDH2000" manufactured by Nippon Denshoku Industries Co., Ltd. as a measuring instrument. In addition, an uncoated glass substrate was used as a reference sample for the optical property measurement, and only the optical properties of the coating film were measured.
[0150] [Table 2]
[0151]
[0152] *1: Not rated
[0153] It was found that the copper oxidation of Examples 1 to 5 using the dispersion containing the composite material of the present invention was low, and the evaluations of antiviral property, antibacterial and deodorizing effect, electrical conductivity, and transmittance were good.
Claims
1. A composite material, wherein: have: a core material composed of cellulose nanofibers; and The cladding layer is composed of copper covering the core material.
2. The composite material according to claim 1, wherein The coating layer has a thickness of 1 nm or more and 150 nm or less.
3. The composite material according to claim 1 or 2, wherein: The coverage of the cladding layer with respect to the core material is 0.5% or more and 99% or less.
4. The composite material according to any one of claims 1 to 3, wherein The cellulose nanofibers have an average fiber diameter of 3 nm or more and 100 nm or less.
5. The composite material according to any one of claims 1 to 4, wherein The composite material comprises a plating layer covering the covering layer.
6. A dispersion liquid in which the composite material according to any one of claims 1 to 5 is dispersed.
7. A spray, wherein: The spray comprises the composite material according to any one of claims 1 to 5 or the dispersion according to claim 6.
8. A sanitary material, wherein: The sanitary material comprises the composite material according to any one of claims 1 to 5 or the dispersion according to claim 6.
9. A filter, wherein: The filter comprises the composite material according to any one of claims 1 to 5 or the dispersion according to claim 6.
10. A coating agent, wherein The coating agent comprises the composite material according to any one of claims 1 to 5 or the dispersion according to claim 6.
11. A method for producing a composite material according to any one of claims 1 to 5, wherein: The cellulose nanofibers are immersed in the copper particle dispersion.
12. The method for producing a composite material according to claim 11, wherein: The average particle diameter of the copper particles contained in the copper particle dispersion is 1 nm or more and 150 nm or less.