Resin sheet, container, carrier tape, and electronic component package

By using a layered structure of polystyrene-based resin substrate sheets and conductive materials within a specific range, the problem of easy deformation of extremely small electronic components in the carrier tape was solved, achieving high-precision molding and deformation resistance, and avoiding pick-up defects.

CN118946616APending Publication Date: 2024-11-12DENKA CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380028746.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-28
Filing Date
2023-03-02
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

In the process of handling miniaturized electronic components, the miniaturized size of the carrier tape's storage section makes it easy for the nozzle to deform upon contact, resulting in poor pickup. Furthermore, the components are prone to tilting during transport, making them difficult to pick up.

Method used

The polystyrene-based resin sheet has a maximum puncture modulus of 2.4–6.4 MPa, a storage modulus E'1 of 1.0 × 10⁸ Pa to 1.0 × 10¹⁰ Pa at 25°C, and a storage modulus E'2 of 1.0 × 10⁶ Pa at the loss tangent peak temperature of +20°C. Combined with a conductive material laminate structure, a resin sheet with excellent deformation resistance and formability is formed.

Benefits of technology

It achieves good formability of the carrier tape storage section and resistance to deformation of the pick-up nozzle during the handling of extremely small parts, thus suppressing the occurrence of pick-up defects.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118946616A_ABST
    Figure CN118946616A_ABST
Patent Text Reader

Abstract

The resin sheet is provided with a base sheet containing a polystyrene resin, and has a maximum puncture elastic modulus of 2.4-6.4 MPa as calculated according to the following steps. [Maximum puncture elastic modulus calculation step] A measurement sample is fixed to a flat jig having a hole having a diameter of 1.0 mm provided in the center thereof, and the load L (N) and the strain amount epsilon in the puncture direction are measured when the surface of the measurement sample is vertically punctured by a cylindrical needle having a planar tip shape and a diameter of 0.8 mm at a speed of 0.5 mm / min. The maximum puncture elastic modulus is the value when the ratio between the stress difference and the strain amount difference calculated by the formula ([delta] L / S) / [delta] [epsilon] (in the formula, S represents the area (mm2) of the tip surface of the needle) is the maximum in 0.1 < = [epsilon] < = 5.0.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a resin sheet, a container, a carrier tape and an electronic component package. Background Art

[0002] Vacuum-formed trays and embossed carrier tapes obtained by heat-forming resin sheets are used as packaging containers for intermediate products of industrial products such as electronic devices and automobiles. In addition, resin sheets having a laminated structure in which a surface layer containing a thermoplastic resin and a conductive material such as carbon black is laminated on a base layer formed of a thermoplastic resin are used as sheets for packaging containers for ICs that are sensitive to static electricity and various components having ICs (for example, see the following Patent Documents 1 to 3).

[0003] In the production of the embossed carrier tape, a resin sheet is molded using a molding method such as press molding to provide a storage portion that matches the shape of the component being transported.

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: Japanese Patent Application Laid-Open No. 9-76422

[0007] Patent Document 2: Japanese Patent Application Laid-Open No. 9-76425

[0008] Patent Document 3: Japanese Patent Application Laid-Open No. 9-174769 Summary of the invention

[0009] Problems to be solved by the invention

[0010] In recent years, various electronic components such as capacitors, resistors, ICs, LEDs, connectors, and switching elements are being miniaturized. In the carrier tape that carries such extremely small components, the size of the storage section is minimized, so when the electronic components are installed, the nozzle that picks up the components is easy to contact the carrier tape. If the opening of the storage section is excessively deformed due to the contact of the nozzle, poor picking up may occur, such as the inability to remove the components. In addition, poor picking up of components sometimes occurs due to other major factors. If the extremely small components stored in the storage section move and tilt during transportation, it becomes difficult to adsorb. Therefore, high precision is required for the molding of the storage section of extremely small components.

[0011] An object of the present invention is to provide a resin sheet having sufficient moldability and excellent resistance to deformation under local load, and a container, a carrier tape, and an electronic component package obtained using the same.

[0012] Means for solving problems

[0013] One aspect of the present invention relates to the following [1] to [7].

[0014] [1] A resin sheet comprising a base sheet containing a polystyrene resin, wherein the maximum puncture elastic modulus calculated according to the following steps is 2.4 to 6.4 MPa,

[0015] [Calculation steps for maximum puncture elastic modulus]

[0016] The sample for measurement was fixed to a flat fixture with a hole of 1.0 mm in diameter at the center. The load L (N) and the strain ε in the puncture direction when a needle with a circular tip (diameter 0.8 mm) was vertically punctured into the surface of the sample for measurement at a speed of 0.5 mm / min were measured under an environment of 23°C. The load L (N) and the strain ε in the puncture direction were measured using the formula: (ΔL / S) / Δε (where S represents the area of ​​the tip surface of the needle (mm 2 The value at which the ratio of the calculated stress difference to the strain difference becomes the maximum in the range of 0.1≤ε≤5.0 is taken as the maximum puncture elastic modulus.

[0017] [2] The resin sheet according to [1], wherein the storage modulus E'1 at 25°C is 1.0×10 8 Pa above 1.0×10 10 Pa or less, and the storage modulus E'2 at the peak temperature of the loss tangent +20°C is 1.0×10 6 Below Pa.

[0018] [3] The resin sheet according to [1] or [2], wherein the base sheet contains 50% by mass or more of one or more of a general-purpose polystyrene resin and an impact-resistant polystyrene resin in total, based on the total amount of the styrene-based resin.

[0019] [4] A resin sheet comprising a base sheet containing a thermoplastic resin, wherein the storage modulus E'1 at 25°C is 1.0×10 8 Pa above 1.0×10 10 Pa or less, and the storage modulus E'2 at the peak temperature of the loss tangent +20°C is 1.0×10 6 Below Pa.

[0020] [5] A container which is a molded product of the resin sheet according to any one of [1] to [4] above.

[0021] [6] A carrier tape which is a molded product of the resin sheet according to any one of [1] to [4] above and has a storage portion capable of storing articles.

[0022] [7] An electronic component package comprising: the carrier tape according to [6] above; the electronic component accommodated in the accommodation portion of the carrier tape; and a cover film adhered to the carrier tape as a cover material.

[0023] In order to solve the above-mentioned problems, one aspect of the present invention provides a resin sheet including a base sheet containing a polystyrene-based resin and having a maximum puncture elastic modulus of 2.4 to 6.4 MPa calculated according to the following procedure.

[0024] [Calculation steps for maximum puncture elastic modulus]

[0025] The sample for measurement was fixed to a flat fixture with a hole of 1.0 mm in diameter at the center. The load L (N) and the strain ε in the puncture direction when a needle with a circular tip (diameter 0.8 mm) was vertically punctured into the surface of the sample for measurement at a speed of 0.5 mm / min were measured under an environment of 23°C. The load L (N) and the strain ε in the puncture direction were measured using the formula: (ΔL / S) / Δε (where S represents the area of ​​the tip surface of the needle (mm 2 The value at which the ratio of the calculated stress difference to the strain difference becomes the maximum in the range of 0.1≤ε≤5.0 is taken as the maximum puncture elastic modulus.

[0026] According to the resin sheet, by containing a polystyrene resin and having a maximum puncture elastic modulus within the above-mentioned specific range, it is possible to have both the characteristic of not being easily deformed by a local load and the moldability of a molded body being able to be obtained with sufficient accuracy when performing molding such as press molding. According to the carrier formed of such a resin sheet, in the use of conveying extremely small parts, it is possible to have a well-molded storage portion, and the deformation caused by the contact of the pickup nozzle can be sufficiently suppressed, and the occurrence of the above-mentioned pick-up failure can be suppressed.

[0027] When the dynamic viscoelasticity of the resin sheet is measured, the storage modulus E'1 at 25°C is 1.0×10 8 Pa above 1.0×10 10 Pa or less, and the storage modulus E'2 at the peak temperature of the loss tangent +20°C can be 1.0×10 6 Below Pa.

[0028] The base sheet may contain 50% by mass or more of one or more of a general-purpose polystyrene resin and an impact-resistant polystyrene resin in total, based on the total amount of the polystyrene resin.

[0029] Another aspect of the present invention provides a resin sheet comprising a base sheet containing a thermoplastic resin, wherein the storage modulus E'1 at 25°C is 1.0×10 8Pa above 1.0×10 10 Pa or less, and the storage modulus E'2 at the peak temperature of the loss tangent +20°C is 1.0×10 6 Below Pa.

[0030] The above-mentioned resin sheet can have both the characteristics of not being easily deformed by local loads and the moldability of a molded body with sufficient accuracy when performing heat molding such as press molding by making the storage modulus E'1 and the storage modulus E'2 within the above-mentioned specific range. According to the carrier formed by such a resin sheet, in the use of conveying extremely small parts, it is possible to have a well-molded storage part, and can fully ensure the deformation resistance to the contact of the pickup nozzle, which can suppress the occurrence of the above-mentioned pick-up defects.

[0031] Another aspect of the present invention provides a container which is a molded product of the above-mentioned resin sheet.

[0032] Another aspect of the present invention provides a carrier tape which is a molded product of the above-mentioned resin sheet and is provided with a storage portion capable of storing articles.

[0033] Another aspect of the present invention provides an electronic component package including: the carrier tape described above; the electronic component accommodated in the accommodation portion of the carrier tape; and a cover film adhered to the carrier tape as a cover material.

[0034] Effects of the Invention

[0035] According to the present invention, it is possible to provide a resin sheet having sufficient moldability and capable of obtaining a carrier tape having excellent deformation resistance against a local load, and a container, a carrier tape, and an electronic component package obtained using the same. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] [ Figure 1 ] is a schematic cross-sectional view showing an embodiment of a resin sheet.

[0037] [ Figure 2 ] is a partially cutaway stereoscopic view showing one embodiment of a carrier tape.

[0038] [ Figure 3 ] is a partially cutaway perspective view showing an embodiment of an electronic component package.

[0039] [ Figure 4 ] is a diagram for illustrating a method for evaluating the formability of a resin sheet. DETAILED DESCRIPTION

[0040] Hereinafter, preferred embodiments of the present invention will be described in detail.

[0041] [Resin sheet]

[0042] The resin sheet of the present embodiment includes a base sheet containing a thermoplastic resin. The resin sheet of the present embodiment may further include a surface layer containing a conductive material and a thermoplastic resin and laminated on at least one surface of the base sheet.

[0043] Figure 1 It is a schematic cross-sectional view showing an embodiment of the resin sheet of this embodiment. Figure 1 The resin sheet 10 shown in (a) is composed of a base sheet 1 . Figure 1 The resin sheet 12 shown in (b) includes a base sheet 1 and a surface layer 2 provided on one surface of the base sheet 1 . Figure 1 The resin sheet 14 shown in (c) comprises a substrate sheet 1, a surface layer 2 laminated on one side of the substrate sheet, and a second surface layer 3 laminated on the other side of the substrate sheet. The surface layer 2 and the second surface layer 3 may have the same composition or different compositions.

[0044] (First resin sheet)

[0045] The resin sheet of the present embodiment may include a base sheet (hereinafter also referred to as a “first resin sheet”) containing a polystyrene-based resin.

[0046] The maximum puncture elastic modulus of the first resin sheet calculated according to the following procedure is 2.4 to 6.4 MPa.

[0047] [Calculation steps for maximum puncture elastic modulus]

[0048] The sample for measurement was fixed to a flat fixture with a hole of 1.0 mm in diameter at the center. The load L (N) and the strain ε in the puncture direction when a needle with a circular tip (diameter 0.8 mm) was vertically punctured into the surface of the sample for measurement at a speed of 0.5 mm / min were measured under an environment of 23°C. The load L (N) and the strain ε in the puncture direction were measured using the formula: (ΔL / S) / Δε (where S represents the area of ​​the tip surface of the needle (mm 2 ). In the case of the above needle, the value when the ratio of the calculated stress difference to the strain difference is the maximum in 0.1≤ε≤5.0 is taken as the maximum puncture elastic modulus. It should be noted that when the displacement in the puncture direction is set to D (mm) and the thickness of the resin sheet is set to t (mm), the strain ε is represented by D / t.

[0049] The sample for measurement can be of a size of 5 cm in length and 5 cm in width. The above-mentioned puncture test can be carried out using a tensile tester (Strograph VE-1D manufactured by Toyo Seiki Seisaku-sho, Ltd.).

[0050] By having the maximum puncture elastic modulus in the above-mentioned specific range, it is possible to have both the characteristic of not being easily deformed by a local load and the moldability of a molded body being able to be obtained with sufficient accuracy when performing molding such as press molding. According to the carrier formed of such a resin sheet, in the use of conveying extremely small parts, it is possible to have a well-molded storage portion, and the deformation caused by the contact of the pickup nozzle can be sufficiently suppressed, and the occurrence of the above-mentioned pickup failure can be suppressed.

[0051] From the viewpoint of achieving both high levels of moldability and deformation resistance against local loads, the maximum puncture elastic modulus of the first resin sheet may be 3.0 MPa to less than 6.2 MPa, or 4.0 MPa to less than 6.0 MPa.

[0052] In the puncture test, when the load (maximum load) measured when fracture occurs is taken as the puncture strength, the puncture strength of the first resin sheet may be 7.0 to 14.0 N or 8.0 to 13.0 N from the viewpoint of deformation resistance to local load.

[0053] The first resin sheet has a storage modulus E'1 of 1.0×10 8 Pa above 1.0×10 10 Pa or less, and the storage modulus E'2 at the peak temperature of the loss tangent (hereinafter sometimes referred to as "Tg") + 20°C can be 1.0×10 6 Pa or less. In addition, the dynamic viscoelasticity measurement of the resin sheet was performed under the following conditions.

[0054] The resin sheet was cut into a size of 40 mm in length and 3 mm in width to prepare a sample for measurement. The sample for measurement was subjected to dynamic viscoelasticity measurement using a dynamic viscoelasticity apparatus RAS-G2 (manufactured by TA Instruments) under the following measurement conditions.

[0055] [Measurement conditions]

[0056] Deformation mode: Sine wave stretching mode (Linear tension, linear stretching)

[0057] Measuring temperature: 20℃~200℃

[0058] Measuring frequency: 1Hz

[0059] Heating rate: 10℃ / min

[0060] Initial value of static tensile load: 0.2N

[0061] Initial (at 20°C) gap distance: 10mm

[0062] In addition, when the thickness of the resin sheet is larger than 1 mm, the width of the measurement sample may be adjusted to 3 to 10 mm to perform the above-mentioned dynamic viscoelasticity measurement.

[0063] From the viewpoint of further improving the deformation resistance against local load, the storage modulus E'1 may be 1.0×10 9 Pa or above.

[0064] From the perspective of further improving moldability, the storage modulus E'2 can be 5.0×10 5 Pa or less. In addition, from the viewpoint of suppressing the unexpected deformation of the sheet due to heating, the storage modulus E'2 may be 1.0×10 3 Pa or more, and can also be 1.0×10 4 Pa or above.

[0065] Examples of the polystyrene resin contained in the substrate sheet include general-purpose polystyrene resins, impact-resistant polystyrene resins, and copolymers of styrene and monomers other than styrene monomers. These polystyrene resins can be used alone or in combination of two or more.

[0066] General-purpose polystyrene resin is a resin generally referred to as GPPS, and has styrene as the main monomer, but may contain one or more aromatic vinyl compounds such as o-methylstyrene, p-methylstyrene, p-tert-butylstyrene, 1,3-dimethylstyrene, α-methylstyrene, vinylnaphthalene, vinylanthracene, 1,1-diphenylethylene, etc. as trace components. Commercially available general-purpose polystyrene resins may also be used.

[0067] The weight average molecular weight (Mw) of the general-purpose polystyrene resin may be 80,000 to 220,000, or 140,000 to 220,000. In the present specification, the weight average molecular weight (Mw) can be obtained from a molecular weight distribution curve calculated in terms of standard polystyrene obtained by a conventional method using GPC.

[0068] High-impact polystyrene resin is a resin generally referred to as HIPS, and a polystyrene resin containing microparticles of grafted rubber grafted with a styrene-based monomer can be used. The styrene-based monomer is mainly composed of styrene, and can contain one or more of the above-mentioned aromatic vinyl compounds other than styrene as trace components. The grafted rubber is a substance formed by grafting and copolymerizing a styrene-based monomer to a rubber component to form a graft branch. As the rubber component in the grafted rubber, for example, a diene rubber using 1,3-butadiene (butadiene), 2-methyl-1,3-butadiene (isoprene), 2,3-dimethyl-1,3-butadiene, 1,3-pentadiene, 1,3-hexadiene, 2-methylpentadiene, etc. as monomers can be used. As the grafted rubber, a thermoplastic elastomer in which the diene component is a styrene-conjugated diene block copolymer of 50% by mass or more can also be used.

[0069] The graft rubber in the high-impact polystyrene resin may have a particle size of 2.0 μm to 3.0 μm, or 2.3 μm to 2.7 μm, from the viewpoint of transparency. The particle size of the graft rubber refers to the average particle size of the graft rubber measured by a laser diffraction particle analyzer.

[0070] The weight average molecular weight (Mw) of the high-impact polystyrene resin may be 150,000 to 210,000, or 150,000 to 190,000.

[0071] Monomers other than the polystyrene monomers in the copolymer include conjugated diene monomers, acrylonitrile, and methyl methacrylate. Conjugated diene monomers may be compounds having conjugated double bonds in their structures, such as 1,3-butadiene (butadiene), 2-methyl-1,3-butadiene (isoprene), 2,3-dimethyl-1,3-butadiene, 1,3-pentadiene, 1,3-hexadiene, and 2-methylpentadiene.

[0072] Examples of the above-mentioned copolymer include styrene-conjugated diene block copolymers, AS resins, ABS resins, AES resins, and MS resins.

[0073] The styrene-conjugated diene block copolymer can use a polymer containing a polymer block mainly composed of a styrene-based monomer and a polymer block mainly composed of a conjugated diene monomer. As the conjugated diene monomer, any compound having a conjugated double bond in its structure can be used, for example, 1,3-butadiene (butadiene), 2-methyl-1,3-butadiene (isoprene), 2,3-dimethyl-1,3-butadiene, 1,3-pentadiene, 1,3-hexadiene, 2-methylpentadiene, etc.

[0074] The first resin sheet may contain 50% by mass or more, 60% by mass or more, or 100% by mass of the polystyrene resin based on the total amount of the resin component contained in the substrate sheet from the viewpoint of moldability.

[0075] Regarding the first resin sheet, from the viewpoint of moldability, the base sheet may contain 50% by mass or more, or 60% by mass or more of one or more of a general-purpose polystyrene resin and an impact-resistant polystyrene resin, based on the total amount of the polystyrene resin.

[0076] From the viewpoint of imparting practical impact resistance to the resin sheet, the base sheet contains a general-purpose polystyrene resin and an impact-resistant polystyrene resin, and the mass ratio of these resins [GPPS:HIPS] may be 0:100 to 90:10.

[0077] The substrate sheet may contain a conductive material, a filler, a plasticizer, a processing aid, an antioxidant, an anti-blocking agent, and the like.

[0078] The thickness of the base sheet can be appropriately set according to the application, and may be, for example, 50 μm to 1 mm, 100 μm to 1 mm, or 150 to 600 μm.

[0079] The thickness of the substrate sheet can be set to 60 to 99% relative to the overall thickness of the resin sheet. When the surface layer is provided on both sides of the substrate sheet, the thickness of the substrate sheet can be set to 60 to 98% relative to the overall thickness of the resin sheet. When the surface layer is provided on only one side of the substrate sheet, the thickness of the substrate sheet can be set to 60 to 99% relative to the overall thickness of the resin sheet.

[0080] The first resin sheet may further include a surface layer including a conductive material and a thermoplastic resin, which is laminated on at least one surface of the base sheet.

[0081] As the thermoplastic resin contained in the surface layer, polystyrene resin, polyolefin resin, polycarbonate resin and polyester resin can be used. These thermoplastic resins can be used alone or in combination of two or more.

[0082] Examples of the polystyrene resin include the above-mentioned resins and hydrogenated styrene thermoplastic elastomers. Examples of the hydrogenated styrene thermoplastic elastomer include polystyrene-poly(ethylene / propylene) block (SEP), polystyrene-poly(ethylene / propylene) block-polystyrene (SEPS), polystyrene-poly(ethylene / butylene) block-polystyrene (SEBS), and polystyrene-poly(ethylene-ethylene / propylene) block-polystyrene (SEEPS).

[0083] Examples of polyolefin resins include polyethylene resins such as high-density polyethylene, ultra-low-density polyethylene, and linear low-density polyethylene; polypropylene resins; ethylene-α-olefin copolymers obtained by copolymerizing ethylene with α-olefin hydrocarbons having a C3 or higher group such as propylene, 1-butene, and 1-hexene; copolymers of olefins and monomers having polar groups copolymerizable with olefins, etc. Examples of copolymers of olefins and monomers having polar groups copolymerizable with olefins include ethylene-vinyl acetate copolymers, ethylene-acrylic acid copolymers, ethylene-ethyl acrylate copolymers, ethylene-methacrylate copolymers, ethylene-vinyl acetate-vinyl chloride copolymers, and terpolymers with acid anhydrides, etc.

[0084] As polycarbonate resin, aromatic polycarbonate resin, aliphatic polycarbonate resin, aromatic-aliphatic polycarbonate resin can be mentioned. Aromatic polycarbonate resin is a resin generally classified as engineering plastics, and the aromatic polycarbonate resin obtained by the polycondensation of bisphenol A and phosgene or the polycondensation of bisphenol A and carbonate can be used. From the aspect of mechanical strength, aromatic polycarbonate resin is preferably used.

[0085] As polyester resin, resins obtained by polycondensation reaction of dicarboxylic acid and diol can be used. As dicarboxylic acid, for example, phthalic acid, isophthalic acid, terephthalic acid, 2-methylterephthalic acid, 4,4'-diphenyl dicarboxylic acid, 5-sulfoisophthalic acid, 2,6-naphthalene dicarboxylic acid, malonic acid, succinic acid, glutaric acid, adipic acid, maleic acid, and maleic anhydride can be mentioned. They can be used alone or in combination of two or more. As diol, for example, ethylene glycol, diethylene glycol, polyethylene glycol, propylene glycol, polypropylene glycol, 1,3-propylene glycol, and 1,4-butanediol can be mentioned. They can be used alone or in combination of two or more.

[0086] Examples of the conductive material contained in the surface layer include carbon black, graphite, CNT, graphite, Ketjen black, etc. These conductive materials can be used alone or in combination of two or more.

[0087] The conductive material may be in the form of particles, and in this case, the average primary particle size of the conductive material may be 10 nm to 5.0 μm, or 20 to 50 nm. The average primary particle size of the particles may be determined by the following method.

[0088] First, an ultrasonic disperser was used to disperse the particle sample in chloroform for 10 minutes at 150kHz and 0.4kW to prepare a dispersed sample. The dispersed sample was sprinkled on a carbon-reinforced support film and fixed, and photographed using a transmission electron microscope (JEOL, JEM-2100). From the image magnified 50,000 to 200,000 times, the particle size of more than 1,000 particles (the maximum diameter in the case of shapes other than spherical) was randomly measured using Endter's device, and the average value was taken as the average primary particle size.

[0089] The content of the conductive material in the surface layer may be 10 to 30% by mass, or 15 to 25% by mass, based on the total amount of the surface layer.

[0090] The surface resistivity of the surface layer is preferably 10 4 ~10 8 Ω / □. When the surface resistivity of the surface layer is within this range, it is easy to prevent the destruction of electronic components due to static electricity or the destruction of electronic components due to the inflow of electricity from the outside.

[0091] Various additives such as lubricants, plasticizers, and processing aids can be added to the surface layer.

[0092] The thickness of the surface layer can be appropriately set according to the application, and may be, for example, 1 μm to 200 μm, 1 μm to 100 μm, or 2 μm to 50 μm.

[0093] (Second resin sheet)

[0094] The storage modulus E'1 of the resin sheet of the present embodiment at 25°C was 1.0×10 8 Pa above 1.0×10 10 Pa or less, and the storage modulus E'2 at the peak temperature of the loss tangent (hereinafter sometimes referred to as "Tg") + 20°C can be 1.0×10 6 Pa or less (hereinafter also referred to as "second resin sheet"). In addition, the dynamic viscoelasticity measurement of the resin sheet was performed under the above-mentioned conditions.

[0095] The second resin sheet having the storage modulus E'1 and the storage modulus E'2 within the above-specified ranges can have both the property of being less likely to deform under a local load and the moldability of being able to obtain a molded body with sufficient accuracy when molding by press molding or the like.

[0096] The substrate sheet in the second resin sheet can be constructed in the same manner as the substrate sheet in the first resin sheet. In addition, the second resin sheet can further include a surface layer containing a conductive material and a thermoplastic resin laminated on at least one side of the substrate sheet. In this case, the surface layer can be constructed in the same manner as the surface layer in the first resin sheet.

[0097] The resin sheet of the present embodiment can be formed into a shape according to the intended use by a known thermoforming method such as vacuum forming, pressure forming, or press forming.

[0098] The resin sheet of this embodiment can be used as a material for packaging containers of active components such as ICs, components equipped with ICs, passive components such as capacitors and connectors, and mechanical components, and can be suitably used in vacuum-formed trays, magazines, embossed carriers (embossed carriers), etc.

[0099] [Method for producing resin sheet]

[0100] The resin sheet involved in the present embodiment can be manufactured by a common method. For example, it can be manufactured in the following manner: as a composition for forming a substrate layer for forming a substrate sheet, a mixture of raw materials constituting the substrate sheet is prepared, or pellets are prepared by kneading and granulating using a known method such as an extruder, and as required, as a composition for forming a surface layer, a mixture of raw materials constituting the surface layer is prepared, or pellets are prepared by kneading and granulating using a known method such as an extruder, and using these pellets, a resin sheet is made using a known method such as an extruder. The extruder temperature can be set, for example, to 200 to 300°C.

[0101] When the resin sheet has a surface layer, for the substrate sheet and the surface layer, after the substrate layer forming composition and the surface layer forming composition are respectively formed into sheets or films using different extruders, they can be stacked in stages using a heat lamination method, a dry lamination method, an extrusion lamination method, or the like. Alternatively, the surface layer formed by the surface layer forming composition can be stacked on one or both sides of a substrate sheet previously formed from the substrate layer forming composition by a method such as extrusion coating.

[0102] In addition, for the resin sheet with a surface layer, the raw materials (for example, the above-mentioned pellets) constituting the substrate sheet and the surface layer can be supplied to different extruders respectively, and manufactured by using a multi-layer co-extrusion method such as extrusion molding using a multi-layer T-die with a multi-manifold or T-die extrusion molding using a feed head. This method can obtain a resin sheet by one process, which is preferred from this point of view.

[0103] [container]

[0104] The container of the present embodiment is a molded product of the resin sheet of the present embodiment described above. The container can be obtained by molding the resin sheet of the present embodiment into a shape corresponding to the application.

[0105] As the molding method, a known thermoforming method such as vacuum molding, pressure molding, and press molding can be used.

[0106] The molding temperature is, for example, 120 to 200° C. When molding is performed using a mold, for example, a resin sheet heated to a temperature higher than the peak temperature of the loss tangent may be placed in the mold, and after molding, the molded body may be released from the mold at a temperature lower than the peak temperature of the loss tangent.

[0107] [Carrier tape]

[0108] The carrier tape of the present embodiment is a molded product of the resin sheet according to the present embodiment described above, and is provided with a storage portion capable of storing articles. Figure 2 It is a perspective view showing one embodiment of a carrier tape. Figure 2 The carrier tape 100 shown is an embossed carrier tape formed of a molded body 16 of a resin sheet according to the present embodiment, and has a storage portion 20 formed by embossing. The molded body 16 has a transfer hole 30 that can be used for transporting various electronic components such as ICs during the sealing process.

[0109] The carrier tape of this embodiment can be wound into a reel shape.

[0110] The carrier tape of this embodiment is suitable as a container for packaging electronic components. Examples of electronic components include ICs, LEDs (light emitting diodes), resistors, liquid crystals, capacitors, transistors, piezoelectric resistors, filters, quartz oscillators, quartz resonators, diodes, connectors, switches, potentiometers (volumes), relays, inductors, and the like. The electronic components may be intermediate products using the above components or final products.

[0111] According to the carrier tape formed of the resin sheet of the present embodiment, in the application of conveying extremely small components, it is possible to have a well-shaped storage portion and to sufficiently suppress deformation due to contact with a pickup nozzle.

[0112] [Electronic component packaging]

[0113] The electronic component package of the present embodiment includes: the carrier tape of the present embodiment described above; the electronic component accommodated in the accommodation portion of the carrier tape; and a cover film bonded to the carrier tape as a cover material. Figure 3 This is a partially cutaway perspective view showing one embodiment of an electronic component package. Figure 3The electronic component package 200 shown includes: an embossed carrier tape formed of a resin sheet molded body 16 according to the present embodiment and provided with a storage portion 20 and a feed hole 30; an electronic component 40 stored in the storage portion 20; and a cover film 50 bonded to the embossed carrier tape.

[0114] Examples of the cover film include cover films disclosed in Japanese Patent No. 4630046 and Japanese Patent No. 5894578.

[0115] The cover film can be bonded to the upper surface of the embossed carrier tape storing the electronic components by heat sealing.

[0116] The electronic component package of the present embodiment can be used for storage and transportation of electronic components in the form of a carrier tape wound in a reel shape.

[0117] Example

[0118] Hereinafter, the present invention will be described in more detail using Examples and Comparative Examples, but the present invention is not limited to the following Examples.

[0119] [Production of resin sheets]

[0120] (Examples 1 to 9 and Comparative Examples 1 to 4)

[0121] The raw materials shown in Tables 1 and 2 were weighed so as to have the composition ratios (parts by mass) shown in the same tables, and uniformly mixed using a high-speed mixer. The mixture was kneaded by a vented twin-screw extruder and pelletized by a strand cutting method to obtain a resin composition for forming a surface layer.

[0122] On the other hand, the raw materials shown in Tables 1 and 2 were measured so as to have the composition ratios (parts by mass) shown in the same tables, and were uniformly mixed using a high-speed mixer to obtain a resin composition for forming a base sheet.

[0123] Using the pelletized surface layer forming resin composition and the substrate sheet forming resin composition, Single screw extruder (L / D = 28), used for forming the surface layer A single screw extruder (L / D=26) and a 500 mm wide T-die feed head method were used to produce a resin sheet having a laminated structure of surface layer / base sheet / surface layer. It should be noted that the thickness of the base sheet and the surface layer were adjusted so that the thickness of the resin sheet was 200 μm and the ratio of the thickness of the surface layer / base sheet / surface layer was 1:18:1.

[0124] Details of the raw materials shown in Tables 1 and 2 are as follows.

[0125] GPPS: General purpose polystyrene resin (manufactured by TOYO STYRENE Co., Ltd., product name "Toyo Styrol GP·G200C")

[0126] HIPS: High-impact polystyrene resin (manufactured by TOYO STYRENE Co., Ltd., product name "Toyo Styrol HIE640N")

[0127] EEA: Ethylene-ethyl acrylate copolymer resin (manufactured by ENEOS NUC, product name "DPDJ-6169")

[0128] HDPE: High-density polyethylene resin (manufactured by Prime Polymer, product name "HI-ZEX 5000H")

[0129] SEBS: Hydrogenated styrene-based thermoplastic elastomer (manufactured by Asahi Kasei Corporation, product name "Tuftec P2000")

[0130] SBC: Styrene-butadiene block copolymer (manufactured by Denka, product name "Clearen 200TR")

[0131] ABS: ABS resin (manufactured by Denka, product name "Denka ABS SE-10")

[0132] PC: Polycarbonate resin (manufactured by Teijin Co., Ltd., product name "Panlite L-1225L")

[0133] PBT: polybutylene terephthalate resin (manufactured by Mitsubishi Engineering-Plastics, product name "NOVADURAN 5010R8 M")

[0134] CB: Carbon black (manufactured by Denka Co., Ltd., product name “Denka Black Granular”, average primary particle size 35 nm)

[0135] [Evaluation of resin sheet]

[0136] The samples were taken in the extrusion direction of the resin sheet and evaluated by the following method. The results are summarized in Tables 1 and 2.

[0137] (1) Puncture strength and maximum puncture elastic modulus

[0138] The puncture strength and maximum puncture elastic modulus were calculated using the following steps.

[0139] (i) A resin sheet having a thickness of 0.2 mm was cut into a size of 5 cm in length and 5 cm in width to prepare a sample for measurement.

[0140] (ii) The sample for measurement is fixed to a flat fixture having a hole with a diameter of 1.0 mm in the center, and a tensile tester (Strograph VE-1D manufactured by Toyo Seiki Seisaku-sho, Ltd.) is used to vertically puncture the surface of the sample for measurement from above at a speed of 0.5 mm / min with a needle having a circular tip (diameter 0.8 mm) to measure the load L (N) and the strain ε in the puncture direction. It should be noted that when the displacement in the puncture direction is D (mm) and the thickness of the resin sheet is t (mm), the strain ε is represented by D / t.

[0141] (iii) The formula: (ΔL / S) / Δε (where S represents the area of ​​the front end of the needle (mm) 2 The value when the ratio of the calculated stress difference to the strain difference is the maximum in 0.1≤ε≤5.0 (i.e., 0.02mm≤D≤1.0mm) is taken as the maximum puncture elastic modulus. In addition, the load (maximum load) measured when the fracture occurs is taken as the puncture strength.

[0142] (2) Dynamic viscoelasticity of resin sheet

[0143] A resin sheet with a thickness of 0.2 mm was cut into a size of 40 mm in length and 3 mm in width to prepare a sample for measurement. The sample for measurement was subjected to dynamic viscoelasticity measurement using a dynamic viscoelasticity apparatus RAS-G2 (manufactured by TA Instruments) under the following measurement conditions, and the storage modulus E'1 at 25°C and the storage modulus E'2 at the peak temperature Tg+20°C of the loss tangent (tanδ) were calculated.

[0144] [Measurement conditions]

[0145] Deformation mode: Sine wave stretching mode (linear stretching)

[0146] Measuring temperature: 20℃~200℃

[0147] Measuring frequency: 1Hz

[0148] Heating rate: 10℃ / min

[0149] Initial value of static tensile load: 0.2N

[0150] Initial (at 20°C) gap distance: 10mm

[0151] (3) Component pressure evaluation

[0152] The evaluation sample was prepared by cutting a resin sheet with a thickness of 0.2 mm into a length of 5 cm and a width of 5 cm. On the surface of the evaluation sample, 4 stacked ceramic capacitors (size: 0.4 mm × 0.2 mm, height 0.2 mm) were placed at the four corners of a 2 cm square, and a SUS plate with a length of 5 cm, a width of 5 cm, a thickness of 0.2 mm, and a weight of 4.0 g was placed on it. Then, a weight of 100 g to 1000 g was placed on the SUS plate, and after standing for 1 minute, the amount of depression on the surface of the evaluation sample was measured using a laser microscope VK-X100 (Keyence). The weight of the weight (hereinafter referred to as "depression load") when the depression amount becomes more than 5 μm was confirmed, and the deformation resistance to the load applied to a very small area was evaluated using the following judgment criteria. It should be noted that the stacked ceramic capacitor has electrodes (length 0.1 mm) at both ends and the size between the electrodes becomes smaller, so the electrode portion contacts the resin sheet.

[0153] <Judgment Criteria>

[0154] A: Depression load greater than 1000g (when the weight is 1000g, the depression amount on the surface of the resin sheet is less than 5μm)

[0155] B: Depression load is between 800g and 1000g

[0156] C: Depression load is 500g or more and less than 800g

[0157] D: Depression load less than 500g

[0158] (4) Evaluation of formability

[0159] A resin sheet with a thickness of 0.2 mm was cut into 8 mm widths, and both sides of the sheet were heated to Tg°C calculated in (2) above + 20°C using a contact heater using a press molding machine, and then five containers with openings of (A dimension) 0.23 mm × (B dimension) 0.43 mm and a depth (D) of 0.25 mm were molded using an upper mold and a lower mold (see Figure 4 ). It should be noted that Figure 4 (a) is a top view of the container. Figure 4 (b) is along Figure 4 (a) Schematic cross-sectional view of line II. Figure 4 The container 110 shown has a concave shape having a bottom wall portion 7 and side walls 5 and 6 erected from the periphery of the bottom wall portion 7. In addition, the upper mold is designed so that the angles θ1 and θ2 formed by the inner side surface of the bottom wall portion 7 and the inner side surface of the side wall portion 6 are right angles. The A-dimension cross section obtained by cutting out the center of the B-dimension of the obtained container (see FIG. 1 ) was observed using a laser microscope VK-X100 (manufactured by Keyence Corporation). Figure 4 (b)), measure the angle (θ) formed by the bottom surface and the side surface of the inner side of the container at 2 locations, and take the average value of the total 10 locations as the pocket angle (pocket angle) θp. The moldability is evaluated from the pocket angle θp obtained using the following criteria.

[0160] <Judgment Criteria>

[0161] A: Pocket angle θp is less than 92.0°

[0162] B: Pocket angle θp is greater than 92.0° and less than 94.0°

[0163] C: Pocket angle θp is 94.0° or more and less than 96.0°

[0164] D: Pocket angle θp is 96.0° or more [Table 1]

[0165]

[0166] [Table 2]

[0167]

[0168] Description of Reference Numerals

[0169] 1…base material sheet, 2…surface layer, 3…second surface layer, 5, 6…side wall portions, 7…bottom wall portion, 10, 12, 14…resin sheet, 20…storage portion, 30…transport hole, 40…electronic component, 50…cover film, 100…carrier tape, 200…electronic component package.

Claims

1. A resin sheet comprising a base sheet containing a polystyrene resin, The maximum puncture elastic modulus calculated according to the following steps is 2.4 to 6.4 MPa. [Calculation steps for maximum puncture elastic modulus] The sample for measurement was fixed to a flat fixture with a hole of 1.0 mm in diameter at the center. The load L (N) and the strain ε in the puncture direction when a needle with a circular tip (diameter 0.8 mm) was vertically punctured into the surface of the sample for measurement at a speed of 0.5 mm / min were measured under an environment of 23°C. The load L (N) and the strain ε in the puncture direction were measured using the formula: (ΔL / S) / Δε (where S represents the area of ​​the tip surface of the needle (mm 2 The value at which the ratio of the calculated stress difference to the strain difference becomes the maximum in the range of 0.1≤ε≤5.0 is taken as the maximum puncture elastic modulus.

2. The resin sheet according to claim 1, wherein In the dynamic viscoelasticity measurement, the storage modulus E'1 at 25°C is 1.0×10 8 Pa above 1.0×10 10 Pa or less, and the storage modulus E'2 at the peak temperature of the loss tangent +20°C is 1.0×10 6 Below Pa.

3. The resin sheet according to claim 1, wherein The base sheet contains at least one of a general-purpose polystyrene resin and an impact-resistant polystyrene resin in an amount of 50% by mass or more in total based on the total amount of the styrene-based resin.

4. A resin sheet comprising a base sheet containing a thermoplastic resin, wherein: In the dynamic viscoelasticity measurement, the storage modulus E'1 at 25°C is 1.0×10 8 Pa above 1.0×10 10 Pa or less, and the storage modulus E'2 at the peak temperature of the loss tangent +20°C is 1.0×10 6 Below Pa. 5 . A container, which is a molded product of the resin sheet according to claim 1 . 6 . A carrier tape, which is a molded product of the resin sheet according to claim 1 and has a storage portion capable of storing articles.