Polypropylene-based resin foamed particles, polypropylene-based resin

By using a specific ratio of recycled resin and carbon black in polypropylene resin foam granules, combined with a specific manufacturing process, the problems of insufficient blackness and flame retardancy of recycled polypropylene resin foam molded articles have been solved, achieving excellent blackness and flame retardancy while reducing environmental burden.

CN118946620APending Publication Date: 2024-11-12KANEKA CORP
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202380030600.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-30
Filing Date
2023-03-29
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

When using recycled polypropylene resin to make polypropylene resin foamed molded articles, the blackness and flame retardancy are not sufficient and there is still room for improvement.

Method used

The carbon black is made of polypropylene resin foam particles containing a base resin, which includes non-recycled polypropylene resin, recycled polypropylene resin or recycled polyethylene resin. The number of carbon black particles with a structural size of less than 1×104 nm2 accounts for 10% to 50% of the total. The carbon black is manufactured through a specific process, including granulation, dispersion, heating, pressurization and release steps.

Benefits of technology

It provides polypropylene resin foamed molded parts with excellent blackness and flame retardancy, reducing environmental pollution, plastic waste and the amount of plastic in manufacturing, which is in line with sustainable development goals.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005061157180000171
    Figure BDA0005061157180000171
  • Figure BDA0005061157180000172
    Figure BDA0005061157180000172
  • Figure BDA0005061157180000181
    Figure BDA0005061157180000181
Patent Text Reader

Abstract

The present invention addresses the problem of providing polypropylene-based resin foam particles which contain a regenerated resin and which can provide a polypropylene-based resin foam molded article having excellent blackness and flame retardancy. Provided are foamed polypropylene resin particles containing carbon black and a base resin containing a predetermined amount of a regenerated resin, the foamed polypropylene resin particles being characterized in that the ratio of the number of carbon black having a structural size per structure of less than 1 * 104 nm2 to the total number of carbon black is 10-50%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to polypropylene resin foamed particles, polypropylene resin foamed molded products and a method for producing polypropylene resin foamed particles. Background Art

[0002] Polypropylene resin foam molded products are used in various applications including automobile interior parts, core materials for automobile bumpers, thermal insulation materials, cushioning packaging materials, shipping boxes, and the like (for example, Patent Document 1).

[0003] In recent years, in order to reduce environmental burden, the use of recycled resins has been required when manufacturing resin products, and the use of recycled resins has attracted much attention (for example, Patent Document 2).

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: WO2006 / 075491

[0007] Patent Document 2: Japanese Patent Application Publication No. 2011-173273 Summary of the invention

[0008] Problem that the invention aims to solve

[0009] However, when a polypropylene resin foam molded article is produced using recycled polypropylene resin, the blackness and flame retardancy of the polypropylene resin foam molded article are still insufficient, and there is still room for further improvement.

[0010] One embodiment of the present invention has been made in view of the above-mentioned problems, and an object of the present invention is to provide polypropylene resin foamed particles containing recycled resin and capable of providing a polypropylene resin foamed molded product having excellent blackness and flame retardancy.

[0011] Solutions for solving problems

[0012] The polypropylene resin foamed particles according to one embodiment of the present invention are polypropylene resin foamed particles containing a base resin and carbon black, wherein the base resin includes a non-recycled polypropylene resin and a recycled polypropylene resin and / or a recycled polyethylene resin, the total content of the recycled polypropylene resin and the recycled polyethylene resin is 10 to 60 parts by weight in 100 parts by weight of the base resin, and the carbon black has a structure size of less than 1×10 4 nm 2 The ratio of the number of carbon blacks to the total number of carbon blacks is 10% to 50%.

[0013] The method for producing polypropylene resin foamed particles according to one embodiment of the present invention comprises: a granulation step of preparing a granulated particle containing a non-recycled polypropylene resin, a recycled material and a particle having an average structure size of 0.2×10 4 nm 2 Above and less than 4.0×10 4 nm 2 The invention relates to a method for preparing a polypropylene resin particle, comprising: preparing a polypropylene resin particle, a polypropylene resin particle having an average structure size of 5.0×10 4 nm 2 Above and less than 9.0×10 4 nm 2 The carbon black B used in the above-mentioned recycled material is as follows: in 100 parts by weight of the base resin containing the above-mentioned non-recycled polypropylene resin and the above-mentioned recycled polypropylene resin and / or the above-mentioned recycled polyethylene resin, the total content of the above-mentioned recycled polypropylene resin and the above-mentioned recycled polyethylene resin is 10 parts by weight to 60 parts by weight.

[0014] One embodiment of the present invention includes the following configurations.

[0015] Effects of the Invention

[0016] According to one embodiment of the present invention, there is provided an effect of being able to provide polypropylene resin foamed particles containing recycled resin and capable of providing a polypropylene resin foam molded body having excellent blackness and flame retardancy. DETAILED DESCRIPTION

[0017] Hereinafter, an embodiment of the present invention will be described, but the present invention is not limited thereto. The present invention is not limited to the various configurations described below, and various changes can be made within the scope indicated in the claims. In addition, embodiments or embodiments obtained by combining the technical means respectively disclosed in different embodiments or examples are also included in the technical scope of the present invention. Furthermore, by combining the technical means respectively disclosed in each embodiment, new technical features can be formed. It should be noted that all academic literature and patent literature described in this specification are cited in this specification as references. In addition, in this specification, unless otherwise specified, "A to B" indicating a numerical range means, "Above A (including A and greater than A) and below B (including B and less than B)".

[0018] In this specification, a "structural unit derived from X monomer" contained in a polymer, a copolymer or a resin may be referred to as an "X unit".

[0019] In this specification, unless otherwise specified, X 1 Unit, X 2 Unit, ··· and X n A copolymer having a unit (n is an integer greater than 2) as a structural unit is also referred to as "X 1 / X 2 / ··· / X n Copolymer". As X 1 / X 2 / ··· / X n The copolymer is not particularly limited in the polymerization method unless otherwise specified, and may be a random copolymer, an alternating copolymer, a block copolymer, or a graft copolymer.

[0020] [1. Polypropylene resin foam particles]

[0021] The polypropylene resin foamed particles according to one embodiment of the present invention are polypropylene resin foamed particles containing a base resin and carbon black, wherein the base resin includes a non-recycled polypropylene resin and a recycled polypropylene resin and / or a recycled polyethylene resin, the total content of the recycled polypropylene resin and the recycled polyethylene resin is 10 to 60 parts by weight in 100 parts by weight of the base resin, and the carbon black has a structure size of less than 1×10 4 nm 2 The ratio of the number of carbon blacks to the total number of carbon blacks is 10% to 50%.

[0022] The polypropylene resin foamed particles according to one embodiment of the present invention can be molded by a known method to provide a polypropylene resin foamed molded article.

[0023] In this specification, "polypropylene resin foamed particles" are sometimes referred to as "foamed particles", "polypropylene resin foamed particles involved in one embodiment of the present invention" are sometimes referred to as "present foamed particles", and "polypropylene resin foamed molded article" are sometimes referred to as "foamed molded article".

[0024] The foamed particles have the aforementioned structure, and therefore have the following advantages: they can provide a foamed molded body with excellent blackness and flame retardancy. In addition, as described above, the foamed particles contain recycled polypropylene resin and / or recycled polyethylene resin. Therefore, it can be said that the environmental burden of the foamed particles is small. In other words, in one embodiment of the present invention, due to the use of recycled polypropylene resin and / or recycled polyethylene resin, one embodiment of the present invention can not only reduce environmental pollution, but also significantly reduce the amount of plastic waste generated and the amount of plastic used in manufacturing. Thus, one embodiment of the present invention can, for example, contribute to the realization of Goal 12 of the Sustainable Development Goals (SDGs) "ensuring sustainable consumption and production patterns" and Goal 14 "protecting sea / ocean resources and using them in a sustainable manner for sustainable development" of the SDGs.

[0025] <Ingredients>

[0026] (2-1. Base material resin)

[0027] In this specification, the base resin refers to the resin component that substantially constitutes the polypropylene resin particles, polypropylene resin foamed particles and polypropylene resin foamed molded bodies. The base resin contains at least non-recycled polypropylene resin and recycled polypropylene resin and / or recycled polyethylene resin.

[0028] In the present specification, the "polypropylene-based resin" refers to a resin containing 50 mol% or more of propylene units in 100 mol% of all structural units constituting the resin.

[0029] In this specification, a "structural unit derived from a propylene monomer" may be referred to as a "propylene unit".

[0030] In the present specification, the "polyethylene-based resin" refers to a resin containing 50 mol% or more of ethylene units in 100 mol% of all structural units constituting the resin.

[0031] In this specification, a "structural unit derived from an ethylene monomer" may be referred to as an "ethylene unit".

[0032] In addition, in this specification, the resin which contains 50 mol% of propylene units and 50 mol% of ethylene units as 100 mol% of all structural units constituting the resin is referred to as "polypropylene-based resin".

[0033] In this specification, "recycled polypropylene resin" refers to a polypropylene resin that has undergone one or more polypropylene resin product forms (e.g., foamed particles, foamed molded bodies, films, food trays, bags, bottles and other packaging containers, clothing boxes, transparent folders and other supplies, etc.) and has become a polypropylene resin (or polypropylene resin particles) again by melting or other methods. In addition, in this specification, "recycled polyethylene resin" refers to a polyethylene resin that has undergone one or more polyethylene resin product forms (e.g., foamed particles, foamed molded bodies, films, food trays, bags, bottles and other packaging containers, clothing boxes, transparent folders and other supplies, etc.) and has become a polyethylene resin (or polyethylene resin particles) again by melting or other methods. In this specification, recycled polypropylene resin or recycled polyethylene resin is sometimes referred to as "recycled resin", and recycled polypropylene resin and recycled polyethylene resin are sometimes collectively referred to as "recycled resin". In addition, in this specification, "non-recycled polypropylene resin" refers to a polypropylene resin that has not undergone a polypropylene resin product form once.

[0034] The method for producing the recycled resin, in other words, the method for reusing the polypropylene resin product and the polyethylene resin product, is not particularly limited, and a known method can be adopted. For example, a method for crushing or melting the polypropylene resin product or the polyethylene resin product, and a method for cutting these products can be cited.

[0035] (Structure of polypropylene resin)

[0036] In this item only, unless otherwise specified, "polypropylene resin" means both non-recycled polypropylene resin and recycled polypropylene resin. The structure of the polypropylene resin is described below.

[0037] The polypropylene resin may be (i) a homopolymer of propylene, (ii) a block copolymer, alternating copolymer, random copolymer or graft copolymer of propylene and a monomer other than propylene, or (iii) a mixture of two or more thereof.

[0038] The polypropylene resin may have one or more structural units derived from monomers other than the propylene monomer in addition to the propylene unit, and may have one or more types. The "monomers other than the propylene monomer" used in the production of the polypropylene resin is sometimes referred to as a "comonomer". The "structural unit derived from monomers other than the propylene monomer" contained in the polypropylene resin is sometimes referred to as a "comonomer unit".

[0039] Examples of the comonomer include α-olefins having 2 or 4 to 12 carbon atoms, such as ethylene, 1-butene, isobutylene, 1-pentene, 3-methyl-1-butene, 1-hexene, 4-methyl-1-pentene, 3,4-dimethyl-1-butene, 1-heptene, 3-methyl-1-hexene, 1-octene and 1-decene.

[0040] Specific examples of the polypropylene resin include: polypropylene homopolymer, ethylene / propylene block copolymer, 1-butene / propylene block copolymer, ethylene / 1-butene / propylene block copolymer, ethylene / propylene alternating copolymer, 1-butene / propylene alternating copolymer, ethylene / 1-butene / propylene alternating copolymer, ethylene / propylene random copolymer, 1-butene / propylene random copolymer, ethylene / 1-butene / propylene random copolymer, propylene / vinyl chloride copolymer, propylene / maleic anhydride copolymer, styrene-modified polypropylene resin, etc. As the polypropylene resin, one of them may be used alone, or two or more of them may be used in combination.

[0041] From the viewpoint of molding processability, the non-recycled polypropylene resin is preferably (a) an alternating copolymer composed of propylene units and comonomer units, and the two units are arranged alternately, and / or (b) a random copolymer composed of propylene units and comonomer units, and the two units are arranged in a random order. From the perspective of easy availability, the non-recycled polypropylene resin more preferably includes one or more selected from the group consisting of ethylene / propylene alternating copolymers, ethylene / 1-butene / propylene alternating copolymers, ethylene / propylene random copolymers, and ethylene / 1-butene / propylene random copolymers.

[0042] From the viewpoint of molding processability and easy availability, the non-recycled polypropylene resin preferably contains 60% by weight or more, more preferably 70% by weight or more, more preferably 80% by weight or more, further preferably 90% by weight or more, and particularly preferably 95% by weight or more of one or more selected from the group consisting of ethylene / propylene alternating copolymers, ethylene / 1-butene / propylene alternating copolymers, ethylene / propylene random copolymers, and ethylene / 1-butene / propylene random copolymers in 100% by weight of the non-recycled polypropylene resin. The non-recycled polypropylene resin is most preferably composed of only one or more selected from the group consisting of ethylene / propylene alternating copolymers, ethylene / 1-butene / propylene alternating copolymers, ethylene / propylene random copolymers, and ethylene / 1-butene / propylene random copolymers.

[0043] From the viewpoint of molding processability, the recycled polypropylene resin is preferably (a) a block copolymer consisting of a propylene unit and a comonomer unit and consisting of a block structure comprising only propylene units and a block structure comprising only comonomer units, (b) an alternating copolymer consisting of a propylene unit and a comonomer unit and two units arranged alternately, and / or (c) a random copolymer consisting of a propylene unit and a comonomer unit and two units arranged in a random order. In the aforementioned block copolymer, the arrangement order of the block structure comprising only propylene units and the block structure comprising only comonomer units is not particularly limited. From the aspect of being easily available, the recycled polypropylene resin is more preferably included in the group consisting of ethylene / propylene block copolymers, ethylene / 1-butene / propylene block copolymers, ethylene / propylene alternating copolymers, ethylene / 1-butene / propylene alternating copolymers, ethylene / propylene random copolymers and ethylene / 1-butene / propylene random copolymers. One or more.

[0044] From the viewpoint of molding processability and easy availability, the recycled polypropylene resin preferably contains 60% by weight or more, more preferably 70% by weight or more, more preferably 80% by weight or more, further preferably 90% by weight or more, and particularly preferably 95% by weight or more of one or more selected from the group consisting of ethylene / propylene alternating copolymers, ethylene / 1-butene / propylene alternating copolymers, ethylene / propylene random copolymers, and ethylene / propylene random copolymers in 100% by weight of the recycled polypropylene resin. The recycled polypropylene resin is most preferably composed of only one or more selected from the group consisting of ethylene / propylene block copolymers, ethylene / 1-butene / propylene block copolymers, ethylene / propylene alternating copolymers, ethylene / 1-butene / propylene alternating copolymers, ethylene / propylene random copolymers, and ethylene / 1-butene / propylene random copolymers.

[0045] (Physical properties of non-recycled polypropylene resin)

[0046] The melting point of the non-recycled polypropylene resin according to one embodiment of the present invention is not particularly limited, but is preferably 135° C. to 160° C., more preferably 137° C. to 155° C., and even more preferably 139° C. to 153° C. When the melting point of the non-recycled polypropylene resin is (i) 135° C. or higher, the foamed molded article obtained from the present foamed beads has excellent heat resistance, and when it is (ii) 160° C. or lower, the expansion ratio of the foamed beads can be easily increased when the present foamed beads are produced.

[0047] In this specification, the melting point of the non-recycled polypropylene resin is a value obtained by differential scanning calorimetry (hereinafter referred to as "DSC method"). The specific operation steps are as follows: (1) the temperature of 5 mg to 6 mg of the non-recycled polypropylene resin is increased from 40°C to 220°C at a heating rate of 10°C / min, thereby melting the non-recycled polypropylene resin; (2) then, the temperature of the molten non-recycled polypropylene resin is decreased from 220°C to 40°C at a cooling rate of 10°C / min, thereby crystallizing the non-recycled polypropylene resin; (3) then, the temperature of the crystallized non-recycled polypropylene resin is further increased from 40°C to 220°C at a heating rate of 10°C / min. The temperature of the peak (melting peak) of the DSC curve of the non-recycled polypropylene resin obtained at the second heating (i.e., at (3)) can be obtained as the melting point of the non-recycled polypropylene resin. It should be noted that, when there are multiple peaks (melting peaks) in the DSC curve of the non-recycled polypropylene resin obtained by the above method at the second temperature increase, the temperature of the peak (melting peak) with the largest melting heat is taken as the melting point of the non-recycled polypropylene resin. As a differential scanning calorimeter, for example, DSC7020 manufactured by Hitachi High-Tech Corporation can be used.

[0048] The MFR of the non-recycled polypropylene resin used in one embodiment of the present invention at 230°C is not particularly limited, but is preferably 1 g / 10 min to 40 g / 10 min, more preferably 2 g / 10 min to 35 g / 10 min, further more preferably 3 g / 10 min to 30 g / 10 min, and particularly preferably 3 g / 10 min to 10 g / 10 min. When the MFR of the non-recycled polypropylene resin at 230°C is 1 g / 10 min or more, there is a tendency to easily increase the expansion ratio of the foamed particles when the present foamed particles are produced. When the MFR of the non-recycled polypropylene resin at 230°C is 40 g / 10 min or less, there is no concern that the bubbles of the obtained foamed particles will be interconnected, and as a result, there is a tendency that (i) the compressive strength of the foamed molded article obtained from the present foamed particles is good or (ii) the surface properties of the foamed molded article are good. It should be noted that in this specification, the "bubbles" of the foamed particles are sometimes referred to as "cells". That is, in this specification, "bubbles" may be replaced with "cells", and "cells" may be replaced with "bubbles".

[0049] In addition, the case where the MFR of the non-recycled polypropylene resin at 230°C is in the range of 1 g / 10 minutes to 40 g / 10 minutes is considered. In this case, polypropylene resin foamed particles having a relatively large expansion ratio are easily obtained. Furthermore, in this case, there are the following advantages: the surface aesthetics of the foamed molded article obtained from the present foamed particles is excellent and the dimensional shrinkage is small.

[0050] In this specification, the MFR value of the non-recycled polypropylene resin at 230°C is a value obtained by measuring using an MFR measuring instrument described in JIS K7210:1999 under the following conditions: the diameter of the orifice is The length of the orifice was 8.000±0.025 mm, the load was 2.16 kgf, and the temperature was 230° C. (230±0.2° C.).

[0051] (Physical properties of recycled polypropylene resin)

[0052] The melting point of the recycled polypropylene resin according to one embodiment of the present invention is not particularly limited, but is preferably 135° C. to 160° C., more preferably 137° C. to 155° C., and even more preferably 139° C. to 153° C. When the melting point of the recycled polypropylene resin is (i) 135° C. or higher, the foamed molded article obtained from the present foamed beads has excellent heat resistance, and when it is (ii) 160° C. or lower, the expansion ratio of the foamed beads can be easily increased when the present foamed beads are produced.

[0053] In this specification, the melting point of the recycled polypropylene resin is a value obtained by measuring by the above-mentioned DSC method in the same manner as the melting point of the non-recycled polypropylene resin, except that the recycled polypropylene resin is used instead of the non-recycled polypropylene resin.

[0054] The MFR of the recycled polypropylene resin used in one embodiment of the present invention at 230°C is not particularly limited, and is preferably 1 g / 10 min to 40 g / 10 min, more preferably 2 g / 10 min to 35 g / 10 min, further more preferably 3 g / 10 min to 30 g / 10 min, and particularly preferably 3 g / 10 min to 10 g / 10 min. When the MFR of the recycled polypropylene resin at 230°C is (a) 1.0 g / 10 min or more, there is the following advantage: it is easy to increase the expansion ratio of the foamed particles when the present foamed particles are manufactured, and when it is (b) 40.0 g / 10 min or less, there is the following advantage: there is no need to worry about the bubbles of the obtained foamed particles becoming interconnected.

[0055] In this specification, the MFR value of the recycled polypropylene resin at 230° C. is a value measured by the same method as the MFR value of the non-recycled polypropylene resin at 230° C., except that the recycled polypropylene resin is used instead of the non-recycled polypropylene resin.

[0056] The non-recycled polypropylene resin can be obtained by a known method. The polymerization catalyst used in the synthesis of the polypropylene resin is not particularly limited, and a Ziegler catalyst or the like can be used.

[0057] The base resin preferably contains 80 to 100 parts by weight, more preferably 90 to 100 parts by weight of polypropylene resin (non-recycled polypropylene resin and recycled polypropylene resin) in 100 parts by weight of the base resin. This configuration has the advantage that the strength of the obtained foamed molded article is less reduced.

[0058] The base resin includes at least one of a recycled polypropylene resin and a recycled polyethylene resin. The base resin may also include a non-recycled polyethylene resin. In this specification, "non-recycled polyethylene resin" refers to a polyethylene resin that has never been in the form of a polyethylene resin product.

[0059] (Structure of polyethylene resin)

[0060] In this item only, unless otherwise specified, "polyethylene resin" means both non-recycled polyethylene resin and recycled polyethylene resin. The structure of the polyethylene resin is described below.

[0061] The polyethylene resin may be (a) a homopolymer of ethylene, (b) a block copolymer, alternating copolymer, random copolymer or graft copolymer of ethylene and a monomer other than ethylene, or (c) a mixture of two or more thereof.

[0062] The polyethylene resin may have one or more structural units derived from monomers other than the ethylene monomer in addition to the ethylene unit, or may have one or more structural units. The "structural units derived from monomers other than the ethylene monomer" contained in the polyethylene resin is sometimes referred to as a "comonomer unit".

[0063] Examples of the comonomer include: (a) α-olefins having 3 to 12 carbon atoms, such as propylene, 1-butene, isobutylene, 1-pentene, 3-methyl-1-butene, 1-hexene, 4-methyl-1-pentene, 3,4-dimethyl-1-butene, 1-heptene, 3-methyl-1-hexene, 1-octene, and 1-decene; and (b) vinyl monomers such as vinyl acetate.

[0064] Specific examples of polyethylene resins include: (a) polyethylene homopolymers, (b) ethylene / propylene block copolymers, 1-butene / ethylene block copolymers, ethylene / 1-butene / propylene block copolymers, ethylene / propylene alternating copolymers, 1-butene / ethylene alternating copolymers, ethylene / 1-butene / propylene alternating copolymers, ethylene / propylene random copolymers, 1-butene / ethylene random copolymers, ethylene / 1-butene / propylene random copolymers and other ethylene / α-olefin copolymers, (c) ethylene / vinyl chloride copolymers, ethylene / maleic anhydride copolymers and other ethylene / vinyl unit copolymers, (d) styrene-modified polyethylene resins, and (e) chlorinated polyethylene, etc. As the polyethylene resin, one of these may be used alone, or two or more of them may be used in combination.

[0065] As polyethylene resins, from the perspective of different densities, high-density polyethylene (HDPE or PE-HD), medium-density polyethylene (MDPE or PE-MD), low-density polyethylene (LDPE or PE-LD), etc. can also be listed. For HDPE, MDPE and LDPE, JIS K 6760 stipulates that the density range of each is HDPE: 942 kg / m 3 Above, MDPE: 930kg / m 3 Above and less than 942kg / m 3 , LPDE: 910kg / m 3 Above and less than 930kg / m 3 .

[0066] Low-density polyethylene (LPDE) can be further classified into (a) low-density polyethylene produced by a high-pressure method, which has long-chain branches on the basis of short-chain branches such as ethyl (hereinafter also referred to as branched low-density polyethylene) and (b) low-density polyethylene produced using a transition metal catalyst under medium-low pressure, which has short-chain branches (hereinafter also referred to as linear low-density polyethylene (LLDPE or PE-LLD)). Branched low-density polyethylene is a homopolymer of polyethylene. Linear low-density polyethylene is a copolymer obtained by polymerizing ethylene and α-olefins such as 1-butene, 1-hexene and / or 4-methyl-1-pentene into a linear chain, and has short-chain branches derived from the side chains of the α-olefin. Therefore, linear low-density polyethylene can also be called ethylene / α-olefin copolymer.

[0067] The recycled polyethylene-based resin may include one or more selected from the group consisting of high-density polyethylene, medium-density polyethylene, and low-density polyethylene.

[0068] (Physical properties of recycled polyethylene resin)

[0069] In one embodiment of the present invention, the melting point of the recycled polyethylene resin is not particularly limited, but is preferably 100° C. to 140° C., and more preferably 110° C. to 130° C. When the melting point of the recycled polyethylene resin is (a) 100° C. or higher, there is an advantage that the impact resistance of the foamed molded article is unlikely to decrease, and when it is (b) 140° C. or lower, there is an advantage that the elongation of the foamed molded article surface is good.

[0070] In this specification, the melting point of the recycled polyethylene resin is a value obtained by measuring by the above-mentioned DSC method in the same manner as the melting point of the non-recycled polypropylene resin, except that the recycled polyethylene resin is used instead of the non-recycled polypropylene resin.

[0071] In one embodiment of the present invention, the total content of the recycled polypropylene resin and the recycled polyethylene resin is 10 to 60 parts by weight, preferably 10 to 60 parts by weight, more preferably 15 to 60 parts by weight, further preferably 18 to 60 parts by weight, and particularly preferably 20 to 60 parts by weight in 100 parts by weight of the base resin. This configuration has the following advantages: the burden on the environment can be further reduced.

[0072] In one embodiment of the present invention, when the total content of the recycled polypropylene resin and the recycled polyethylene resin is 100 parts by weight, preferably (a) the recycled polypropylene resin is 60 to 100 parts by weight and the recycled polyethylene resin is 0 to 40 parts by weight, more preferably (b) the recycled polypropylene resin is 70 to 100 parts by weight and the recycled polyethylene resin is 0 to 30 parts by weight, more preferably (c) the recycled polypropylene resin is 80 to 100 parts by weight and the recycled polyethylene resin is 0 to 20 parts by weight, further preferably (d) the recycled polypropylene resin is 90 to 100 parts by weight and the recycled polyethylene resin is 0 to 10 parts by weight, and particularly preferably (e) the recycled polypropylene resin is 95 to 100 parts by weight and the recycled polyethylene resin is 0 to 5 parts by weight. According to this configuration, there are the following advantages: the impact resistance and surface elongation of the foamed molded body are good.

[0073] The base resin preferably contains 80 to 100 parts by weight, more preferably 90 to 100 parts by weight, and further preferably 95 to 100 parts by weight of polypropylene resin (non-recycled polypropylene resin and recycled polypropylene resin) and recycled polyethylene resin in total in 100 parts by weight of the base resin. According to this constitution, there is an advantage that the strength of the obtained foamed molded body decreases little. As the base resin, it can be composed only of polypropylene resin (non-recycled polypropylene resin and recycled polypropylene resin) and recycled polyethylene resin.

[0074] (Other resins, etc.)

[0075] Without prejudice to the effects of one embodiment of the present invention, the substrate resin may also include resins other than non-recycled polypropylene resins, recycled polypropylene resins, and recycled polyethylene resins (sometimes referred to as other resins, etc.). As the aforementioned other resins, etc., there may be listed: (a) styrene resins such as polystyrene, styrene / maleic anhydride copolymers, and styrene / ethylene copolymers, (b) polyolefin waxes such as propylene-α-olefin waxes, and (c) olefin rubbers such as ethylene / propylene rubber, ethylene / butene rubber, ethylene / hexene rubber, and ethylene / octene rubber. The content of other resins is preferably 10 parts by weight or less, and more preferably 5 parts by weight or less, relative to a total of 100 parts by weight of non-recycled polypropylene resins, recycled polypropylene resins, and recycled polyethylene resins.

[0076] (2-2. Carbon black)

[0077] The foamed particles contain carbon black. More specifically, the foamed particles contain carbon black, each of which has a structure size of less than 1×10 4 nm 2 The carbon black contained in the foamed particles has a structural size of less than 1×10 4 nm 2 The ratio of the number of carbon blacks to the total number of carbon blacks is 10% to 50%. The inventors of the present invention have independently obtained the following new insights through in-depth research: surprisingly, foamed particles containing carbon blacks of the above structural size within the above range can provide foamed molded products with excellent blackness and flame retardancy. In addition, the inventors of the present invention have independently obtained the following new insights through in-depth research: surprisingly, foamed particles containing carbon blacks of the above structural size within the above range can provide foamed molded products with excellent color unevenness.

[0078] The method for measuring the structural size of carbon black will be described in detail in the examples described below.

[0079] The carbon black is not particularly limited, and examples thereof include channel black, roll black, pan black, gas phase furnace black, oil phase furnace black, thermal black, acetylene black, etc. The carbon black may be used alone or in combination of two or more.

[0080] The shape of carbon black is not particularly limited, and may be spherical or substantially spherical.

[0081] The structural size of each structure in the foamed particles is less than 1×10 4 nm 2The ratio of the number of carbon blacks to the total number of carbon blacks is 10% to 50%, preferably 15% to 30%. According to this structure, there is the advantage that even when recycled resin is used, a foamed molded body with uneven color, excellent blackness and flame retardancy can be obtained.

[0082] In one embodiment of the present invention, in order to improve the blackness of the foamed particles and the foamed particle molded body, an average structure size of 0.2×10 4 nm 2 Above and less than 4.0×10 4 nm 2 In other words, the present expanded particles contain carbon black A. The average structural size of the carbon black A in the expanded particles is preferably 0.2×10 4 nm 2 Above and less than 4.0×10 4 nm 2 , more preferably 0.2×10 4 nm 2 More than and less than 3.5×10 4 nm 2 , more preferably 0.5×10 4 nm 2 More than and less than 3.5×10 4 nm 2 , more preferably 1.0×10 4 nm 2 More than and less than 3.5×10 4 nm 2 , more preferably 1.5×10 4 nm 2 More than and less than 3.5×10 4 nm 2 , more preferably 2.0×10 4 nm 2 More than and less than 3.5×10 4 nm 2 , and more preferably 2.5×10 4 nm 2 More than and less than 3.5×10 4 nm 2 , particularly preferably 3.0×10 4 nm 2 More than and less than 3.5×10 4 nm 2 According to this configuration, there is an advantage that even when a recycled resin is used, a foamed molded product having uneven color, excellent blackness and flame retardancy can be obtained.

[0083] The foamed particles contain an average structural size of 5.0×104 nm 2 Above and less than 9.0×10 4 nm 2 The average structural size of carbon black B is preferably 5.0×10 4 nm 2 Above and less than 9.0×10 4 nm 2 , more preferably 5.0×10 4 nm 2 Above and less than 8.0×10 4 nm 2 , more preferably 5.0×10 4 nm 2 More than and less than 7.5×10 4 nm 2 , more preferably 5.0×10 4 nm 2 Above and less than 7.0×10 4 nm 2 , and more preferably 5.0×10 4 nm 2 Above and less than 6.5×10 4 nm 2 , particularly preferably 5.0×10 4 nm 2 Above and less than 6.0×10 4 nm 2 According to this configuration, there is an advantage that even when recycled resin is used, a foamed molded product with uneven color, excellent blackness and flame retardancy can be obtained. As described later, the recycled material may include an average structural size of 5.0×10 4 nm 2 Above and less than 9.0×10 4 nm 2 Carbon black, that is, carbon black B. Therefore, the source of carbon black B can be a recycled material. It should be noted that carbon black B different from recycled materials can be used.

[0084] In one embodiment of the present invention, it is preferred not to use an average structure size of 10×10 4 nm 2 In other words, the average structural size of the foamed beads is preferably 10×10 4 nm 2 For example, the foamed particles preferably do not contain an average structural size of 10×10 4 nm 2The above carbon black C, or more than 0 weight part and less than 0.5 weight part of the above carbon black C relative to 100 weight parts of the above base resin. The present inventors have independently obtained the following new findings in the course of intensive research: surprisingly, according to this structure, a foamed molded product with better flame retardancy can be obtained.

[0085] The content of carbon black A in the present foamed particles is preferably 0.1 to 5.0 parts by weight, more preferably 0.3 to 4.5 parts by weight, more preferably 0.5 to 4.3 parts by weight, more preferably 1.0 to 4.0 parts by weight, further preferably 1.5 to 3.5 parts by weight, further preferably 2.0 to 3.5 parts by weight, and particularly preferably 2.5 to 3.0 parts by weight, relative to 100 parts by weight of the base resin. The inventors of the present invention have independently obtained the following new insight in the process of in-depth research: surprisingly, according to this structure, a foamed molded body with a better blackness can be obtained.

[0086] The content of carbon black B in the foamed particles is preferably 0.10 to 2.00 parts by weight, more preferably 0.10 to 1.80 parts by weight, and further preferably 0.30 to 1.80 parts by weight, relative to 100 parts by weight of the base resin. In the process of in-depth research, the inventors independently obtained the following new insights: surprisingly, according to this structure, a foamed molded body with uneven color and better flame retardancy can be obtained.

[0087] (2-3. Additives)

[0088] The present foamed particles may optionally contain additives in addition to (a) non-regenerated polypropylene resin, (b) recycled polypropylene resin and / or recycled polyethylene resin, and (c) carbon black A and B. As additives, colorants other than carbon black, water-absorbing substances, foaming nucleating agents, antistatic agents, flame retardants, antioxidants, light stabilizers, crystallization nucleating agents, conductive agents, lubricants, etc. may be listed. Such additives may also be directly added to the blend or polypropylene resin composition described later when manufacturing the polypropylene resin particles.

[0089] (Foaming nucleating agent)

[0090] The foaming nucleating agent is a substance that can be used in the manufacture of the present foaming particles and can form a foaming nucleus when the resin particles are foamed. In the manufacture of the present foaming particles, the foaming nucleating agent is preferably used, in other words, the present foaming particles preferably contain the foaming nucleating agent. According to this configuration, there is the following advantage: the cell structure of the foaming particles is uniform.

[0091] In this specification, the foaming nucleating agent is an inorganic compound and refers to a substance that does not burn and remains as a residue when burned at 750°C for more than 1 hour, and is sometimes referred to as "ash" in this specification. Examples include silicon dioxide, silicates, alumina, diatomaceous earth, calcium carbonate, magnesium carbonate, calcium phosphate, feldspar apatite, barium sulfate, zinc borate, and the like. Examples of silicates include talc, magnesium silicate, kaolin, halloysite, dickite, aluminum silicate, zeolite, and the like. It should be noted that these foaming nucleating agents may be used alone or in combination of two or more. In addition, when two or more foaming nucleating agents are used in combination, the mixing ratio may be appropriately adjusted according to the purpose.

[0092] Since there is a tendency that the cell structure of the expanded particles becomes more uniform and the color non-uniformity of the expanded particles decreases, in one embodiment of the present invention, the expansion nucleating agent preferably contains talc, preferably talc.

[0093] The amount of the foaming nucleating agent used in the manufacture of the present foamed beads, in other words, the content of the foaming nucleating agent in the present foamed beads is described. It should be noted that the content of the foaming nucleating agent in the present foamed beads refers to the total amount of the foaming nucleating agent in the present foamed beads, including the content of the foaming nucleating agent contained in the recycled material. From the viewpoint of uniformity of the average bubble diameter, the content of the foaming nucleating agent in the present foamed beads is preferably 0.001 to 2.00 parts by weight, more preferably 0.01 to 1.00 parts by weight, further preferably 0.020 to 0.50 parts by weight, further preferably 0.05 to 0.50 parts by weight, more preferably 0.05 to 0.50 parts by weight, more preferably 0.10 to 0.50 parts by weight, further preferably 0.20 to 0.50 parts by weight, and particularly preferably 0.20 to 0.45 parts by weight. In the in-mold foaming molded product formed by the conventional foamed particles, if 0.20 weight part or more of talc is contained, there is a tendency to easily produce color unevenness. Even if the in-mold foaming molded product formed by the present foamed particles contains 0.20 weight part or more of talc, there is no color unevenness and the blackness is good.

[0094] The method for determining the type of the foaming nucleating agent is not particularly limited, and known qualitative analysis can be applied. As a specific method of qualitative analysis of the present foaming nucleating agent, for example, it can be a method of analyzing the ash content by infrared spectroscopy as described in detail in the following embodiments, it can be a method of using chloroform for solvent fractionation and analyzing the chloroform insoluble matter by infrared spectroscopy, or it can be a method of using heated xylene for melt fractionation and analyzing the xylene insoluble matter by X-ray diffraction.

[0095] As flame retardants that can be used in one embodiment of the present invention, for example, there can be listed: intumescent flame retardants, hindered amine flame retardants, bromine flame retardants, phosphorus flame retardants, phosphate flame retardants, etc. The polyolefin resin foamed particles of the present invention contain hindered amine flame retardants, so that the target flame retardancy can be obtained with a small amount of flame retardant added.

[0096] The present foamed beads preferably contain a hindered amine flame retardant. According to this configuration, the effect of achieving the desired flame retardancy with a relatively small amount of the flame retardant added is achieved.

[0097] In this specification, "hindered amine" refers to a hindered amine having an OR group (here, R is a saturated or unsaturated monovalent hydrocarbon group) directly substituted on the N atom (hereinafter sometimes referred to as an N-substituted hindered amine). The hindered amine is not particularly limited as long as it is a hindered amine having an OR group directly substituted on the N atom, and a known hindered amine can be used. As the hindered amine, one hindered amine may be used alone, or two or more hindered amines may be used in combination.

[0098] As the hindered amine, an N-substituted hindered amine containing a triazine component (hereinafter sometimes referred to as a "triazine skeleton-containing hindered amine") is preferred because it can exhibit a flame retardant effect over a wide temperature range. The hindered amine containing a triazine skeleton is not particularly limited, but preferably is (i) a compound of CAS No. 191680-81-6 (which is (i-1) a reaction product of a peroxidized N-butyl-2,2,6,6-tetramethyl-4-piperidinamine and a reaction product of 2,4,6-trichloro-1,3,5-triazine with cyclohexane and N,N'-bis(3-aminopropyl)ethylenediamine, which can also be (i-2) a reaction product of 2,4-bis((1-cyclohexyloxy-2,2,6,6-tetramethylpiperidin-4-yl)butylamino)-6-chloro-S-triazine with N,N'-bis(3-aminopropyl)ethylenediamine). The corresponding product can also be said to be (i-3) N,N',N"'-tri{2,4-bis[(1-hydrocarbyloxy-2,2,6,6-tetramethylpiperidin-4-yl)alkylamino]-s-triazine-6-yl}-3,3'-ethylenediiminobispropylamine) and / or (ii) bis(1-undecanyloxy-2,2,6,6-tetramethylpiperidin-4-yl)carbonate. In addition, isomers of the above-mentioned triazine skeleton-containing hindered amines and cross-linked derivatives of the above-mentioned triazine skeleton-containing hindered amines can also be used. Regarding the triazine skeleton-containing hindered amines, more details are disclosed in the specification of European Patent No. 0889085 on page 2, line 32 to page 4, line 6.

[0099] As the triazine skeleton-containing hindered amine, commercially available products can also be preferably used. Examples of commercially available products of the triazine skeleton-containing hindered amine include BASF's FLAMSTAB (registered trademark) NOR116 (a compound with CAS number 191680-81-6), CLARIANT's HOSTAVIN (registered trademark) NOW XP, and Adeka Stab LA-81 (bis(1-undecyloxy-2,2,6,6-tetramethylpiperidin-4-yl) carbonate) manufactured by Adeka.

[0100] In one embodiment of the present invention, the hindered amine may be a compound represented by the following structural formula (iv):

[0101]

[0102] In the above structural formula (iv), G 1 and G 2 Independently for C 1-8 Alkyl or pentamethylene; Z 1 and Z 2 Methyl or Z 1 and Z 2 Together they form a bonding component, and the bonding component can be replaced by an ester group, an ether group, an amide group, an amino group, a carboxyl group or a carbamate group; and E is C 1-8 Alkoxy, C 5-12 Cycloalkoxy C 7-15 Aralkyloxy, -OC(O)-C 1-18 Alkyl or -OT-(OH) b Here, T is (i) C 1-18 Alkylene chain, (ii) C 5-18 Cycloalkylene chain, (iii) C 5-18 Cycloalkenylene chain, or (iv) phenyl or C 1-4 Alkyl substituted phenyl substituted C 1-4 Alkylene chain; b is 1 to 3 and is less than the number of carbon atoms possessed by T. In addition, when b is 2 or 3, each hydroxyl group is connected to a different carbon atom of T.

[0103] The compound represented by the above structural formula (iv) is disclosed in more detail in the specification of European Patent No. 2225318, and more specifically, in page 5, line 35 to page 25, line 48 of the specification of European Patent No. 2225318.

[0104] In one embodiment of the present invention, the hindered amine may be a compound represented by the following structural formula (v):

[0105]

[0106] In the above structural formula (v), R is hydrogen or methyl, and R 1 C 1-18 Alkyl, C 2-18 Alkenyl, C 2-18 Alkynyl, C 5-12 Cycloalkyl, C 5-8 Cycloalkenyl, C 6-10 Aryl or C 7-9 Aralkyl.

[0107] The compound represented by the above structural formula (v) is disclosed in more detail in page 3, line 33 to page 8, line 58 of European Patent No. 0309402.

[0108] In one embodiment of the present invention, the hindered amine may be a compound represented by the following structural formula (vi):

[0109]

[0110] In the above structural formula (vi), E, ​​k, Y, W, R1 to R7 and G1 to G4 are as defined in the specification of U.S. Patent No. 8,598,369.

[0111] The compound represented by the above structural formula (vi) is disclosed in more detail in Examples 1 to 12 and Tables 1 to 5 of US Pat. No. 8,598,369.

[0112] The amount of flame retardant used in the manufacture of the present foamed beads, in other words, the content of the flame retardant in the present foamed beads is described. The content of the flame retardant in the present foamed beads is preferably 0.05 to 1.00 parts by weight, more preferably 0.05 to 0.20 parts by weight, and further preferably 0.05 to 0.10 parts by weight, relative to 100 parts by weight of the base resin. When the aforementioned content of the flame retardant is (i) 0.05 parts by weight or more, the flame retardant effect can be fully obtained, and when it is (ii) 0.10 parts by weight or less, there is no need to worry about uneven or fine bubble diameters of the obtained foamed beads.

[0113] <Physical Properties>

[0114] The physical properties of the present expanded beads are described below.

[0115] (DSC ratio of foamed particles)

[0116] The present foamed beads preferably have at least two melting peaks in the DSC curve obtained by differential scanning calorimetry described later. Among the melting peaks, the melting heat obtained from the melting peak on the high temperature side is recorded as "high temperature side melting heat", and the melting heat obtained from the melting peak on the low temperature side is recorded as "low temperature side melting heat". In addition, when there are three or more melting peaks, the melting heat obtained from the highest temperature melting peak is recorded as "high temperature side melting heat", and the melting heat obtained from the other melting peaks is recorded as "low temperature side melting heat".

[0117] The DSC ratio of the present foamed particles is not particularly limited, and is preferably 10.0% to 50.0%, more preferably 15.0% to 40.0%, and further preferably 20.0% to 30.0%. When the DSC ratio of the foamed particles is 10.0% or more, there is the following advantage: the foamed particles can provide a foamed molded body with sufficient strength. On the other hand, when the DSC ratio of the foamed particles is 40% or less, there is the following advantage: the foamed particles can be molded at a relatively low temperature (molding temperature) to provide a foamed molded body.

[0118] The method for measuring the DSC ratio of expanded beads will be described in detail in Examples described later.

[0119] The DSC ratio of the present foamed particles is also a value that serves as a reference for the amount of crystals with a high melting point contained in the foamed particles. That is, a DSC ratio of 10.0% to 50.0% indicates that the foamed particles contain a large amount of crystals with a high melting point. In addition, the DSC ratio of the foamed particles is largely related to the viscoelasticity of the resin particles and the foamed particles when the resin particles are foamed and when the foamed particles are expanded. That is, when the DSC ratio of the foamed particles is 10.0% to 50.0%, the resin particles and the foamed particles can respectively exhibit excellent foaming properties and expandability when the resin particles are foamed and when the foamed particles are molded. As a result, there is the following advantage: the foamed particles can obtain a foamed molded body with excellent internal fusion properties and excellent mechanical strength such as compression strength at a low molding pressure.

[0120] In the present foamed beads, as a method for controlling the DSC ratio within a predetermined range, there can be cited a method of adjusting the conditions during the production of the present foamed beads (especially the foaming temperature, foaming pressure, retention time, and the temperature of the region (space) where the dispersion liquid is released, etc.) etc. From the viewpoint of easy adjustment, as a method for controlling the DSC ratio within a predetermined range, a method of adjusting the foaming temperature, foaming pressure and / or retention time is preferred.

[0121] For example, if the foaming temperature is increased, the DSC ratio tends to decrease, and conversely, if the foaming temperature is decreased, the DSC ratio tends to increase. This is because the amount of unmelted crystals changes due to the foaming temperature. In addition, if the foaming pressure is increased, the DSC ratio tends to decrease, and conversely, if the foaming pressure is decreased, the DSC ratio tends to increase. This is because the degree of plasticization changes due to the foaming pressure, which causes the amount of unmelted crystals to change. In addition, there is a tendency for the DSC ratio to become larger as the holding time is extended. This is because the growth amount of unmelted crystals changes due to the holding time.

[0122] (Expansion ratio of foamed particles)

[0123] The expansion ratio of the foamed particles is preferably 10 to 50 times, more preferably 15 to 40 times, and further preferably 15 to 30 times. If the expansion ratio of the foamed particles is (i) 10 times or more, a lightweight foamed molded article can be obtained with good production efficiency, and if it is (ii) 50 times or less, there is no need to worry about the insufficient strength of the obtained foamed molded article.

[0124] The method for calculating the expansion ratio of the foamed beads will be described in detail in the examples described later.

[0125] (Average bubble diameter of foamed particles)

[0126] The average bubble diameter of the present foamed particles is not particularly limited, and is preferably 100 μm to 500 μm, more preferably 120 μm to 400 μm, more preferably 120 μm to 300 μm, and further preferably 140 μm to 250 μm. When the average bubble diameter of the present foamed particles is (i) 100 μm or more, there is the following advantage: the foamed particles can provide a polypropylene resin foamed molded body without color unevenness, excellent colorability and excellent compression strength. When (ii) the average bubble diameter of the present foamed particles is 500 μm or less, there is the following advantage: there is no need to worry about the molding cycle of the in-mold foamed molded body becoming longer, and the productivity is good. Here, the molding cycle refers to the time from the start of in-mold foaming molding to the completion of molding when the obtained molded body is demolded from the mold by in-mold foaming molding using foamed particles.

[0127] The method for measuring the average cell diameter of the foamed beads will be described in detail in Examples described later.

[0128] <Method for producing polypropylene resin foamed particles>

[0129] The method for producing polypropylene resin foamed particles according to one embodiment of the present invention comprises: a granulation step of preparing a granulated particle containing a non-recycled polypropylene resin, a recycled material and a particle having an average structure size of 0.2×10 4 nm 2 Above and less than 4.0×10 4 nm 2 The mixture of carbon black A and carbon black A is melt-kneaded to obtain polypropylene resin particles; a dispersion step is performed to disperse the polypropylene resin particles, aqueous dispersion medium and foaming agent in a container; a heating step is performed to heat the temperature in the container to a temperature above the softening temperature of the polypropylene resin particles; a pressurization step is performed to pressurize the pressure in the container; and a release step is performed to open one end of the container to release the dispersion in the container to an area with a pressure lower than the pressure in the container. In the method for producing polypropylene resin foamed particles according to one embodiment of the present invention, the recycled material comprises recycled polypropylene resin and / or recycled polyethylene resin, and comprises an average structural size of 5.0×10 4 nm 2 Above and less than 9.0×10 4 nm 2 The carbon black B used in the above-mentioned recycled material is as follows: in 100 parts by weight of the base resin containing the above-mentioned non-recycled polypropylene resin and the above-mentioned recycled polypropylene resin and / or the above-mentioned recycled polyethylene resin, the total content of the above-mentioned recycled polypropylene resin and the above-mentioned recycled polyethylene resin is 10 parts by weight to 60 parts by weight.

[0130] The method for producing the foamed particles has the aforementioned structure, and therefore has the following advantages: it is possible to provide polypropylene resin foamed particles that can provide polypropylene resin foamed moldings with excellent blackness and flame retardancy. In addition, in the method for producing the foamed particles, recycled polypropylene resin and / or recycled polyethylene resin are used as described above. Therefore, it can be said that the method for producing the foamed particles has a small environmental burden.

[0131] Recycled materials currently circulating in the market (especially recycled materials containing recycled polypropylene resins) may contain carbon black. This is because carbon black is added in the recycling process for the purpose of adding carbon black as a colorant to the product before recycling or for the purpose of eliminating the color of the product before recycling with carbon black to make the color of the recycled material beautiful. It should be noted that the inventors measured the average structural size of carbon black contained in recycled polypropylene resin as an example of recycled materials by the above method, and the result was that the average structural size was, for example, 5.0×10 4 nm 2 Above and less than 9.0×10 4 nm 2 In this specification, the average structure size is 5.0×104 nm 2 Above and less than 9.0×10 4 nm 2 The carbon black contained in the recycled material is referred to as “carbon black B”. In other words, the recycled material may contain carbon black B.

[0132] In addition, the inventors have found that the blackness of a foamed molded article formed by molding foamed particles obtained using recycled materials (e.g., recycled polypropylene resin and / or recycled polyethylene resin) is poor, and have conducted in-depth research to provide a foamed molded article with excellent blackness even when foamed particles obtained using recycled materials are used.

[0133] The inventors have independently obtained the following new insights during the course of their in-depth research: if carbon black having an average structural size smaller than that contained in the recycled material (e.g., 0.2×10 4 nm 2 Above and less than 4.0×10 4 nm 2 ) carbon black, surprisingly, can provide a foamed molded product with excellent blackness. In this specification, the average structure size is 0.2×10 4 nm 2 Above and less than 4.0×10 4 nm 2 The carbon black of is referred to as "carbon black A". In other words, the present inventors have independently obtained the new finding that a foamed molded product having excellent blackness can be provided if foamed particles obtained by using (adding) carbon black A to recycled materials.

[0134] The present inventors used foamed particles obtained by using (adding) carbon black A to recycled materials, and measured the average structural size of carbon black in the foamed particles by the above method. As a result, in at least a portion of the foamed particles, the structural size of each structure in the foamed particles was less than 1×10 4 nm 2 The ratio of the number of carbon black to the total number of carbon black is 10% to 50%. That is, the present production method can provide the foamed beads according to one embodiment of the present invention. It should be noted that the structural size of each structure in the aforementioned foamed beads is less than 1×10 4 nm 2 The source of the carbon black may be the carbon black B in the recycled material, or may be the carbon black A used additionally (added).

[0135] Furthermore, the inventors independently obtained the following new finding: by appropriately adjusting the average structural size and amount of carbon black used in addition to the recycled material, the structural size of each structure in the foamed particles is less than 1×10 4 nm 2 The polypropylene resin foamed particles in which the ratio of the number of carbon blacks to the total number of carbon blacks is 10% to 50% can provide polypropylene resin foamed particles containing recycled resin and capable of providing a polypropylene resin foam molded body having excellent blackness and flame retardancy.

[0136] Hereinafter, one embodiment of the method for producing the present foamed beads will be described in detail, and except for the matters described in detail below, the description of the above-mentioned section [2. Polypropylene resin foamed beads] is appropriately cited. It should be noted that the method for producing the present foamed beads is not limited to the following production method.

[0137] (Granulation process)

[0138] The granulation step can also be said to be a step of preparing polypropylene resin particles, wherein the polypropylene resin particles contain: (a) a base resin containing non-recycled polypropylene resin and recycled polypropylene resin and / or recycled polyethylene resin, and (b) carbon black. The amount of recycled materials used in the present production method (e.g., granulation step) is an amount in which the total content of recycled polypropylene resin and recycled polyethylene resin in the obtained polypropylene resin particles is 10 to 60 parts by weight in 100 parts by weight of the base resin contained in the polypropylene resin particles. In this specification, "polypropylene resin particles" are sometimes referred to as "resin particles".

[0139] The polypropylene resin pellets in the present production method contain a base resin. It can also be said that the polypropylene resin pellets obtained through the above-mentioned granulation step contain a base resin.

[0140] In the granulation process, it is preferred to also use a foaming nucleating agent. In other words, the polypropylene resin particles in the present manufacturing method preferably contain a foaming nucleating agent. Specific examples of foaming nucleating agents are the same as those described in the aforementioned (foaming nucleating agent) section, so the description is cited and omitted here. The foaming nucleating agent in the present manufacturing method (for example, granulation process) is preferably used in the following amount: the content of the foaming nucleating agent in the obtained polypropylene resin particles is the amount described in the aforementioned (foaming nucleating agent) section relative to 100 parts by weight of the base resin in the polypropylene resin particles.

[0141] In the melt kneading of the mixture, there is no particular limitation, for example, an extruder may be used. In the granulation step, there is no particular limitation except for the melt kneading of the mixture. For example, polypropylene resin pellets can be prepared by sequentially performing the following (1) to (3) on the melt kneaded mixture: (1) extruding the mixture through a die provided by an extruder; (2) solidifying the extruded mixture by cooling it through water or the like; (3) then cutting the solidified mixture into a desired shape such as a cylinder, an ellipse, a sphere, a cube, a cuboid, a hollow cylinder, a polygonal column, etc. using a cutter. Alternatively, the melt kneaded mixture may be extruded directly into water through a die provided by an extruder, and the mixture may be cut into pellets immediately after extrusion, cooled, and solidified.

[0142] In the granulation process, a mixture containing non-recycled polypropylene resin, recycled materials, and carbon black A is melt-kneaded. Carbon black A can be used in its original state or in the state of a masterbatch pre-kneaded with a polypropylene resin. In the granulation process, carbon black B and carbon black C can be further used on the basis of carbon black A. The respective amounts of carbon black A, B, and C used in the granulation process can become the respective contents of carbon black A, B, and C in the obtained foamed particles. Therefore, regarding the respective amounts of carbon black A, B, and C used in the present manufacturing method (e.g., granulation process), it is preferably the following amount: the respective contents of carbon black A, B, and C in the obtained polypropylene resin particles are the amounts described in the aforementioned (2-2. Carbon black) item relative to 100 parts by weight of the base resin in the polypropylene resin particles. In addition, the respective average structures of carbon black A, B, and C used in the granulation process are also the same as the contents of the respective average structures of carbon black A, B, and C described above, so the description is cited and omitted here. It should be noted that the amount of carbon black B used in the present production method (for example, the granulation step) refers to the total amount of carbon black B contained in the recycled material used and the amount of carbon black B not used as recycled material but optionally used separately.

[0143] The total amount of non-recycled polypropylene resin and recycled materials used in the present manufacturing method (e.g., granulation step) is preferably the following amount: the total content of the non-recycled polypropylene resin, the recycled polypropylene resin, and the recycled polyethylene resin in the polypropylene resin particles is the amount described in the aforementioned (2-1. Base material resin) item.

[0144] (Dispersion process)

[0145] The dispersion step can also be said to be a step of preparing a dispersion in which, for example, resin particles, a foaming agent, and, if necessary, a dispersant and / or a dispersing aid are dispersed in an aqueous dispersion medium.

[0146] The container used in the dispersion step is not particularly limited, but is preferably a container that can withstand the foaming temperature and foaming pressure described below.

[0147] Examples of the container include a pressure-resistant container and an autoclave-type pressure-resistant container. The container may include a stirrer in the container.

[0148] The aqueous dispersion medium is not particularly limited as long as it can uniformly disperse the resin particles, the foaming agent, and the like.

[0149] As the aqueous dispersion medium, for example, there can be mentioned: (a) a dispersion medium obtained by adding methanol, ethanol, ethylene glycol, glycerol, etc. to water, (b) water such as tap water and industrial water, and (c) a solution (aqueous solution) containing a salt such as sodium chloride or sodium sulfate, etc. From the viewpoint of being able to stably produce foamed particles, as the aqueous dispersion medium, pure water and ultrapure water such as RO water (water purified by reverse osmosis membrane method), distilled water, and deionized water (water purified by ion exchange resin) are preferably used.

[0150] Examples of the foaming agent include: (a) (a-1) inorganic gases such as nitrogen, carbon dioxide, and air (a mixture of oxygen, nitrogen, and carbon dioxide); and (a-2) inorganic foaming agents such as water; and (b) (b-1) saturated hydrocarbons having 3 to 5 carbon atoms such as propane, n-butane, isobutane, n-pentane, isopentane, and neopentane; (b-2) ethers such as dimethyl ether, diethyl ether, and methyl ethyl ether; and (b-3) halogenated hydrocarbons such as monochloromethane, ethyl chloride, and hydrofluoroolefins.

[0151] As the blowing agent, halogenated hydrocarbons such as dichloromethane and dichlorodifluoroethane may be used.

[0152] In the method for producing the foamed particles, it is preferred to use a dispersant (for example, an inorganic substance such as calcium phosphate and kaolin) and a dispersing aid (for example, an anionic surfactant such as sodium dodecylbenzene sulfonate). According to this configuration, the adhesion (sometimes referred to as adhesion) of the resin particles to each other can be reduced, and the stability of the dispersion in the container can be improved. As a result, there is the following advantage: the foamed particles can be produced stably.

[0153] The aqueous dispersion medium and the foaming agent may be used alone or in combination of two or more.

[0154] The present production method includes, between the dispersing step and the releasing step, a heating step of heating the temperature in the container to a temperature above the softening temperature of the polypropylene resin particles; and a pressurizing step of increasing the pressure in the container to, for example, a certain pressure. The heating step and the pressurizing step may be performed in different orders or simultaneously. In addition, the present production method may further include a holding step after the heating step and the pressurizing step, in which the temperature in the container is kept at a temperature above the softening temperature of the polypropylene resin particles and the pressure in the container is kept at a certain pressure.

[0155] (Heating process, pressurizing process and holding process)

[0156] In this specification, (a) "temperature higher than the softening temperature of polypropylene resin particles" in the heating step, the pressurizing step, and the holding step may be referred to as "foaming temperature", and (b) a certain pressure may be referred to as "foaming pressure". In this specification, "higher than the softening temperature of polypropylene resin particles" means higher than the melting point -10°C of the polypropylene resin constituting the polypropylene resin particles, and when two or more polypropylene resins are used, means the melting point -10°C of the polypropylene resin with the highest melting point.

[0157] The foaming temperature in the heating process varies depending on the types of non-recycled polypropylene resin and recycled materials, the type of foaming agent, the desired apparent density of the foamed particles, etc., and therefore cannot be generally specified. In the heating process, as long as the temperature in the container is heated to a temperature above the softening temperature of the polypropylene resin particles, there is no particular limitation on how many degrees the temperature in the container is heated to. The heating process of one embodiment of the present invention is preferably a process for heating the temperature in the container to a temperature above (i) the softening temperature of the polypropylene resin particles and below the softening temperature of the polypropylene resin particles + 10.0°C, more preferably a process for heating the temperature in the container to a temperature above (ii) the softening temperature of the polypropylene resin particles and below the softening temperature of the polypropylene resin particles + 8.0°C, and further preferably a process for heating the temperature in the container to a temperature above (iii) the softening temperature of the polypropylene resin particles and below the softening temperature of the polypropylene resin particles + 6.0°C. According to this configuration, there is an advantage that there is no need to worry about the polypropylene resin particles sticking to each other in the container.

[0158] In the pressurizing step, there is no particular limitation on the degree to which the pressure in the container is pressurized. The pressurizing step of one embodiment of the present invention is preferably a step of pressurizing the pressure in the container to (i) a pressure of 1.0 MPa (gauge pressure) to 10.0 MPa (gauge pressure), more preferably a step of pressurizing the pressure in the container to (ii) a pressure of 1.5 MPa (gauge pressure) to 5.0 MPa (gauge pressure), and further preferably a step of pressurizing the pressure in the container to (iii) a pressure of 1.5 MPa (gauge pressure) to 3.5 MPa (gauge pressure). In the case where the pressurizing step is a step of pressurizing the pressure in the container to a pressure of 1.0 MPa (gauge pressure) or more, foamed particles with a suitable density can be obtained.

[0159] In the holding process, the time (holding time) for which the temperature in the container (temperature of the dispersion) is maintained at the foaming temperature and the pressure in the container is maintained near the foaming pressure is not particularly limited. The holding time is preferably 10 minutes to 60 minutes, more preferably 12 minutes to 55 minutes, and further preferably 15 minutes to 50 minutes. When the holding time is more than 10 minutes, there is a sufficient amount of unmelted crystals (crystallization of the substrate resin), and as a result, there is the following advantage: the shrinkage of the obtained foamed particles and / or the increase in the continuous bubble rate can be reduced. On the other hand, when the holding time is less than 60 minutes, there is no excessive unmelted crystals, and therefore there is the following advantage: the foamed particles can be molded at a lower molding temperature.

[0160] (Release process)

[0161] The releasing step may be performed (a) after the heating step and the pressurizing step when the holding step is not performed, or (b) after the holding step when the holding step is performed. The releasing step allows the resin particles to be foamed, and as a result, foamed particles can be obtained.

[0162] In the release process, "a region with a pressure lower than the pressure in the container" means "a region at a pressure lower than the pressure in the container" or "a space at a pressure lower than the pressure in the container", and can also be said to be "an atmosphere at a pressure lower than the pressure in the container". A region with a pressure lower than the pressure in the container can also be said to be a region with a pressure lower than the foaming pressure, and can be, for example, a region at atmospheric pressure.

[0163] In the release step, when the dispersion is released to a region where the pressure is lower than the pressure in the container, the dispersion may be released through an open throttle hole with a diameter of 1 mm to 5 mm in order to adjust the flow rate of the dispersion and reduce the variation in the expansion ratio of the obtained foamed particles.

[0164] The low-pressure region is, for example, a gas phase. In order to improve the foaming property, the low-pressure region (space) may be filled with saturated steam.

[0165] As described above, the process of producing foamed beads from resin particles is referred to as a "primary foaming process", and the obtained foamed beads are referred to as "primary foamed beads".

[0166] (Two-stage foaming process)

[0167] In order to obtain foamed particles with a high expansion ratio, the first-stage foamed particles obtained in the first-stage foaming process can be foamed again. The process of increasing the expansion ratio of the first-stage foamed particles is called the "second-stage foaming process", and the polyolefin resin foamed particles obtained by the second-stage foaming process are called "second-stage foamed particles". The specific method of the second-stage foaming process is not particularly limited, and a known method can be used.

[0168] [3. Polypropylene resin foamed molded article]

[0169] One embodiment of the present invention also provides a polypropylene resin foamed molded product, which is formed by molding the polypropylene resin foamed particles described in the above-mentioned [2. Polypropylene resin foamed particles]. The polypropylene resin foamed molded product involved in one embodiment of the present invention can also be said to be a foamed molded product containing the polypropylene resin foamed particles described in the above-mentioned [2. Polypropylene resin foamed particles].

[0170] In this specification, "the polypropylene-based resin foamed molded product according to one embodiment of the present invention" may be referred to as "the present foamed molded product".

[0171] The present foamed molded product has the above-mentioned structure, and therefore has the following advantages: excellent blackness and flame retardancy (self-extinguishing property). Specifically, a foamed molded product having excellent blackness and an L value of less than 28 measured by a spectrocolorimeter can be obtained. The present foamed molded product also has the following advantages: excellent color unevenness and surface properties. Specifically, a foamed molded product having a standard deviation of less than 2 and suppressed color unevenness of the L value measured by a spectrocolorimeter can be obtained. The determination and evaluation methods of the blackness, color unevenness, flame retardancy and surface properties of the foamed molded product are described in detail in the following embodiments.

[0172] The density of the molded body of the present foamed molded article is not particularly limited. The aforementioned molded body density is preferably 20g / L to 90g / L, more preferably 20g / L to 60g / L. According to this structure, there is the following advantage: it is possible to take into account both the excellent lightness and excellent impact resistance of the molded body. The method for measuring the density of the molded body of the foamed molded article is described in detail in the following examples.

[0173] <Method for producing foamed molded article>

[0174] As long as the foaming particles can be molded (preferably in-mold foaming) to obtain a foaming molded body, other methods are not particularly limited, and known methods can be applied. As a method for manufacturing the foaming molded body, for example, the method described in the <Method for Manufacturing Foamed Molded Body> of International Publication WO2022 / 149538 can be suitably adopted.

[0175] One embodiment of the present invention may have the following configuration.

[0176] [1] A polypropylene resin foamed particle comprising a base resin and carbon black, wherein the base resin comprises a non-recycled polypropylene resin and a recycled polypropylene resin and / or a recycled polyethylene resin, the total content of the recycled polypropylene resin and the recycled polyethylene resin is 10 to 60 parts by weight per 100 parts by weight of the base resin, and the carbon black has a structure size of less than 1×10 4 nm 2 The ratio of the number of carbon blacks to the total number of carbon blacks is 10% to 50%.

[0177] [2] The polypropylene resin foamed particles according to [1], comprising an average structural size of 0.2×10 4 nm 2 Above and less than 4.0×10 4 nm 2 The average structure size of carbon black A is 5.0×10 4 nm 2 Above and less than 9.0×10 4 nm 2 of carbon black B.

[0178] [3] The polypropylene resin foamed particles according to [1] or [2], further comprising a foaming nucleating agent.

[0179] [4] The polypropylene resin foamed particles according to [3], wherein the content of the foaming nucleating agent is 0.05 to 0.50 parts by weight based on 100 parts by weight of the base resin.

[0180] [5] The polypropylene resin foamed particles according to [3], wherein the content of the foaming nucleating agent is 0.20 to 0.50 parts by weight based on 100 parts by weight of the base resin.

[0181] [6] The polypropylene resin foamed particles according to any one of [3] to [5], wherein the foaming nucleating agent is talc.

[0182] [7] The polypropylene resin foamed particles according to any one of [1] to [6], further comprising a hindered amine flame retardant.

[0183] [8] The polypropylene resin foamed particles according to [2], wherein the content of the carbon black A is 0.1 to 5.0 parts by weight based on 100 parts by weight of the base resin.

[0184] [9] The polypropylene resin foamed particles according to [2], wherein the content of the carbon black B is 0.10 to 2.00 parts by weight based on 100 parts by weight of the base resin.

[0185]

[10] The polypropylene resin foamed particles according to any one of [1] to [9], wherein the base resin comprises the recycled polyethylene resin, and the recycled polyethylene resin comprises a recycled high-density polyethylene resin.

[0186]

[11] The polypropylene resin foamed particles according to any one of [1] to

[10] , wherein, when the total content of the recycled polypropylene resin and the recycled polyethylene resin is set to 100 parts by weight, the recycled polypropylene resin is 60 parts by weight to 100 parts by weight, and the recycled polyethylene resin is 0 parts by weight to 40 parts by weight.

[0187]

[12] The polypropylene resin foamed particles according to any one of [1] to

[11] , which do not contain an average structural size of 10.0×10 4 nm 2 The above carbon black C, or the carbon black C is contained in an amount of less than 0.5 parts by weight based on 100 parts by weight of the base resin.

[0188]

[13] The polypropylene resin foamed particles according to any one of [1] to

[12] , wherein the non-recycled polypropylene resin contains 60 wt % or more of one or more selected from the group consisting of ethylene / propylene alternating copolymers, ethylene / 1-butene / propylene alternating copolymers, ethylene / propylene random copolymers and ethylene / 1-butene / propylene random copolymers in 100 wt % of the non-recycled polypropylene resin.

[0189]

[14] The polypropylene resin foamed particles according to any one of [1] to

[13] , wherein the base resin comprises the recycled polypropylene resin, and the recycled polypropylene resin comprises one or more selected from the group consisting of ethylene / propylene alternating copolymers, ethylene / 1-butene / propylene alternating copolymers, ethylene / propylene random copolymers and ethylene / propylene random copolymers.

[0190]

[15] The polypropylene resin foamed particles according to any one of [1] to

[14] , wherein the substrate resin contains a total of 80 to 100 parts by weight of the non-recycled polypropylene resin, the recycled polypropylene resin and the recycled polyethylene resin per 100 parts by weight of the substrate resin.

[0191]

[16] The polypropylene resin foamed particles according to any one of [1] to

[15] , wherein the polypropylene resin foamed particles have a DSC ratio of 10.0% to 50.0%.

[0192]

[17] The polypropylene resin foamed particles according to any one of [1] to

[16] , wherein the foamed polypropylene resin particles have an expansion ratio of 10 to 50 times.

[0193]

[18] The polypropylene resin foamed particles according to any one of [1] to

[17] , wherein the average cell diameter of the polypropylene resin foamed particles is 100 μm to 500 μm.

[0194]

[19] A polypropylene resin foam molded product obtained by molding the polypropylene resin foamed particles according to any one of [1] to

[18] .

[0195]

[20] The polypropylene resin foam molded product according to

[19] , wherein the molded product density of the polypropylene resin foam molded product is 20 g / L to 90 g / L.

[0196]

[21] The polypropylene resin foam molded product according to

[19] or

[20] , wherein the polypropylene resin foam molded product has self-extinguishing properties.

[0197]

[22] The polypropylene resin foam molded product according to any one of

[19] to

[21] , wherein the L value of the polypropylene resin foam molded product measured by a spectrocolorimeter is less than 28.

[0198]

[23] The polypropylene resin foam molded product according to any one of

[19] to

[22] , wherein the standard deviation of the L value of the polypropylene resin foam molded product measured by a spectrocolorimeter is less than 2.

[0199]

[24] A method for producing polypropylene resin foamed particles, comprising: a granulation step of preparing a particle containing non-recycled polypropylene resin, recycled materials and an average structural size of 0.2×10 4 nm 2 Above and less than 4.0×10 4 nm 2The invention relates to a method for preparing a polypropylene resin particle, comprising: melt-kneading a mixture of carbon black A and carbon black A to obtain polypropylene resin particles; a dispersing step of dispersing the polypropylene resin particles, the aqueous dispersion medium and the foaming agent in a container; a heating step of heating the temperature in the container to a temperature above the softening temperature of the polypropylene resin particles; a pressurizing step of increasing the pressure in the container; and a releasing step of opening one end of the container to release the dispersion in the container to a region with a lower pressure than that in the container.

[0200] The aforementioned recycled material comprises recycled polypropylene resin and / or recycled polyethylene resin, and comprises an average structural size of 5.0×10 4 nm 2 Above and less than 9.0×10 4 nm 2 The carbon black B used in the above-mentioned recycled material is as follows: in 100 parts by weight of the base resin containing the above-mentioned non-recycled polypropylene resin and the above-mentioned recycled polypropylene resin and / or the above-mentioned recycled polyethylene resin, the total content of the above-mentioned recycled polypropylene resin and the above-mentioned recycled polyethylene resin is 10 parts by weight to 60 parts by weight.

[0201]

[25] The method for producing polypropylene resin foamed particles according to

[24] , wherein the heating step is a step of heating the temperature in the container to a temperature above the softening temperature of the polypropylene resin particles and below the softening temperature of the polypropylene resin particles + 10.0°C.

[0202]

[26] The method for producing polypropylene resin foamed particles according to

[24] or

[25] , wherein the pressurizing step is a step of increasing the pressure in the container to a pressure of 1.0 MPa (gauge pressure) to 10.0 MPa (gauge pressure).

[0203]

[27] The method for producing polypropylene resin foamed particles according to any one of

[24] to

[26] , wherein the polypropylene resin particles further contain a foaming nucleating agent.

[0204]

[28] The method for producing polypropylene resin foamed particles according to

[27] , wherein the content of the foaming nucleating agent in the polypropylene resin particles is 0.05 to 0.50 parts by weight relative to 100 parts by weight of the base resin.

[0205]

[29] The method for producing polypropylene resin foamed particles according to

[27] , wherein the content of the foaming nucleating agent in the polypropylene resin particles is 0.20 to 0.50 parts by weight relative to 100 parts by weight of the base resin.

[0206]

[30] The method for producing polypropylene resin foamed particles according to any one of

[27] to

[29] , wherein the foaming nucleating agent is talc.

[0207]

[31] The method for producing polypropylene resin foamed particles according to any one of

[24] to

[30] , wherein the polypropylene resin particles further contain a hindered amine flame retardant.

[0208]

[32] A method for producing polypropylene resin foamed particles according to any one of

[24] to

[31] , wherein the amount of the carbon black A used is as follows: the content of the carbon black A is 0.1 parts by weight to 5.0 parts by weight relative to 100 parts by weight of the base resin.

[0209]

[33] A method for producing polypropylene resin foamed particles according to any one of

[24] to

[32] , wherein the amount of the carbon black B used is as follows: the content of the carbon black B is 0.10 parts by weight to 2.00 parts by weight relative to 100 parts by weight of the base resin.

[0210]

[34] The method for producing polypropylene resin foamed particles according to any one of

[24] to

[33] , wherein the recycled material comprises the recycled polyethylene resin, and the recycled polyethylene resin comprises a recycled high-density polyethylene resin.

[0211]

[35] A method for producing polypropylene resin foamed particles according to any one of

[24] to

[34] , wherein, in the aforementioned recycled material, when the total content of the aforementioned recycled polypropylene resin and the aforementioned recycled polyethylene resin is set to 100 parts by weight, the aforementioned recycled polypropylene resin is 60 parts by weight to 100 parts by weight, and the aforementioned recycled polyethylene resin is 0 parts by weight to 40 parts by weight.

[0212]

[36] The method for producing polypropylene resin foamed particles according to any one of

[24] to

[35] , wherein the particles having an average structure size of 10.0×10 4 nm 2 The above carbon black C may be used in an amount such that the content of the carbon black C is less than 0.5 parts by weight relative to 100 parts by weight of the base resin.

[0213]

[37] A method for producing polypropylene resin foamed particles according to any one of

[24] to

[36] , wherein the non-recycled polypropylene resin contains 60 wt% or more of one or more selected from the group consisting of ethylene / propylene alternating copolymers, ethylene / 1-butene / propylene alternating copolymers, ethylene / propylene random copolymers and ethylene / 1-butene / propylene random copolymers in 100 wt% of the non-recycled polypropylene resin.

[0214]

[38] A method for producing polypropylene resin foamed particles according to any one of

[24] to

[37] , wherein the recycled material comprises the recycled polypropylene resin, and the recycled polypropylene resin comprises one or more selected from the group consisting of ethylene / propylene alternating copolymers, ethylene / 1-butene / propylene alternating copolymers, ethylene / propylene random copolymers and ethylene / propylene random copolymers.

[0215]

[39] A method for producing polypropylene resin foamed particles according to any one of

[24] to

[38] , wherein the total amount of the non-recycled polypropylene resin and the recycled material used is as follows: the total content of the non-recycled polypropylene resin, the recycled polypropylene resin and the recycled polyethylene resin in the polypropylene resin particles is 80 to 100 parts by weight per 100 parts by weight of the base material resin in the polypropylene resin particles.

[0216]

[40] The method for producing polypropylene resin foamed particles according to any one of

[24] to

[39] , wherein the DSC ratio of the polypropylene resin foamed particles is 10.0% to 50.0%.

[0217]

[41] The method for producing polypropylene resin foamed particles according to any one of

[24] to

[40] , wherein the foaming ratio of the polypropylene resin foamed particles is 10 to 50 times.

[0218]

[42] The method for producing polypropylene resin foamed particles according to any one of

[24] to

[41] , wherein the average bubble diameter of the polypropylene resin foamed particles is 100 μm to 500 μm.

[0219]

[43] A method for producing a polypropylene resin foam molded product, comprising the step of molding the polypropylene resin foam particles described in any one of [1] to

[18] or the polypropylene resin foam particles obtained by the method for producing polypropylene resin foam particles described in any one of

[24] to

[42] .

[0220]

[44] The method for producing a polypropylene resin foam molded product according to

[43] , wherein the polypropylene resin foam molded product has a molded product density of 20 g / L to 90 g / L.

[0221]

[45] The method for producing a polypropylene resin foam molded product according to

[43] or

[44] , wherein the polypropylene resin foam molded product has self-extinguishing properties.

[0222]

[46] The method for producing a polypropylene resin foam molded product according to any one of

[43] to

[45] , wherein the L value of the polypropylene resin foam molded product measured by a spectrocolorimeter is less than 28.

[0223]

[47] The method for producing a polypropylene resin foam molded product according to any one of

[43] to

[46] , wherein the standard deviation of the L value of the polypropylene resin foam molded product measured by a spectrocolorimeter is less than 2.

[0224] Example

[0225] Hereinafter, an embodiment of the present invention will be described in more detail with reference to Examples and Comparative Examples, but the present invention is not limited to the Examples. In Examples and Comparative Examples, the substances used are as follows, and were used without any particular purification or the like.

[0226] <Materials>

[0227] (Non-recycled polypropylene resin)

[0228] Ethylene / 1-butene / propylene random copolymer [ethylene content 1.0 wt%, 1-butene content 4 parts by weight, melting point 148°C]

[0229] (Recycled materials)

[0230] Recycled material-1: a mixture comprising 96.2 parts by weight of an ethylene / propylene random copolymer [ethylene content 9.0% by weight and melting point 151° C.], 3 parts by weight of carbon black B and 0.8 parts by weight of talc.

[0231] The average structural size of carbon black B in recycled material-1 was measured by the following method and the result was 5.8×10 4 nm 2 The content of carbon black B in recycled material-1 is a value measured by the following method. The ash content in recycled material-1 was measured by the following method and the result was 0.8 parts by weight. The ash content was qualitatively analyzed by the following method and was found to be talc.

[0232] ·Recycled material-2; high-density polyethylene [melting point 126°C]

[0233] (Carbon Black)

[0234] Carbon black A [average structure size: 3.2×10 4 nm 2 (Minimum value of the structure: 0.01×10 4 nm 2 , Maximum value of structure: 5.0×10 4 nm 2 )]

[0235] Carbon black B (carbon black contained in recycled material-1) [average structural size: 5.8×10 4 nm 2 (The minimum value of the structure is 1.0×10 4 nm 2 , maximum value 9.9×10 4 nm 2 )]

[0236] (Foaming nucleating agent)

[0237] ·Talc [Manufactured by Hayashi Kasei Co., Ltd., Talc PK-S]

[0238] (Water-absorbent substances)

[0239] · Glycerin [LION Corporation, purified glycerin D]

[0240] (Flame Retardant)

[0241] ·Hindered amine flame retardant [manufactured by BASF, NOR116]

[0242] <Method for determining melting point>

[0243] The melting points of non-recycled polypropylene resin, recycled polypropylene resin and recycled polyethylene resin are recorded as values ​​obtained by DSC measurement using a differential scanning calorimeter (DSC7020 manufactured by Hitachi High-Tech Corporation). The specific operation steps are as follows (1) to (3): (1) The temperature of 5 mg to 6 mg of a sample (non-recycled polypropylene resin, recycled polypropylene resin or recycled polyethylene resin) is increased from 40°C to 220°C at a heating rate of 10°C / min to melt the sample; (2) Then, the temperature of the molten sample is decreased from 220°C to 40°C at a cooling rate of 10°C / min to crystallize the sample; (3) Then, the temperature of the crystallized sample is further increased from 40°C to 220°C at a heating rate of 10°C / min. The temperature of the peak (melting peak) of the DSC curve of the sample obtained at the second heating (i.e., at (3)) is recorded as the melting point of the sample.

[0244] <Measurement of structural dimensions of carbon black>

[0245] The structural size of the carbon black in the foamed particles is determined by the following measurement method: (1) using a slicer to cut the polypropylene resin foamed particles into approximately half; (2) using a transmission electron microscope to take a photograph of the cross section of the cell membrane of the obtained polypropylene resin foamed particles at a magnification of 40,000 times to obtain a cross-sectional photograph; (3) in the obtained cross-sectional photograph under the transmission electron microscope, 30 carbon black structures are randomly extracted and the areas of these carbon blacks are measured. Specifically, a line is drawn along the outline of the carbon black structure, and the area of ​​the portion surrounded by the line is measured using the area measurement function of the PDF file editing software [made by Adobe, Adobe Acrobat DC].

[0246] In the above (3), the structural size of the carbon black in the recycled material was measured by the same method as above, except that an image obtained by magnifying the recycled material by 40,000 times using a transmission electron microscope was used. In the above (3), the structural size of the carbon black A or B added (used) was measured by the same method as above, except that an image obtained by magnifying the carbon black A or B by 40,000 times using a transmission electron microscope was used.

[0247] <Determination of carbon black content in recycled materials>

[0248] The carbon black content in the recycled material was measured using a thermogravimetric analysis-differential thermal analyzer [manufactured by Hitachi High-Tech Corporation, STA200RV]. The specific operation steps are as follows (1) to (3): (1) 6 to 8 mg of the recycled material was weighed into a Pt measuring container; (2) The temperature of the sample was raised to 600°C at 10°C / min in a nitrogen atmosphere, then cooled to 400°C at 10°C / min, and then changed to a simulated air (mixed gas of oxygen: nitrogen = 21%: 79%) atmosphere and the temperature was raised to 800°C at 10°C / min; (3) In the TG weight loss rate curve obtained in the process of the above (2), the weight ratio of carbon black [weight %] was calculated based on the difference between the weight loss rate [weight %] at 400°C and the weight loss rate [weight %] at 800°C in the process of heating from 400°C to 800°C.

[0249] <Measurement of ash content in recycled materials>

[0250] The ash content in the recycled material is calculated based on the weight of the recycled material and the weight of the recycled material after the recycled material is burned. The specific operation steps are as follows (1) to (4): (1) Heat the recycled material at 150°C for 1 hour to completely remove the moisture; (2) Put 1 to 2 g of the recycled material into a crucible with a weight of W1, and measure the weight of the crucible containing the recycled material, which is recorded as W2; (3) Use an electric furnace to keep the crucible containing the recycled material at 300°C for more than 30 minutes, and then keep it at 750°C for more than 1 hour to burn the recycled material; (4) Take the crucible out of the electric furnace and cool it in a dryer at 23°C for 1 hour; (5) Measure the weight of the crucible after cooling, which is recorded as W3; (6) Determine the ash content A according to the following formula.

[0251] W1: Crucible weight

[0252] W2: Crucible before burning + weight of recycled materials

[0253] W3: weight of crucible after burning + recycled materials

[0254] A = (W3-W1) × 100 / (W2-W1).

[0255] <Qualitative analysis of ash>

[0256] The ash content of talc in the recycled material was determined by infrared spectroscopy. The specific operation steps are as follows (1) to (2): (1) The ash obtained above was pressed onto the crystal part of a total reflection measuring device [PerkinElmer Japan, Spectrum Two] with a resolution of 4 cm -1 The total reflection measurement was performed 16 times to obtain the -1 ~4000cm -1 (2) In the obtained spectrum, at 3700cm -1 Nearby, 1020cm -1 Nearby, 670cm -1 Nearby and 550cm -1 Peaks were observed at 4 locations near 3700 cm -1 Nearby, 1020cm -1 Nearby, 670cm -1 Nearby and 550cm -1 The spectral shape of the peaks observed at four nearby locations is a spectral shape unique to talc, and therefore it was determined that the ash contained in the recycled material was talc.

[0257] <Determination of DSC ratio of polypropylene resin foamed particles>

[0258] The DSC ratio of the foamed particles is measured using a differential scanning calorimeter [DSC7020 manufactured by Hitachi High-Tech Corporation]. The specific operation steps are as shown in the following (1) to (5): (1) 5 mg to 6 mg of polypropylene resin foamed particles are weighed; (2) the temperature of the foamed particles is increased from 40°C to 220°C at a heating rate of 10°C / min to melt the foamed particles; (3) in the DSC curve of the foamed particles obtained in the process of the above (2) (DSC curve of the foamed particles when the temperature is increased for the first time), (a) the maximum point between the highest temperature melting peak and the melting peak adjacent to the melting peak (low temperature side) is connected with a straight line to the point indicating the temperature before the start of melting, and (b) the above maximum point is connected with the point indicating the end of melting. The points of the temperature after melting are connected by a straight line; (4) (a) the heat calculated by the line segment (a-1) connecting the aforementioned maximum point and the point indicating the temperature after melting ends and (a-2) the area surrounded by the DSC curve of the melting peak with the highest temperature is recorded as the high-temperature side melting heat Qh, (b) the heat calculated by the line segment (b-1) connecting the aforementioned maximum point and the point indicating the temperature before melting starts and (b-2) the area surrounded by the DSC curve of the adjacent (low-temperature side) melting peak with the maximum point is recorded as the low-temperature side melting heat Ql, (c) is recorded as the high-temperature side melting heat Qh; (5) the DSC ratio is calculated by the following formula:

[0259] DSC ratio (%)=Qh / (Qh+Ql)×100.

[0260] <Expansion ratio of polypropylene resin foam particles>

[0261] The method for measuring the expansion ratio of the foamed particles is as shown in the following (1) to (4): (1) The weight w (g) of the foamed particles is measured; (2) Then, the foamed particles used for the weight measurement are sunk into ethanol contained in a measuring cylinder, and the volume v (cm2) of the foamed particles is measured based on the amount of rise in the liquid level position of the measuring cylinder. 3 ); (3) by dividing the weight w (g) by the volume v (cm 3 ), calculate the density ρ1 of the foamed particles; (4) divide the density ρ2 of the polypropylene resin particles used in the manufacture of the foamed particles by the density ρ1 of the foamed particles to obtain the value (ρ2 / ρ1) as the foaming ratio of the foamed particles.

[0262] <Average cell diameter of foamed particles>

[0263] The method for determining the average bubble diameter of the foamed particles is as shown in the following (1) to (5): (1) While paying full attention not to break the bubble membrane (cell membrane) of the foamed particles, use a razor (Hi-Stainless Double Edge Blade manufactured by FEATHER) to cut the foamed particles in a manner passing through the center of the foamed particles; (2) Use a microscope [RH-2000 manufactured by HIROX] to observe the cut surface of the foamed particles and obtain an image of the observed surface; (3) On the obtained image, draw a line segment equivalent to a length of 2000 μm at any part of the foamed particles excluding the surface layer; (4) Measure the number of bubbles n passed by the line segment, and calculate the bubble diameter according to the formula (bubble diameter = 2000 / n (μm)); (5) Perform the same operation on 10 foamed particles, and record the arithmetic mean of the bubble diameters calculated respectively as the average bubble diameter of the foamed particles.

[0264] <Density of Foam Molded Article>

[0265] The weight (g) of the foamed molded product was measured (denoted as W). Next, the vertical, horizontal and thickness dimensions of the foamed molded product were measured with a vernier caliper to calculate the volume (unit: 1000 cm 3 , namely L) (denoted as V). Next, the density (g / L) of the foamed molded article is determined by the formula (density of the foamed molded article=W / V).

[0266] <Measurement of blackness and color unevenness of foamed molded articles>

[0267] Use spectrophotometer [CM-26dG made by Konicaminolta Co., Ltd.] to measure the L value of 50 points at any position on the foaming molding surface, and its average value is recorded as blackness. It should be noted that the reflected light during measurement is only diffuse reflected light. In addition, the standard deviation of the L value measured is recorded as color unevenness. Blackness and color unevenness are evaluated with the following benchmarks respectively. The larger the numerical value, the more excellent blackness and color unevenness are.

[0268] (Blackness)

[0269] 1 (Excellent): The average value of the measured L value is less than 28

[0270] 0 (bad): The average value of the measured L value is 28 or more

[0271] (Uneven color)

[0272] 1 (Excellent): The standard deviation of the measured L values ​​is less than 2

[0273] 0 (bad): The standard deviation of the measured L value is 2 or more

[0274] <Evaluation of flame retardancy of polypropylene resin in-mold foamed articles>

[0275] A flame retardancy test sample of 350 mm in length × 100 mm in width × 12 mm in thickness was cut from the obtained foamed molded body, and a marking line A was set at a position of 38 mm from one end of the length direction of the sample, and a marking line B was set at a position of 292 mm. The flame retardancy evaluation was carried out according to the combustion test method specified in FMVSS302. Using the FMVSS flammability tester [manufactured by Suga Test Instruments Co., Ltd.], at one end of the length direction of the sample, the sample end was made the center of the flame, and the flame of the burner adjusted to a height of 38 mm was contacted for 15 seconds. According to the combustion situation at this time, the flame retardancy was evaluated according to the following criteria. The larger the value, the better the flame retardancy.

[0276] 1 (Excellent): The flame goes out before reaching the A mark, or within 60 seconds or 50 mm after passing the A mark. This is called "self-extinguishing".

[0277] 0 (poor): The burning speed is 100 mm / min or less when the flame burns beyond the A mark line [38 mm from the end of the sample in contact with the flame] and burns to the B mark line [292 mm from the end of the sample in contact with the flame], and when the flame burns beyond the A mark line and extinguishes more than 60 seconds or more than 50 mm after passing the A mark line. This is called "delayed ignition".

[0278] -1 (very poor): Neither self-extinguishing property nor delayed ignition property can be determined. This is called "flammability".

[0279] <Evaluation of Surface Properties of Polypropylene Resin In-Mold Foam Molded Articles>

[0280] The surface of the molded foamed body obtained by visual observation was judged by the following criteria. The particle gap (the gap between the polypropylene resin foamed particles) as one of the evaluation indicators of surface property was judged by visually counting the number of particles present in the 50 mm square on the surface of the central part of the molded body. The larger the value, the better the surface property.

[0281] 2 (good): The interparticle gap (the interparticle gap between polypropylene resin foam particles) is 0 to 1, there are no wrinkles, and the appearance is beautiful.

[0282] 1 (acceptable): There are 2 to 3 gaps between particles and no wrinkles.

[0283] 0 (Not acceptable): There are 4 or more interparticle spaces and wrinkles are visible.

[0284] Hereinafter, the production methods of the polypropylene resin particles, the polypropylene resin foamed particles, and the polypropylene resin in-mold foamed molded products in Examples and Comparative Examples will be described.

[0285] (Example 1)

[0286] [Production of resin pellets]

[0287] A mixture was obtained by dry-blending (a) 75 parts by weight of a non-recycled polypropylene resin (ethylene / 1-butene / propylene random copolymer), (b) 25 parts by weight of recycled material-1, (c) 3 parts by weight of carbon black A, (d) 0.2 parts by weight of glycerol, (e) 0.05 parts by weight of talc, and (f) 0.10 parts by weight of a hindered amine flame retardant using a mixer. The obtained mixture was melt-kneaded at a resin temperature of 220° C. using a twin-screw extruder [TEM26-SX manufactured by Toshiba Machine Co., Ltd.], and the extruded strand was water-cooled in a water tank with a length of 2 m and then cut to produce polypropylene resin pellets (1.2 mg / pellet).

[0288] [Production of Foamed Particles and Foamed Molded Articles]

[0289] In a 10L pressure-resistant autoclave, 100 parts by weight (2.4 kg) of the polypropylene resin particles obtained as described above, 200 parts by weight of water, 0.3 parts by weight of kaolin [ASP170 manufactured by BASF] as a dispersant, and 0.038 parts by weight of an aqueous solution of sodium dodecylbenzenesulfonate [NEOPELEX G-15 manufactured by Kao Corporation, an aqueous solution of 16% sodium dodecylbenzenesulfonate] as a dispersant were placed, and then 4 parts by weight of carbon dioxide as a foaming agent was added under stirring. The contents of the autoclave were heated to a foaming temperature of 155.5°C, and after maintaining for 10 minutes, additional carbon dioxide was pressurized to increase the pressure inside the autoclave to a foaming pressure of 2.2 MPa. After maintaining at the above-mentioned foaming temperature and foaming pressure for 20 minutes, the valve at the bottom of the autoclave was opened, and the mixture was released to atmospheric pressure through an opening orifice with a diameter of 3.6 mm, thereby obtaining polypropylene resin foamed particles having a foaming ratio of 17 times. At this time, in order to prevent the pressure in the container from decreasing during release, carbon dioxide is pressed in to maintain the pressure.

[0290] The obtained expanded beads were dried at 80°C, impregnated with pressurized air in a pressure-resistant container to an internal pressure of 0.3 MPa (absolute pressure), and then contacted with water vapor of 0.07 MPa (gauge pressure) to perform two-stage expansion. The expansion ratio of the obtained two-stage expanded beads was 25 times.

[0291] The obtained two-stage foamed particles are put into a pressure-resistant container, impregnated with pressurized air, and the polypropylene resin foamed particles with a pre-adjusted foamed particle internal pressure of 0.20MPa (absolute pressure) are filled into a mold of 370mm in length × 320mm in width × 50mm in thickness. Then, the mold cavity is heated with 0.30MPa water vapor to fuse the foamed particles to each other. After the mold and the surface of the molded body are water-cooled, the molded body is taken out to obtain a polypropylene resin in-mold foamed body. The obtained in-mold foamed body is left to stand at 23°C for 2 hours, and then aged at 75°C for 16 hours.

[0292] (Examples 2 and 3)

[0293] In [Production of Resin Particles], the formula was changed as shown in Table 1 or Table 2, and in [Production of Foamed Particles and Foamed Molded Articles], the foaming conditions were changed as shown in Table 1 or Table 2. Except for this, polypropylene resin particles, polypropylene resin foamed particles, and polypropylene resin in-mold foamed molded articles were produced by the same operation as in Example 1.

[0294] (Examples 4 and 5)

[0295] A mixer was used to dry-blend (a) non-recycled polypropylene resin in the amount shown in Table 1, (b) recycled material-1 and recycled material-2 in the amounts shown in Table 1, (c) 3 parts by weight of carbon black A, (d) 0.2 parts by weight of glycerol, (e) 0.05 parts by weight of talc, and (f) 0.10 parts by weight of hindered amine flame retardant to obtain a mixture. The obtained mixture was melt-kneaded at a resin temperature of 220°C using the same twin-screw extruder as in Example 1, and the extruded strands were water-cooled in a water tank of 2 m in length and then cut to produce polypropylene resin particles (1.2 mg / particle). Polypropylene resin foamed particles and polypropylene resin in-mold foamed bodies were produced by the same operation as in Example 1 except that the foaming conditions were changed as shown in Table 1 in [Production of Foamed Particles and Foamed Molded Body].

[0296] (Comparative Example 1)

[0297] A mixer was used to dry-blend (a) non-recycled polypropylene resin in the amount shown in Table 1, (b) recycled material-1 and recycled material-2 in the amounts shown in Table 1, (c) 0.2 parts by weight of glycerol, (d) 0.05 parts by weight of talc, and (e) 0.10 parts by weight of hindered amine flame retardant to obtain a mixture. The obtained mixture was melt-kneaded at a resin temperature of 220°C using the same twin-screw extruder as in Example 1, and the extruded strands were water-cooled in a water tank of 2 m in length and then cut to produce polypropylene resin particles (1.2 mg / particle). In [Production of Foamed Particles and Foamed Molded Articles], the foaming conditions were changed as shown in Table 2, and the same operation as in Example 1 was used to produce polypropylene resin foamed particles and polypropylene resin in-mold foamed molded articles.

[0298] (Comparative Example 2)

[0299] A mixer was used to dry-blend (a) the amount of recycled material-1 shown in Table 1, (b) 3 parts by weight of carbon black A, (c) 0.2 parts by weight of glycerol, (d) 0.05 parts by weight of talc, and (e) 0.10 parts by weight of a hindered amine flame retardant to obtain a mixture. The obtained mixture was melt-kneaded at a resin temperature of 220°C using the same twin-screw extruder as in Example 1, and the extruded strands were water-cooled in a water tank of 2 m in length and then cut to produce polypropylene resin particles (1.2 mg / particle). In [Production of Foamed Particles and Foamed Molded Articles], the foaming conditions were changed as shown in Table 2, and the same operation as in Example 1 was used to produce polypropylene resin foamed particles and polypropylene resin in-mold foamed molded articles.

[0300] (Comparative Example 3)

[0301] A mixer was used to dry-blend (a) recycled material-1 and recycled material-2 in the amounts shown in Table 1, (b) 3 parts by weight of carbon black A, (c) 0.2 parts by weight of glycerol, (d) 0.05 parts by weight of talc, and (e) 0.10 parts by weight of a hindered amine flame retardant to obtain a mixture. The obtained mixture was melt-kneaded at a resin temperature of 220°C using the same twin-screw extruder as in Example 1, and the extruded strands were water-cooled in a water tank of 2 m in length and then cut to produce polypropylene resin particles (1.2 mg / particle). Polypropylene resin foamed particles and polypropylene resin in-mold foamed bodies were produced by the same operation as in Example 1 except that the foaming conditions were changed as shown in Table 2 in [Production of Foamed Particles and Foamed Molded Body].

[0302] (Reference Example 1)

[0303] A mixer was used to dry-blend (a) 100 parts by weight of non-recycled polypropylene resin, (b) 3 parts by weight of carbon black A, (c) 0.2 parts by weight of glycerol, (d) 0.05 parts by weight of talc, and (e) 0.10 parts by weight of hindered amine flame retardant to obtain a mixture. The obtained mixture was melt-kneaded at a resin temperature of 220°C using the same twin-screw extruder as in Example 1, and the extruded strands were water-cooled in a water tank of 2m in length and then cut to produce polypropylene resin particles (1.2mg / particle). In [Preparation of Foamed Particles and Foamed Molded Articles], the foaming conditions were changed as shown in Table 2. Otherwise, the same operation as in Example 1 was used to produce polypropylene resin foamed particles and polypropylene resin in-mold foamed molded articles. The evaluation results of the obtained polypropylene resin foamed particles and polypropylene resin in-mold foamed molded articles are shown in Table 2.

[0304] (Reference Example 2)

[0305] A mixer was used to dry-blend (a) 100 parts by weight of non-recycled polypropylene resin, (b) 3 parts by weight of carbon black A, (c) 0.2 parts by weight of glycerol, (d) 0.25 parts by weight of talc, and (e) 0.10 parts by weight of hindered amine flame retardant to obtain a mixture. The obtained mixture was melt-kneaded at a resin temperature of 220°C using the same twin-screw extruder as in Example 1, and the extruded strands were water-cooled in a water tank of 2 m in length and then cut to produce polypropylene resin particles (1.2 mg / particle). In [Production of Foamed Particles and Foamed Molded Articles], the foaming conditions were changed as shown in Table 2. Otherwise, the same operation as in Example 1 was used to produce polypropylene resin foamed particles and polypropylene resin in-mold foamed molded articles.

[0306] The formulations for producing polypropylene resin pellets in each of the Examples, Comparative Examples and Reference Examples are shown in Table 1 or Table 2. In Table 1 or Table 2, (i) the amount of carbon black B is the total amount of carbon black B derived from recycled materials and the amount of carbon black B added separately, and (ii) the amount of talc is the total amount of talc derived from recycled materials and the amount of talc added separately.

[0307] Various measurements and evaluations were performed on the polypropylene resin foamed particles and the polypropylene resin in-mold foamed products obtained in the examples, comparative examples and reference examples.

[0308] [Table 1]

[0309]

[0310] [Table 2]

[0311]

[0312] Reference Examples 1 and 2 show the evaluation results of existing foamed particles that do not contain recycled materials. According to the comparison between Reference Examples 1 and 2, when the amount of talc contained in the existing resin particles is increased from 0.05 parts by weight to 0.25 parts by weight, it is confirmed that the average bubble diameter becomes smaller and the color unevenness worsens. Examples 1 to 5 show the evaluation results of polypropylene resin foamed particles and polypropylene resin in-mold foamed bodies involved in one embodiment of the present invention. It can be seen from Examples 1 to 5 that the in-mold foamed body formed by the polypropylene resin foamed particles obtained by the present manufacturing method has no color unevenness even if it contains 0.25 parts by weight or more of talc, and has excellent blackness and surface appearance and good flame retardancy. As in Comparative Examples 1 to 3, the structural size is less than 1.0×10 4 nm 2 When the ratio of carbon black is reduced, the blackness and flame retardancy can be improved.

[0313] Industrial Applicability

[0314] The polypropylene foamed particles according to one embodiment of the present invention have the following advantages: the blackness and flame retardancy after molding can be improved. The polypropylene foamed molded body can be applied to various uses such as cushioning packaging materials, logistics materials, insulation materials, civil engineering and construction parts, and automobile parts.

Claims

1. A polypropylene resin foam particle comprising a base resin and carbon black, The base resin comprises a non-recycled polypropylene resin and a recycled polypropylene resin and / or a recycled polyethylene resin, The total content of the recycled polypropylene resin and the recycled polyethylene resin is 10 parts by weight to 60 parts by weight in 100 parts by weight of the base resin. In the carbon black, the structural size of each structure is less than 1×10 4 nm 2 The ratio of the number of carbon blacks to the total number of carbon blacks is 10% to 50%.

2. The polypropylene resin foamed particles according to claim 1, comprising an average structural size of 0.2×10 4 nm 2 Above and less than 4.0×10 4 nm 2 The average structure size of carbon black A is 5.0×10 4 nm 2 Above and less than 9.0×10 4 nm 2 of carbon black B. The polypropylene resin foamed particles according to claim 1 or 2, further comprising a foaming nucleating agent.

4. The polypropylene resin foamed particles according to claim 3, wherein The content of the foaming nucleating agent is 0.05 parts by weight to 0.50 parts by weight based on 100 parts by weight of the base resin.

5. The polypropylene resin foamed particles according to claim 3, wherein The content of the foaming nucleating agent is 0.20 parts by weight to 0.50 parts by weight based on 100 parts by weight of the base resin.

6. The polypropylene resin foamed particles according to any one of claims 3 to 5, wherein The foaming nucleating agent is talc. 7 . The polypropylene resin foamed particles according to claim 1 , further comprising a hindered amine flame retardant.

8. The polypropylene resin foamed particles according to claim 2, wherein The content of the carbon black A is 0.1 parts by weight to 5.0 parts by weight based on 100 parts by weight of the base resin.

9. The polypropylene resin foamed particles according to claim 2, wherein The content of the carbon black B is 0.10 parts by weight to 2.00 parts by weight based on 100 parts by weight of the base resin.

10. The polypropylene resin foamed particles according to any one of claims 1 to 9, wherein The base resin includes the recycled polyethylene resin, and the recycled polyethylene resin includes a recycled high-density polyethylene resin.

11. The polypropylene resin foamed particles according to any one of claims 1 to 10, wherein When the total content of the recycled polypropylene resin and the recycled polyethylene resin is 100 parts by weight, the recycled polypropylene resin is 60 parts by weight to 100 parts by weight, and the recycled polyethylene resin is 0 parts by weight to 40 parts by weight.

12. The polypropylene resin foamed particles according to any one of claims 1 to 11, which do not contain an average structural size of 10.0×10 4 nm 2 The above carbon black C, or the carbon black C is contained in an amount of less than 0.5 parts by weight relative to 100 parts by weight of the base resin.

13. The polypropylene resin foamed particles according to any one of claims 1 to 12, wherein The non-recycled polypropylene resin contains 60% by weight or more of one or more selected from the group consisting of ethylene / propylene alternating copolymers, ethylene / 1-butene / propylene alternating copolymers, ethylene / propylene random copolymers and ethylene / 1-butene / propylene random copolymers in 100% by weight of the non-recycled polypropylene resin.

14. The polypropylene resin foamed particles according to any one of claims 1 to 13, wherein The base resin includes the recycled polypropylene resin, and the recycled polypropylene resin includes one or more selected from the group consisting of ethylene / propylene alternating copolymers, ethylene / 1-butene / propylene alternating copolymers, ethylene / propylene random copolymers, and ethylene / propylene random copolymers.

15. The polypropylene resin foamed particles according to any one of claims 1 to 14, wherein The base resin includes 80 to 100 parts by weight of the non-recycled polypropylene resin, the recycled polypropylene resin, and the recycled polyethylene resin in total per 100 parts by weight of the base resin. 16 . A polypropylene resin foam molded product obtained by molding the polypropylene resin foamed particles according to claim 1 .

17. A method for producing polypropylene resin foamed particles, comprising: The granulation process contains non-recycled polypropylene resin, recycled materials and an average structure size of 0.2×10 4 nm 2 Above and less than 4.0×10 4 nm 2 The mixture of carbon black A and carbon black A is melt-kneaded to obtain polypropylene resin particles; A dispersing step of dispersing the polypropylene resin particles, the aqueous dispersion medium and the foaming agent in a container; A heating step of heating the temperature in the container to a temperature above the softening temperature of the polypropylene resin particles; A pressurizing step of increasing the pressure in the container; and In the release step, one end of the container is opened to release the dispersion in the container to an area with a lower pressure than the pressure in the container. The recycled material comprises recycled polypropylene resin and / or recycled polyethylene resin, and comprises an average structural size of 5.0×10 4 nm 2 Above and less than 9.0×10 4 nm 2 Carbon black B, The amount of the recycled material used is as follows: in 100 parts by weight of the base resin containing the non-recycled polypropylene resin and the recycled polypropylene resin and / or the recycled polyethylene resin, the total content of the recycled polypropylene resin and the recycled polyethylene resin is 10 parts by weight to 60 parts by weight.

Citation Information

Cited By

  • Flame-retardant foamed polypropylene composite material and preparation method thereof

    CN119192732A