Recycled 6xxx alloy plates and methods of manufacture
Through the specific composition of aluminum alloy plates and process flow, the problem of recycling of coated plates is solved, efficient production of automobile body parts is achieved, and carbon emissions and resource waste is reduced.
Patent Information
- Application Number
- CN202380030041.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-04-02
- Filing Date
- 2023-03-31
- Publication Date
- 2024-11-12
AI Technical Summary
The prior art is difficult to efficiently recover and reuse the clad plate waste containing different alloys, especially in the manufacturing of automotive body parts, resulting in waste of resources and increased carbon emissions.
Using specific composition aluminum alloy plates, including alloys of elements such as Si, Fe, Cu, Mn, Mg, Ti, Cr and Zn, through semi-continuous vertical casting, hot rolling, cold rolling, solid solution heat treatment and quenching, etc. An aluminum alloy plate with excellent moldability and corrosion resistance was prepared, which is suitable for the production of automotive body parts.
It has achieved the production of aluminum alloy plates with excellent stamping, mechanical properties and corrosion resistance from recycling of clad plate waste, which reduces carbon emissions, improves resource utilization, and meets the use needs of automotive body parts.
Smart Images

Figure CN118946679A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of aluminum alloy plates intended for stamping and manufacturing of body parts of automobile body-in-white. Background Art
[0002] Aluminum alloys are increasingly used in automotive construction to reduce vehicle weight, thereby reducing fuel consumption and greenhouse gas emissions.
[0003] It is also necessary to reduce greenhouse gas emissions during the production of the alloy. This reduction can be obtained by recycling aluminum alloy scrap and waste, thereby reducing or even avoiding the use of primary aluminum produced by electrolysis and / or addition of alloying elements.
[0004] The carbon footprint of an optimal electrolysis plant using hydroelectricity, taking into account the use of carbon anodes, is 4 tons of CO2 equivalent (CO2 eq) per ton of cast plate. The typical carbon footprint of one ton of electrolytic aluminum cast plate produced in Europe is 7 tons of CO2 eq. The carbon footprint of one ton of cast plate obtained only from scrap and waste is 0.5 tons of CO2 eq per cast plate. CO2 equivalent emissions are the carbon dioxide (CO2) emissions that cause the same combined radiative forcing as the emissions of one or more greenhouse gases (GHGs) over a time horizon of 100 years. CO2 equivalent emissions are calculated by multiplying the emissions of GHGs by their global warming potential (GWP) over a time horizon of 100 years. In the case of a mixture of GHGs, CO2 equivalent emissions are calculated by adding the CO2 equivalent emissions of each gas. When a plate is partly produced using recycled alloy, the CO2 equivalent of this plate is evaluated by linear interpolation between the above electrolytic plate (0% recycling) and the plate obtained only from scrap and waste (100% recycling). The recovery or recycling rate is the ratio of the weight of aluminium alloy scrap and waste used to produce the plate to the weight of the plate, with the remainder of the alloy being primary aluminium and / or alloying elements.
[0005] Simple recycling includes closed-loop recycling, i.e. recycling aluminium alloy scrap and waste to obtain the same alloy as when it was produced. However, there are products that cannot be recycled in this way. This applies in particular to clad sheets as defined in EN 12258-1 (2012) §2.6.26, especially when they contain very different alloys. This is the case for clad sheets used in the production of brazed heat exchangers, as they are usually made of a core part made of a 3xxx alloy (sometimes with small amounts of Cu and / or Mg) and one or more cladding layers made of 4xxx and / or 7xxx and / or 1xxx and / or 3xxx alloys. Currently, these clad sheets are mainly recycled for cast parts, which usually use 4xxx alloys. However, the transition from internal combustion engine drive to electric drive will shake up this recycling branch. Aluminium alloy sheets on vehicles, especially those for body and structural components, are in the prior art 5xxx and 6xxx alloys, which are not suitable for large-scale recycling of 4xxx alloys due to their composition. The evolution of alloys due to research and development also makes it difficult to recycle old scrap, which according to EN 12258-1 is the waste generated after the use of products. This is the case with old scrap generated after the demolition of buildings, which usually contains Si: 0.5%, Fe: 0.2%, Cu: 0.1%, Mn: 0.1%, Mg: 0.1%.
[0006] Application US20210108293 discloses an aluminum alloy sheet, the chemical composition of which includes Si: 2.3-3.8 mass%, Mn: 0.35-1.05 mass%, Mg: 0.35-0.65 mass%, Fe: 0.01-0.45 mass%, and at least one element selected from Cu: 0.0010-1.0 mass%, Cr: 0.0010-0.10 mass%, Zn: 0.0010-0.50 mass% and Ti: 0.0050-0.20 mass%. The ratio of Si content to Mn content is greater than or equal to 2.5 and less than or equal to 9.0. At a nominal strain of 3%, the elongation of the aluminum alloy sheet is greater than or equal to 23%, and the strain hardening index is greater than or equal to 0.28. This aluminum alloy sheet is very suitable for stamping (stamping) applications, such as forming automotive body skins.
[0007] Application WO2018 / 175876 discloses a technique for casting high strength and high formability metal products from recycled metal scrap without adding much or any amount of primary aluminum. Additional alloying elements, such as magnesium, can be added to the metal scrap, which can be cast and processed to produce the desired metal coil having the desired metallurgical and mechanical properties, such as high strength and formability, at the final specification. Thus, cheap and recycled metal scrap can be effectively reused in new applications, such as automotive applications and beverage can blanks.
[0008] The technical problem to be solved by the application JP2005298922 is to provide an aluminum alloy plate to be formed at a low cost, which has sufficient hemming-bending formability, low bending anisotropy and greater baking hardenability after coating, causes less aging at room temperature, and has sufficient wrinkle resistance. The solution is an aluminum alloy plate of Al-Mg-Si based alloy or Al-Mg-Si-Cu based alloy; under the conditions of (C(sub 1 / 10)+C(sub 1 / 4)) / 2>C(sub 1 / 2) and 30<(C(sub 1 / 10)+C(sub1 / 4))<500, C(sub 1 / 10), C(sub 1 / 4) and C(sub 1 / 2) are defined as the cubic orientation density at 1 / 10, 1 / 4 and 1 / 2 depth from the plate surface in the plate thickness direction, respectively; in the region from 1 / 10 to 1 / 4 depth from the plate surface in the plate thickness direction, {001} <210> The orientation density is 2 to 50; and the 0-degree and 90-degree earing rates are 5% or more. The manufacturing method includes strictly specified casting and hot rolling conditions. The metallographic structure conditions of the cast slab and the hot-rolled plate as intermediate products are specified.
[0009] Application WO2022 / 026825 discloses a new 6xxx aluminum alloy. In one method, a new 6xxx aluminum alloy may include 0.25 to 0.60 wt% iron, 0.8 to 1.2 wt% silicon, 0.35 to 1.1 wt% Mg, 0.05 to 0.8 wt% Mn, up to 0.30 wt% Cu, up to 0.35 wt% Zn, up to 0.15 wt% Ti, up to 0.15 wt% Cr, Zr and V each, the balance being aluminum, incidental elements and impurities. The new 6xxx aluminum alloy can be made from recycled aluminum alloy.
[0010] Therefore, there is a need to recycle cladding sheet scrap and waste to produce body panels for the automotive industry.
[0011] Ask a question
[0012] The problem to be solved is to develop a 6xxx series alloy plate with the aim of achieving an excellent compromise between:
[0013] Recycling of scrap and waste, preferably cladding sheet. Cladding sheet is usually made of very different alloys,
[0014] For example, the core part uses a 3xxx series alloy, a 4xxx and / or 7xxx series cladding. The average composition of the clad sheet is difficult to recycle into another sheet, as it does not correspond to a known alloy. Furthermore, recycling activities, especially when it comes to old scrap generated after the use of a product, are inseparable from contamination phenomena that arise from mixing with other materials, such as steel, and that can reduce the properties of the material obtained after recycling.
[0015] The formability of the plate is evaluated in the T4 state after natural aging, which corresponds to the quenching of the plate.
[0016] The time of transport and storage between the fire and the stamped parts. Formability The LDH (Limiting Dome Height) test is used to characterize the deformability and the yield strength is used to characterize the force required to obtain said deformation.
[0017] The properties necessary for the use of the part in the automobile are evaluated on the finished part, therefore after stamping, painting and baking of the sheet. The person skilled in the art also calls baking "baking hardening" because it can simultaneously harden the stamped sheet by aging, thereby obtaining the properties necessary for the use of the part in the automobile. Here, the suitability for automotive use is characterized by the yield strength of the sheet after a deformation of 2% and a heat treatment of 170°C for 20 minutes (representing the baking heat treatment). In industry, baking can be carried out at a temperature of 170°C to 195°C for 10 to 30 minutes.
[0018] Corrosion, evaluated on naturally aged panels. After heat treatment at 170°C for 20 minutes,
[0019] The panels were subjected to filiform corrosion testing to evaluate corrosion. Summary of the invention
[0020] An object of the present invention is an aluminum alloy plate, the composition of which is calculated in weight %:
[0021] Si: about 1.25% to about 1.55%,
[0022] Fe: ≤ about 0.60%,
[0023] Cu: ≤ about 0.37%,
[0024] Mn: about 0.22% - about 0.65%,
[0025] Mg: about 0.25% - about 0.55%,
[0026] Ti: ≤ about 0.15%,
[0027] Cr≤about 0.30%,
[0028] Cr+Mn+Fe: ≤ about 0.90%,
[0029] Zn≤about 0.15%,
[0030] Other elements: each ≤ 0.05%, total ≤ 0.15%,
[0031] Remainder: Al.
[0032] Another object of the present invention is a method for manufacturing an aluminum alloy rolled plate according to the present invention, comprising the following successive steps:
[0033] a. producing an alloy, preferably comprising scrap and waste, preferably clad sheet,
[0034] b. casting the alloy into plates, preferably by semi-continuous vertical casting,
[0035] c. homogenizing the plate at a homogenizing temperature, preferably between 540°C and 580°C, preferably above 550°C,
[0036] d. Hot rolled plate,
[0037] e. Cold rolling of hot rolled sheet,
[0038] f. Solution heat treatment followed by quenching,
[0039] g. pre-aging at a pre-aging temperature of 60 to 100 ° C for 2 to 16 hours, preferably obtained by coiling, and then cooled to room temperature,
[0040] h. Natural aging: 72 hours to 6 months. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] [ Figure 1 ]: This figure shows the LDH depending on recyclability.
[0042] [ Figure 2 ]: This figure shows the LDH depending on the alloy Fe, Mn and Cr contamination.
[0043] [ Figure 3 ]: This figure shows the compromise between LDH and yield strength in the T4 state.
[0044] [ Figure 4 ]: This figure shows the trade-off between LDH and yield strength after paint baking simulation.
[0045] [ Figure 5 ]: This figure shows the yield strength in the T4 state depending on the recyclability of the panel according to the invention.
[0046] [ Figure 6 ]: This figure shows the yield strength after a paint baking simulation as a function of the recyclability of the panels according to the invention.
[0047] [ Figure 7 ]: This figure shows the filiform corrosion depending on the Cu content.
[0048] [ Figure 8 ]: This image shows the LDH measurement tool.
[0049] [ Fig. 9 ]: The board according to the invention makes it possible to recycle the cladding board.
[0050] [ Fig.10 ]: This photo shows an example of samples going through the Luoping line, grades 1, 2 and 3 (1 average - 3 excellent).
[0051] illustrate
[0052] Unless otherwise stated, all aluminum alloys discussed below are named according to the rules and names defined by the Aluminum Association in its periodically published "Register Series". Unless otherwise stated, the composition is expressed in weight %. The expression 1.4Cu means that the copper content expressed in weight % is 1.4%.
[0053] The metallurgical conditions in question are named according to European Standard EN-515.
[0054] The static tensile mechanical properties, in other words the ultimate tensile strength Rm, the conventional yield strength at 0.2% elongation Rp0.2, the shrinkage elongation Ag% and the elongation at break A%, are determined by tensile tests according to NF EN ISO 6892-1, the directions of sampling and testing being defined by EN 485-1.
[0055] The strain hardening factor n is evaluated according to EN ISO 10275.
[0056] The elastic modulus is measured according to ASTM 1876.
[0057] The Lankford anisotropy coefficient is measured according to EN ISO 10113.
[0058] The bending angle, called α range, is determined by a three-point bending test according to NF EN ISO 7438 and VDA 238-100 and VDA 239-200 version 2017 procedures.
[0059] Unless otherwise stated, the definitions in standard EN 12258 apply.
[0060] The LDH parameter is widely used to evaluate the suitability of stamping sheets. It has been the subject of many publications, especially R. Thompson, "The LDH test to evaluate sheet metal formability-Final Report of the LDH Committee of the North American Deep Drawing Research Group", SAE conference, Detroit, 1993, SAE Paper no.930815. This is an example of a stamping test with a blank locked on the periphery by a ring. The blank-clamping pressure is adjusted to prevent slipping in the ring. The blank with dimensions of 120 mm × 160 mm is stressed in a manner close to a planar deformation. The punch used is hemispherical. Figure 8 The dimensions of the tool used to perform this test are shown. Lubrication between the punch and the strip is provided by graphite grease. The punch is lowered at a rate of 50 mm / min. The so-called LDH value is the value of the punch displacement at break, i.e. the limiting depth of the punch. The so-called LDH value actually corresponds to the average of three tests, giving a 95% confidence interval for the 0.2 mm measurement.
[0061] The standard for measuring intergranular corrosion is ASTM G110.
[0062] The standard for filiform corrosion is EN 3665.
[0063] The roping line is measured in the following manner. A strip of about 270 mm (in the transverse direction) x 50 mm (in the rolling direction) is cut from the plate. Subsequently, a traction pre-deformation of 15% is applied perpendicular to the rolling direction (i.e. the length direction of the strip). Subsequently, the strip is subjected to the action of P800 type sandpaper to reveal the roping line. The latter is then visually evaluated and classified by a scale of 1 (significant roping line) to 3 (complete absence of roping line). Fig.10 Examples of Luo Ping lines corresponding to values 1 to 3 are shown in .
[0064] Room temperature is any temperature suitable for human activities, from 5 to 35°C. Room temperature can be 5°C, 6°C, 7°C, 8°C, 9°C, 10°C, 11°C, 12°C, 13°C, 14°C, 15°C, 16°C, 17°C, 18°C, 19°C, 20°C, 21°C, 22°C, 23°C, 24°C, 25°C, 26°C, 27°C, 28°C, 29°C, 30°C, 31°C, 32°C, 33°C, 34°C, 35°C.
[0065] When used in connection with a measurable numerical variable, the term "about" refers to the indicated value of the variable and all values of the variable within the experimental error range of the indicated value, or within ±10% of the indicated value, retaining the highest value. DETAILED DESCRIPTION
[0066] The present invention is based on the Applicant's observation that, thanks to a suitable composition and manufacturing process, it is possible to produce from recycled cladding sheets sheets having acceptable stamping properties, good corrosion resistance and mechanical properties, suitable for the production of automobile bodies.
[0067] A typical composition of the alloy according to the invention is as follows (in wt. %):
[0068] Si: 1.25% - about 1.55%,
[0069] Fe: ≤ about 0.60%,
[0070] Cu: ≤ about 0.37%,
[0071] Mn: 0.22% - about 0.65%,
[0072] Mg: about 0.25% - about 0.55%,
[0073] Ti: ≤ about 0.15%,
[0074] Cr≤about 0.30%,
[0075] Cr+Mn+Fe: ≤ about 0.90%,
[0076] Zn≤about 0.15%,
[0077] Other elements: each ≤ 0.05%, total ≤ 0.15%,
[0078] Remainder: Al.
[0079] Therefore, the concentration range imposed on the constituent elements of such alloys can be explained by the following reasons:
[0080] Si: Silicon, together with magnesium, is the first alloying element to form the intermetallic compounds Mg2Si or Mg5Si6 in the aluminum-magnesium-silicon system (AA6xxx family), which contributes to the structural hardening of these alloys. High silicon content is beneficial for recyclability, considering that certain plates are clad with Si-rich alloys (such as AA4343, AA4045, AA4004 and other alloys), the silicon content of these alloys can reduce the melting point. Relative to the weight percentage of Mg, Si is excessive. Preferably, the excess of silicon is at least 0.70 weight%, more preferably 0.80 weight%, and preferably at most 1.20 weight%, more preferably 1.15 weight%. The purpose of this excess is to improve the ductility required for plate forming, but within the scope of the present invention, the Si content has a small effect on the formability measured by LDH. The Si content is from 1.25% to about 1.55%. In one embodiment, the Si content is up to about 1.35%, preferably about 1.30%. This embodiment makes it possible to have a low value of the yield strength in the T4 state, thereby reducing the punching force. In another embodiment, the Si content is at least about 1.30%, preferably at least about 1.35%, preferably about 1.40%, preferably about 1.45%, and / or a maximum of about 1.50%. This embodiment makes it possible to obtain high values of yield strength after paint baking.
[0081] In one embodiment, the Si content is at least 1.25%, and at most about 1.30%, or at most about 1.35%, or at most about 1.40%, or at most about 1.45%, or at most about 1.50%, or at most about 1.55%. In another embodiment, the Si content is at least about 1.30%, and at most about 1.35%, or at most about 1.40%, or at most about 1.45%, or at most about 1.50%, or at most about 1.55%. In one embodiment, the Si content is at least about 1.35%, and at most about 1.40%, or at most about 1.45%, or at most about 1.50%, or at most about 1.55%. In one embodiment, the Si content is at least about 1.40%, and at most about 1.45%, or at most about 1.50%, or at most about 1.55%. In one embodiment, the Si content is at least about 1.40%, and at most about 1.45%, or at most about 1.50%, or at most about 1.55%. In one embodiment, the Si content is at least about 1.45%, and at most about 1.50%, or at most about 1.55%. In one embodiment, the Si content is at least about 1.50%, and at most about 1.55%.
[0082] Fe: Iron is generally considered an unwanted impurity. The presence of iron-containing intermetallic compounds is generally associated with a reduction in local formability. The maximum Fe content is about 0.60%, preferably about 0.50%, and more preferably about 0.40%. Reducing the Fe content can improve the formability measured by LDH. However, very pure iron alloys are expensive on the one hand, and on the other hand, scrap and waste are naturally contaminated with Fe through mixtures with steel. Therefore, it is preferred that the iron content is at least about 0.05%, preferably about 0.10%, more preferably about 0.15%, and more preferably about 0.20%. According to the present invention, the Fe content must also be controlled in combination with Mn and Cr, taking into account the maximum Cr+Mn+Fe contaminant content: ≤ about 0.90%, in order to control the LDH of the plate.
[0083] In one embodiment, the Fe content is at least about 0.25%, and at most about 0.30%, or at most about 0.35%, or at most about 0.40%, or at most about 0.45%, or at most about 0.50%, or at most about 0.55%, or at most about 0.60%. In one embodiment, the Fe content is at least about 0.30%, and at most about 0.35%, or at most about 0.40%, or at most about 0.45%, or at most about 0.50%, or at most about 0.55%, or at most about 0.60%. In one embodiment, the Fe content is at least about 0.35%, and at most about 0.40%, or at most about 0.45%, or at most about 0.50%, or at most about 0.55%, or at most about 0.60%. In one embodiment, the Fe content is at least about 0.40%, and at most about 0.45%, or at most about 0.50%, or at most about 0.55%, or at most about 0.60%. In one embodiment, the Fe content is at least about 0.45%, and at most about 0.50%, or at most about 0.55%, or at most about 0.60%. In one embodiment, the Fe content is at least about 0.50%, and at most about 0.55%, or at most about 0.60%. In one embodiment, the Fe content is at least about 0.55%, and at most about 0.60%.
[0084] Cu: In the AA6000 family of alloys, copper is an element that participates in hardening precipitation and is beneficial to improving the yield strength of the alloy in the T4 state and after baking. However, Cu is known to reduce corrosion resistance. The Cu content is up to about 0.37%, preferably about 0.32%, preferably about 0.27%, and more preferably 0.25% to ensure an acceptable level of filiform corrosion. Increasing the maximum Cu content can improve the recyclability of clad plates containing Cu, such as the clad plates disclosed in application WO02 / 40729. Increasing the Cu content can also improve the formability characterized by the LDH test. This effect is beneficial because it can increase the contaminant content, especially Mn, because the Cu content increases the LDH, which can compensate for the decreasing effect of the LDH caused by these contaminants. Therefore, in one embodiment, the Cu content is at least about 0.20%. In one embodiment, the Cu content is a maximum of about 0.20%. This embodiment is advantageous because it allows avoiding the addition of Cu, a metal more expensive than aluminum, for recycling Cu-free cladding plates, such as cladding plates whose core portion is made of the reference alloy AA3003, well known to those skilled in the art of cladding plates.
[0085] In one embodiment, the Cu content is at least about 0.05%, and at most about 0.07%, or at most about 0.12%, or at most about 0.17%, or at most about 0.22%, or at most about 0.27%, or at most about 0.32%, or at most about 0.37%. In one embodiment, the Cu content is at least about 0.07%, and at most about 0.12%, or at most about 0.17%, or at most about 0.22%, or at most about 0.27%, or at most about 0.32%, or at most about 0.37%. In one embodiment, the Cu content is at least about 0.12%, and at most about 0.17%, or at most about 0.22%, or at most about 0.27%, or at most about 0.32%, or at most about 0.37%. In one embodiment, the Cu content is at least about 0.17%, and at most about 0.22%, or at most about 0.27%, or at most about 0.32%, or at most about 0.37%. In one embodiment, the Cu content is at least about 0.22%, and at most about 0.27%, or at most about 0.32%, or at most about 0.37%. In one embodiment, the Cu content is at least about 0.27%, and at most about 0.32%, or at most about 0.37%. In one embodiment, the Cu content is at least about 0.32%, and at most about 0.37%.
[0086] Mn: Manganese has a similar effect to iron through its contribution to the precipitation of common intermetallic compounds. Reducing the Mn content can improve the formability measured by LDH. Increasing the maximum Mn content can improve the recyclability of clad sheet scrap and waste. In particular, this can increase the recyclability of clad sheet containing alloys, said alloys including Mn such as AA3003 or the alloys disclosed in application WO02 / 40729. A compromise is a Mn content of at least 0.22% and up to 0.65%, preferably about 0.60%, preferably 0.55%, preferably a minimum Mn content of at least about 0.25%, preferably about 0.30%, preferably about 0.35%, preferably about 0.40%, preferably about 0.44%. Taking into account the maximum Cr+Mn+Fe contaminant content: ≤ about 0.90%, the Mn content must also be controlled in combination with Fe and Cr to control the LDH of the plate of the present invention. Mn may slightly reduce the yield strength in the T4 state, which is undoubtedly due to its contaminant effect and is not relevant to the present invention.
[0087] In one embodiment, the Mn content is at least about 0.22%, and at most about 0.25%, or at most about 0.30%, or at most about 0.35%, or at most about 0.40%, or at most about 0.45%, or at most about 0.50%, or at most about 0.55%, or at most about 0.60%, or at most about 0.65%. In one embodiment, the Mn content is at least about 0.25%, and at most about 0.30%, or at most about 0.35%, or at most about 0.40%, or at most about 0.45%, or at most about 0.50%, or at most about 0.55%, or at most about 0.60%, or at most about 0.65%. In one embodiment, the Mn content is at least about 0.30%, and at most about 0.35%, or at most about 0.40%, or at most about 0.45%, or at most about 0.50%, or at most about 0.55%, or at most about 0.60%, or at most about 0.65%. In one embodiment, the Mn content is at least about 0.35%, and at most about 0.40%, or at most about 0.45%, or at most about 0.50%, or at most about 0.55%, or at most about 0.60%, or at most about 0.65%. In one embodiment, the Mn content is at least about 0.40%, and at most about 0.45%, or at most about 0.50%, or at most about 0.55%, or at most about 0.60%, or at most about 0.65%. In one embodiment, the Mn content is at least about 0.45%, and at most about 0.50%, or at most about 0.55%, or at most about 0.60%, or at most about 0.65%. In one embodiment, the Mn content is at least about 0.50%, and at most about 0.55%, or at most about 0.60%, or at most about 0.65%. In one embodiment, the Mn content is at least about 0.55%, and at most about 0.60%, or at most about 0.65%. In one embodiment, the Mn content is at least about 0.60%, and at most about 0.65%.
[0088] Mg: Generally, the mechanical property level of AA6xxx family alloys increases with increasing magnesium content, which combines with silicon to form intermetallic compounds Mg2Si or Mg5Si6, which is beneficial for reducing the thickness of the plate and making the vehicle lighter, especially after annealing the paint. Magnesium helps to increase the yield strength in the T4 state, thereby increasing the punching force, and also helps to increase the yield strength after the paint is baked, which can make the body parts lighter. In particular, Mg enhances the response to the paint baking, which is the difference between the yield strength after the paint baking and the yield strength in the T4 state. Mg is about 0.25% to about 0.55%. In one embodiment, Mg is at least about 0.30%, preferably about 0.35%, and / or up to about 0.50%, preferably about 0.45%. Limiting the Mg content can maintain a low yield strength in the T4 state, which promotes formability by avoiding excessive punching forces. In one embodiment, Mg is about 0.45%, preferably about 0.50%. Adding Mg can improve the response to the paint baking to obtain a higher yield strength after the paint baking. Increasing the Mg content can improve the recyclability of the clad plate, especially the clad plate containing Mg in the cladding, such as AA4004, or the clad plate containing Mg in the core part, such as certain alloys disclosed in patent FR2797454.
[0089] In one embodiment, the Mg content is at least about 0.25%, and at most about 0.30%, or at most about 0.35%, or at most about 0.40%, or at most about 0.45%, or at most about 0.50%, or at most about 0.55%. In one embodiment, the Mg content is at least about 0.30%, and at most about 0.35%, or at most about 0.40%, or at most about 0.45%, or at most about 0.50%, or at most about 0.55%. In one embodiment, the Mg content is at least about 0.35%, and at most about 0.40%, or at most about 0.45%, or at most about 0.50%, or at most about 0.55%. In one embodiment, the Mg content is at least about 0.40%, and at most about 0.45%, or at most about 0.50%, or at most about 0.55%. In one embodiment, the Mg content is at least about 0.45%, and at most about 0.50%, or at most about 0.55%. In one embodiment, the Mg content is at least about 0.45%, and at most about 0.50%, or at most about 0.55%. In one embodiment, the Mg content is at least about 0.50%, and at most about 0.55%.
[0090] Cr: It is added to refine the grains and stabilize the structure. Reducing the Cr content can improve the formability measured by LDH, due to its contaminant effect. High contents can improve the recyclability of the alloy of the present invention. In fact, scrap and waste can be contaminated by steel mixtures containing Cr. Cr is up to about 0.30%. The compromise between formability and recyclability is Cr+M+Fe≤about 0.90%. In one embodiment, in order to improve formability, Cr is up to about 0.20%, preferably about 0.15%, preferably about 0.10%, preferably about 0.05%. In one embodiment, Cr is an impurity.
[0091] Ti: The maximum content is about 0.15%, preferably 0.10%, to avoid the formation of primary phases during vertical casting, which has a negative impact on all the claimed properties. This element facilitates solid solution hardening to achieve the required level of mechanical properties, and this element also has a favorable effect on service ductility and corrosion resistance. In one embodiment, the Ti content is up to about 0.01%.
[0092] In one embodiment, the Ti content is at most about 0.05%, or at most about 0.10%, or at most about 0.15%. In one embodiment, the Ti content is at least about 0.01%, and at most about 0.05%, or at most about 0.10%, or at most about 0.15%.
[0093] Zn: The content is up to about 0.15%. Since Zn is an alloying element in aluminum alloys, it is advantageous to accept Zn in order to recycle aluminum scrap or waste, especially aluminum scrap and waste from scrapped vehicles. In fact, Zn is used in certain cladding alloys of certain cladding plates, especially AA7072 with a cladding thickness of 10%. Application WO02 / 55256 discloses another Zn-containing cladding alloy. Taking into account the Zn content of AA7072 or the alloy of the above application, this content is not limited to the use of this cladding plate for the production of the alloy according to the present invention. However, Zn is known for its sensitivity to corrosion. Therefore, limiting the Zn content can improve corrosion resistance. In a preferred embodiment, Zn is up to about 0.10%. In one embodiment, Zn is up to about 0.05%. In one embodiment, Zn is an impurity.
[0094] Typically, other elements are impurities, and their content is kept at less than or equal to 0.05%, preferably strictly less than 0.05%, and less than 0.15% in total; the balance is aluminum.
[0095] The contaminant content of Fe, Mn and Cr must be controlled. The term contamination is used to indicate that these elements may be present in the alloy according to the present invention in some cases due to recycling. However, without being bound by any theory, the inventors have found that their effect is not harmful and may have an unexpectedly favorable effect on the properties obtained in the claimed proportions. Increasing the contamination content can improve recyclability. Reducing the contamination content can increase the LDH. Preferably, the compromise is a contaminant content from at least about 0.64% to at most about 0.90%. In one embodiment, the contaminant content is about Cu+0.41% to about Cu+0.59%, preferably about 0.45%+Cu to about 0.55%+Cu. This embodiment is advantageous because it can maintain high LDH values. In a more preferred embodiment, the contaminant content is greater than about 0.70%, which can improve the recyclability of the copper-containing clad plate.
[0096] In one embodiment, the plate according to the present invention has an LDH less than or equal to 26.0 mm. The LDH is measured with a 1 mm thick plate in the T4 state. Limiting the LDH is a compromise, which can improve the recyclability of the plate according to the present invention. Limiting the LDH is a compromise, which can increase the amount of contaminants in the plate according to the present invention. Limiting the LDH is a compromise, which can increase the yield strength of the plate according to the present invention in the T4 state and after painting. In one embodiment, the plate according to the present invention has an LDH greater than or equal to 24.0 mm, preferably greater than or equal to 24.5 mm, more preferably greater than or equal to 25.0 mm, more preferably greater than or equal to 25.5 mm. Increasing the LDH value can increase the formability of the stamping.
[0097] In one embodiment, the board according to the present invention has a minimum yield strength Rp0.2 of 100 MPa, preferably 110 MPa, more preferably 115 MPa in the T4 state and / or has a maximum yield strength Rp0.2 of 150 MPa, preferably 145 MPa, more preferably 140 MPa in the T4 state. Too low a yield strength in the T4 state will limit the yield strength after baking paint. Too high a yield strength in the T4 state will increase the punching force. Limiting the maximum yield strength in the T4 state is a compromise, which can improve the formability measured by LDH. In a sub-embodiment, the yield strength Rp0.2 in the T4 state is at most 135 MPa. This sub-embodiment is a compromise, which can increase recyclability.
[0098] In one embodiment, the board according to the invention has a minimum yield strength Rp0.2 of 200 MPa, preferably 210 MPa after baking and / or a maximum yield strength Rp0.2 of 250 MPa, preferably 240 MPa after baking. Increasing the yield strength after baking is advantageous in reducing the thickness of the component. In a sub-embodiment, the yield strength after baking is at most 220 MPa, preferably 215 MPa. This sub-embodiment is a compromise, which can increase recyclability.
[0099] In a preferred embodiment, the panels according to the invention have excellent filiform corrosion resistance after painting and baking, less than about 0.25 cm on average according to EN 3665. Painting includes all operations known per se, surface treatment, electrophoresis and painting. Baking, also known as baking hardening, can be simulated by a treatment at 170° C. for 20 minutes.
[0100] The method for manufacturing a plate according to the invention comprises the casting of the plate, preferably by vertical semi-continuous casting, followed by homogenization thereof.
[0101] The plate is cast with an alloy according to the aforementioned composition. The alloy is preferably partially produced with waste and waste, preferably clad plate. This clad plate waste and waste can also be a finished product to be recycled (old waste according to EN 12258-1), a part of which is made of clad plate. This is advantageous because these finished products are usually also made of very different alloy components, and it is not necessary to coat all components, such as 3xxx series alloys and Zn-containing alloys, such as 7xxxx series alloys or alloys disclosed in application EP1446511. Cladding plate waste and waste can be used directly or indirectly to produce the alloy. When clad plate waste and waste are coated with paint or varnish, or when clad plate waste and waste are equipped with plastic parts, indirect use is advantageous. In these cases, it is preferably remelted in a professional unit known to technicians in the recycling field, where coatings or plastic parts will be properly handled, such as by filtering smoke. Direct use is advantageous because it is easy and economical to organize, because it includes directly charging waste and waste into a melting furnace to produce alloys.
[0102] The recyclability is evaluated in the following way. First, for each element, it is necessary to calculate, estimate or measure the average composition of the scrap or waste, preferably clad sheet. Then, for each element, the ratio of the maximum value of the alloy of the sheet according to the invention to the percentage of the content of this element in the average composition of the clad sheet scrap and waste is calculated. The recyclability is the minimum between all these ratios. Therefore, this recyclability is the maximum value of the clad sheet scrap and waste that can be added to the sheet alloy according to the invention, the composition of the sheet alloy according to the invention being obtained by adding raw aluminum and / or alloying elements.
[0103] Increasing recyclability can reduce the amount of CO2 equivalent emitted for cast plate. Preferably, the plate is produced with at least 10% scrap and waste, preferably at least 20%, preferably at least 30%, preferably at least 39%, preferably at least 46%, preferably at least 48%. In one embodiment, up to 45% recyclability is a compromise that can increase the yield strength in the T4 state or after paint baking.
[0104] Preferred dimensions of the panels according to the invention are a thickness of 200 to 600 mm, a width of 1,000 to 3,000 mm and a length of 2,000 to 8,000 mm.
[0105] The plate is usually homogenized to a homogenization temperature above the alloy solvus temperature while avoiding local melting or incipient melting for a minimum of 2 hours, preferably 3 hours, more preferably 4 hours, and a maximum of 7 hours, preferably 6 hours, more preferably 5 hours. The homogenization temperature is preferably at most 580°C, preferably 570°C, preferably 560°C, more preferably 555°C, and at least 540°C, preferably 550°C. Too high or too low a temperature will reduce the mechanical properties of the plate.
[0106] The plate is then transferred to a hot roller. Optionally, it is transferred directly from homogenization to hot rolling, during which the temperature can naturally drop by 5°C to 35°C. Optionally, the plate is cooled from the homogenization temperature to the hot rolling start temperature by forced cooling. This forced cooling is preferably carried out at a direct cooling rate of at least 150°C per hour. Advantageously, the direct cooling rate is at most 500°C / hour. Cooling can generally be achieved by a machine such as that described in application WO2016012691. Preferably, this cooling is accomplished in two steps, one being spraying and the other being homogenization. Optionally, this cooling can be achieved in two steps by a machine such as that described in application WO2016012691.
[0107] The homogenized plate is then typically hot rolled to a thickness of 4 mm (preferably 3 mm) to 8 mm. The temperature at the start of hot rolling is typically 520 to 550°C. Optionally, the hot rolling temperature after cooling is 390°C to 510°C or 490°C or 470°C or 450°C or 430°C or 410°C. Optionally, the hot rolling temperature after cooling is 410°C to 510°C or 490°C or 470°C or 450°C or 430°C. Optionally, the hot rolling temperature after cooling is 430°C to 510°C or 490°C or 470°C or 450°C. Optionally, the hot rolling temperature after cooling is 450°C to 510°C or 490°C or 470°C. Optionally, the hot rolling temperature after cooling is 470°C to 510°C or 490°C. Optionally, the hot rolling temperature after cooling is 490°C to 510°C.
[0108] The temperature variation between the start and the end of hot rolling is due to the cooling of the plate by normal heat exchange with the air at room temperature of the plant, to the thermal equipment of the rolling mill, such as, without limitation, the cylinders of the conveyor rollers, and to the usual lubricating or cooling fluids and to the heating associated with the deformation energy. Preferably, the end temperature of hot rolling is preferably between 350°C and 450°C.
[0109] The hot rolled sheet is then cold rolled, usually to a sheet thickness of 0.7 to 1.5 mm. Intermediate annealing can also be carried out between two cold rolling steps. Annealing can be carried out in a static furnace or a continuous furnace.
[0110] The plate is then solution heat treated at a solution temperature above the solvus temperature of the alloy while avoiding local melting or incipient melting, and then quenched, preferably in a continuous furnace. Too cold a solution heat treatment and / or too short a solution heat treatment time may reduce the mechanical properties of the plate due to inadequate solution heat treatment. Too hot a solution heat treatment may result in incipient melting, reducing the mechanical properties. Too long a solution heat treatment time reduces productivity. Preferably, the solution heat treatment lasts from 15 seconds to 300 seconds. The solution heat treatment temperature is preferably at least 530°C and at most 570°C.
[0111] The plate is then quenched with water or air or a continuous combination of water or air at a rate typically exceeding 30°C / s and preferably at least 100°C / s. Preferably, the plate is quenched to 60 to 100°C. Insufficient cooling rates will reduce the mechanical properties of the plate because the solution heat treatment is incomplete.
[0112] The sheet is then heated for pre-aging at a pre-aging temperature of 60°C to 100°C for 2 to 16 hours. Heating is useful when the sheet undergoes a surface treatment between quenching and pre-aging at a temperature lower than the pre-aging. Preferably, the pre-aging is obtained by coiling and then cooling to room temperature, preferably for at least 40 hours. Pre-aging can improve the response to paint baking, i.e. the difference between the yield strength in the T4 state and the yield strength after paint baking.
[0113] The pre-aged panels are in the T4 temper and are subsequently naturally aged at room temperature for 72 hours to 6 months. This step is a limitation associated with storage before forming. Despite the natural aging, the panels according to the invention can still be formed.
[0114] The panels according to the invention are advantageously used for the production of automotive body parts. In one embodiment, the panels according to the invention are panels for linings, such as door linings or hood linings. For automotive parts, in particular linings, the thickness is 0.7 to 1.5 mm. A thickness of less than 0.7 mm will not ensure the rigidity of the element containing the lining. A thickness of more than 1.5 mm would make the element containing the lining too heavy for the user and the vehicle. Since the lining is not a visible component on the outside of the vehicle, the surface condition of the lining panel in the delivery state and after painting is not comparable to the surface condition of the external parts of the vehicle body. In one embodiment, the roping line of the panel according to the invention is optimally 1.
[0115] Example
[0116] The present disclosure is further illustrated by the following examples. These examples are intended only to illustrate the present invention, not to limit it.
[0117] Plates of various compositions were cast according to the alloys in Table 1. Alloy A is a typical alloy of application US20210108293. Alloy B is a typical production alloy providing body panels made of AA6016 alloy. In Table 1, examples according to the invention are marked with E and comparative examples are marked with CE.
[0118] [Table 1]
[0119] Si Fe Cu Mn Mg Cr Ti Zn Fe+Mn+Cr A CE 2.32 0.29 0.18 0.49 0.48 0.01 0.05 0.78 B CE 1.11 0.22 0.13 0.12 0.44 0.01 0.05 0.35 C CE 1.54 0.24 0.42 0.55 0.38 0.01 0.06 0.80 D CE 1.49 0.25 0.19 0.56 0.70 0.01 0.05 0.81 E CE 1.56 0.23 0.64 0.54 0.38 0.01 0.06 0.78 F CE 1.51 0.25 0.42 0.56 0.73 0.01 0.05 0.83 G CE 1.89 0.24 0.42 0.89 0.42 0.01 0.05 1.14 H CE 1.50 0.49 0.17 0.59 0.41 0.01 0.05 1.09 I CE 1.47 0.49 0.38 0.58 0.41 0.05 0.05 1.12 J CE 1.91 0.24 0.61 0.53 0.41 0.01 0.05 0.78 K E 1.28 0.23 0.25 0.52 0.35 0.001 0.01 <0.01 0.75 L E 1.47 0.23 0.24 0.52 0.34 0.001 0.01 <0.01 0.75 M E 1.48 0.24 0.20 0.44 0.36 0.001 0.01 <0.01 0.68 N E 1.27 0.24 0.20 0.44 0.45 0.001 0.01 <0.01 0.68 O E 1.41 0.26 0.18 0.50 0.37 0.010 0.05 0.77 P E 1.39 0.26 0.23 0.49 0.38 0.010 0.05 0.76
[0120] Recyclability was evaluated with a clad board as disclosed in application WO 02 / 40729, by selecting 10% of the cladding on each surface of the central part. In order to recycle this board, the average composition of the clad board was calculated as shown in the following table.
[0121] [Table 2]
[0122] Si Fe Cu Mn Mg Cr Ti Zn Center 0.19 0.19 0.62 1.33 0.01 0.002 0.09 0.039 Cladding 7.21 0.25 0.08 Average composition 1.59 0.20 0.50 1.08 0.01 0.002 0.07 0.03
[0123] The recyclability of the various alloys A to P was evaluated by calculating the maximum amount of the average composition of each element in Table 2 below. Values above 100% mean that the cladding plate does not provide the amount of the element in question, so there is no restriction on the introduction of the cladding plate to produce the alloy of the element in question. Values below 100% mean that the cladding plate provides too much of the element in question, so the introduction of cladding plate must be limited to produce the alloy. Therefore, in order to determine the recyclability of each alloy evaluated, it is necessary to consider only the minimum value of all its elements. For Cr and Ti, the calculated recyclability is not calculated with the Ti and Cr content of the test alloy, but with a value of 0.05%, which corresponds to the conventional maximum value of 0.05% for impurities.
[0124] [Table 3]
[0125] Si Fe Cu Mn Mg Cr Ti Recyclability A >100% >100% 36% 45% >100% >100% 69% 36% B 70% >100% 25% 11% >100% >100% 69% 11% C 94% 100% 84% 51% >100% >100% 69% 51% D 94% 100% 38% 52% >100% >100% 69% 38% E >100% 100% >100% 50% >100% >100% 69% 50% F 94% >100% 84% 52% >100% >100% 69% 52% G >100% 100% 84% 82% >100% >100% 69% 69% H 94% >100% 35% 54% >100% >100% 69% 35% I >100% 100% >100% 49% >100% >100% 69% 49% J 94% >100% 76% 54% >100% >100% 69% 54% K 81% >100% 49% 48% >100% >100% 69% 48% L 92% >100% 48% 48% >100% >100% 69% 48% M 93% >100% 40% 41% >100% >100% 69% 40% N 80% >100% 39% 41% >100% >100% 69% 39% O 89% >100% 36% 46% >100% >100% 71% 36% P 87% >100% 46% 45% >100% >100% 71% 45%
[0126] Plates A to N were homogenized at 555°C for 4 hours and then hot rolled at a thickness of 6 mm with a hot rolling start temperature of 550°C and then cold rolled to 1 mm thick plates. These plates were then solution heat treated at a temperature above 530°C for 15 seconds and then quenched to 60°C. The plates were then pre-aged at 80°C for 16 hours.
[0127] Plates O and P were homogenized at 560°C for 2 hours and then forced cooled at a hot rolling start temperature of 400°C. The plates were cold rolled to a thickness of 3 mm at a temperature of 305°C. The plates were then cold rolled to a thickness of 1.2 mm and then solution heat treated at a PMT (peak metal temperature) of 560°C and then quenched. Pre-aging was then carried out by heating to a temperature of 65°C and then by coiling and then naturally cooling to room temperature.
[0128] Mechanical properties tests were carried out in the T4 state. The results are shown in Table 4. The last column is the yield strength of these samples after 7 days of natural aging after a paint simulation (bake hardening or BH) heat treatment at 170°C for 20 minutes. The TL direction is the direction transverse to the rolling direction.
[0129] [Table 4]
[0130]
[0131] Figure 1 It is shown that boards K, L, M, N, O and P according to the invention are a good compromise between formability and recyclability. In fact, board B is slightly better in formability, but has very low recyclability. Other boards may have better recyclability, but with a much reduced formability.
[0132] Figure 2 It is shown that plates K, L, M, N, O and P according to the invention are a good compromise between formability and Fe, Cr and Mn contamination levels. In fact, plate B is slightly better in terms of formability, but uses a high purity alloy with a low contaminant content. The other plates have higher Fe, Cr and Mn contaminant levels, but the formability is greatly reduced.
[0133] Figure 3 and Figure 4 The compromise between LDH (formability) and Rp0.2 in the T4 state (forming force) and the compromise between LDH and Rp0.2 after the paint baking simulation (BH or bake hardening) are shown. Plates K, L, M, N, O and P have a better compromise than the other plates (except plate B, but plate B does not comply with the invention because it has a lower content of Mn, one of the contaminants). Plates K and L have a similar formability level to plates M and N due to the Cu content compensating the Mn+Cr+Fe contamination level.
[0134] Figure 5 Two different favorable compromises between recyclability and yield strength in the T4 state and after painting are shown. Panel N has better yield strength in the T4 state and after painting, and slightly lower recyclability. Panel L has better recyclability in the T4 state and after painting, and slightly lower yield strength.
[0135] Since boards K and L have a higher Mn content than boards M and N, they have better recyclability.
[0136] Plate N is able to achieve the best yield strength after paint baking by increasing Mg relative to Plate M, while reducing Si content to maintain the yield strength in the T4 state comparable to Plate M. Mn content less than 0.50% can compensate for the hardening effect in the T4 state to maintain the LDH level.
[0137] Plates A to P were subjected to filiform corrosion tests according to standard EN3665. For this purpose, the samples were subjected to surface and paint treatments known to those skilled in the art. The samples were subsequently subjected to a paint baking heat treatment at 170°C for 20 minutes. The specimens were then scratched in the longitudinal direction of rolling (L) and in the long transverse direction perpendicular to the rolling direction (TL). The results of the filiform corrosion tests are shown in the following table.
[0138] [Table 5]
[0139] Ref Average value in TL direction (cm) Average value in L direction (cm) A 0.12 0.09 B 0.22 0.16 C 0.54 0.36 D 0.21 0.16 E 0.65 0.46 F 0.74 0.49 G 0.70 0.38 H 0.09 0.08 I 0.72 0.46 J 0.47 0.29 K 0.19 0.11 L 0.11 0.08 M 0.21 0.12 N 0.19 0.11 O 0.19 0.14 P 0.22 0.18
[0140] Only samples A, B, D, H, K, L, M, N, O, and P, whose copper contents were less than 0.37%, showed filiform corrosion with an average length of less than 0.25 cm.
[0141] Panels B, H, K, L, M, N, O, and P were also characterized after 90 days of natural aging. These panels were still not very sensitive to natural aging.
[0142] [Table 6]
[0143]
Claims
1. Aluminum alloy plate, the composition of which is expressed in weight % as follows: Si: 1.25% - about 1.55%, Fe: ≤ about 0.60%, Cu: ≤ about 0.37%, Mn: 0.22% - about 0.65%, Mg: about 0.25% - about 0.55%, Ti: ≤ about 0.15%, Cr≤about 0.30%, Cr+Mn+Fe: ≤ about 0.90%, Zn≤about 0.15%, Other elements: each ≤ 0.05%, total ≤ 0.15%, Remainder: Al.
2. The plate according to claim 1, characterized in that Cu is ≤ about 0.32%, preferably about ≤ 0.27%, more preferably ≤ 0.25%.
3. The plate according to claim 1 or 2, characterized in that Mn≥ about 0.30%, preferably about ≥ 0.35%, preferably about ≥ 0.40%, and / or Mn is about ≤ 0.60%, preferably about ≤ 0.55%.
4. A plate according to any one of claims 1 to 3, characterized in that Mg≥ about 0.30%, preferably about ≥ 0.35% and / or Mg≤ about 0.50%, preferably about ≤ 0.45%.
5. The plate according to any one of claims 1 to 4, characterized in that Cr ≤ about 0.15%, preferably ≤ about 0.10%, preferably ≤ about 0.05%.
6. A plate according to any one of claims 1 to 5, characterized in that Ti≤about 0.10%, preferably Ti≤about 0.05% or Ti≥about 0.01%.
7. A plate according to any one of claims 1 to 6, characterized in that Zn≤about 0.10%, preferably Zn≤about 0.05%.
8. A plate according to any one of claims 1 to 7, characterised in that Si ≤ about 1.50% and / or ≥ about 1.30%; preferably about ≥ 1.35%, preferably about ≥ 1.40%.
9. A plate according to any one of claims 1 to 8, characterised in that The LDH of the plate is less than or equal to 26.0 mm and / or greater than or equal to 24.0 mm, preferably greater than or equal to 24.5 mm, preferably greater than or equal to 25.0 mm, the LDH being measured with a plate having a thickness of 1 mm in the T4 state.
10. A plate according to any one of claims 1 to 9, characterised in that The minimum yield strength Rp0.2 of the plate in the T4 state is 100 MPa, preferably 110 MPa, more preferably 115 MPa and / or the maximum yield strength Rp0.2 in the T4 state is 150 MPa, preferably 145 MPa, more preferably 140 MPa.
11. A method for manufacturing a panel according to any one of claims 1 to 10, comprising the following consecutive steps: a. producing an alloy, preferably comprising scrap and waste, preferably clad sheet, b. casting the alloy into plates, preferably by semi-continuous vertical casting, c. homogenizing the plate at a homogenizing temperature, preferably at 540°C to 580°C, preferably at 550°C to 580°C, d. Hot rolled plate, e. Cold rolling of hot rolled sheet, f. Solution heat treatment followed by quenching, g. pre-aging at a pre-aging temperature of 60 to 100 ° C for 2 to 16 hours, preferably obtained by coiling, and then cooled to room temperature, h. Natural aging: 72 hours to 6 months.
Citation Information
Cited By
Medium-strength 7xxx series recycled aluminum alloy parts with high recycled material ratio and their preparation method
TWI934433B