Photosensitive resin film, printed wiring board, semiconductor package, and method for manufacturing printed wiring board
By introducing specific components into the photosensitive resin film and controlling the difference in fluorine atom concentration, the problem of balancing dielectric properties and conductor adhesion was solved, enabling efficient and low-cost manufacturing of printed wiring boards.
Patent Information
- Application Number
- CN202380030798.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-31
- Filing Date
- 2023-03-30
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing technologies struggle to balance dielectric properties and conductor adhesion in the manufacture of high-density printed wiring boards, especially when using fluorinated resins, which result in decreased adhesive strength, low efficiency in via formation, and high costs.
A photosensitive resin film containing olefinic unsaturated compounds, thermosetting resin, inorganic filler, fluorinated resin and photopolymerization initiator is used. By controlling the difference in fluorine atom concentration, an interlayer insulating layer with excellent dielectric properties and conductor adhesion is formed, and small-diameter through holes are formed by photolithography.
This invention enables printed wiring boards with low high-frequency signal transmission loss, improves the adhesion strength between conductors and copper plating, reduces manufacturing costs, and increases manufacturing efficiency.
Smart Images

Figure CN118946852A_ABST
Abstract
Description
Technical Field
[0001] The present disclosure relates to a photosensitive resin film, a printed wiring board, a semiconductor package, and a method for producing the printed wiring board. Background Art
[0002] In recent years, electronic devices have been miniaturized and improved in performance, and printed wiring boards have been increasingly densified due to the increase in the number of circuit layers and the miniaturization of wiring. In particular, semiconductor packages such as BGA (ball grid array) and CSP (chip size package) equipped with semiconductor chips have become more and more dense. Therefore, printed wiring boards require not only miniaturization of wiring, but also thinning of interlayer insulation layers and reduction of the diameter of through holes used for interlayer connections.
[0003] As a method for manufacturing a printed wiring board that has been used in the past, there can be cited a method for manufacturing a multilayer printed wiring board based on a build-up method (for example, see Patent Document 1) in which an interlayer insulating layer and a conductor circuit layer are stacked in sequence. In a multilayer printed wiring board, as circuits become more miniaturized, a semi-additive method for forming circuits by plating has become the mainstream. In the conventional semi-additive method, a thermosetting resin film is used to form an interlayer insulating layer.
[0004] Laser processing is the mainstream method for forming through holes in an interlayer insulating layer formed of a thermosetting resin film. However, the reduction in the diameter of through holes using laser processing is reaching its limit. In addition, in the formation of through holes based on laser processing, each through hole needs to be formed one by one. Therefore, in the case where a plurality of through holes need to be formed due to high density, the formation of the through holes requires a lot of time, and there are problems such as high manufacturing cost and poor manufacturing efficiency.
[0005] Under such circumstances, a method of collectively forming a plurality of small-diameter through holes by photolithography using a photosensitive resin film has been proposed (for example, refer to Patent Document 2).
[0006] Prior art literature
[0007] Patent Literature
[0008] Patent Document 1: Japanese Patent Application Laid-Open No. 7-304931
[0009] Patent Document 2: Japanese Patent Application Publication No. 2017-116652 Summary of the invention
[0010] Problems to be solved by the invention
[0011] However, in recent years, the signals used in electronic devices have been increasingly being used at higher speeds and with higher capacity. As a result, printed wiring board substrate materials are required to have dielectric properties that can reduce the transmission loss of high-frequency signals [hereinafter sometimes referred to as "high-frequency properties"]. That is, low relative dielectric constant and low dielectric loss tangent.
[0012] In order to improve the dielectric properties of the substrate material, the inventors have studied the use of a fluorine-containing resin with a low relative dielectric constant in the photosensitive resin film used to form the interlayer insulating layer. However, if the photosensitive resin film is simply made to contain a fluorine-containing resin, even if the relative dielectric constant of the interlayer insulating layer can be reduced, the adhesion of the conductor, especially the bonding strength with the copper plating layer, will also be reduced. Therefore, it is difficult to achieve both excellent dielectric properties and conductor adhesion.
[0013] In view of such a situation, an object of the present embodiment is to provide a photosensitive resin film capable of forming an interlayer insulating layer having excellent dielectric properties and conductor adhesion, a printed wiring board using the photosensitive resin film, a method for producing the same, and a semiconductor package.
[0014] Means for solving problems
[0015] The present inventors have studied to solve the above-mentioned problems, and as a result, have found that the above-mentioned problems can be solved by the present embodiment described below.
[0016] That is, this embodiment relates to the following [1] to
[12] .
[0017] [1] A photosensitive resin film comprising: (A) a compound having an ethylenically unsaturated group, (B) a thermosetting resin, (C) a photopolymerization initiator, (D) an inorganic filler, and (E) a fluorine-containing resin,
[0018] The photosensitive resin film has a first surface and a second surface opposite to the first surface.
[0019] The fluorine atom concentration at a depth of 1 μm from the first surface is lower than the fluorine atom concentration at a depth of 1 μm from the second surface.
[0020] [2] The photosensitive resin film according to the above [1], comprising a compound having an ethylenically unsaturated group and an acidic substituent as the (A) compound having an ethylenically unsaturated group.
[0021] [3] The photosensitive resin film according to [1] or [2], comprising at least one selected from the group consisting of epoxy resins, maleimide resins, allyl resins, and vinyl resins as the (B) thermosetting resin.
[0022] [4] The photosensitive resin film according to any one of [1] to [3] above, comprising silicon dioxide as the inorganic filler (D), wherein the content of the silicon dioxide is 2 to 60% by mass.
[0023] [5] The photosensitive resin film according to any one of [1] to [4] above, comprising a film having a true density of 1,500 kg / m or less. 3 Silica is used as the above-mentioned (D) inorganic filler.
[0024] [6] The photosensitive resin film according to any one of [1] to [5] above, wherein the content of the fluorine-containing resin (E) is 5 to 80% by mass based on the total amount of the resin components of the photosensitive resin film.
[0025] [7] The photosensitive resin film according to any one of [1] to [6] above, further comprising (F) an elastomer.
[0026] [8] The photosensitive resin film according to any one of [1] to [7] above, wherein the first surface is a surface on which a circuit pattern is formed by copper plating, and the second surface is a pasting surface when the photosensitive resin film is laminated.
[0027] [9] The photosensitive resin film according to any one of [1] to [8], which is used for forming an interlayer insulating layer having an optical through hole.
[0028]
[10] A printed wiring board having an interlayer insulating layer which is a cured product of the photosensitive resin film according to any one of [1] to [9] above.
[0029]
[11] A semiconductor package comprising the printed wiring board described in
[10] above.
[0030]
[12] A method for manufacturing a printed wiring board, comprising the following (1) to (4).
[0031] (1): The photosensitive resin film according to any one of the above [1] to [9] is laminated on one or both surfaces of a circuit board in a state where the second surface serves as an attachment surface.
[0032] (2): The photosensitive resin film laminated in the above (1) is exposed and developed to form an interlayer insulating layer having a through hole.
[0033] (3): The interlayer insulating layer having the through-hole is heated and cured.
[0034] (4) A circuit pattern is formed on a surface of the interlayer insulating layer opposite to the circuit substrate.
[0035] Effects of the Invention
[0036] According to the present embodiment, a photosensitive resin film capable of forming an interlayer insulating layer having excellent dielectric properties and conductor adhesion, a printed wiring board using the photosensitive resin film, a method for producing the same, and a semiconductor package can be provided. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] [ Figure 1 ] is a schematic diagram showing one method of manufacturing a printed wiring board using the photosensitive resin film of the present embodiment as a material for an interlayer insulating layer.
[0038] [ Figure 2 ] is a cross-sectional SEM image for illustrating the measurement position of the fluorine atom concentration. DETAILED DESCRIPTION
[0039] In the numerical range described in this specification, the lower limit and upper limit of the numerical range can be replaced by the values shown in the embodiments. In addition, the lower limit and upper limit of the numerical range can be arbitrarily combined with the lower limit or upper limit of other numerical ranges. In the expression of the numerical range "AA to BB", the numerical values AA and BB at both ends are included in the numerical range as the lower limit and upper limit, respectively.
[0040] In this specification, for example, a statement such as "greater than or equal to 10" refers to 10 and a value greater than 10, and this applies even if the values are different. In addition, for example, a statement such as "less than or equal to 10" refers to 10 and a value less than 10, and this applies even if the values are different.
[0041] In the present specification, when there are plural substances corresponding to each component, the content of each component refers to the total content of the plural substances unless otherwise specified.
[0042] In this specification, "solid content" refers to non-volatile components other than volatile substances such as solvents. That is, "solid content" refers to components that remain when the resin composition is dried without evaporation, and also includes components that are liquid, syrupy, and waxy at room temperature. Here, in this specification, room temperature refers to 25°C.
[0043] In the present specification, the "ring carbon number" refers to the number of carbon atoms required to form a ring, and does not include the number of carbon atoms of substituents possessed by the ring. For example, the number of ring carbon atoms of a cyclohexane skeleton and a methylcyclohexane skeleton are both 6.
[0044] The expression "(meth)acrylate XX ester" refers to one or both of acrylate XX ester and the corresponding methacrylate XX ester. In addition, "(meth)acryloyl group" refers to one or both of acryloyl group and methacryloyl group.
[0045] In this specification, when a "layer" such as an interlayer insulating layer is expressed as a "layer", in addition to a solid layer, a layer in which a part is not a solid layer but is island-shaped, a layer with holes, and a layer in which the interface with the adjacent layer is unclear are also included in the "layer".
[0046] The action mechanism described in this specification is a guess, and does not limit the mechanism by which the effects of the present embodiment are achieved.
[0047] A mode in which the matters described in this specification are arbitrarily combined is also included in this embodiment.
[0048] [Photosensitive resin film]
[0049] The photosensitive resin film of this embodiment contains: (A) a compound having an ethylenically unsaturated group, (B) a thermosetting resin, (C) a photopolymerization initiator, (D) an inorganic filler, and (E) a fluorine-containing resin.
[0050] The photosensitive resin film has a first surface and a second surface opposite to the first surface.
[0051] The fluorine atom concentration at a depth of 1 μm from the first surface is lower than the fluorine atom concentration at a depth of 1 μm from the second surface.
[0052] In addition, in this specification, each component may be appropriately abbreviated as "(A) component", "(B) component" or the like.
[0053] In the following description, the fluorine atom concentration at a depth of 1 μm from the first surface is sometimes referred to as “fluorine atom concentration at the first surface”, and the fluorine atom concentration at a depth of 1 μm from the second surface is sometimes referred to as “fluorine atom concentration at the second surface”.
[0054] The photosensitive resin film of this embodiment can form a pattern such as a through hole by exposure and development. Therefore, the photosensitive resin film of this embodiment is suitable for forming an interlayer insulating layer having a through hole. It should be noted that in this specification, "through hole" refers to a through hole formed by photolithography, that is, exposure and development.
[0055] The thickness of the entire photosensitive resin film of the present embodiment is not particularly limited, and may be, for example, 2 μm to 110 μm, 4 μm to 60 μm, or 7 μm to 50 μm.
[0056] <Fluorine Atom Concentration>
[0057] In the photosensitive resin film of this embodiment, the fluorine atom concentration on the first surface is lower than that on the second surface. Therefore, the interlayer insulating layer formed by curing the photosensitive resin film of this embodiment exhibits high bonding strength with the copper plating on the first surface.
[0058] The reasons can be inferred as follows. (E) Fluorine-containing resin is difficult to dissolve in the roughening process before forming the copper plating layer compared with other resin components due to its high alkali resistance. Therefore, for a surface containing a large amount of (E) fluorine-containing resin, it is believed that after the roughening process, a large amount of dissolved residual (E) fluorine-containing resin is exposed on the surface, which becomes the main reason for the reduced adhesion to the copper plating layer. In contrast, in the photosensitive resin film of the present embodiment, since the fluorine atom concentration of the first surface is lower than the fluorine atom concentration of the second surface, it is believed that the amount of (E) fluorine-containing resin exposed on the first surface after the roughening process is suppressed, and the adhesion of the surface to the copper plating layer is improved.
[0059] In order to fully exhibit this effect, in the photosensitive resin film of this embodiment, it is preferred that the first surface is a surface on which a circuit pattern is formed by copper plating, and the second surface is a pasting surface when the photosensitive resin film is laminated.
[0060] Here, in the present embodiment, the fluorine atom concentrations of the first surface and the second surface can be measured by the following method.
[0061] By observing the cross section of the cured product of the photosensitive resin film of the present embodiment, a reference line equivalent to a surface is determined. Elemental analysis is performed on a measurement line that is 1 μm away from the reference line to the inside of the cured product and is parallel to the reference line, and the fluorine atom concentration of the mass reference measured is used as the fluorine atom concentration of one surface side. Similarly, the fluorine atom concentration of the other surface side is measured, and the fluorine atom concentration of the lower side is determined as the fluorine atom concentration of the first surface, and the fluorine atom concentration of the higher side is determined as the fluorine atom concentration of the second surface. It should be noted that the cured product of the photosensitive resin film can be produced by exposure and heating. The fluorine atom concentration in the cured product obtained by exposing and heating the photosensitive resin film of the present embodiment can be regarded as the fluorine atom concentration of the photosensitive resin film before curing.
[0062] A more detailed method for measuring the fluorine atom concentrations of the first surface and the second surface is described in the Examples.
[0063] The fluorine atom concentration of the first surface is not particularly limited, but is preferably 0 to 7 mass %, more preferably 0 to 6 mass %, and even more preferably 0 to 5 mass % from the viewpoint of forming an interlayer insulating layer having better dielectric properties and conductor adhesion.
[0064] The fluorine atom concentration of the second surface is not particularly limited as long as it is higher than that of the first layer. From the viewpoint of forming an interlayer insulating layer having better dielectric properties and conductor adhesion, the fluorine atom concentration is preferably 8 to 60 mass %, more preferably 10 to 35 mass %, and further preferably 15 to 30 mass % within the range higher than that of the first surface.
[0065] In order to set a difference in fluorine atom concentration between the first surface and the second surface, the photosensitive resin film of this embodiment is preferably manufactured using a resin composition for forming the first surface of the photosensitive resin film (hereinafter also referred to as "resin composition (1)") and a resin composition for forming the second surface (hereinafter also referred to as "resin composition (2)").
[0066] The resin composition (1) preferably contains (A) a compound having an ethylenically unsaturated group, (B) a thermosetting resin, (C) a photopolymerization initiator, and (D) an inorganic filler, and contains silica as the (D) inorganic filler.
[0067] The resin composition (2) preferably contains (A) a compound having an ethylenically unsaturated group, (B) a thermosetting resin, (C) a photopolymerization initiator, (D) an inorganic filler, and (E) a fluorine-containing resin.
[0068] Hereinafter, each component contained in the photosensitive resin film of this embodiment is demonstrated, and the preferable aspect of the resin composition (1) and the resin composition (2) is also demonstrated.
[0069] <(A) Compound Having Ethylenically Unsaturated Group>
[0070] (A) The component is not particularly limited as long as it is a compound having an ethylenically unsaturated group.
[0071] (A) The component may be used alone or in combination of two or more.
[0072] (A) The component is a compound that exhibits photopolymerization, particularly radical polymerization, due to having an ethylenically unsaturated group.
[0073] It should be noted that, in the present specification, "ethylenically unsaturated group" refers to a substituent containing an ethylenically unsaturated bond. In addition, "ethylenically unsaturated bond" refers to a carbon-carbon double bond that can undergo an addition reaction, and does not include a double bond of an aromatic ring.
[0074] Examples of the ethylenically unsaturated group include a vinyl group, an allyl group, a (meth)acryloyl group, a propargyl group, a butenyl group, an ethynyl group, a phenylethynyl group, a maleimide group, and a nadicimide group. Among them, a (meth)acryloyl group is preferred from the viewpoint of reactivity.
[0075] From the viewpoint of being able to perform alkali development, the photosensitive resin film of this embodiment preferably contains (A1) a compound having an ethylenically unsaturated group and an acidic substituent, and from the viewpoint of forming an interlayer insulating layer having better heat resistance and dielectric properties, it preferably contains (A2) a monomer having two or more ethylenically unsaturated groups together with the component (A1). The components (A1) and (A2) are described below.
[0076] <(A1) Compound Having an Ethylenically Unsaturated Group and an Acidic Substituent>
[0077] Examples of the acidic substituent that the component (A1) has include a carboxyl group, a sulfonic acid group, and a phenolic hydroxyl group. Among these, a carboxyl group is preferred from the viewpoint of resolution.
[0078] The acid value of the component (A1) is not particularly limited, but is preferably 20 to 200 mgKOH / g, more preferably 40 to 180 mgKOH / g, and even more preferably 70 to 150 mgKOH / g.
[0079] When the acid value of the component (A1) is equal to or greater than the above lower limit, the alkali developability tends to be better. When the acid value of the component (A1) is equal to or less than the above upper limit, the relative dielectric constant tends to be better.
[0080] In addition, the acid value of (A1) component can be measured by the method described in Examples.
[0081] The weight average molecular weight (Mw) of the component (A1) is not particularly limited, but is preferably 600 to 30,000, more preferably 800 to 20,000, further preferably 1,000 to 10,000, and particularly preferably 1,200 to 4,000.
[0082] When the weight average molecular weight (Mw) of the component (A1) is within the above range, an interlayer insulating layer having better bonding strength with the copper plating layer, heat resistance, and insulation reliability tends to be formed.
[0083] In addition, in this specification, the weight average molecular weight (Mw) is a value calculated|required by the gel permeation chromatography (GPC) method using tetrahydrofuran as a solvent and standard polystyrene conversion, More specifically, it is a value measured by the method described in an Example.
[0084] From the viewpoint of lowering the relative dielectric constant and lowering the dielectric loss tangent, the component (A1) preferably contains an alicyclic skeleton.
[0085] As the alicyclic skeleton possessed by the component (A1), from the viewpoint of resolution and dielectric properties, an alicyclic skeleton having 5 to 20 ring carbon atoms is preferred, an alicyclic skeleton having 5 to 18 ring carbon atoms is more preferred, an alicyclic skeleton having 6 to 16 ring carbon atoms is further preferred, an alicyclic skeleton having 7 to 14 ring carbon atoms is particularly preferred, and an alicyclic skeleton having 8 to 12 ring carbon atoms is most preferred.
[0086] From the viewpoint of resolution and dielectric properties, the alicyclic skeleton possessed by the component (A1) is preferably composed of 2 or more rings, more preferably composed of 2 to 4 rings, and further preferably composed of 3 rings. Examples of the alicyclic skeleton composed of 2 or more rings include a norbornane skeleton, a decalin skeleton, a bicycloundecane skeleton, and a saturated dicyclopentadiene skeleton. Among them, from the viewpoint of resolution and dielectric properties, a saturated dicyclopentadiene skeleton is preferred.
[0087] From the same viewpoint, the component (A1) preferably includes an alicyclic skeleton represented by the following general formula (A1-1).
[0088] [Chemistry 1]
[0089]
[0090] (Where R A1 represents an alkyl group having 1 to 12 carbon atoms, which may be substituted at any position of the above-mentioned alicyclic skeleton. 1 is an integer from 0 to 6. * represents a bonding site. )
[0091] In the above general formula (A1-1), R A1 Examples of the alkyl group having 1 to 12 carbon atoms include methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, tert-butyl, n-pentyl, etc. The alkyl group is preferably an alkyl group having 1 to 6 carbon atoms, more preferably an alkyl group having 1 to 3 carbon atoms, and still more preferably a methyl group.
[0092] In the above general formula (A1-1), m 1 It is an integer of 0 to 6, preferably an integer of 0 to 2, and more preferably 0. m 1 When it is an integer from 2 to 6, multiple R A1 They may be the same or different. A1 The substitutions may be made on the same carbon atom or on different carbon atoms within the possible range.
[0093] In the above general formula (A1-1), * is a bonding site with other structures.
[0094] The single bond having the bonding site * may be bonded to any carbon atom on the alicyclic skeleton, and preferably to the carbon atom represented by either 1 or 2 and the carbon atom represented by either 3 or 4 in the following general formula (A1-1').
[0095] [Chemistry 2]
[0096]
[0097] (Where R A1 、m 1 and * are the same as those in the above general formula (A1-1).
[0098] The component (A1) is preferably a compound obtained by reacting a compound obtained by reacting (a1) an epoxy resin with (a2) a (meth)acryloyl group-containing organic acid and (a3) a saturated or unsaturated group-containing polybasic acid anhydride.
[0099] In the following description, a compound obtained by reacting (a1) an epoxy resin and (a2) a (meth)acryloyl group-containing organic acid may be referred to as "component (A')".
[0100] In addition, the compound obtained by reacting the component (A') with the polybasic acid anhydride (a3) containing a saturated group or an unsaturated group may be referred to as an "acid-modified (meth)acryloyl group-containing epoxy resin derivative".
[0101] Hereinafter, preferred embodiments of the component (A1) will be described.
[0102] ((a1) Epoxy resin)
[0103] The (a1) epoxy resin preferably has two or more epoxy groups.
[0104] (a1) The epoxy resin may be used alone or in combination of two or more.
[0105] (a1) Epoxy resins can be classified into, for example, glycidyl ether type epoxy resins, glycidyl amine type epoxy resins, glycidyl ester type epoxy resins, etc. Among them, glycidyl ether type epoxy resins are preferred.
[0106] (a1) Epoxy resins can also be classified into various epoxy resins according to the difference in the main skeleton, for example, epoxy resins having an alicyclic skeleton, novolac epoxy resins, bisphenol epoxy resins, aralkyl epoxy resins, other epoxy resins, etc. Among them, epoxy resins having an alicyclic skeleton and novolac epoxy resins are preferred.
[0107] [Epoxy resin having an alicyclic skeleton]
[0108] The alicyclic skeleton of the epoxy resin having an alicyclic skeleton is described in the same manner as the alicyclic skeleton of the component (A1), and preferred aspects are also the same.
[0109] As the epoxy resin having an alicyclic skeleton, an epoxy resin represented by the following general formula (A1-2) is preferred.
[0110] [Chemistry 3]
[0111]
[0112] (Where R A1 Each independently represents an alkyl group having 1 to 12 carbon atoms, and may be substituted at any position of the alicyclic skeleton. A2 Each independently represents an alkyl group having 1 to 12 carbon atoms. 1 is an integer from 0 to 6, m 2 is an integer from 0 to 3. n is a number from 0 to 50. )
[0113] In the above general formula (A1-2), R A1 and R in the above general formula (A1-1) A1 The same, the preferred method is also the same.
[0114] As R in the above general formula (A1-2) A2 Examples of the alkyl group having 1 to 12 carbon atoms include methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, tert-butyl, n-pentyl, etc. The alkyl group is preferably an alkyl group having 1 to 6 carbon atoms, more preferably an alkyl group having 1 to 3 carbon atoms, and still more preferably a methyl group.
[0115] In the above general formula (A1-2), m 1 and m in the above general formula (A1-1) 1 The same, the preferred method is also the same.
[0116] In the above general formula (A1-2), m 2 It is an integer of 0 to 3, preferably 0 or 1, and more preferably 0.
[0117] In the general formula (A1-2), n represents the number of structural units in parentheses, and is a number from 0 to 50. Usually, epoxy resins are mixtures of substances having different numbers of structural units in parentheses, and in this case, n is represented by the average value of the mixture. As n, a number of 0 to 30 is preferred.
[0118] As the epoxy resin having an alicyclic skeleton, a commercially available product can be used. Examples of the commercially available products include "ZXR-1807H" (trade name, manufactured by Nippon Kayaku Co., Ltd.), "XD-1000" (trade name, manufactured by Nippon Kayaku Co., Ltd.), and "EPICLON (registered trademark) HP-7200" (trade name, manufactured by DIC Corporation).
[0119] [Novolac type epoxy resin]
[0120] Examples of the novolac epoxy resin include bisphenol novolac epoxy resins such as bisphenol A novolac epoxy resin, bisphenol F novolac epoxy resin, and bisphenol S novolac epoxy resin; phenol novolac epoxy resin, cresol novolac epoxy resin, biphenyl novolac epoxy resin, and naphthol novolac epoxy resin.
[0121] As the novolac-type epoxy resin, an epoxy resin having a structural unit represented by the following general formula (A1-3) is preferred.
[0122] [Chemistry 4]
[0123]
[0124] (Where R A3 Each independently represents a hydrogen atom or a methyl group, Y A1 Each independently represents a hydrogen atom or a glycidyl group. A1 At least one of them is a glycidyl group.)
[0125] From the viewpoint of resolution, R in the above general formula (A1-3) A3 Preferably, all of them are hydrogen atoms. From the same viewpoint, Y in the above general formula (A1-3) A1 Preferably, both are glycidyl groups.
[0126] The number of the structural units in the epoxy resin (a1) having the structural unit represented by the general formula (A1-3) is 1 or more, preferably 10 to 100, more preferably 13 to 80, and further preferably 15 to 70. When the number of the structural units is within the above range, there is a tendency that an interlayer insulating layer having better conductor adhesion, heat resistance, and insulation reliability can be formed.
[0127] As the epoxy resin having the structural unit represented by the general formula (A1-3), a commercially available product may be used. Examples of the commercially available product include the "EXA-7376" series (manufactured by DIC Corporation, trade name, wherein R in the general formula (A1-3) is A3 are hydrogen atoms, Y A1are all epoxy resins containing glycidyl groups), "EPON SU8" series (manufactured by Mitsubishi Chemical Corporation, trade name, R in the above general formula (A1-3) A3 All are methyl, Y A1 are all glycidyl epoxy resins) and the like.
[0128] 〔Bisphenol type epoxy resin〕
[0129] As a bisphenol type epoxy resin, a bisphenol A type epoxy resin, a bisphenol F type epoxy resin, a bisphenol S type epoxy resin, 3,3',5,5'-tetramethyl-4,4'-diglycidyloxydiphenylmethane etc. are mentioned, for example.
[0130] 〔Aralkyl type epoxy resin〕
[0131] As an aralkyl type epoxy resin, a phenol aralkyl type epoxy resin, a biphenyl aralkyl type epoxy resin, a naphthol aralkyl type epoxy resin etc. are mentioned, for example.
[0132] 〔Other epoxy resins〕
[0133] Examples of other epoxy resins include stilbene-type epoxy resins, naphthalene-type epoxy resins, naphthylene ether-type epoxy resins, biphenyl-type epoxy resins, dihydroanthracene-type epoxy resins, cyclohexanedimethanol-type epoxy resins, trimethylol-type epoxy resins, alicyclic epoxy resins, aliphatic chain epoxy resins, heterocyclic epoxy resins, spiro-ring-containing epoxy resins, and rubber-modified epoxy resins.
[0134] ((a2) (meth)acryloyl-containing organic acid)
[0135] As the (a2) (meth)acryloyl group-containing organic acid, a (meth)acryloyl group-containing monocarboxylic acid is preferred.
[0136] Examples of the monocarboxylic acid containing a (meth)acryloyl group include acrylic acid derivatives such as acrylic acid, a dimer of acrylic acid, methacrylic acid, β-furfuryl acrylic acid, β-styryl acrylic acid, cinnamic acid, crotonic acid, and α-cyanocinnamic acid; half-ester compounds that are reaction products of hydroxyl-containing acrylic acid esters and dibasic acid anhydrides; monoglycidyl ethers containing a (meth)acryloyl group or half-ester compounds that are reaction products of monoglycidyl esters containing a (meth)acryloyl group and dibasic acid anhydrides; and the like.
[0137] The component (a2) may be used alone or in combination of two or more.
[0138] In the reaction of component (a1) and component (a2), the amount of component (a2) used is not particularly limited, but is preferably 0.6 to 1.1 equivalents, more preferably 0.8 to 1.05 equivalents, and still more preferably 0.9 to 1.02 equivalents relative to 1 equivalent of the epoxy group of component (a1). By reacting component (a1) and component (a2) at the above ratio, there is a tendency that the polymerizability of component (a1) is improved and the resolution is improved.
[0139] It is preferred that the components (a1) and (a2) are dissolved in an organic solvent and reacted while heating. In the reaction, a known reaction catalyst, polymerization inhibitor, etc. may be used as necessary.
[0140] When a monocarboxylic acid containing a (meth)acryloyl group is used as the component (a2), the component (A') obtained by reacting the components (a1) and (a2) has a hydroxyl group formed by a ring-opening addition reaction between the epoxy group of the component (a1) and the carboxyl group of the component (a2). Next, the component (A') is reacted with a polyacid anhydride containing a saturated or unsaturated group (a3), thereby obtaining an acid-modified epoxy resin derivative containing a (meth)acryloyl group, which is obtained by half-esterification of the hydroxyl group of the component (A') and the acid anhydride group of the component (a3). It should be noted that the hydroxyl group of the component (A') may also include the hydroxyl group originally present in the component (a1).
[0141] ((a3) polyacid anhydride)
[0142] As (a3) component, it is possible to contain a saturated group or an unsaturated group. As (a3) component, for example, succinic anhydride, maleic anhydride, tetrahydrophthalic anhydride, phthalic anhydride, methyltetrahydrophthalic anhydride, ethyltetrahydrophthalic anhydride, hexahydrophthalic anhydride, methylhexahydrophthalic anhydride, ethylhexahydrophthalic anhydride, itaconic anhydride etc. can be listed. Among them, from the viewpoint of resolution, tetrahydrophthalic anhydride is preferred. (a3) component can be used alone or in combination of two or more.
[0143] In the reaction between the components (A') and (a3), for example, by reacting 0.1 to 1.0 equivalent of the component (a3) per 1 equivalent of the hydroxyl groups in the component (A'), the acid value of the acid-modified (meth)acryloyl group-containing epoxy resin derivative can be well adjusted.
[0144] <(A2) Monomer having two or more ethylenically unsaturated groups>
[0145] The component (A2) is mainly used as a crosslinking agent for the component (A1).
[0146] The photosensitive resin film of this embodiment contains the component (A2) together with the component (A1), thereby increasing the crosslinking density due to the photoradical polymerization reaction, improving the alkaline developer resistance and the resolution, and tending to form an interlayer insulating layer having better heat resistance.
[0147] In addition, the component (A2) may or may not have an acidic substituent.
[0148] The number of ethylenically unsaturated groups possessed by component (A2) is 2 or more, preferably 2 to 10, more preferably 2 to 8, and even more preferably 2 to 7 from the viewpoint of resolution and forming an interlayer insulating layer having better heat resistance and dielectric properties.
[0149] (A2) As a component, a bifunctional monomer which has two ethylenically unsaturated groups, a polyfunctional monomer which has three or more ethylenically unsaturated groups, etc. are mentioned.
[0150] Examples of the difunctional monomer having two ethylenically unsaturated groups include aliphatic di(meth)acrylates such as trimethylolpropane di(meth)acrylate, polypropylene glycol di(meth)acrylate, and polyethylene glycol di(meth)acrylate; di(meth)acrylates having an alicyclic skeleton such as dicyclopentadiene di(meth)acrylate and tricyclodecane dimethanol di(meth)acrylate; and aromatic di(meth)acrylates such as 2,2-bis(4-(meth)acryloyloxypolyethoxypolypropoxyphenyl)propane and bisphenol A diglycidyl ether di(meth)acrylate.
[0151] Examples of the polyfunctional monomer having three or more ethylenically unsaturated groups include (meth)acrylate compounds having a skeleton derived from trimethylolpropane, such as trimethylolpropane tri(meth)acrylate; (meth)acrylate compounds having a skeleton derived from tetramethylolmethane, such as tetramethylolmethane tri(meth)acrylate and tetramethylolmethane tetra(meth)acrylate; (meth)acrylate compounds having a skeleton derived from pentaerythritol, such as pentaerythritol tri(meth)acrylate and pentaerythritol tetra(meth)acrylate; (meth)acrylate compounds having a skeleton derived from dipentaerythritol, such as dipentaerythritol penta(meth)acrylate and dipentaerythritol hexa(meth)acrylate; (meth)acrylate compounds having a skeleton derived from di(trimethylolpropane), such as di(trimethylolpropane) tetra(meth)acrylate; (meth)acrylate compounds having a skeleton derived from diglycerol, and the like.
[0152] Here, the above-mentioned “(meth)acrylate compound having a skeleton derived from XXX” (wherein XXX is a compound name) refers to an esterification product of XXX and (meth)acrylic acid, and the esterification product also includes compounds modified with an alkyleneoxy group.
[0153] Among the above options, from the viewpoint of resolution and the viewpoint of forming an interlayer insulating layer with better conductor adhesion, the (A2) component is preferably a polyfunctional monomer having three or more ethylenically unsaturated groups, and more preferably a (meth)acrylate compound having a skeleton derived from trimethylolpropane or a (meth)acrylate compound having a skeleton derived from dipentaerythritol.
[0154] Component (A) may or may not contain compounds other than components (A1) and (A2). Components other than components (A1) and (A2) include, for example, monofunctional monomers having one ethylenically unsaturated group and no acidic substituent.
[0155] (Content of component (A))
[0156] The content of the component (A) in the photosensitive resin film of the present embodiment is not particularly limited, but is preferably 10 to 80% by mass, more preferably 15 to 60% by mass, and even more preferably 20 to 50% by mass, based on the total amount of the resin components in the photosensitive resin film, from the viewpoint of resolution and dielectric properties of the formed interlayer insulating layer.
[0157] Here, in this specification, "resin component" refers to a resin and a compound that forms a resin by a curing reaction. For example, in the photosensitive resin film of this embodiment, component (A), component (B), component (E), and component (F) are classified as resin components.
[0158] On the other hand, the component (C), the component (D), the component (G), and the component (H) are not contained in the resin component.
[0159] When the photosensitive resin film of the present embodiment contains the component (A1), the content thereof is not particularly limited, but is preferably 5 to 50% by mass, more preferably 10 to 40% by mass, and even more preferably 15 to 30% by mass, based on the total amount of the resin components in the photosensitive resin film, from the viewpoint of resolution and dielectric properties of the formed interlayer insulating layer.
[0160] When the photosensitive resin film of the present embodiment contains components (A1) and (A2), the content of component (A2) is not particularly limited. From the viewpoint of resolution and dielectric properties of the formed interlayer insulating layer, the content of component (A2) is preferably 10 to 90 parts by mass, more preferably 30 to 80 parts by mass, and even more preferably 50 to 70 parts by mass, relative to 100 parts by mass of component (A1) in the photosensitive resin film of the present embodiment.
[0161] (Content of component (A) in resin composition (1))
[0162] The content of the component (A) in the resin composition (1) is not particularly limited, but is preferably 10 to 80% by mass, more preferably 20 to 60% by mass, and even more preferably 30 to 50% by mass, based on the total amount of the resin components in the resin composition (1), from the viewpoint of the resolution of the photosensitive resin film and the dielectric properties of the interlayer insulating layer to be formed.
[0163] When the resin composition (1) contains the component (A1), the content of the component (A1) in the resin composition (1) is not particularly limited. From the viewpoint of resolution and dielectric properties of the interlayer insulating layer to be formed, it is preferably 5 to 70% by mass, more preferably 10 to 50% by mass, and even more preferably 20 to 40% by mass, based on the total amount of the resin components in the resin composition (1).
[0164] When the resin composition (1) contains the components (A1) and (A2), the content of the component (A2) in the resin composition (1) is not particularly limited. However, from the viewpoint of resolution and dielectric properties of the interlayer insulating layer to be formed, the content is preferably 5 to 120 parts by mass, more preferably 10 to 60 parts by mass, and even more preferably 20 to 40 parts by mass, relative to 100 parts by mass of the component (A1) in the resin composition (1).
[0165] (Content of component (A) in resin composition (2))
[0166] The content of the component (A) in the resin composition (2) is not particularly limited, but is preferably 10 to 80% by mass, more preferably 15 to 60% by mass, and even more preferably 20 to 50% by mass, based on the total amount of the resin components in the resin composition (2), from the viewpoint of resolution and dielectric properties of the interlayer insulating layer to be formed.
[0167] When the resin composition (2) contains the component (A1), the content of the component (A1) in the resin composition (2) is not particularly limited. From the viewpoint of resolution and dielectric properties of the interlayer insulating layer to be formed, it is preferably 3 to 60% by mass, more preferably 5 to 40% by mass, and even more preferably 10 to 30% by mass, based on the total amount of the resin components in the resin composition (2).
[0168] When the resin composition (2) contains the components (A1) and (A2), the content of the component (A2) in the resin composition (2) is not particularly limited. However, from the viewpoint of resolution and dielectric properties of the interlayer insulating layer to be formed, the content is preferably 20 to 100 parts by mass, more preferably 40 to 90 parts by mass, and even more preferably 60 to 80 parts by mass, relative to 100 parts by mass of the component (A1) in the resin composition (2).
[0169] <(B) Thermosetting resin>
[0170] (B) The thermosetting resin is not particularly limited as long as it is a thermosetting resin.
[0171] The photosensitive resin film of the present embodiment contains the (B) thermosetting resin, so that the heat resistance of the interlayer insulating layer to be formed tends to be improved.
[0172] (B) Thermosetting resins may be used alone or in combination of two or more.
[0173] Examples of the thermosetting resin (B) include epoxy resins, isocyanate resins, maleimide resins, phenolic resins, cyanate resins, benzoic acid resins, Oxazine resin, oxetane resin, amino resin, unsaturated polyester resin, allyl resin, vinyl resin, dicyclopentadiene resin, silicone resin, triazine resin, melamine resin, other well-known thermosetting resins, etc.
[0174] Among the above options, from the viewpoint of forming an interlayer insulating layer with better heat resistance and conductor adhesion, the photosensitive resin film of the present embodiment preferably contains one or more selected from the group consisting of epoxy resin, maleimide resin, allyl resin and vinyl resin as component (B), and more preferably contains epoxy resin.
[0175] (Epoxy resin)
[0176] As the epoxy resin, an epoxy resin having two or more epoxy groups is preferred.
[0177] Epoxy resins can be classified into, for example, glycidyl ether epoxy resins, glycidyl amine epoxy resins, glycidyl ester epoxy resins, etc. Among them, glycidyl ether epoxy resins are preferred.
[0178] In addition, epoxy resins can also be classified into various epoxy resins according to the difference of the main skeleton. Among the above-mentioned various types of epoxy resins, they can be further classified as follows. Specifically, epoxy resins can be classified into bisphenol-based epoxy resins such as bisphenol A epoxy resin, bisphenol F epoxy resin, and bisphenol S epoxy resin; bisphenol A novolac epoxy resin; bisphenol F novolac epoxy resin and other bisphenol novolac epoxy resins; phenol novolac epoxy resins other than the above-mentioned bisphenol novolac epoxy resins such as phenol novolac epoxy resin, cresol novolac epoxy resin, and biphenyl novolac epoxy resin; phenol aralkyl epoxy resin; stilbene epoxy resin ; Epoxy resins containing naphthalene skeletons such as naphthol novolac type epoxy resin, naphthol type epoxy resin, naphthol aralkyl type epoxy resin, and naphthylene ether type epoxy resin; biphenyl type epoxy resin; biphenyl aralkyl type epoxy resin; benzyl dimethyl type epoxy resin; dihydroanthracene type epoxy resin; alicyclic epoxy resins such as saturated dicyclopentadiene type epoxy resin; heterocyclic epoxy resin; epoxy resin containing spiro ring; cyclohexanedimethanol type epoxy resin; trimethylol type epoxy resin; aliphatic chain epoxy resin; rubber modified epoxy resin, etc.
[0179] Among them, the epoxy resin is preferably a bisphenol epoxy resin, a naphthalene skeleton-containing epoxy resin, or a biphenyl aralkyl type epoxy resin, and more preferably an epoxy resin containing a naphthalene skeleton or a biphenyl aralkyl type epoxy resin.
[0180] (isocyanate resin)
[0181] As isocyanate resin, for example, aliphatic isocyanates such as trimethylene diisocyanate, tetramethylene diisocyanate, pentamethylene diisocyanate, hexamethylene diisocyanate, and trimethylhexamethylene diisocyanate; alicyclic isocyanates such as 1,3-cyclopentane diisocyanate, 1,4-cyclohexane diisocyanate, 1,2-cyclohexane diisocyanate, isophorone diisocyanate, and norbornane diisocyanate; aromatic isocyanates such as xylylene diisocyanate, 2,4-toluene diisocyanate, and 2,6-toluene diisocyanate; their biuret bodies; their urate bodies, etc. Among them, aliphatic isocyanates are preferred, and hexamethylene diisocyanate is more preferred.
[0182] (Maleimide resin)
[0183] As maleimide resin, for example, aromatic maleimide compounds having N-substituted maleimide groups directly bonded to an aromatic ring, aliphatic maleimide compounds having N-substituted maleimide groups directly bonded to an aliphatic hydrocarbon group, etc. Among them, aromatic maleimide compounds are preferred, and aromatic bismaleimide compounds are more preferred, from the viewpoint of heat resistance and handling properties.
[0184] Examples of the aromatic maleimide compound include bis(4-maleimidephenyl)methane, 2,2-bis[4-(4-maleimidephenoxy)phenyl]propane, 3,3'-dimethyl-5,5'-diethyl-4,4'-diphenylmethane bismaleimide, polyphenylmethane maleimide, biphenyl aralkyl maleimide resins, and aromatic bismaleimide resins having an indane skeleton. Among them, aromatic bismaleimide resins having an indane skeleton are preferred.
[0185] (Content of component (B))
[0186] The content of the (B) thermosetting resin in the photosensitive resin film of the present embodiment is not particularly limited, but is preferably 1 to 60% by mass, more preferably 10 to 50% by mass, and further preferably 15 to 40% by mass, based on the total amount of the resin component in the photosensitive resin film, from the viewpoint of forming an interlayer insulating layer having better conductor adhesion and heat resistance.
[0187] When the photosensitive resin film of the present embodiment contains an epoxy resin as the (B) thermosetting resin, the content thereof is not particularly limited, but is preferably 1 to 50% by mass, more preferably 2 to 30% by mass, and even more preferably 3 to 25% by mass, based on the total amount of the resin component in the photosensitive resin film, from the viewpoint of forming an interlayer insulating layer having better conductor adhesion, heat resistance, and dielectric properties.
[0188] When the photosensitive resin film of the present embodiment contains an isocyanate resin as the (B) thermosetting resin, the content thereof is not particularly limited, but is preferably 0.1 to 20% by mass, more preferably 0.5 to 15% by mass, and even more preferably 0.8 to 10% by mass, based on the total amount of the resin components in the photosensitive resin film, from the viewpoint of forming an interlayer insulating layer having better conductor adhesion, heat resistance, and dielectric properties.
[0189] When the photosensitive resin film of the present embodiment contains a maleimide resin as the (B) thermosetting resin, the content thereof is not particularly limited, but is preferably 1 to 40% by mass, more preferably 3 to 30% by mass, and even more preferably 5 to 20% by mass, based on the total amount of the resin components in the photosensitive resin film, from the viewpoint of forming an interlayer insulating layer having better conductor adhesion, heat resistance, and dielectric properties.
[0190] (Content of component (B) in resin composition (1))
[0191] The content of the thermosetting resin (B) in the resin composition (1) is not particularly limited, but is preferably 10 to 90% by mass, more preferably 30 to 80% by mass, and even more preferably 40 to 70% by mass, based on the total amount of the resin components in the resin composition (1), from the viewpoint of forming an interlayer insulating layer having better conductor adhesion and heat resistance.
[0192] When the resin composition (1) contains an epoxy resin as the (B) thermosetting resin, the content of the epoxy resin in the resin composition (1) is not particularly limited. From the viewpoint of forming an interlayer insulating layer having better conductor adhesion and heat resistance, the content of the epoxy resin is preferably 10 to 80% by mass, more preferably 20 to 70% by mass, and even more preferably 30 to 60% by mass, based on the total amount of the resin components in the resin composition (1).
[0193] From the viewpoint of forming an interlayer insulating layer having better conductor adhesion, the content of the epoxy resin in the resin composition (1) is preferably larger than the content of the epoxy resin in the resin composition (2).
[0194] When the resin composition (1) contains an isocyanate resin as the (B) thermosetting resin, the content of the isocyanate resin in the resin composition (1) is not particularly limited. From the viewpoint of forming an interlayer insulating layer having better conductor adhesion and heat resistance, the content is preferably 1 to 30% by mass, more preferably 3 to 20% by mass, and even more preferably 5 to 15% by mass, based on the total amount of the resin components in the resin composition (1).
[0195] (Content of component (B) in resin composition (2))
[0196] The content of the thermosetting resin (B) in the resin composition (2) is not particularly limited, but is preferably 1 to 50% by mass, more preferably 5 to 40% by mass, and even more preferably 10 to 30% by mass, based on the total amount of the resin components in the resin composition (2), from the viewpoint of forming an interlayer insulating layer having better heat resistance and dielectric properties.
[0197] When the resin composition (2) contains an epoxy resin as the (B) thermosetting resin, the content of the epoxy resin in the resin composition (2) is not particularly limited. From the viewpoint of forming an interlayer insulating layer having better heat resistance and dielectric properties, the content is preferably 1 to 50% by mass, more preferably 3 to 30% by mass, and even more preferably 5 to 20% by mass, based on the total amount of the resin components in the resin composition (2).
[0198] When the resin composition (2) contains an isocyanate resin as the (B) thermosetting resin, the content of the isocyanate resin in the resin composition (2) is not particularly limited. From the viewpoint of forming an interlayer insulating layer having better heat resistance and dielectric properties, the content is preferably 1 to 20% by mass, more preferably 2 to 15% by mass, and even more preferably 4 to 10% by mass, based on the total amount of the resin components in the resin composition (2).
[0199] When the resin composition (2) contains a maleimide resin as the (B) thermosetting resin, the content of the maleimide resin in the resin composition (2) is not particularly limited. From the viewpoint of forming an interlayer insulating layer having better heat resistance and dielectric properties, the content is preferably 1 to 40% by mass, more preferably 3 to 30% by mass, and even more preferably 5 to 20% by mass, based on the total amount of the resin components in the resin composition (2).
[0200] <(C) Photopolymerization Initiator>
[0201] The (C) photopolymerization initiator is a polymerization initiator that mainly initiates the photoradical polymerization reaction of the ethylenically unsaturated group contained in the (A) component.
[0202] The photosensitive resin film of the present embodiment tends to have a further improved resolution by containing the (C) photopolymerization initiator.
[0203] (C) The photopolymerization initiator may be used alone or in combination of two or more.
[0204] (C) The photopolymerization initiator includes, for example, benzoin compounds such as benzoin, benzoin methyl ether, and benzoin isopropyl ether; acetophenone compounds such as acetophenone, 2,2-dimethoxy-2-phenylacetophenone, 2,2-diethoxy-2-phenylacetophenone, 1,1-dichloroacetophenone, 1-hydroxycyclohexyl phenyl ketone, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-1-butanone, 2-[4-(methylthio)benzoyl]-2-(4-morpholino)propane, and N,N-dimethylaminoacetophenone; anthraquinone compounds such as 2-methylanthraquinone, 2-ethylanthraquinone, 2-tert-butylanthraquinone, 1-chloroanthraquinone, 2-amylanthraquinone, and 2-aminoanthraquinone; ketal compounds such as acetophenone dimethyl ketal and benzyl dimethyl ketal; 9-phenylacridine, 1- ,7-bis(9,9'-acridinyl)heptane and other acridinium compounds; phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide and other acylphosphine oxide compounds; 1,2-octanedione-1-[4-(phenylthio)phenyl]-2-(O-benzoyl oxime), 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazole-3-yl]ethanone 1-(O-acetyl oxime) , 1-phenyl-1,2-propanedione-2-[O-(ethoxycarbonyl)oxime] and other oxime ester compounds; 2,4-dimethylthioxanthone, 2,4-diethylthioxanthone, 2-chlorothioxanthone, 2,4-diisopropylthioxanthone and other thioxanthone compounds; 4,4'-bis(dimethylamino)benzophenone, 4,4'-bis(diethylamino)benzophenone and other benzophenone compounds, etc. Among them, phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide and 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazole-3-yl]ethanone 1-(O-acetyloxime) are preferred.
[0205] (Content of component (C))
[0206] The content of the (C) photopolymerization initiator in the photosensitive resin film of the present embodiment is not particularly limited, but is preferably 0.01 to 10 parts by mass, more preferably 0.05 to 5 parts by mass, and even more preferably 0.1 to 1 part by mass, relative to 100 parts by mass of the (A) component in the photosensitive resin film, from the viewpoint of easily obtaining a moderate polymerization reaction promotion effect.
[0207] (Content of Component (C) in Resin Composition (1))
[0208] The content of the photopolymerization initiator (C) in the resin composition (1) is not particularly limited, but is preferably 0.01 to 10 parts by mass, more preferably 0.05 to 5 parts by mass, and even more preferably 0.1 to 1 part by mass, relative to 100 parts by mass of the component (A) in the resin composition (1), from the viewpoint of easily obtaining a moderate polymerization reaction promoting effect.
[0209] (Content of component (C) in resin composition (2))
[0210] The content of the photopolymerization initiator (C) in the resin composition (2) is not particularly limited, but is preferably 0.01 to 10 parts by mass, more preferably 0.05 to 5 parts by mass, and even more preferably 0.1 to 1 part by mass, relative to 100 parts by mass of the component (A) in the resin composition (2), from the viewpoint of easily obtaining a moderate polymerization reaction promoting effect.
[0211] <(D) Inorganic filler>
[0212] When the photosensitive resin film of the present embodiment contains the (D) inorganic filler, the interlayer insulating layer formed tends to have further improved low thermal expansion, heat resistance, and flame retardancy.
[0213] (D) The inorganic filler may be used alone or in combination of two or more.
[0214] From the viewpoint of expressing high bonding strength with the copper plating layer, the photosensitive resin film of the present embodiment preferably contains silicon dioxide as the (D) inorganic filler.
[0215] As silica, for example, precipitated silica with high water content produced by a wet process, dry process silica produced by a dry process and containing almost no bound water, etc., etc. can be cited. In addition, as dry process silica, for example, crushed silica, fumed silica, fused silica, etc. can also be cited depending on the production method.
[0216] Silica may be surface-treated with a coupling agent such as a silane coupling agent.
[0217] Examples of silica include (D1) having a true density of more than 1,500 kg / m 3 Silica (hereinafter also referred to as "(D1) component"), (D2) true density less than or equal to 1,500 kg / m 3 Silicon dioxide (hereinafter also referred to as "(D2) component") and the like.
[0218] The component (D1) tends to have a low dielectric loss tangent. Therefore, from the viewpoint of forming an interlayer insulating layer having more excellent dielectric properties, the resin composition (1) preferably contains the component (D1).
[0219] From the viewpoint of low thermal expansion, the true density of silica as the component (D1) is preferably greater than 1,500 and less than or equal to 2,200 kg / m 3 , more preferably 1,600 to 2,200 kg / m 3 , more preferably 1,800 to 2,200 kg / m3 .
[0220] The component (D2) tends to have a small relative dielectric constant. Therefore, from the viewpoint of forming an interlayer insulating layer having more excellent dielectric properties, the resin composition (2) preferably contains the component (D2).
[0221] From the viewpoint of dielectric properties, the true density of silicon dioxide as the component (D2) is preferably 1,000 to 1,500 kg / m 3 , more preferably 1,100 to 1,500 kg / m 3 , more preferably 1,200 to 1,500 kg / m 3 , particularly preferably 1,250 to 1,450 kg / m 3 , most preferably 1,250 to 1,400 kg / m 3 .
[0222] In addition, the true density of silica can be measured using a dry type automatic density meter "AccuPycII 1340" (manufactured by Shimadzu Corporation).
[0223] Examples of the (D) inorganic filler other than silica include alumina, titanium oxide, mica, beryllium oxide, barium titanate, potassium titanate, strontium titanate, calcium titanate, aluminum carbonate, magnesium hydroxide, aluminum hydroxide, aluminum silicate, calcium carbonate, calcium silicate, magnesium silicate, silicon nitride, boron nitride, clay, talc, aluminum borate, and silicon carbide.
[0224] (D) Volume average particle size of the inorganic filler (D 50 ) is not particularly limited, but from the viewpoint of resolution, it is preferably 0.01 to 3.0 μm, more preferably 0.1 to 2.5 μm, and even more preferably 0.3 to 2.0 μm.
[0225] It should be noted that in this specification, the volume average particle size (D 50 ) can be determined as follows: using a submicron particle analyzer (manufactured by Beckman Coulter, Ltd., trade name: N5), in accordance with international standard ISO13321, particles dispersed in a solvent are measured with a refractive index of 1.38, and the particle size is determined as the particle size equivalent to the cumulative value of 50% (volume basis) in the particle size distribution.
[0226] (Content of component (D))
[0227] The content of the (D) inorganic filler in the photosensitive resin film of the present embodiment is not particularly limited, but is preferably 2 to 60 mass %, more preferably greater than or equal to 3 mass % and less than 60 mass %, further preferably 4 to 55 mass %, further preferably 5 to 50 mass %, and particularly preferably 6 to 40 mass %, from the viewpoint of forming an interlayer insulating layer having low thermal expansion, heat resistance, flame retardancy and better conductor adhesion.
[0228] The content of silicon dioxide in the photosensitive resin film of the present embodiment is not particularly limited, but is preferably 2 to 60 mass %, more preferably greater than or equal to 3 mass % and less than 60 mass %, further preferably 4 to 55 mass %, further preferably 5 to 50 mass %, and particularly preferably 6 to 40 mass %, from the viewpoint of forming an interlayer insulating layer having low thermal expansion, heat resistance, flame retardancy and better conductor adhesion.
[0229] When the photosensitive resin film of the present embodiment contains the component (D1), the content thereof is not particularly limited. From the viewpoint of forming an interlayer insulating layer having low thermal expansion, heat resistance, flame retardancy and better conductor adhesion, the content thereof is preferably 10 to 100% by mass, more preferably 20 to 90% by mass, and even more preferably 30 to 80% by mass, relative to the total amount (100% by mass) of the (D) inorganic filler in the photosensitive resin film.
[0230] When the photosensitive resin film of the present embodiment contains component (D2), its content is not particularly limited. From the viewpoint of forming an interlayer insulating layer having low thermal expansion, heat resistance and flame retardancy, the content is preferably 5 to 80% by mass, more preferably 10 to 60% by mass, and further preferably 20 to 50% by mass, relative to the total amount (100% by mass) of component (D) in the photosensitive resin film.
[0231] (Content of (D) Inorganic Filler in Resin Composition (1))
[0232] The content of the inorganic filler (D) in the resin composition (1) is not particularly limited, but is preferably 5 to 70% by mass, more preferably 15 to 60% by mass, and even more preferably 25 to 50% by mass, relative to the total solid content of the resin composition (1), from the viewpoint of forming an interlayer insulating layer having low thermal expansion, heat resistance, flame retardancy and better conductor adhesion.
[0233] When the resin composition (1) contains silica, the content of silica in the resin composition (1) is not particularly limited. From the viewpoint of forming an interlayer insulating layer having low thermal expansion, heat resistance, flame retardancy and better conductor adhesion, the content is preferably 5 to 70% by mass, more preferably 15 to 60% by mass, and even more preferably 25 to 50% by mass, relative to the total solid content of the resin composition (1).
[0234] From the viewpoint of forming an interlayer insulating layer having better conductor adhesion, the content of silicon dioxide in the resin composition (1) is preferably larger than the content of silicon dioxide in the resin composition (2).
[0235] When the resin composition (1) contains the component (D1), the content of the component (D1) in the resin composition (1) is not particularly limited. From the viewpoint of forming an interlayer insulating layer having low thermal expansion, heat resistance, flame retardancy and better conductor adhesion, the content is preferably 60 to 100 mass %, more preferably 70 to 100 mass %, and even more preferably 80 to 100 mass % relative to the total amount (100 mass %) of the (D) inorganic filler in the resin composition (1).
[0236] (Content of (D) Inorganic Filler in Resin Composition (2))
[0237] The content of the (D) inorganic filler in the resin composition (2) is not particularly limited. From the viewpoint of forming an interlayer insulating layer having low thermal expansion, heat resistance and flame retardancy, it is preferably 1 to 60% by mass, more preferably greater than or equal to 2% by mass and less than 60% by mass, further preferably 3 to 55% by mass, further preferably 4 to 50% by mass, and particularly preferably 5 to 40% by mass, relative to the total solid content of the resin composition (2).
[0238] When the resin composition (2) contains silica, the content of silica in the resin composition (2) is not particularly limited. From the viewpoint of forming an interlayer insulating layer having low thermal expansion, heat resistance, flame retardancy and better conductor adhesion, the content of silica is preferably 1 to 60% by mass, more preferably greater than or equal to 2% by mass and less than 60% by mass, further preferably 3 to 55% by mass, further preferably 4 to 50% by mass, and particularly preferably 5 to 40% by mass, relative to the total solid content of the resin composition (2).
[0239] When the resin composition (2) contains the component (D2), the content of the component (D2) in the resin composition (2) is not particularly limited. From the viewpoint of forming an interlayer insulating layer having low thermal expansion, heat resistance and flame retardancy, the content is preferably 60 to 100% by mass, more preferably 70 to 100% by mass, and even more preferably 80 to 100% by mass, relative to the total amount (100% by mass) of the component (D) in the resin composition (2).
[0240] <(E) Fluorine-containing resin>
[0241] When the photosensitive resin film of the present embodiment contains the (E) fluorine-containing resin, the interlayer insulating layer formed of the photosensitive resin film of the present embodiment tends to have a lower relative dielectric constant.
[0242] (E) The fluorine-containing resin may be used alone or in combination of two or more.
[0243] (E) As a fluorine-containing resin, a polymer of an olefin containing a fluorine atom (hereinafter also referred to as "fluorine-containing olefin") is mentioned, for example.
[0244] The fluorine-containing olefin may be one in which a part of hydrogen atoms in carbon-hydrogen bonds are substituted with fluorine atoms, but preferably one in which all hydrogen atoms in carbon-hydrogen bonds are substituted with fluorine atoms from the viewpoint of further reducing the relative dielectric constant.
[0245] (E) The fluorine-containing resin includes, for example, polymonofluoroethylene, polydifluoroethylene, polytrifluoroethylene, polytetrafluoroethylene, polyhexafluoropropylene, polyvinyl fluoride, polyvinylidene fluoride, etc. Among them, polytetrafluoroethylene is preferred.
[0246] (E) The fluorine-containing resin is preferably in the form of particles.
[0247] The volume average particle size (D) of the fluorine-containing resin (E) as particles 50 ) is not particularly limited, but from the viewpoint of resolution, it is preferably 0.01 μm to 3.0 μm, more preferably 0.05 μm to 2.5 μm, and further preferably 0.1 μm to 2.0 μm.
[0248] (Content of component (E))
[0249] The content of the (E) fluorine-containing resin in the photosensitive resin film of the present embodiment is not particularly limited, but is preferably 5 to 80% by mass, more preferably 10 to 70% by mass, and further preferably 15 to 60% by mass, based on the total amount of the resin component in the photosensitive resin film, from the viewpoint of forming an interlayer insulating layer having better heat resistance and conductor adhesion.
[0250] (Content of component (E) in resin composition (1))
[0251] The resin composition (1) may contain (E) a fluorine-containing resin, but preferably contains no (E) fluorine-containing resin from the viewpoint of resolution and from the viewpoint of forming an interlayer insulating layer having more excellent conductor adhesion.
[0252] When the resin composition (1) contains the fluorine-containing resin (E), the content of the fluorine-containing resin (E) in the resin composition (1) is preferably as low as possible. From the same viewpoint as described above, the content is preferably 20% by mass or less, more preferably 10% by mass or less, and even more preferably 1% by mass or less, based on the total amount of the resin components in the resin composition (1).
[0253] (Content of component (E) in resin composition (2))
[0254] The content of the fluorine-containing resin (E) in the resin composition (2) is not particularly limited, but is preferably 10 to 80% by mass, more preferably 15 to 70% by mass, and even more preferably 20 to 65% by mass, based on the total amount of the resin components in the resin composition (2), from the viewpoint of resolution and the formation of an interlayer insulating layer having better insulation reliability, relative dielectric constant, heat resistance and conductor adhesion.
[0255] <(F) Elastomer>
[0256] The photosensitive resin film of the present embodiment may further contain (F) an elastomer.
[0257] Since the photosensitive resin film of the present embodiment contains the (F) elastomer, the interlayer insulating layer formed tends to have further improved adhesiveness to a conductor.
[0258] It should be noted that the “elastomer” herein refers to a polymer having a glass transition temperature of 25° C. or less as measured by differential scanning calorimetry in accordance with JIS K 6240:2011.
[0259] (F) The elastomer may be used alone or in combination of two or more.
[0260] (F) Elastomers include, for example, polybutadiene elastomers, polyester elastomers, styrene elastomers, olefin elastomers, urethane elastomers, polyamide elastomers, acrylic elastomers, silicone elastomers, and derivatives of these elastomers. Among these, polybutadiene elastomers are preferred from the viewpoint of compatibility with the resin component and from the viewpoint of forming an interlayer insulating layer with better conductor adhesion.
[0261] Preferred examples of the polybutadiene-based elastomer include those derived from 1,3-butadiene and containing a 1,2-vinyl group.
[0262] From the viewpoint of resolution, the polybutadiene-based elastomer is preferably a polybutadiene-based elastomer having an acid anhydride group, and more preferably a polybutadiene-based elastomer having an acid anhydride group derived from maleic anhydride.
[0263] When the polybutadiene elastomer has an acid anhydride group, the number of the acid anhydride groups in one molecule is not particularly limited, but is preferably 1 to 12, more preferably 3 to 11, and even more preferably 6 to 10 from the viewpoint of resolution and forming an interlayer insulating layer with a better relative dielectric constant.
[0264] The number average molecular weight (Mn) of the (F) elastomer is not particularly limited, but is preferably 1,000 to 100,000, more preferably 2,000 to 50,000, further preferably 3,000 to 10,000, and particularly preferably 4,000 to 7,000.
[0265] In addition, in this specification, the number average molecular weight (Mn) is a value calculated|required by the gel permeation chromatography (GPC) method using tetrahydrofuran as a solvent and standard polystyrene conversion, More specifically, it is a value measured by the method described in an Example.
[0266] (Content of component (F))
[0267] The content of the (F) elastomer in the photosensitive resin film of the present embodiment is not particularly limited, but is preferably 0.5 to 20% by mass, more preferably 1 to 15% by mass, and even more preferably 2 to 10% by mass, based on the total amount of the resin components in the photosensitive resin film, from the viewpoint of forming an interlayer insulating layer having better heat resistance and conductor adhesion.
[0268] (Content of component (F) in resin composition (1))
[0269] When the resin composition (1) contains the (F) elastomer, the content of the (F) elastomer in the resin composition (1) is not particularly limited. From the viewpoint of forming an interlayer insulating layer having better heat resistance and conductor adhesion, the content is preferably 1 to 30% by mass, more preferably 3 to 20% by mass, and even more preferably 5 to 15% by mass, based on the total amount of the resin components in the resin composition (1).
[0270] (Content of component (F) in resin composition (2))
[0271] When the resin composition (2) contains the (F) elastomer, the content of the (F) elastomer in the resin composition (2) is not particularly limited. From the viewpoint of forming an interlayer insulating layer having better heat resistance and conductor adhesion, the content is preferably 0.5 to 20% by mass, more preferably 1 to 15% by mass, and even more preferably 2 to 10% by mass, based on the total amount of the resin components in the resin composition (2).
[0272] <(G) Organic peroxide>
[0273] The photosensitive resin film of the present embodiment preferably further contains (G) an organic peroxide. The (G) organic peroxide is mainly a polymerization initiator for the thermal radical polymerization reaction of the ethylenically unsaturated group possessed by the component (A) and, if necessary, the component (B).
[0274] Since the photosensitive resin film of the present embodiment contains the (G) organic peroxide, the interlayer insulating layer formed tends to have further improved heat resistance, dielectric properties, and the like.
[0275] (G) The organic peroxide may be used alone or in combination of two or more.
[0276] Examples of the organic peroxide (G) include peroxyketals such as 1,1-di(tert-butylperoxy)cyclohexane, 2,2-di(tert-butylperoxy)butane, 2,2-di(4,4-di-tert-butylperoxycyclohexyl)propane, and 1,1-di(tert-amylperoxy)cyclohexane; hydroperoxides such as cumene hydroperoxide and tert-butyl hydroperoxide; alkyl peroxides such as tert-butyl peroxyacetate and tert-amyl peroxyisononanoate; tert-butyl Dialkyl peroxides such as cumyl peroxide, di-tert-butyl peroxide, dicumyl peroxide, di-tert-hexyl peroxide, and 1,3-di(tert-butylperoxyisopropyl)benzene; peroxyesters such as tert-butyl peroxyacetate, tert-butyl peroxybenzoate, and tert-butyl peroxyisopropylmonocarbonate; peroxycarbonates such as tert-butyl peroxyisopropylcarbonate and polyether tetra(tert-butylperoxycarbonate); diacyl peroxides such as dibenzoyl peroxide, etc. Among them, 1,3-di(tert-butylperoxyisopropyl)benzene is preferred.
[0277] (Content of component (G))
[0278] When the photosensitive resin film of the present embodiment contains (G) an organic peroxide, the content thereof is not particularly limited. From the viewpoint of forming an interlayer insulating layer having better heat resistance and conductor adhesion, the content is preferably 0.1 to 10 parts by mass, more preferably 1 to 7 parts by mass, and even more preferably 1.5 to 4 parts by mass, relative to 100 parts by mass of the component (A) in the photosensitive resin film.
[0279] (Content of component (G) in resin composition (1))
[0280] When the resin composition (1) contains (G) an organic peroxide, the content of the (G) organic peroxide in the resin composition (1) is not particularly limited. However, from the viewpoint of forming an interlayer insulating layer having better heat resistance and conductor adhesion, the content is preferably 0.1 to 10 parts by mass, more preferably 1 to 7 parts by mass, and even more preferably 1.5 to 4 parts by mass, relative to 100 parts by mass of the component (A) in the resin composition (1).
[0281] (Content of component (G) in resin composition (2))
[0282] When the resin composition (2) contains (G) an organic peroxide, the content of the (G) organic peroxide in the resin composition (2) is not particularly limited. However, from the viewpoint of forming an interlayer insulating layer having better heat resistance and conductor adhesion, the content is preferably 0.1 to 10 parts by mass, more preferably 1 to 7 parts by mass, and even more preferably 1.5 to 4 parts by mass, relative to 100 parts by mass of the component (A) in the resin composition (2).
[0283] <(H) Curing Accelerator>
[0284] The photosensitive resin film of the present embodiment preferably further contains (H) a curing accelerator.
[0285] Since the photosensitive resin film of the present embodiment contains the (H) curing accelerator, the interlayer insulating layer formed tends to have further improved heat resistance, dielectric properties, and the like.
[0286] (H) The curing accelerator may be used alone or in combination of two or more.
[0287] Examples of the (H) curing accelerator include imidazole compounds such as 2-methylimidazole, 2-ethyl-4-methylimidazole, 1-benzyl-2-methylimidazole, 2-phenylimidazole, 2-phenyl-1-benzyl-1H-imidazole, 2-phenyl-4-methyl-5-hydroxymethylimidazole, and isocyanate-masked imidazole (addition reaction product of hexamethylene diisocyanate resin and 2-ethyl-4-methylimidazole); tertiary amines such as trimethylamine, N,N-dimethyloctylamine, N-benzyldimethylamine, pyridine, N-methylmorpholine, hexa(N-methyl)melamine, 2,4,6-tris(dimethylaminophenol), tetramethylguanidine, and m-aminophenol; organic phosphines such as tributylphosphine, triphenylphosphine, and tri-2-cyanoethylphosphine; tri-n-butyl(2,5-dihydroxyphenyl)bromide; Hexadecyl tributyl chloride wait Salts; quaternary ammonium salts such as benzyltrimethylammonium chloride and phenyltributylammonium chloride; the above-mentioned polyacid anhydrides; diphenyl iodide Tetrafluoroborate, triphenylsulfonium hexafluoroantimonate, 2,4,6-triphenylthiopyran Hexafluorophosphate, etc.
[0288] Among them, imidazole compounds are preferred from the viewpoint of obtaining an excellent curing effect.
[0289] (Content of component (H))
[0290] When the photosensitive resin film of the present embodiment contains a curing accelerator (H), the content thereof is not particularly limited. From the viewpoint of forming an interlayer insulating layer having better heat resistance and conductor adhesion, the content thereof is preferably 0.1 to 10 parts by mass, more preferably 0.5 to 7 parts by mass, and even more preferably 1 to 4 parts by mass, relative to 100 parts by mass of the component (B) in the photosensitive resin film.
[0291] (Content of component (H) in resin composition (1))
[0292] When the resin composition (1) contains a curing accelerator (H), the content of the curing accelerator (H) in the resin composition (1) is not particularly limited. However, from the viewpoint of forming an interlayer insulating layer having better heat resistance and conductor adhesion, the content is preferably 0.1 to 10 parts by mass, more preferably 0.5 to 7 parts by mass, and even more preferably 1 to 4 parts by mass, relative to 100 parts by mass of the component (B) in the resin composition (1).
[0293] (Content of component (H) in resin composition (2))
[0294] When the resin composition (2) contains a curing accelerator (H), the content of the curing accelerator (H) in the resin composition (2) is not particularly limited. From the viewpoint of forming an interlayer insulating layer having better heat resistance and conductor adhesion, the content is preferably 0.1 to 10 parts by mass, more preferably 0.5 to 7 parts by mass, and even more preferably 1 to 4 parts by mass, relative to 100 parts by mass of the component (B) in the resin composition (2).
[0295] <(I) Other ingredients>
[0296] The photosensitive resin film of the present embodiment may contain components other than the above-mentioned components as (I) other components as necessary.
[0297] Examples of (I) other components include resins other than the above-mentioned components, organic fillers other than (E) component, photosensitizers, polymerization inhibitors, foam stabilizers, pigments, adhesion aids such as melamine, foam stabilizers such as silicone compounds, thickeners, flame retardants, and the like.
[0298] These may be used alone or in combination of two or more.
[0299] The content of (I) other components in the photosensitive resin film of the present embodiment may be appropriately adjusted depending on the purpose, and each may be 0.01 to 10% by mass, 0.05 to 5% by mass, or 0.1 to 1% by mass.
[0300] <Method for producing photosensitive resin film>
[0301] The photosensitive resin film of the present embodiment can be produced using, for example, the resin composition (1) and the resin composition (2).
[0302] The resin composition (1) and the resin composition (2) can be produced by mixing the components to be blended in each layer and a diluent used as required. The components can be mixed using, for example, a roll mill, a bead mill, a planetary mixer, a rotation and revolution mixer, or the like.
[0303] The resin composition (1) and the resin composition (2) are coated on respective carrier films and dried as required to form a film of the resin composition (1) with a carrier film and a film of the resin composition (2) with a carrier film. Then, the resin composition films of the resin composition (1) with a carrier film and the resin composition (2) with a carrier film can be laminated to each other to produce a photosensitive resin film having carrier films on both sides.
[0304] As another method, the photosensitive resin film of this embodiment can be manufactured by coating any one of the resin compositions on a carrier film in advance and coating any other of the resin compositions on the resin composition on the one side. After coating one of the resin compositions and before coating the other of the resin compositions, drying can be performed as needed.
[0305] Examples of the method for applying the resin composition (1) and the resin composition (2) include methods using a coating apparatus such as a notch wheel coater, a bar coater, a kiss coater, a roll coater, a gravure coater, and a die coater.
[0306] The drying temperature when drying the coating film of the resin composition (1) and the resin composition (2) is not particularly limited, but is preferably 60° C. to 150° C., more preferably 70° C. to 120° C., and even more preferably 80° C. to 100° C. The drying time is not particularly limited, but is preferably 1 minute to 60 minutes, more preferably 2 minutes to 30 minutes, and even more preferably 5 minutes to 20 minutes.
[0307] Examples of the material of the carrier film include polyesters such as polyethylene terephthalate and polybutylene terephthalate, and polyolefins such as polypropylene and polyethylene. The thickness of the carrier film is not particularly limited, but is preferably 5 μm to 100 μm, more preferably 10 μm to 60 μm, and even more preferably 15 μm to 45 μm.
[0308] [Printed wiring board and method for manufacturing the same]
[0309] The printed wiring board of the present embodiment is a printed wiring board having an interlayer insulating layer which is a cured product of the photosensitive resin film of the present embodiment.
[0310] It should be noted that the “interlayer insulating layer” included in the printed wiring board of the present embodiment also includes an interlayer insulating layer in a state after various processing or treatments such as formation of through holes and wirings and roughening are performed.
[0311] The method for producing a printed wiring board according to the present embodiment is not particularly limited as long as it is a method using the photosensitive resin film according to the present embodiment, but a method for producing a printed wiring board including the following (1) to (4) is preferred.
[0312] (1): The photosensitive resin film of the present embodiment is laminated on one or both surfaces of a circuit board in a state where the second surface is the pasting surface (hereinafter also referred to as "lamination step (1)").
[0313] (2): The photosensitive resin film laminated in the above (1) is exposed and developed to form an interlayer insulating layer having a through hole (hereinafter also referred to as "through hole forming step (2)").
[0314] (3): The interlayer insulating layer having the through-hole is heated and cured (hereinafter also referred to as "heat-curing step (3)").
[0315] (4): A circuit pattern is formed on the surface of the interlayer insulating layer on the opposite side to the circuit substrate (hereinafter also referred to as "circuit pattern forming step (4)").
[0316] Below, refer to Figure 1 A method for manufacturing a printed wiring board according to the present embodiment will be described.
[0317] It should be noted that, in this specification, for convenience, a predetermined operation may be referred to as "XX step" in some cases, but this "XX step" is not limited to the method specifically described in this specification.
[0318] (Lamination process (1))
[0319] In the lamination step (1), the photosensitive resin film of the present embodiment is laminated on one or both surfaces of the circuit board in a state where the second surface serves as an attachment surface.
[0320] Figure 1 (a) shows a process of forming a photosensitive layer 103 on both surfaces of a substrate 101 having a circuit pattern 102 .
[0321] The photosensitive layer 103 can be formed by laminating the photosensitive resin film of this embodiment on both surfaces of the substrate 101 such that the second surface serves as an attachment surface.
[0322] Lamination may be performed by pressure bonding while applying pressure and heat using, for example, a vacuum laminator or the like.
[0323] When a carrier film is attached to the photosensitive layer 103 after lamination, the carrier film may be peeled off before exposure described later or after exposure.
[0324] (Through-hole forming step (2))
[0325] In the through-hole forming step (2), the photosensitive layer formed in the lamination step (1) is exposed and developed to form an interlayer insulating layer having a through-hole.
[0326] Figure 1 (b) shows a process of forming the interlayer insulating layer 104 having the through hole 105 by exposing and developing the photosensitive layer 103 .
[0327] The photosensitive layer 103 is exposed to light, thereby initiating a photoradical polymerization reaction and curing the photosensitive resin film.
[0328] The exposure method of the photosensitive layer 103 can be, for example, a mask exposure method in which active light is irradiated in an image form through a negative or positive mask pattern called an artwork, or a method in which active light is irradiated in an image form through a direct drawing exposure method such as an LDI (Laser Direct Imaging) exposure method or a DLP (Digital Light Processing) exposure method.
[0329] Examples of the light source for active light rays include carbon arc lamps, mercury vapor arc lamps, high pressure mercury lamps, xenon lamps, gas lasers such as argon lasers, solid lasers such as YAG lasers, and known light sources that efficiently radiate ultraviolet rays or visible light such as semiconductor lasers.
[0330] The exposure amount can be appropriately adjusted according to the light source used and the thickness of the photosensitive layer. For example, when a photosensitive layer having a thickness of 1 μm to 100 μm is exposed using ultraviolet light from a high-pressure mercury lamp, the exposure amount is not particularly limited, but is preferably 10 to 1,000 mJ / cm 2 , more preferably 50 to 700 mJ / cm 2 , more preferably 150 to 400 mJ / cm 2 .
[0331] Next, if a carrier film exists on the photosensitive layer 103, the carrier film is removed and then development is performed. In the development, the uncured portion of the photosensitive layer 103 is removed, so that the photocured portion is formed as the interlayer insulating layer 104 on the substrate.
[0332] The developing method may be wet developing or dry developing, but wet developing is preferred. As a method based on wet developing, a spray method is preferred from the viewpoint of improving resolution.
[0333] Examples of the developer include alkaline aqueous solutions, water-based developers, and organic solvent-based developers. Among these, alkaline aqueous solutions are preferred.
[0334] After exposure and development, post-exposure may be performed from the viewpoint of improving the curing degree of the interlayer insulating layer. The exposure amount in the post-exposure is not particularly limited, but is preferably 0.2 to 10 J / cm 2 , more preferably 0.5 to 5 J / cm 2 .
[0335] The shape of the through hole is not particularly limited. If described in terms of cross-sectional shape, for example, a quadrilateral, an inverted trapezoid, etc. can be listed. It should be noted that an inverted trapezoid is a shape in which the upper side is longer than the lower side. In addition, if described in terms of a top view, a circle, a quadrilateral, etc. can be listed.
[0336] In the through-hole formation by photolithography of the present embodiment, a through-hole having an inverted trapezoidal cross-sectional shape can be formed. A through-hole having such a shape is preferred because the copper plating layer has high coverage (recovery) on the through-hole wall surface.
[0337] In the through-hole formation based on the photolithography method of this embodiment, the diameter of the through-hole can be made smaller than the diameter of the through-hole made by laser processing. The diameter of the through-hole formed by the manufacturing method of this embodiment can be, for example, less than or equal to 40 μm, less than or equal to 35 μm, or less than or equal to 30 μm. The lower limit of the diameter of the through-hole is not particularly limited, for example, it can be greater than or equal to 15 μm, or greater than or equal to 20 μm.
[0338] (Heating and curing step (3))
[0339] In the heat curing step (3), the interlayer insulating layer having the through hole is heat cured.
[0340] That is, in the heat curing step (3), the curing reaction of the thermosetting component contained in the photosensitive multilayer resin film of the present embodiment is advanced by heating.
[0341] The heating temperature is not particularly limited, but is preferably 100 to 300° C., more preferably 120 to 200° C., and further preferably 150 to 180° C. The heating time is not particularly limited, but is preferably 0.3 to 3 hours, more preferably 0.5 to 2 hours, and further preferably 0.75 to 1.5 hours.
[0342] (Circuit pattern forming step (4))
[0343] Next, a circuit pattern is formed on the surface of the interlayer insulating layer formed above on the side opposite to the circuit substrate. The surface of the interlayer insulating layer on the side opposite to the circuit substrate is a surface corresponding to the first surface after curing.
[0344] From the viewpoint of forming fine wiring, the circuit pattern is preferably formed by a semi-additive method in which roughening treatment, formation of a seed layer, formation of a resist pattern, formation of a copper circuit layer, and removal of the resist pattern are sequentially performed.
[0345] Roughening treatment is a treatment for roughening the surface of the interlayer insulating layer to form a concave and convex anchor point. In the case where smear is generated in the through-hole forming step (2), a roughening liquid can be used to simultaneously perform the roughening treatment and remove the smear. Examples of the roughening liquid include alkaline permanganate roughening liquids such as sodium permanganate roughening liquid, chromium / sulfuric acid roughening liquid, sodium fluoride / chromium / sulfuric acid roughening liquid, and the like.
[0346] Figure 1 (c) shows the step of forming the seed layer 106 .
[0347] The seed layer 106 is used to form a power supply layer for performing copper electroplating.
[0348] The seed layer 106 can be formed by performing chemical copper plating on the entire surface of the through-hole bottom, the through-hole wall surface, and the interlayer insulating layer using a palladium catalyst or the like.
[0349] Figure 1 (d) shows a step of forming a resist pattern 107 on the seed layer 106 .
[0350] The resist pattern 107 can be formed, for example, by thermally pressing a dry film resist onto the seed layer 106 using a roll laminator or the like, and then exposing and developing the resist. As the dry film resist, a commercially available product can be used.
[0351] The exposure of the dry film resist can be performed through a mask having a desired wiring pattern drawn thereon. After exposure, the dry film resist is developed using an alkaline aqueous solution to remove the unexposed portion, thereby forming a resist pattern 107. Then, a plasma treatment can be performed to remove the development residue of the dry film resist as needed.
[0352] Figure 1 (e) shows the step of forming the copper circuit layer 108.
[0353] The copper circuit layer 108 is preferably formed by copper electroplating.
[0354] As the copper electroplating solution used for copper electroplating, for example, a commercially available copper electroplating solution such as a copper electroplating solution containing copper sulfate can be used.
[0355] After copper electroplating, the resist pattern 107 is removed using an alkaline aqueous solution or an amine stripper, and then flash etching to remove the seed layer 106 between wirings and removal of the palladium catalyst are appropriately performed by a known method. Furthermore, a post-baking treatment for sufficiently thermally curing the unreacted thermal curing component may be performed as needed.
[0356] Figure 1 (f) shows a multilayer printed wiring board 100A which is multilayered by repeating the above-mentioned steps and has a solder resist layer 109 on the outermost surface.
[0357] The solder resist layer 109 can be formed using a known photosensitive resin film for solder resist.
[0358] In the above, the method for manufacturing a printed wiring board in which a through hole is formed using the photosensitive resin film of the present embodiment is described, but the photosensitive resin film of the present embodiment is excellent in pattern resolution and is therefore also suitable for forming a cavity for a built-in chip or passive element, for example. With regard to the cavity, for example, in the description of the printed wiring board described above, the cavity can be appropriately formed by setting the drawing pattern when the photosensitive resin film is exposed to form a pattern to form a desired cavity.
[0359] [Semiconductor packaging]
[0360] The semiconductor package of the present embodiment is a semiconductor package including the printed wiring board of the present embodiment.
[0361] The semiconductor package of the present embodiment can be manufactured by, for example, mounting a semiconductor element such as a semiconductor chip or a memory at a predetermined position on a printed wiring board of the present embodiment and sealing the semiconductor element with a sealing resin or the like.
[0362] Example
[0363] Hereinafter, the present embodiment will be described in more detail with reference to Examples, but the present embodiment is not limited to these Examples.
[0364] [Measurement method of acid value]
[0365] The acid value was calculated from the amount of potassium hydroxide aqueous solution required to neutralize the object of measurement.
[0366] [Method for measuring weight average molecular weight (Mw) and number average molecular weight (Mn)]
[0367] The weight average molecular weight (Mw) and number average molecular weight (Mn) were measured by the following GPC measuring device and measuring conditions, and converted and obtained using a calibration curve of standard polystyrene. In the preparation of the calibration curve, 5 sample sets ("PStQuick MP-H" and "PStQuick B", manufactured by Tosoh Corporation) were used as standard polystyrene.
[0368] (GPC measurement device)
[0369] GPC device: High-speed GPC device "HCL-8320GPC", detector is differential refractometer or UV, manufactured by Tosoh Corporation
[0370] Column: Column TSKgel SuperMultipore HZ-H (column length: 15cm, column inner diameter: 4.6mm), manufactured by Tosoh Corporation
[0371] (Measurement conditions)
[0372] Solvent: Tetrahydrofuran (THF)
[0373] Measurement temperature: 40℃
[0374] Flow rate: 0.35ml / min
[0375] Sample concentration: 10mg / THF 5ml
[0376] Injection volume: 20μl
[0377] [Measurement method of fluorine atom concentration]
[0378] The photosensitive resin film with a carrier film produced in each example was irradiated with a light intensity of 400 mJ / cm using a flat exposure machine in a state where the carrier films were provided on both sides. 2 Then, the carrier films on both sides were peeled off and the UV exposure machine was used to irradiate the film at a light intensity of 2 J / cm 2 (wavelength 365nm) ultraviolet rays. Then, a hot air circulation dryer was used to heat at 170°C for 1 hour to obtain a cured photosensitive resin film. The cured photosensitive resin film obtained was embedded with an embedding resin and cured, and then polished using a grinder (manufactured by Refinetec Co., Ltd., trade name "Refine Polisher") to cut out a cross section of the cured photosensitive resin film as a test piece.
[0379] Next, a cross section of the cured product of the photosensitive resin film was observed at 3,000 times using a scanning electron microscope (SEM) (manufactured by Hitachi High-Technologies Corporation, trade name "SU-5000") equipped with an energy dispersive X-ray spectrometer (EDX) as an elemental analysis device. Figure 2 An example of a cross-sectional image 10 of a cured product of a photosensitive resin film is shown in FIG.
[0380] exist Figure 2In the cross-sectional image 10 shown, a reference line BL1 corresponding to one surface and a reference line BL2 corresponding to the other surface are defined.
[0381] It should be noted that when it is determined that the surface of baseline BL1 or baseline BL2 is uneven, at least 10 points can be drawn at equal intervals on the surface position of each layer within the entire range of the cross-sectional image, and the straight line obtained by approximating them by the least squares method can be used as baseline BL1 or baseline BL2.
[0382] Elemental analysis was performed using the above-mentioned elemental analysis device on a measurement line L1 parallel to the baseline BL1 and 1 μm away from the baseline BL1 toward the inner side of the cured product, and a measurement line L2 parallel to the baseline BL2 and 1 μm away from the baseline BL2 toward the inner side of the cured product. It should be noted that the line lengths for elemental analysis were set to 40 μm. The lower fluorine atom concentration of the calculated average fluorine atom concentration was determined as the fluorine atom concentration of the first surface, and the higher fluorine atom concentration was determined as the fluorine atom concentration of the second surface.
[0383] [Manufacturing of photosensitive resin film]
[0384] Examples 1 to 6, Comparative Examples 1 to 3
[0385] The components were mixed according to the composition shown in Table 1 (the units of the numerical values in the table are parts by mass, and in the case of a solution, the amount is calculated as solid content), and kneaded using a three-roll mill and a rotation and revolution mixer. Then, methyl ethyl ketone was added so that the solid content concentration became 65% by mass, thereby obtaining resin compositions (1) and resin compositions (2), respectively.
[0386] Next, the resin composition (1) was coated on a carrier film (PET film, manufactured by Teijin Limited, trade name "G2-16", thickness 16 μm) and dried at 100° C. for 10 minutes using a hot air convection dryer to form a resin composition (1) film with a carrier film (the thickness of the resin composition (1) film was 5 μm).
[0387] In addition, the resin composition (2) was coated on a carrier film different from the above (PET film manufactured by Teijin Limited, trade name "G2-16", thickness 16 μm), and dried at 100°C for 10 minutes using a hot air convection dryer to form a resin composition (2) film with a carrier film (the thickness of the resin composition (2) film was 20 μm).
[0388] The resin composition films of the resin composition (1) with a carrier film and the resin composition (2) with a carrier film obtained above were bonded together to obtain a photosensitive resin film with a carrier film (photosensitive resin film thickness: 25 μm).
[0389] The following evaluations were performed using the produced photosensitive resin film. The evaluation results are shown in Table 2 together with the content of each component in the photosensitive resin film.
[0390] [Determination of relative dielectric constant (Dk) and dielectric loss tangent (Df)]
[0391] Two films were prepared in which the carrier film on the second surface side of the photosensitive resin film with a carrier film produced in each example was peeled off and removed, and the second surfaces were bonded together.
[0392] Next, with the carrier films on both sides, the substrate was irradiated with a light intensity of 400 mJ / cm using a flat exposure machine. 2 Next, the carrier films on both sides were peeled off and the UV exposure machine was used to irradiate the film at a light intensity of 2 J / cm 2 Then, the sample was heated at 170°C for 1 hour using a hot air circulation dryer and cut into pieces of 7 cm x 10 cm in size to prepare a sample for measuring relative dielectric constant (Dk) and dielectric loss tangent (Df).
[0393] The obtained measurement sample was dried at 105°C for 10 minutes using a hot air circulation dryer, and then the relative dielectric constant (Dk) and dielectric loss tangent (Df) were measured in the 10 GHz frequency band using a separated column dielectric resonator method (SPDR method), and evaluated according to the following criteria.
[0394] (Evaluation criteria for relative dielectric constant (Dk))
[0395] A: Less than or equal to 2.8
[0396] B: greater than 2.8 to less than or equal to 3.0
[0397] C: greater than 3.0
[0398] (Evaluation criteria for dielectric loss tangent (Df))
[0399] A: Less than or equal to 0.0100
[0400] B: greater than 0.0100 to less than or equal to 0.0120
[0401] C: greater than 0.0120
[0402] [Evaluation of through-hole resolution]
[0403] (1) Preparation of evaluation laminate
[0404] The copper foil surface of a printed wiring board substrate (Showa Denko Materials Co., Ltd., trade name "MCL-E-679") with copper foil (thickness 12 μm) laminated on a glass epoxy substrate was roughened using a roughening pretreatment liquid (manufactured by MEC Co., Ltd., trade name "CZ-8100"), and then washed and dried. Next, the carrier film on the second surface side of the photosensitive resin film with a carrier film manufactured in each example was peeled off and removed, and laminated on the copper foil of the printed wiring board substrate after the above roughening pretreatment in such a way that the exposed second surface becomes the adhesive surface. It should be noted that a pressing vacuum laminator (manufactured by Meiki Manufacturing Co., Ltd., trade name "MVLP-500") was used for lamination, and the lamination conditions were set to a pressing hot plate temperature of 70°C, a vacuuming time of 20 seconds, a lamination pressing time of 30 seconds, an air pressure of less than or equal to 4 kPa, and a crimping pressure of 0.4 MPa. After the lamination treatment, the film was left to stand at room temperature for 1 hour or more, thereby obtaining a laminate for evaluation in which a photosensitive resin film and a carrier film were laminated in this order on the copper foil surface of the printed wiring board substrate.
[0405] (2) Sensitivity measurement
[0406] A 41-step exposure meter was placed on the carrier film of the evaluation laminate obtained above. Then, exposure was performed using a direct imaging exposure device (manufactured by ORC Manufacturing Co., Ltd., trade name "DXP-3512") using an ultra-high pressure mercury lamp as a light source. The exposure pattern used was The points are arranged in a grid-like dot pattern.
[0407] After exposure, the film was left at room temperature for 30 minutes, and then the carrier film on the first surface side of the evaluation laminate obtained above was removed. The photosensitive resin film in the unexposed part was spray-developed for 60 seconds using a 1 mass % sodium carbonate aqueous solution at 30°C. After development, the exposure energy when the gloss residual stage number of the 41-stage step exposure meter reached 4.0 was taken as the sensitivity of the photosensitive resin film (unit: mJ / cm 2 ). Using the pattern exposed at this sensitivity, evaluation was performed according to the following evaluation criteria.
[0408] (3) Evaluation of through-hole resolution
[0409] The resolution of the through-holes was evaluated by observing a through-hole pattern formed by exposure and spray development at the exposure energy, which is the sensitivity of the photosensitive resin film obtained in (2), using an optical microscope and evaluating the resolution based on the following criteria.
[0410] (Evaluation Criteria)
[0411] A: Dot pattern The through hole is partially opened.
[0412] C: Dot pattern The through hole portion is not opened.
[0413] [Evaluation of bonding strength with copper plating]
[0414] (1) Preparation of evaluation laminate and measurement of sensitivity of photosensitive resin film
[0415] In the steps (1) and (2) of the above-mentioned [Evaluation of the resolution of through holes], except that the exposure machine used was changed to a parallel light exposure machine using an ultra-high pressure mercury lamp as a light source (manufactured by ORC Manufacturing Co., Ltd., trade name "EXM-1201"), the same operations as in the steps (1) and (2) of the above-mentioned [Evaluation of the resolution of through holes] were performed to prepare a laminate for evaluation, and the exposure energy when the gloss residual stage number was 8.0 was determined and used as the sensitivity of the photosensitive resin film (unit: mJ / cm 2 ).
[0416] (2) Exposure and Development Process
[0417] The carrier film on the first surface side of the evaluation laminate was peeled off and the entire surface was exposed at the sensitivity, i.e., exposure energy, to cure the photosensitive resin film. After exposure, the film was left at room temperature for 30 minutes, and then the unexposed portion of the photosensitive resin film was spray developed for 60 seconds using a 1 mass % sodium carbonate aqueous solution at 30°C.
[0418] (3) Post-curing treatment
[0419] Next, a high-pressure mercury lamp irradiation type UV delivery device (manufactured by ORC Manufacturing Co., Ltd.) was used to expose the sample at an exposure dose of 2 J / cm 2 The film was then post-cured with UV light at a conveying speed of 1.50°C. Then, it was heated at 170°C for 1 hour using a hot air circulation dryer.
[0420] (4) Roughening treatment
[0421] The heated evaluation laminate was treated with a swelling liquid "Swelling Dip Securiganth P" at 70°C for 5 minutes, and then roughened with a roughening liquid "Dosing Securiganth P500J" at 70°C for 10 minutes. Next, a neutralization treatment was performed at 50°C for 5 minutes using a neutralizing liquid "Reduction Conditioner Securiganth P500". Then, a hydrofluoric acid treatment was performed at room temperature for 10 minutes using a buffered hydrofluoric acid "LAL1800 SA High Purity Buffered Hydrofluoric Acid". It should be noted that the swelling liquid, the roughening liquid, and the neutralizing liquid were all made by ATOTECH JAPAN Co., Ltd., and the buffered hydrofluoric acid was made by Stella Chemifa Co., Ltd.
[0422] (5) Plating treatment
[0423] The roughened laminate was subjected to chemical plating at 30°C for 15 minutes using a chemical plating solution "Priganth MSK-DK" (manufactured by ATOTECH JAPAN Co., Ltd.). Then, the roughened laminate was subjected to chemical plating at 24°C, 2 A / dm 2 The electroplating treatment was performed for 1.5 hours to form copper plating on the interlayer insulating layer. The thickness of the copper plating was 25 μm.
[0424] (6) Measurement of bonding strength with copper plating
[0425] The adhesive strength with the copper plating layer was evaluated by measuring the vertical peel strength at 23° C. in accordance with JIS C6481:1996 based on the following criteria.
[0426] (Evaluation Criteria)
[0427] A: greater than 0.4kN / m
[0428] B: greater than 0.1kN / m to less than or equal to 0.4kN / m
[0429] C: less than or equal to 0.1kN / m
[0430] [Table 1]
[0431]
[0432] [Table 2]
[0433]
[0434] The details of each component described in Table 1 and Table 2 are as follows.
[0435] [(A) ingredient]
[0436] Compound having a carboxyl group and an acryloyl group: manufactured by Nippon Kayaku Co., Ltd., trade name "ZXR-1807H", acid value: 110 mgKOH / g, weight average molecular weight (Mw): 2,000
[0437] [(B) ingredient]
[0438] · Biphenyl aralkyl type epoxy resin: manufactured by Nippon Kayaku Co., Ltd., trade name "NC-3000-L", epoxy equivalent: 272 g / eq
[0439] · Naphthol-type epoxy resin: manufactured by Nippon Steel & Sumitomo Metal Corporation, trade name "ESN-475V", epoxy equivalent: 325 g / eq
[0440] Maleimide resin: Aromatic bismaleimide resin with indane skeleton
[0441] [(C) ingredient]
[0442] Photopolymerization initiator 1: phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide
[0443] Photopolymerization initiator 2: 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazol-3-yl]ethanone 1-(O-acetyl oxime)
[0444] [(D) ingredient]
[0445] Silica 1: manufactured by Admatechs Co., Ltd., trade name "SC2050-MB", average particle size (D 50 ): 0.5μm, true density 2,200kg / m 3
[0446] Silica 2: manufactured by TAT, trade name "BQQ-0710SCB", average particle size (D 50 ): 0.7μm, true density 1,350kg / m 3
[0447] [(E) ingredient]
[0448] Polytetrafluoroethylene particles: manufactured by Mitsubishi Pencil Co., Ltd., trade name "MPT-N8", average particle size (D 50 ): 0.2~0.3μm
[0449] [(F)INGREDIENT]
[0450] Polybutadiene-based elastomer: butadiene-styrene-random copolymer, manufactured by Cray Valley, trade name "Ricon 100", number average molecular weight (Mn): 4,500
[0451] Acid anhydride-modified polybutadiene: manufactured by Cray Valley Corporation, trade name "Ricon 131 MA17", number average molecular weight (Mn): 5,400, number of acid anhydride groups in one molecule: 9
[0452] [(G) ingredient]
[0453] Organic peroxide: 1,3-di(tert-butylperoxyisopropyl)benzene
[0454] [(H) ingredient]
[0455] Curing accelerator: 1-benzyl-2-phenylimidazole
[0456] [(I)INGREDIENTS]
[0457] Sensitizer: 4,4'-bis-(diethylamino)benzophenone
[0458] ·Inhibitor: 4-tert-butylcatechol
[0459] According to Table 2, the cured products formed from the photosensitive resin films of Examples 1 to 6 of the present embodiment all have excellent dielectric properties and high conductor adhesion.
[0460] Description of Reference Numerals
[0461] BL1: Baseline
[0462] BL2: Baseline
[0463] L1: Measurement line
[0464] L2: Measurement line
[0465] 10: Cross-sectional image
[0466] 100A: Multilayer printed wiring board
[0467] 101: Substrate
[0468] 102: Circuit pattern
[0469] 103: Photosensitive layer
[0470] 104: Interlayer insulation layer
[0471] 105: Through hole
[0472] 106: Seed layer
[0473] 107: Resist pattern
[0474] 108: Copper circuit layer
[0475] 109: Solder mask layer.
Claims
1. A photosensitive resin film comprising: (A) a compound having an ethylenically unsaturated group, (B) a thermosetting resin, (C) a photopolymerization initiator, (D) an inorganic filler, and (E) a fluorine-containing resin, The photosensitive resin film has a first surface and a second surface opposite to the first surface. The fluorine atom concentration at a depth of 1 μm from the first surface is lower than the fluorine atom concentration at a depth of 1 μm from the second surface. 2 . The photosensitive resin film according to claim 1 , comprising a compound having an ethylenically unsaturated group and an acidic substituent as the (A) compound having an ethylenically unsaturated group. 3 . The photosensitive resin film according to claim 1 , comprising at least one selected from the group consisting of epoxy resins, maleimide resins, allyl resins, and vinyl resins as the (B) thermosetting resin. 4 . The photosensitive resin film according to claim 1 , comprising silicon dioxide as the (D) inorganic filler, wherein the content of the silicon dioxide is 2 to 60% by mass.
5. The photosensitive resin film according to claim 1, comprising a true density of less than or equal to 1,500 kg / m 3 Silica is used as the (D) inorganic filler. 6 . The photosensitive resin film according to claim 1 , wherein the content of the (E) fluorine-containing resin is 5 to 80% by mass based on the total amount of resin components of the photosensitive resin film. 7 . The photosensitive resin film according to claim 1 , further comprising (F) an elastomer. 8 . The photosensitive resin film according to claim 1 , wherein the first surface is a surface on which a circuit pattern is formed by copper plating, and the second surface is a pasting surface when the photosensitive resin film is laminated. 9 . The photosensitive resin film according to claim 1 , which is used to form an interlayer insulating layer having an optical through hole. 10 . A printed wiring board comprising an interlayer insulating layer which is a cured product of the photosensitive resin film according to claim 1 .
11. A semiconductor package comprising the printed wiring board according to claim 10.
12. A method for manufacturing a printed wiring board, comprising the steps (1) to (4), (1) The photosensitive resin film according to any one of claims 1 to 9 is laminated on one or both surfaces of a circuit board in a state where the second surface serves as an adhesive surface; (2): exposing and developing the photosensitive resin film laminated in (1) to form an interlayer insulating layer having a through hole; (3): heating and curing the interlayer insulating layer having the through hole; (4) A circuit pattern is formed on a surface of the interlayer insulating layer opposite to the circuit substrate.