Conductive paste, electronic component, and laminated ceramic capacitor

By adding rosin derivatives with hydroxyl or amine groups to the conductive paste, the problem of insufficient clinging between conductive paste and substrate in the manufacturing of laminated ceramic capacitors is solved, and high clinging and electrical characteristics are achieved. Suitable for miniaturized and high-capacity electronic components.

CN118946940APending Publication Date: 2024-11-12SUMITOMO METAL MINING CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380030841.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-28
Filing Date
2023-03-28
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

During the manufacturing process of laminated ceramic capacitors, when the crimping time and pressure are shortened, the tightness between the conductive paste and the substrate is insufficient, resulting in a position shift of the dry film, affecting electrical characteristics and yield.

Method used

A conductive slurry containing conductive powder, ceramic powder, binder resin and organic solvent is used, and a rosin derivative having a hydroxyl group or an amine group is added therein to improve the clinging to the substrate.

Benefits of technology

The firmness of the dry film and ceramic green sheet is significantly improved, and the high firmness and electrical characteristics of the laminated ceramic capacitor are ensured, and it is suitable for miniaturized and high-capacity electronic components.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118946940A_ABST
    Figure CN118946940A_ABST
Patent Text Reader

Abstract

Provided is an electroconductive paste capable of further improving adhesion to a base material. The conductive paste contains a conductive powder, an additive, a binder resin, and an organic solvent, and contains, as an additive, a rosin derivative having a hydroxyl group or an amine group.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a conductive paste, an electronic component, and a multilayer ceramic capacitor. Background Art

[0002] As electronic devices such as mobile phones and digital devices become smaller and more powerful, electronic components including multilayer ceramic capacitors are also expected to be smaller and have higher capacity. Multilayer ceramic capacitors have a structure in which multiple dielectric layers and multiple internal electrode layers are alternately stacked. By making the dielectric layers and internal electrode layers thinner, miniaturization and higher capacity can be achieved.

[0003] The multilayer ceramic capacitor is manufactured, for example, in the following manner. First, a layer containing barium titanate (BaTiO 3 ) and a raw sheet of dielectric powder and binder resin, a conductive paste for internal electrodes is printed in a predetermined electrode pattern, and dried to form a dry film (conductive film). Next, the dry film and the raw sheet are stacked in an alternating overlapping manner to obtain a laminate. Next, the laminate is heated and pressed to form a press-bonded body. The press-bonded body is cut, and after the organic binder is removed in an oxidizing atmosphere or an inactive atmosphere, it is fired to obtain a fired chip. Next, the slurry for external electrodes is applied to both ends of the fired chip, and after firing, the surface of the external electrode is plated with nickel, etc. to obtain a multilayer ceramic capacitor.

[0004] In the process of heating, pressing and cutting the laminated body formed by stacking the dry film and the green sheet, if the adhesion between the dry film and the green sheet (substrate) is insufficient, the dry film (conductive film) may peel off from the green sheet (substrate) or the layer structure may shift, and the resulting multilayer ceramic capacitor may not have the desired electrical properties.

[0005] For example, Patent Document 1 discloses a conductive paste, the purpose of which is to improve the adhesion of a conductive paste containing a (meth)acrylic resin as a binder resin to a ceramic green sheet. The conductive paste contains a (meth)acrylic resin as a binder resin, an organic solvent, and a metal powder, wherein the (meth)acrylic resin has a glass transition temperature Tg in the range of -60°C to 120°C, a hydroxyl group in the molecule in the range of 0.01 mass % to 5 mass %, an acid value in the range of 1 mgKOH / g to 50 mgKOH / g, and a weight average molecular weight in the range of 10,000 Mv to 350,000 Mv.

[0006] In addition, Patent Document 2 discloses a conductive paste, the purpose of which is to provide a conductive paste capable of forming a conductive film having excellent adhesion to a substrate, the conductive paste being used to form an electrode layer on a substrate, the conductive paste comprising a conductive powder, a resin binder, an organic additive and an organic solvent, the organic additive comprising a (meth)acrylate compound having two or more (meth)acryloyl groups in one molecule and a number average molecular weight of less than 1000.

[0007] In addition, Patent Document 3 discloses a dry film for internal electrodes of a multilayer ceramic capacitor for the purpose of providing a dry film for internal electrodes that can form internal electrodes that have excellent adhesion to a dielectric layer and whose shape does not significantly change before and after a heat treatment. The dry film is formed from a composition containing a conductive powder and an organic binder resin, and is characterized in that the dry film for internal electrodes has a Vickers hardness of 47 Hv or more and 51 Hv or less.

[0008] Prior art literature

[0009] Patent Literature

[0010] Patent Document 1: International Publication No. 2013 / 187183

[0011] Patent Document 2: Japanese Patent Application Publication No. 2018-055933

[0012] Patent Document 3: Japanese Patent Application Publication No. 2019-121744 Summary of the invention

[0013] Problems to be solved by the invention

[0014] In recent years, in order to improve productivity and reduce costs, in the manufacturing process of multilayer ceramic capacitors, when a laminated body obtained by alternately laminating dry films and ceramic green sheets is subjected to heat compression, the pressing time during compression is sometimes shortened and the pressure is reduced.

[0015] However, when the pressing time during crimping is shortened or the pressure is reduced, conventional conductive pastes sometimes fail to achieve sufficient adhesion between the dry film and the substrate, resulting in positional deviation of the dry film and a reduction in yield. Therefore, conductive pastes that can further improve adhesion to the substrate when forming a dry film are required.

[0016] In view of such circumstances, an object of the present invention is to provide a conductive paste capable of further improving the adhesion with a substrate.

[0017] Means used to solve problems

[0018] In a first aspect of the present invention, there is provided a conductive paste comprising a conductive powder, an additive, a binder resin, and an organic solvent, wherein the conductive paste comprises a rosin derivative having a hydroxyl group or an amine group as the additive.

[0019] In addition, preferably, the rosin derivative is contained in an amount of 0.01 mass % or more and 2.0 mass % or less relative to the whole conductive paste. In addition, preferably, the temperature at which the weight reduction rate of the compound in thermogravimetric analysis reaches the maximum is 200°C or more. In addition, preferably, the molecular weight of the rosin derivative is 250 or more and 3000 or less. Preferably, the conductive paste further contains an acidic dispersant and / or an alkaline dispersant. In addition, preferably, the conductive powder contains at least one metal powder selected from Ni, Pd, Pt, Au, Ag, Cu and their alloys. In addition, preferably, the average particle size of the conductive powder is 0.05 μm or more and 1.0 μm or less. In addition, preferably, the binder resin contains a butyral resin. In addition, preferably, the conductive paste further contains ceramic powder. In addition, preferably, the ceramic powder contains barium titanate. In addition, preferably, the average particle size of the ceramic powder is 0.01 μm or more and 0.5 μm or less. In addition, preferably, the ceramic powder is contained in an amount of 1 mass % or more and 20 mass % or less relative to the whole conductive paste. In addition, preferably, the conductive paste is used for the internal electrodes of the multilayer ceramic component.

[0020] In a second aspect of the present invention, there is provided an electronic component formed using the conductive paste.

[0021] According to a third aspect of the present invention, there is provided a multilayer ceramic capacitor including at least a laminated body in which dielectric layers and internal electrode layers are laminated, wherein the internal electrode layers are formed using the conductive paste.

[0022] Effects of the Invention

[0023] The conductive paste of the present invention can further improve the adhesion to the substrate. In addition, in the manufacturing process of a multilayer ceramic capacitor, the dried film (internal electrode layer) formed using the conductive paste of the present invention has high adhesion to the green sheet (dielectric layer). BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 1 and 2 are a perspective view and a cross-sectional view showing a multilayer ceramic capacitor according to an embodiment. DETAILED DESCRIPTION

[0025] [Conductive paste]

[0026] The conductive paste of the present embodiment includes conductive powder, ceramic powder, a dispersant, a binder resin, and an organic solvent. Hereinafter, each component will be described in detail.

[0027] (Conductive powder)

[0028] As the conductive powder, there is no particular limitation, and metal powder can be used, for example, powders of one or more selected from Ni, Pd, Pt, Au, Ag, Cu and their alloys can be used. Among them, from the viewpoints of conductivity, corrosion resistance and cost, powder of Ni or its alloy (hereinafter sometimes referred to as "Ni powder") is preferred. As Ni alloy, for example, alloys of Ni and at least one element selected from the group consisting of Mn, Cr, Co, Al, Fe, Cu, Zn, Ag, Au, Pt and Pd can be used. The content of Ni in the Ni alloy is, for example, 50% by mass or more, preferably 80% by mass or more. In addition, in order to suppress the rapid gas generation caused by the partial thermal decomposition of the binder resin during the debinding process, the Ni powder can contain about hundreds of ppm of element S.

[0029] The average particle size of the conductive powder is preferably 0.05 μm or more and 1.0 μm or less, and more preferably 0.1 μm or more and 0.5 μm or less. When the average particle size of the conductive powder is within the above range, it can be suitably used as a slurry for internal electrodes of thin-film multilayer ceramic capacitors (multilayer ceramic components). The average particle size is a value obtained by observation using a scanning electron microscope (SEM), and is an average value (SEM average particle size) obtained by measuring the particle size of each of a plurality of particles in an image obtained by observation at a magnification of 10,000 times using an SEM.

[0030] The content of the conductive powder is preferably 30% by mass or more and less than 70% by mass, more preferably 40% by mass or more and 60% by mass or less, relative to the entire conductive paste. When the content of the conductive powder is within the above range, the conductivity and dispersibility are excellent.

[0031] (Ceramic powder)

[0032] The ceramic powder is not particularly limited. For example, in the case of a slurry for internal electrodes of a multilayer ceramic capacitor, a known ceramic powder can be appropriately selected according to the type of multilayer ceramic capacitor to be used. As the ceramic powder, for example, a perovskite oxide containing Ba and Ti can be used, preferably barium titanate (BaTiO 3 ).

[0033] As the ceramic powder, a ceramic powder containing barium titanate as a main component and oxides as a secondary component may be used. Examples of the oxides include oxides of Mn, Cr, Si, Ca, Ba, Mg, V, W, Ta, Nb, and one or more rare earth elements. In addition, as the ceramic powder, for example, barium titanate (BaTiO 3 ) is a perovskite-type oxide ferroelectric ceramic powder in which the Ba atoms and Ti atoms are replaced by other atoms such as Sn, Pb, Zr, etc.

[0034] When used as a conductive paste for internal electrodes, the ceramic powder may be a powder having the same composition as the dielectric ceramic powder constituting the green sheet of the multilayer ceramic capacitor (electronic component). This can suppress the occurrence of cracks caused by the mismatch of shrinkage at the interface between the dielectric layer and the internal electrode layer during the sintering process. Examples of such ceramic powders include ZnO, ferrite, PZT, BaO, Al 2 O 3 、Bi 2 O 3 , R (rare earth elements) 2 O 3 、TiO 2 、Nd 2 O 3 Oxides such as ethylene and ethylene. In addition, the ceramic powder may be used alone or in combination of two or more.

[0035] The average particle size of the ceramic powder is, for example, greater than 0.01 μm and less than 0.5 μm, preferably greater than 0.01 μm and less than 0.3 μm. By setting the average particle size of the ceramic powder to the above range, when used as an internal electrode slurry, a sufficiently fine and thin uniform internal electrode can be formed. The average particle size is a value obtained by observation using a scanning electron microscope (SEM), and is an average value (SEM average particle size) obtained by measuring the particle size of each of a plurality of particles from an image obtained by observation using an SEM at a magnification of 50,000 times.

[0036] The content of the ceramic powder is preferably 1% to 20% by mass, more preferably 3% to 15% by mass, relative to the entire conductive paste. When the content of the ceramic powder is within the above range, dispersibility and sinterability are excellent.

[0037] The content of the ceramic powder is preferably 1 part by mass or more and 30 parts by mass or less, and more preferably 3 parts by mass or more and 30 parts by mass or less, based on 100 parts by mass of the conductive powder.

[0038] (Binder resin)

[0039] As a binder resin, a butyral resin is preferably included. In addition, when used as an internal electrode paste, from the viewpoint of improving the bonding strength with the green sheet, a butyral resin may be included, or a butyral resin may be used alone. As a butyral resin, polyvinyl butyral (PVB) can be cited. When the conductive paste contains a butyral resin, the bonding strength with the green sheet can be further improved.

[0040] The content of the butyral resin can be, for example, 20% by mass or more, 40% by mass or more, more than 50% by mass, or 60% by mass or more relative to the entire binder resin. When the content of the butyral resin is within the above range, the adhesiveness is further improved, and the bonding strength between the dry film and the green sheet (substrate) is improved.

[0041] In addition, the upper limit of the content of the butyral resin is not particularly limited, for example, it can be 90% by mass or less, or 80% by mass or less relative to the entire binder resin. When the content of the butyral resin is within the above range, since the conductive paste has a moderate hardness, it is not easy to cause undesirable situations such as the printed film not being peeled off from the support film and the electrode being broken during thermal compression bonding.

[0042] In addition, the weight average molecular weight (Mw) of the butyral resin can be 30,000 to 300,000, 50,000 to 200,000, or 100,000 to 150,000. In addition, the glass transition temperature Tg of the butyral resin can be 50°C to 90°C, or 60°C to 80°C. By including the additives described below together with the butyral resin having the above-mentioned characteristics, a conductive paste with further improved adhesion can be obtained. In addition, the butyral resin can be used alone or in combination of two or more.

[0043] In addition, resins other than butyral resins may also be included as binder resins. As binder resins other than the above, there are no particular limitations, and known resins may be used, for example, cellulose resins such as methyl cellulose, ethyl cellulose, ethyl hydroxyethyl cellulose, and nitrocellulose, acrylic resins, etc. Among them, from the viewpoints of solubility in solvents, combustion decomposition, etc., it is preferred to include a cellulose resin, and more preferably to include ethyl cellulose.

[0044] For example, when a cellulose resin is included as a binder resin, the weight average molecular weight (Mw) may be 10,000 to 300,000, 30,000 to 250,000, or 50,000 to 200,000. In addition, the hydroxyl value of the cellulose resin is not particularly limited, but is preferably 0.1 mgKOH / g to 15 mgKOH / g, more preferably 0.5 mgKOH / g to 7 mgKOH / g, and further preferably 1.5 mgKOH / g to 3 mgKOH / g. In addition, the cellulose resin may contain one alone or two or more. When the content of the cellulose resin is high, the glass transition temperature Tg described later sometimes increases and reduces the adhesion, so it is preferred that the combination contains a butyral resin.

[0045] In addition, when the binder resin includes a cellulose resin and a butyral resin, from the viewpoint of improving adhesion, relative to the total content (100% by mass) of the cellulose resin and the butyral resin, the butyral resin may be included in an amount of 20% by mass or more, 40% by mass or more, more than 50% by mass, or more than 60% by mass. When the content of the two resins is within the above range, sometimes the adhesion is further improved, and the bonding strength between the dry film and the raw sheet (substrate) is improved. In addition, the upper limit of the content of the butyral resin is not particularly limited, and may be less than 100% by mass, or less than 90% by mass, or less than 80% by mass. When the content of the two resins is within the above range, the conductive paste can have a moderate hardness, and it is not easy to have undesirable conditions such as the printed film not peeling off from the supporting film and the electrode breaking during hot pressing, and it has high adhesion with the raw sheet.

[0046] The content of the binder resin is preferably 0.5% by mass or more and 10% by mass or less, and more preferably 1% by mass or more and 7% by mass or less, relative to the entire conductive paste. When the content of the binder resin is within the above range, the conductivity and dispersibility are excellent.

[0047] The content of the binder resin is preferably 1 part by mass or more and 20 parts by mass or less, and more preferably 1 part by mass or more and 14 parts by mass or less, based on 100 parts by mass of the conductive powder.

[0048] (Organic Solvent)

[0049] The organic solvent is not particularly limited, and any known organic solvent that can dissolve the binder resin can be used. Examples of the organic solvent include terpene solvents, acetate solvents, ether solvents, and ketone solvents.

[0050] Examples of the terpene solvent include terpineol, dihydroterpineol, and dihydroterpineol acetate.

[0051] Examples of the acetate solvent include isobornyl acetate, isobornyl propionate, isobornyl butyrate, and isobornyl isobutyrate; glycol ether acetates such as ethylene glycol monobutyl ether acetate, diethylene glycol monobutyl ether acetate, diethylene glycol monoethyl ether acetate, dipropylene glycol methyl ether acetate, 3-methoxy-3-methylbutyl acetate, and 1-methoxypropyl-2-acetate; glycol diacetates such as propylene glycol diacetate, 1,4-butanediol diacetate, 1,3-butanediol diacetate, and 1,6-hexanediol diacetate; and cyclohexanol acetate.

[0052] Examples of the ether solvent include propylene glycol monoalkyl ethers such as propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monopropyl ether, and propylene glycol monobutyl ether; glycol ethers such as diethylene glycol mono-2-ethylhexyl ether, ethylene glycol mono-2-ethylhexyl ether, diethylene glycol monohexyl ether, and ethylene glycol monohexyl ether; dipropylene glycol methyl-n-propyl ether, dipropylene glycol methyl-n-butyl ether, and dipropylene glycol dimethyl ether.

[0053] Examples of the ketone solvent include methyl isobutyl ketone, diisobutyl ketone, etc. When the ketone solvent is contained, the viscosity can be adjusted without impairing the dispersibility, and the drying property can be improved.

[0054] As the organic solvent, at least one selected from the group consisting of terpineol, dihydroterpineol, dihydroterpineol acetate, propylene glycol monobutyl ether, and diethylene glycol monobutyl ether acetate is preferably included. By including the above organic solvent, the compatibility with the binder resin is excellent, and the dispersibility of the filler is excellent.

[0055] The content of the organic solvent (total) is preferably 20% by mass or more and 60% by mass or less, and more preferably 25% by mass or more and 45% by mass or less, relative to the total amount of the conductive paste. When the content of the organic solvent is within the above range, the conductivity and dispersibility are excellent.

[0056] The content of the organic solvent is preferably 50 parts by mass or more and 130 parts by mass or less, and more preferably 60 parts by mass or more and 90 parts by mass or less, relative to 100 parts by mass of the conductive powder. When the content of the organic solvent is within the above range, the conductivity and dispersibility are excellent.

[0057] In addition, the organic solvent may be used alone or in combination of two or more. For example, when two or more organic solvents are included, at least one selected from the group consisting of terpineol, dihydroterpineol, dihydroterpineol acetate (DHTA), propylene glycol monobutyl ether, and diethylene glycol monobutyl ether acetate, and a hydrocarbon solvent may be included. In addition, at least one selected from methyl isobutyl ketone and diisobutyl ketone may be included together with the above organic solvents.

[0058] Examples of hydrocarbon solvents include solvents containing tridecane, nonane, cyclohexane, etc., mineral spirits, cycloalkane solvents, etc. Among them, mineral spirits are preferably contained. The content of the hydrocarbon solvent may be 10% by mass or more and 50% by mass or less, or 20% by mass or more and 40% by mass or less relative to the total amount of the organic solvent.

[0059] (additive)

[0060] (a) Rosin derivatives

[0061] The conductive paste according to the present embodiment contains a rosin derivative having a hydroxyl group or an amine group (hereinafter, also simply referred to as a “rosin derivative”) as an additive.

[0062] Here, the rosin derivative refers to a compound derived from abietic acid and the like, and examples thereof include abietic acid and its derivatives such as dehydroabietic acid, dihydroabietic acid, tetrahydroabietic acid, diabietic acid, neoabietic acid, pimaric acid-type resin acids such as levorotatory pimaric acid, hydrogenated rosins obtained by hydrogenating these, and disproportionated rosins obtained by disproportionating these, and compounds having a rosin skeleton. In addition, the rosin skeleton may include a structure in which two or more rosins are bonded, or may include a rosin ester structure.

[0063] As a result of intensive studies, the inventors of the present invention have found that a conductive paste containing a rosin derivative having a hydroxyl group or an amine group can improve the adhesion between a dry film formed from the conductive paste and a ceramic green sheet (dielectric layer).

[0064] The detailed reason is not clear, but it is considered that, for example, by adding the above-mentioned rosin derivative, the interaction between resins is inhibited, thereby making the dry film moderately softened, and the dry film that becomes easily deformed due to the softening and the resin that does not interact with each other are easily entangled at the bonding interface, thereby improving the adhesion between the dry film and the ceramic green sheet (dielectric layer).

[0065] The additive can be any rosin derivative having a hydroxyl group or an amine group without any particular limitation, but from the viewpoint of improving adhesion, it is preferably a rosin derivative having a hydroxyl group, more preferably having one or two hydroxyl groups, and further preferably having two hydroxyl groups. The hydroxyl value of the rosin derivative can be, for example, more than 10 mgKOH / g, more than 20 mgKOH / g, more than 50 mgKOH / g, and further more than 100 mgKOH / g. In addition, the upper limit of the hydroxyl value is not particularly limited, for example, less than 200 mgKOH / g. In addition, the rosin derivative preferably does not have an acidic group such as a carboxyl group. The acid value of the rosin derivative can be, for example, less than 20.0 mgKOH / g, or less than 5.0 mgKOH / g.

[0066] The temperature at which the weight loss rate of the above-mentioned rosin derivative in thermogravimetric analysis reaches the maximum (maximum thermal decomposition temperature) may be, for example, 200° C. or above, or 220° C. or above, and preferably 250° C. or above. When the boiling point or thermal decomposition temperature is within the above range, delamination and cracking of the laminate can be suppressed. In addition, the upper limit of the boiling point or thermal decomposition temperature is not particularly limited, and may be, for example, 450° C. or below, or 420° C. or below.

[0067] In addition, the maximum thermal decomposition temperature can be measured by thermogravimetric determination (TG). Specifically, using a thermal decomposition weight measuring device (NETZSCH manufactured, STA25000REGULUS), under a nitrogen atmosphere, the temperature is raised from 20°C to 550°C at a heating rate of 5°C / min, and when the weight loss at this time is measured, the temperature at which the differential heating loss reaches the maximum is taken as the decomposition temperature.

[0068] The molecular weight of the rosin derivative is preferably 250 to 3000, more preferably 250 to 2000, and even more preferably 250 to 1200. When the molecular weight of the rosin derivative is within the above range, adhesion to the ceramic green sheet (dielectric layer) is further improved.

[0069] In addition, the content of the rosin derivative is preferably 0.01% by mass or more and 1.0% by mass or less relative to the conductive paste as a whole. When the content of the rosin derivative is within the above range, the adhesion between the dry film and the ceramic green sheet (dielectric layer) is improved. In addition, from the viewpoint of further improving the adhesion, the lower limit of the content of the rosin derivative can be 0.05% by mass or more, or 0.1% by mass or more relative to the conductive paste as a whole.

[0070] The upper limit of the content of rosin derivatives can be less than 2 mass %, can be less than 1.8 mass %, can be less than 1.5 mass %, can be less than 1.0 mass %, can be less than 1.0 mass %. When the content of rosin derivatives exceeds 1 mass %, although it has high adhesion, when the pressed body of the laminated body of the dry film and the ceramic green sheet is subjected to the debonding process, thermal decomposition sometimes occurs to produce gas. The content of rosin derivatives can be appropriately adjusted within the above range according to the use environment, etc. In addition, the upper limit of rosin derivatives can be less than 0.7 mass %, and can be less than 0.4 mass %. In the conductive paste of the present embodiment, even if the upper limit of rosin derivatives is the above range, it can have high adhesion.

[0071] In addition, the content of the rosin derivative can be appropriately set according to the type and content of the above-mentioned binder resin. For example, the content of the rosin derivative can be set according to the content of the butyral resin. For example, relative to 100 parts by mass of the butyral resin, the rosin derivative can be contained in an amount of 10 parts by mass or more and 90 parts by mass or less, 10 parts by mass or more and 60 parts by mass or less, or 10 parts by mass or more and 50 parts by mass or less.

[0072] (b) Dispersant

[0073] When the conductive paste contains a dispersant, the dispersibility of the conductive powder and the ceramic powder can be improved. As the dispersant, for example, an acidic dispersant, an alkaline dispersant, a nonionic dispersant, an amphoteric dispersant, etc. may be included, preferably at least one of an acidic dispersant and an alkaline dispersant, and more preferably an acidic dispersant. In addition, the above dispersants may be used alone or in combination of two or more.

[0074] As the acidic dispersant, there may be included carboxylic acid dispersants such as higher fatty acids, polycarboxylic acid dispersants, phosphoric acid dispersants, acidic dispersants having acidic groups such as polymer surfactants, etc., preferably at least one of polycarboxylic acid dispersants and phosphoric acid dispersants. In addition, the polycarboxylic acid dispersant may also be a comb-type carboxylic acid having a comb-type structure.

[0075] The higher fatty acid may be an unsaturated carboxylic acid or a saturated carboxylic acid, and is not particularly limited, and examples thereof include higher fatty acids having 11 or more carbon atoms, such as stearic acid, oleic acid, myristic acid, palmitic acid, linoleic acid, lauric acid, and linolenic acid. Among them, oleic acid or stearic acid is preferred.

[0076] Examples of the acidic dispersant include oleoylsarcosine, which is a compound of glycine and oleic acid, and alkyl monoamine salt-type amide compounds using higher fatty acids such as stearic acid and lauric acid instead of oleic acid.

[0077] In addition, from the viewpoint of further improving the separation inhibition effect of the conductive powder and the ceramic powder, a dicarboxylic acid may also be included. A dicarboxylic acid is a carboxylic acid having two carboxyl groups (COO- groups). In addition, the average molecular weight of the dicarboxylic acid is not particularly limited, and for example, may be 200 or more and 1000 or less.

[0078] Examples of alkaline dispersants include aliphatic amines such as laurylamine, abietamine, cetylamine, myristicamine, and stearylamine. When the conductive paste contains the acidic dispersant and the alkaline dispersant, the dispersibility is sometimes better and the viscosity stability over time is also excellent.

[0079] For example, the conductive paste contains 0.01% to 3% by mass of the dispersant relative to the entire conductive paste. The upper limit of the content of the dispersant may be 2% by mass or less, 1% by mass or less, or 0.5% by mass or less. When the content of the dispersant is within the above range, the dispersibility of the conductive paste can be improved, or sheet erosion and poor peeling of the green sheet can be suppressed.

[0080] (c) Other additives

[0081] The conductive paste of the present embodiment may contain other additives in addition to the above components as necessary. As other additives, for example, conventionally known additives such as a defoamer, a plasticizer, a surfactant, and a thickener may be used.

[0082] (Conductive paste)

[0083] The method for producing the conductive paste according to the present embodiment is not particularly limited, and a conventionally known method can be used. The conductive paste can be produced by stirring and kneading the above components using, for example, a three-roll mill, a ball mill, a mixer, or the like.

[0084] The conductive paste involved in this embodiment can improve the adhesion between the dry film and the green sheet by containing the above-mentioned rosin derivative. As a reason for the improvement of the adhesion, as mentioned above, it is believed that the rosin derivative hinders the interaction between resins, thereby making the dry film moderately softened (lowering the glass transition temperature Tg) and becoming easy to deform.

[0085] For example, when the components other than the conductive powder and the ceramic powder in the conductive paste are dried at 120°C for 40 minutes to prepare a dried body (evaluation sample) from which the organic solvent has been removed, the glass transition temperature Tg of the dried body is preferably lower than the glass transition temperature Tg' of the dried body formed under the same conditions except that the above-mentioned rosin derivative is not contained. The above-mentioned rosin derivative may be a rosin derivative that reduces Tg by 5°C or more or 9°C compared to Tg'. For example, the glass transition temperature Tg of the dried body may be below 65°C or below 60°C. In addition, the lower limit of the glass transition temperature Tg is, for example, above 30°C. When the range of the glass transition temperature Tg is within the above range, high adhesion can be achieved. In addition, when the above-mentioned rosin derivative is used as an additive, high adhesion can be achieved even when the lower limit of the glass transition temperature Tg exceeds 55°C.

[0086] In addition, when the conductive paste contains two or more resins as binder resins, a plurality of glass transition temperatures Tg may be measured depending on the resins contained, but the glass transition temperature Tg of the evaluation sample in this specification represents the glass transition temperature Tg in the lowest temperature region. In addition, the glass transition temperature Tg of the dried body (evaluation sample) can be measured by the method described in the examples.

[0087] In addition, when the conductive paste is applied to the surface of the substrate and dried at 75°C for 20 minutes to form a dry film, the Vickers hardness of the dry film surface at room temperature is preferably not more than 10. The lower limit of the Vickers hardness (room temperature) is, for example, not less than 3.5, but may be not less than 5, or not less than 8.

[0088] The Vickers hardness of the dry film surface at 60°C is preferably 8 or less, preferably 9 or less. The lower limit of the Vickers hardness (60°C) is, for example, 3 or more, and may be 5 or more. When measuring the Vickers hardness (60°C) of the dry film, it is preferred to condition the dry film by leaving it at 60°C for 3 minutes.

[0089] The conductive paste can be suitably used for electronic components such as multilayer ceramic capacitors, and can be particularly suitably used as a paste for internal electrodes of multilayer ceramic capacitors.

[0090] [Multilayer Ceramic Capacitors]

[0091] Hereinafter, embodiments of the multilayer ceramic capacitor of the present invention will be described with reference to the accompanying drawings. In the accompanying drawings, the components may be shown schematically or with a changed scale. Figure 1 The position and direction of the components are described using an XYZ orthogonal coordinate system shown in FIG. In the XYZ orthogonal coordinate system, the X direction and the Y direction are horizontal directions, and the Z direction is a vertical direction (up and down direction).

[0092] Figure 1 A in and Figure 1 B in FIG. 1 is a diagram showing a multilayer ceramic capacitor 1. The multilayer ceramic capacitor 1 includes a ceramic multilayer body 10 in which dielectric layers 12 and internal electrode layers 11 are alternately stacked, and external electrodes 20.

[0093] The following is a method for manufacturing a multilayer ceramic capacitor using the above-mentioned conductive paste as a paste for internal electrodes. First, a conductive paste is printed on a ceramic green sheet and dried to form a dry film. After a plurality of ceramic green sheets having the dry film on the upper surface are stacked by crimping to obtain a laminate, the laminate is fired to be integrated, thereby manufacturing a ceramic laminate 10 in which internal electrode layers 11 and dielectric layers 12 are alternately stacked. Thereafter, a pair of external electrodes 20 are formed at both ends of the ceramic laminate 10 to manufacture a multilayer ceramic capacitor 1. The following is a more detailed description.

[0094] First, a green sheet as an unfired ceramic sheet is prepared. As the green sheet, for example, a dielectric layer slurry obtained by adding a binder resin such as polyvinyl butyral and a solvent such as terpineol to a raw material powder of a predetermined ceramic such as barium titanate is coated on a supporting film such as a PET film in a sheet shape and dried to remove the solvent. In addition, the thickness of the dielectric layer composed of the green sheet is not particularly limited, but from the perspective of the requirement for miniaturization of the multilayer ceramic capacitor, it is preferably 0.05 μm or more and 3 μm or less.

[0095] Next, a plurality of sheets are prepared in which the conductive paste is printed and applied on one side of a green sheet and dried to form a dry film on one side of the green sheet. In addition, from the viewpoint of the requirement for thinning the internal electrode layer 11, the thickness of the dry film formed by the conductive paste is preferably 1 μm or less after drying.

[0096] Next, the green sheet is peeled off from the support film, and the green sheets and the dry films formed on one surface of the green sheets are alternately stacked, and then heated and pressurized to obtain a laminate. In addition, a protective ceramic green sheet not coated with the conductive paste may be further arranged on both sides of the laminate.

[0097] Next, after the laminate is cut into a predetermined size to form a green chip, the green chip is subjected to a binder removal treatment and fired in a reducing atmosphere to produce a laminated ceramic fired body (ceramic laminate 10). In addition, the atmosphere during the binder removal treatment is preferably air or N 2 Gas atmosphere. The temperature during the debinding process is, for example, 200°C to 400°C. In addition, it is preferred that the holding time of the above-mentioned temperature during the debinding process is set to 0.5 hours to 24 hours. In addition, in order to suppress oxidation of the metal used in the internal electrode layer, the firing is performed in a reducing atmosphere. In addition, the temperature during the firing of the laminate is, for example, 1000°C to 1350°C, and the holding time of the temperature during the firing is, for example, 0.5 hours to 8 hours.

[0098] By firing the green chip, the organic binder in the ceramic green sheet is completely removed, and the raw material powder of the ceramic is fired to form the ceramic dielectric layer 12. In addition, the organic vehicle in the dry film is removed, and the nickel powder or the alloy powder containing nickel as the main component is sintered or melted to form an internal electrode layer 11, thereby forming a laminated ceramic fired body in which a plurality of dielectric layers 12 and internal electrode layers 11 are alternately stacked. In addition, from the viewpoint of bringing oxygen into the interior of the dielectric layer to improve reliability and suppressing reoxidation of the internal electrode, the laminated ceramic fired body after firing may be subjected to annealing treatment.

[0099] Then, a pair of external electrodes 20 are provided on the manufactured multilayer ceramic fired body, thereby manufacturing the multilayer ceramic capacitor 1. For example, the external electrode 20 includes an external electrode layer 21 and a plating layer 22. The external electrode layer 21 is electrically connected to the internal electrode layer 11. In addition, as a material of the external electrode 20, for example, copper, nickel, or an alloy thereof can be preferably used. In addition, as an electronic component, an electronic component other than a multilayer ceramic capacitor can also be used.

[0100] Example

[0101] Hereinafter, the present invention will be described in detail based on Examples and Comparative Examples, but the present invention is not limited to these Examples at all.

[0102] [Evaluation method]

[0103] (Adhesion evaluation)

[0104] A conductive paste (sample) is applied to the surface of a pre-made raw sheet containing barium titanate and polyvinyl butyral to form a conductive paste film with a wet film thickness of 35 μm. The obtained raw sheet and the sheet consisting of the conductive paste film for internal electrodes formed on the surface are dried at 75°C for 20 minutes to form a dry film on the raw sheet. The dried sheet (dry film-raw sheet) is overlapped with other raw sheets in the form of the surface coated with the conductive paste being sandwiched by the raw sheets, and then pressed at a temperature of 40°C and a pressure of 20 MPa for 20 seconds to produce a laminate (for evaluation).

[0105] The obtained laminate was cut into 1 cm squares, and both sides of the laminate were respectively set in the clamps of a tensile tester (AGS-50NX manufactured by Shimadzu Corporation) using adhesive tape, and a tensile test was performed. The force at break (the force when the dried film is peeled off from the green sheet) was recorded at a test speed of 20 mm / min. The force at break of Comparative Example 1 was set as 100%, and the force at break of each was evaluated in %.

[0106] (Hardness measurement)

[0107] Using a micro Vickers hardness tester (manufactured by Shimadzu Corporation, HMV-G21DT), under the condition of a test force of 98mN, the surface (dry film side) of the raw sheet formed with a conductive paste film (dry film) made under the same conditions as the adhesion evaluation was measured at n=5 points, and their average values ​​were obtained. The hardness measurement was performed by attaching the sample to a glass substrate and placing it on a heated workbench as a sample stand of the hardness tester, at unheated room temperature (25°C) and heated to 60°C. In addition, when measuring the Vickers hardness (60°C), the previously measured dry film was placed at 60°C for 3 minutes for state adjustment, and then the measurement was performed while maintaining the state after heating at 60°C.

[0108] (Determination of glass transition temperature Tg)

[0109] The components other than the conductive powder and the ceramic powder in the conductive paste, namely, the ethyl cellulose resin, the polyvinyl butyral resin, the additives and the organic solvent were weighed in the same manner as the amounts contained in the conductive paste, and mixed at 2000 rpm for 4 minutes using a rotary mixer (manufactured by THINKY, ARE-310), and then the obtained liquid (mixture) was applied to a PET film with a wet film thickness of 254 μm using an applicator, and dried at 120° C. for 40 minutes to obtain a sample for evaluation. In addition, the organic solvent in the mixture was removed during drying.

[0110] Using a differential scanning calorimeter (NETZSCH Japan Co., Ltd., DSC3100), 10 mg of the dried evaluation sample was placed in an aluminum pan, and the temperature was increased from 0°C to 140°C at a heating rate of 10°C / min under a nitrogen gas flow of 100 mL / min. The glass transition temperature Tg on the low temperature side was determined from the peak of the obtained endothermic curve.

[0111] (Thermal decomposition temperature measurement)

[0112] The thermal decomposition temperature of the additive used in the conductive paste was measured using a thermal decomposition weight measuring device (NETZSCH, STA25000REGULUS). The measurement temperature atmosphere was nitrogen, and the temperature was increased from 20°C to 550°C at a heating rate of 5°C / min. The temperature at which the differential heating loss reached the maximum, that is, the temperature at which the weight loss rate in the thermogravimetric analysis reached the maximum, was taken as the thermal decomposition temperature (maximum thermal decomposition temperature).

[0113] [Materials used]

[0114] (Conductive powder)

[0115] As the conductive powder, Ni powder (SEM average particle size: 0.2 μm) was used.

[0116] (Ceramic powder)

[0117] As ceramic powder, barium titanate (BaTiO 3 , SEM average particle size is 0.10μm).

[0118] (Binder resin)

[0119] As the binder resin, polyvinyl butyral resin (PVB) and ethyl cellulose resin (EC) were used.

[0120] (Dispersant)

[0121] In the examples and comparative examples, as the dispersant (additive) commonly contained, a polycarboxylic acid-based dispersant, which is an acid-based dispersant, was used.

[0122] (additive)

[0123] As the rosin derivative, the compounds shown in the following Table 1 were used. The structures shown in Formulas (1) and (2) in Table 1 represent the structures of Formulas (1) and (2) below. The molecular weight (weight average molecular weight) of the rosin derivative (C) was about 1,000.

[0124] Table 1

[0125] Rosin derivatives Rosin skeleton R / Functional group (A) Chemical(1) <![CDATA[-CH 2 NH 2 ]]> (B) Chemical(1) <![CDATA[-CH 2 OH]]> (C) Disproportionated rosin ester Diol (D) Chemical(1) <![CDATA[-COOCH 3 ]]> (E) Chemical (2) <![CDATA[-COOCH 3 ]]> (F) Chemical (2) -COOH

[0126]

Chemistry 1

[0127]

[0128]

Chemistry 2

[0129]

[0130] As comparative examples, the following additives were used.

[0131] Additive a: polycarboxylic acid having polyoxyalkylene as graft chain

[0132] Additive b: oxyethylene lauryl amine (polyether amine)

[0133] Additive c: dicarboxylic acid

[0134] (Organic Solvent)

[0135] As the organic solvent, dihydroterpineol (DHT) and mineral spirits (MSA) were used.

[0136] [Example 1]

[0137] Conductive powder 49 mass%, ceramic powder 12 mass%, acid dispersant 0.15 mass%, rosin derivative (A) 0.3 mass%, binder resin 2.5 mass% (PVB:EC=7:3 (mass ratio)) and organic solvent (DHT:MSA=60:40 (mass ratio)) as the balance were added, and the total amount was 100 mass%, and these materials were mixed to prepare conductive paste. The content of each material in the conductive paste and the evaluation results are shown in Table 1.

[0138] [Examples 2 to 5, Comparative Examples 1 to 7]

[0139] As shown in Table 1, conductive pastes were prepared and evaluated in the same manner as in Example 1 except that the rosin derivative (A) (additive) was changed to the type and content of the additive shown in Table 1. Table 2 shows the content of each material in the conductive paste and the evaluation results.

[0140]

[0141] (Evaluation results)

[0142] The conductive pastes of Examples 1 to 5 containing the rosin derivative having an amine group or a hydroxyl group have improved adhesion compared to the conductive pastes of Comparative Example 1 containing no rosin derivative or Comparative Examples 2 to 7 containing other additives.

[0143] The glass transition temperatures of the conductive pastes of Examples 1 to 5 were all 64° C. or less, and the glass transition temperature of Comparative Example 1 was 69° C. Therefore, it was confirmed that the glass transition temperatures of the conductive pastes of Examples 1 to 5 were lower than those of Comparative Example 1 by 5° C. or more.

[0144] Industrial Applicability

[0145] When the conductive paste of the present invention is used to form the internal electrodes of a multilayer ceramic capacitor, a multilayer ceramic capacitor with high reliability can be obtained with high productivity. Therefore, the conductive paste of the present invention is particularly suitable for use as a chip component of an electronic device such as a mobile phone or a digital device, that is, an internal electrode of a multilayer ceramic capacitor.

[0146] In addition, the technical scope of the present invention is not limited to the methods described in the above-mentioned embodiments, etc. Sometimes one or more of the requirements described in the above-mentioned embodiments, etc. are omitted. In addition, the requirements described in the above-mentioned embodiments, etc. can be appropriately combined. In addition, as long as the law permits, the disclosure of all the documents cited in the above-mentioned embodiments, etc. is cited as part of the record of this article. In addition, as long as the law permits, the contents of Japanese Patent Application No. 2022-052667, which is a Japanese patent application, are cited as part of the record of this article.

[0147] The embodiments of the present invention may include the following configurations.

[0148] [1] A conductive paste, wherein the conductive paste comprises conductive powder, an additive, a binder resin and an organic solvent,

[0149] The additive includes a rosin derivative having a hydroxyl group or an amine group.

[0150] [2] The conductive paste according to [1], wherein the rosin derivative is contained in an amount of 0.01% by mass or more and 2.0% by mass or less based on the entire conductive paste.

[0151] [3] The conductive paste according to [1] or [2], wherein the temperature at which the weight loss rate of the compound in thermogravimetric analysis reaches a maximum is 200° C. or higher.

[0152] [4] The conductive paste according to any one of [1] to [3], wherein the molecular weight of the rosin derivative is 250 or more and 3000 or less.

[0153] [5] The conductive paste according to any one of [1] to [4], further comprising an acidic dispersant and / or an alkaline dispersant.

[0154] [6] The conductive paste according to any one of [1] to [5], wherein the conductive powder includes at least one metal powder selected from Ni, Pd, Pt, Au, Ag, Cu, and alloys thereof.

[0155] [7] The conductive paste according to any one of [1] to [6], wherein the conductive powder has an average particle size of 0.05 μm or more and 1.0 μm or less.

[0156] [8] The conductive paste according to any one of [1] to [7], wherein the binder resin contains a butyral-based resin.

[0157] [9] The conductive paste according to any one of [1] to [8], further comprising ceramic powder.

[0158]

[10] The conductive paste according to [9], wherein the ceramic powder contains barium titanate.

[0159]

[11] The conductive paste according to [9] or

[10] , wherein the average particle size of the ceramic powder is 0.01 μm or more and 0.5 μm or less.

[0160]

[12] The conductive paste according to any one of [9] to

[11] , wherein the ceramic powder is contained in an amount of 1% by mass or more and 20% by mass or less based on the entire conductive paste.

[0161]

[13] The conductive paste according to any one of [1] to

[12] , wherein the conductive paste is used for an internal electrode of a multilayer ceramic component.

[0162]

[14] An electronic component formed using the conductive paste according to any one of [1] to

[13] .

[0163]

[15] A multilayer ceramic capacitor comprising at least a laminated body in which a dielectric layer and an internal electrode layer are laminated,

[0164] The internal electrode layer is formed using the conductive paste described in

[13] .

[0165] Description of Reference Numerals

[0166] 1: Multilayer ceramic capacitor;

[0167] 10: Ceramic laminate;

[0168] 11: internal electrode layer;

[0169] 12: dielectric layer;

[0170] 20: external electrode;

[0171] 21: external electrode layer;

[0172] 22: Electroplating layer.

Claims

1. A conductive paste, wherein: The conductive paste comprises conductive powder, additives, binder resin and organic solvent. The additive includes a rosin derivative having a hydroxyl group or an amine group.

2. The conductive paste according to claim 1, wherein The rosin derivative is contained in an amount of 0.01 mass % to 2.0 mass % based on the entire conductive paste.

3. The conductive paste according to claim 1, wherein The temperature at which the weight reduction rate of the compound in thermogravimetric analysis reaches a maximum is 200° C. or higher.

4. The conductive paste according to claim 1, wherein The molecular weight of the rosin derivative is 250 or more and 3000 or less.

5. The conductive paste according to claim 1, wherein The conductive paste further includes an acidic dispersant and / or an alkaline dispersant.

6. The conductive paste according to claim 1, wherein The conductive powder includes at least one metal powder selected from the group consisting of Ni, Pd, Pt, Au, Ag, Cu and alloys thereof.

7. The conductive paste according to claim 1, wherein The conductive powder has an average particle size of 0.05 μm or more and 1.0 μm or less.

8. The conductive paste according to claim 1, wherein The binder resin includes a butyral-based resin.

9. The conductive paste according to claim 1, wherein: The conductive paste further includes ceramic powder.

10. The conductive paste according to claim 9, wherein: The ceramic powder includes barium titanate.

11. The conductive paste according to claim 9, wherein The ceramic powder has an average particle size of 0.01 μm or more and 0.5 μm or less.

12. The conductive paste according to claim 9, wherein The ceramic powder is contained in an amount of 1 mass % or more and 20 mass % or less based on the entire conductive paste.

13. The conductive paste according to claim 1, wherein The conductive paste is used for internal electrodes of a multilayer ceramic component.

14. An electronic component, wherein: The electronic component is formed using the conductive paste according to any one of claims 1 to 13.

15. A multilayer ceramic capacitor, wherein: The multilayer ceramic capacitor includes at least a laminated body in which a dielectric layer and an internal electrode layer are laminated. The internal electrode layer is formed using the conductive paste according to claim 13 .