Method for manufacturing electrode for electrochemical device with lead member, and method for manufacturing electrochemical device

By intermittently coating the slurry on the electrode surface and installing lead parts in the uncoated area, and using elastomer to enhance the adhesive, the problems of active layer shedding and increased resistance are solved, and the performance and capacity of the electrochemical device are improved.

CN118946944APending Publication Date: 2024-11-12PANASONIC INTELLECTUAL PROPERTY MANAGEMENT CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380030422.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-29
Filing Date
2023-03-22
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

During the formation of the current collecting foil exposed portion, the active layer is prone to fall off, resulting in an increase in the resistance between the electrode and the lead member, thereby reducing the performance of the electrochemical device.

Method used

By intermittently coating the slurry on the electrode surface, a current collecting foil exposed portion is formed, and a lead member is installed in the uncoated area. The adhesive contains an elastomer and the content of the elastomer is between 0.25% and 3%, so as to Improve the adhesion and adhesion of the active layer, and reduce shedding and resistance.

Benefits of technology

The active layer near the exposed part of the current collecting foil is effectively suppressed, the resistance between the electrode and the lead component is reduced, the performance and capacity of the electrochemical device is improved, and the slight short circuit and capacity reduction are reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118946944A_ABST
    Figure CN118946944A_ABST
Patent Text Reader

Abstract

A method for manufacturing an electrode for an electrochemical device with a lead member includes: a first step of preparing a slurry containing activated carbon and a binder, and a collector foil having a roughened surface; a second step in which the slurry is applied to the surface of the collector foil and dried to form an active layer, thereby obtaining an electrode; and a third step of connecting the electrode and the lead member. In the second step, the paste is intermittently applied to the current collector foil to form an uncoated region in which the surface of the current collector foil is exposed on a portion of the electrode, and in the third step, the lead member is attached to the uncoated region, the binder contains an elastomer, and the content of the elastomer in the active layer is more than 0.25% by mass but less than 3% by mass.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to a method for manufacturing an electrode for an electrochemical device with a lead member and a method for manufacturing an electrochemical device. Background Art

[0002] An example of an electrochemical device is an electric double-layer capacitor. Compared to secondary batteries, electric double-layer capacitors have a longer lifespan, can be quickly charged, and have superior output characteristics. Therefore, electrochemical devices such as electric double-layer capacitors are widely used in backup power supplies and other applications.

[0003] An electric double-layer capacitor, for example, comprises a wound body (capacitor element) formed by winding a pair of polarized electrodes with a separator interposed therebetween, and an electrolyte. The electrodes can be obtained, for example, by applying a slurry containing activated carbon to the surface of a roughened collector foil (e.g., etched aluminum foil) and drying it to form an active layer (e.g., Patent Document 1).

[0004] Leads are connected to the electrodes. The connection between the electrodes and the lead is achieved by forming an exposed area of ​​the collector foil (hereinafter referred to as the "exposed collector foil area") on a portion of the electrode and attaching the lead to the exposed collector foil area. The exposed collector foil area is typically formed by hot-pressing a portion of the active layer formed on the surface of the collector foil and then wiping it with a brush or other similar method. The hot-pressing treatment is performed to facilitate removal of a portion of the active layer with a brush or other similar method.

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: Japanese Patent No. 5278670 Summary of the Invention

[0008] Problems to be solved by the invention

[0009] When the exposed portion of the collector foil is formed by hot pressing and partially cutting away the active layer using a brush, the active layer is prone to falling off the collector foil near the exposed portion. Furthermore, this increases the surface roughness of the exposed portion, which can increase the resistance between the electrode and the lead member. Consequently, the performance of the electrochemical device deteriorates.

[0010] Means for solving problems

[0011] In view of the above situation, one aspect of the present disclosure relates to a method for manufacturing an electrode for an electrochemical device with a lead component, which includes the following steps: a first step of preparing a slurry containing activated carbon and a binder, and a collector foil with a roughened surface; a second step of applying the slurry to the surface of the collector foil, drying it, and forming an active layer to obtain an electrode; and a third step of connecting the electrode to the lead component; in the second step, the slurry is intermittently applied to the collector foil to form an uncoated area on a portion of the electrode where the surface of the collector foil is exposed; in the third step, the lead component is installed in the uncoated area, the binder contains an elastomer, and the content of the elastomer in the active layer exceeds 0.25 mass % and is less than 3 mass %.

[0012] Another aspect of the present disclosure relates to a method for manufacturing an electrochemical device, which includes the following steps: step A, preparing a first electrode with a first lead component and a second electrode with a second lead component; step B, winding the first electrode and the second electrode with a separator to obtain a wound body; and step C, making an electrolyte contain an electrolyte in the wound body; in step A, the above-mentioned method for manufacturing an electrode for an electrochemical device with a lead component is used to obtain at least one of the first electrode with the first lead component and the second electrode with the second lead component.

[0013] Effects of the Invention

[0014] According to the present disclosure, it is possible to suppress degradation in the performance of an electrochemical device.

[0015] The novel features of the present invention are described in the appended claims, and both the configuration and content of the present invention, together with other objects and features of the present invention, will be better understood through the following detailed description with reference to the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 This is a front view schematically showing an example of an electrode with a lead wire.

[0017] Figure 2 This is a cross-sectional view schematically showing an example of an electrode with a lead.

[0018] Figure 3 This is a perspective view with a portion of the electrochemical device cut away. DETAILED DESCRIPTION

[0019] The following describes embodiments of the present invention, but the electrochemical device of the present invention is not limited to the following embodiments. In the following description, specific numerical values ​​and materials are sometimes exemplified, but other numerical values ​​and materials may be applied as long as the effects of the present disclosure are achieved. In this specification, the phrase "numerical value A to numerical value B" includes numerical value A and numerical value B and may be replaced with "numerical value A or greater and numerical value B or less."

[0020] In the following description, the term “comprising…” includes expressions such as “containing…”, “consisting essentially of…” and “consisting of…”.

[0021] A method for manufacturing an electrode for an electrochemical device with a lead component according to one embodiment of the present disclosure includes first to third steps. In the first step, a slurry containing an electrode material and a collector foil with a roughened surface are prepared. In the second step, the slurry is applied to the surface of the collector foil and dried to form an active layer, thereby obtaining an electrode. In the third step, the electrode and the lead component are connected. The electrode material contains activated carbon as an active material and a binder as essential components. The active layer is a layer of the electrode material. The electrode containing activated carbon adsorbs ions during charging and desorbs ions during discharging.

[0022] In the second step, the slurry is intermittently applied to the collector foil to form an uncoated area on a portion of the electrode where the surface of the collector foil is exposed. In the third step, a lead member is attached to the uncoated area.

[0023] Intermittent coating forms the exposed collector foil portion (uncoated area). This prevents the active layer from falling off near the exposed collector foil portion when the exposed collector foil portion is formed by hot pressing or by scraping a portion of the active layer using a brush, for example. Furthermore, the increase in surface roughness of the exposed collector foil portion and the resulting increase in resistance at the connection between the electrode and the lead member are suppressed. Consequently, degradation in the performance of the electrochemical device is suppressed.

[0024] The binder contains an elastomer, and the content of the elastomer in the active layer (electrode material) exceeds 0.25% by mass and is less than 3% by mass. In addition, the content of the elastomer in the active layer (electrode material) refers to the mass ratio (percentage) of the elastomer relative to the entire active layer (electrode material).

[0025] When the elastomer content in the active layer (electrode material) is greater than 0.25% by mass, the binding force of the active layer is improved, and the adhesion between the active layer and the collector foil is improved, thereby achieving an electrochemical device with low internal resistance. Furthermore, the shedding of the active layer is suppressed, and the occurrence of micro-short circuits and reduction in capacity in the electrochemical device are suppressed.

[0026] However, if the elastomer content in the active layer (electrode material) increases to more than 3% by mass, the viscosity of the slurry used to form the active layer increases, and coating tailing occurs when the slurry is intermittently coated on the collector foil, which may reduce the reliability of the exposed portion of the collector foil.

[0027] From the viewpoint of further reducing the internal resistance of the electrochemical device, the content of the elastomer in the active layer is preferably 0.5 mass % or more and 2.5 mass % or less.

[0028] As the collector foil with a roughened surface, an etched metal foil (etched foil) can be used. Compared to ordinary foil, etched foil is more advantageous in improving the adhesion between the active layer and the collector foil. By using etched foil as the collector foil and utilizing a small amount (less than 3% by mass (or less than 2.5% by mass) of an elastomer (such as SBR), the adhesion between the active layer and the collector foil can be effectively improved.

[0029] The active layer containing activated carbon does not experience the same significant expansion and contraction as the active material layer of a lithium-ion secondary battery (LIB). Therefore, an etched foil with appropriate thickness and strength can be used for the collector foil without compromising energy density. Furthermore, LIBs use active materials (such as graphite and Si-based active materials) that intercalate and deintercalate lithium ions, which expand and contract significantly during charge and discharge. Considering the expansion and contraction of the active material layer and the thickness and strength of the collector foil required for LIBs, the use of etched foil in LIBs is difficult.

[0030] (First process)

[0031] (Slurry)

[0032] The slurry is prepared by dispersing the electrode material in a dispersion medium. The electrode material contains at least activated carbon and a binder. The dispersion medium is, for example, water. The water content in the slurry is, for example, 60% to 80% by mass relative to the total slurry.

[0033] There is no particular limitation on the activated carbon (activated carbon particles) used as the active material, and known activated carbon used for electrochemical devices may also be used. Activated carbon can be produced, for example, by subjecting the raw material to heat treatment to carbonization and subjecting the obtained carbide to activation treatment. Examples of raw materials include wood, coconut shells, pulp waste liquid, coal, or coal-based asphalt obtained by thermal decomposition thereof, heavy oil, or petroleum-based asphalt obtained by thermal decomposition thereof, phenolic resin, petroleum coke, coal coke, etc. Examples of activation treatments include gas activation using gases such as water vapor and chemical activation using alkalis such as potassium hydroxide. The activated carbon particles obtained by the above-mentioned activation treatment may also be subjected to a pulverization treatment. Classification treatment may also be performed after the pulverization treatment. The pulverization treatment may be performed using, for example, a ball mill, a jet mill, etc.

[0034] The content of activated carbon in the electrode material (active layer) is not particularly limited and may be 60% by mass or more and 95% by mass or less, or 70% by mass or more and 90% by mass or less. The content of activated carbon in the electrode material (active layer) refers to the mass ratio (percentage) of the activated carbon relative to the total mass of the electrode material (active layer).

[0035] The binder contains at least an elastomer. The elastomer may contain, for example, a rubber component, and may also contain at least one selected from styrene-butadiene rubber (SBR), acrylate rubber, and acrylonitrile-butadiene rubber. Among them, SBR is preferred from the viewpoint of increasing the adhesive force of the active layer and the adhesion between the active layer and the collector foil with a small amount of addition. The binder may consist solely of SBR.

[0036] Styrene-butadiene rubber is a copolymer with styrene and butadiene as main monomers (for example, a copolymer of styrene and butadiene), and may also be a product of modified copolymers.

[0037] Acrylate rubber is a polymer primarily composed of acrylic esters. Examples of acrylic rubber include copolymers of two or more monomers containing acrylic esters and other monomers, as well as modified versions of these copolymers. Examples of other monomers include 2-chloroethyl vinyl ether and acrylonitrile. Examples of acrylic esters include ethyl acrylate, butyl acrylate, and methoxyethyl acrylate. Two or more acrylic esters may be mixed. Acrylate rubber may be fluorinated.

[0038] The binder may contain other components besides the elastomer, for example, a resin component such as polytetrafluoroethylene (PTFE). The proportion of the elastomer in the binder may be 75% by mass or more, 90% by mass or more, or even 100% by mass.

[0039] The electrode material may also contain other components besides activated carbon and a binder. Other components include a conductive agent, a thickener, and the like. As a conductive agent, for example, carbon black such as acetylene black is used. As a thickener, for example, carboxymethyl cellulose (CMC) (including alkali metal salts or ammonium salts of CMC) is used.

[0040] The TI value of the slurry can be more than 2 and less than 4, or more than 2.5 and less than 4. When the TI value of the slurry is more than 2, it is easy to suppress the tailing of the coating film and improve the reliability of the exposed portion formed for the collector foil. When the TI value of the slurry is less than 4, the bonding force of the active layer is easily improved, and the adhesion of the active layer to the collector foil is easily improved. When the proportion of the elastomer (such as SBR) in the electrode material is more than 0.25% by mass and less than 3% by mass (or more than 0.5% by mass and less than 2.5% by mass), it is easy to adjust the TI of the slurry to within the above range.

[0041] The TI value of the slurry is determined as follows.

[0042] Measure the viscosity of the slurry at 25°C using a B-type viscometer or an E-type viscometer. Calculate the viscosity η1 of the slurry at a rotational speed of 1 rpm and the viscosity η2 of the slurry at a rotational speed of 10 rpm. Calculate the ratio of the viscosity η1 to the viscosity η2: η1 / η2, and use this as the TI value.

[0043] (Collector Foil)

[0044] The arithmetic mean roughness Ra of the surface of the collector foil is preferably not less than 0.5 μm and not more than 1 μm. The arithmetic mean roughness Ra of the surface of the collector foil after etching is, for example, not less than 0.5 μm, and may also be not less than 0.6 μm. When the arithmetic mean surface roughness Ra of the surface of the collector foil is not more than 1 μm, the resistance of the connection portion between the electrode (exposed portion of the collector foil) and the lead component is easily reduced. By the above-mentioned intermittent coating, it is possible to easily form a collector exposed portion having a surface with an arithmetic mean roughness Ra within the above-mentioned range. In addition, the arithmetic mean roughness Ra is an index indicating surface roughness, and is obtained in accordance with JIS B 0601:201 3.

[0045] The thickness of the collector foil can be less than 30 μm, or less than 20 μm. By reducing the thickness of the collector foil to less than 20 μm, the filling amount of the active material can be increased to achieve high capacity. In the case of using an elastomer (such as SBR) as a binder for a thin collector foil with a thickness of less than 20 μm, the strength of the collector foil is small due to the large adhesive force of the active layer and the close adhesion between the active layer and the collector foil, making it difficult to remove a portion of the active layer by a brush or the like. Therefore, in the above case, it is effective to form the exposed portion of the collector foil by intermittently applying a slurry to the collector foil.

[0046] Examples of the material for the current collector foil include aluminum, aluminum alloys, nickel, and titanium. Among them, aluminum or aluminum alloys are preferred from the viewpoints of low cost, moderate strength, and high electrical conductivity.

[0047] (Second process)

[0048] In the second step, the slurry is applied to the surface of the collector foil, the coating is dried, and compressed as needed to form an active layer. The dispersion medium in the slurry is removed by drying to form an electrode material layer as an active layer. The thickness of the active layer (the thickness of each side) is, for example, not less than 40 μm and not more than 80 μm. The slurry can be applied to one surface of the collector foil or to both surfaces of the collector foil. The slurry is applied to the collector foil intermittently to form a coated area and an uncoated area. When the slurry is applied to both sides of the collector foil, the coated area and the uncoated area can be formed with the same pattern on both sides of the collector foil.

[0049] The coating method is not particularly limited as long as it is a method capable of intermittent coating, and examples thereof include die coating, comma coating, gravure coating, etc. Among them, die coating is preferably used as the coating method because it is in a sealed state and thus prevents the incorporation of foreign matter, and because the coating amount of the slurry can be easily controlled by using a pump.

[0050] Alternatively, a long collector foil may be supplied to a coating device, and the slurry may be intermittently coated on both sides of the collector foil to form a predetermined coating pattern to form an active layer, which may be cut at predetermined positions to produce a plurality of electrodes having a collector foil exposed portion on a portion thereof.

[0051] (Third Process)

[0052] In the third step, the electrode and the lead member are connected by attaching the lead member to the uncoated area of ​​the electrode. The lead member can be attached to the uncoated area of ​​the electrode by, for example, caulking or cold pressing using a needle-shaped member.

[0053] The lead component, for example, includes a flat tab portion, a lead, and a connection portion connecting the tab portion and the lead. The lead component is not particularly limited as long as it comprises a tab portion, a connection portion, and a lead. For example, it can be prepared as follows: A metal rod-shaped member is prepared, and one end of the member is flattened using a press, for example, to form the tab portion. The other end remains in its rod-like shape as the connection portion. The connection portion and the lead are connected by welding, for example.

[0054] The connection of the electrode and the lead component by riveting is performed, for example, in the following manner. The ear portion of the lead component is arranged on one surface of the uncoated area of ​​the electrode to form an overlapping portion between the ear portion and the uncoated area. A needle-shaped component is used to punch a hole at a predetermined position of the overlapping portion from the ear side to form a through hole. As the through hole is formed, a portion of the ear portion protrudes from the other surface of the uncoated area of ​​the electrode to form a protrusion. Then, the overlapping portion is pressed so that the protrusion is bent and adhered to the other surface of the uncoated area to form a petal-shaped riveted piece. The riveting process is performed, for example, on 2 to 4 predetermined positions in the uncoated area.

[0055] here, Figure 1 This is a front view schematically showing an example of an electrode with a lead member obtained by using the method for manufacturing an electrode with a lead member according to the present embodiment. Figure 2 This is a cross-sectional view schematically showing an example of an electrode with a lead member obtained by using the method for manufacturing an electrode with a lead member according to the present embodiment. Figure 2 The cross section including the rivet portion 40 is shown. The components in the figure are schematically shown, and the relationship between the size and thickness of each component is not limited to this.

[0056] The strip electrode 20 includes a collector foil 21 with a roughened surface and an active layer 22 supported on both surfaces of the collector foil 21. The electrode 20 has a collector foil exposed portion 23 on a portion thereof. The collector foil exposed portions 23 are formed on both surfaces of the electrode 20, and when the electrode 20 is viewed from the normal direction of its main surface, the collector foil exposed portions 23 on both surfaces of the electrode 20 are formed in a substantially uniform manner. Meanwhile, the lead member 30 includes a flat tab portion 31, a connecting portion 32, and a lead 33. The tab portion 31 is placed on the collector foil exposed portion 23 on one surface of the electrode 20 and riveted together for attachment. In this manner, the electrode 20 and the lead member 30 are connected. The rivet portion 40, formed by riveting, has a through-hole 41 and a rivet tab 42 formed on the collector foil exposed portion 23 on the other surface of the electrode 20. Two rivets 40 are provided, but the number of rivets 40 is not limited thereto. In the present embodiment, the collector foil exposed portion 23 is obtained by intermittent coating (formation of an uncoated region).

[0057] [Method for Manufacturing Electrochemical Device]

[0058] The method for manufacturing an electrochemical device according to an embodiment of the present disclosure includes the following steps: Step A, preparing a first electrode with a first lead member and a second electrode with a second lead member; Step B, winding the first and second electrodes with a separator interposed therebetween to form a wound body; and Step C, containing an electrolyte solution in the wound body. In Step A, at least one of the first electrode with a first lead member and the second electrode with a second lead member is obtained using the method for manufacturing an electrode for an electrochemical device with a lead member according to an embodiment of the present disclosure. Hereinafter, the electrode with a lead member obtained using the method for manufacturing an electrode for an electrochemical device with a lead member according to an embodiment of the present disclosure will also be referred to as "electrode with a lead member E."

[0059] As electrochemical devices, electric double layer capacitors (EDLC), lithium ion capacitors (LIC), etc. can be listed. In addition, "capacitor" can also be renamed as "condenser". In the case where the electrochemical device is EDLC, at least one of a pair of electrodes with lead parts can use an electrode E with a lead part. In the case where the electrochemical device is LIC, as long as one of a pair of electrodes with lead parts (positive electrode) uses an electrode E with a lead part, and the other of a pair of electrodes with lead parts (negative electrode) uses a negative electrode with a lead part used in a lithium ion secondary battery. The negative electrode used in a lithium ion secondary battery, for example, contains a negative electrode active material (such as graphite) that can embed and deintercalate lithium ions.

[0060] The electrolyte contains a solvent (non-aqueous solvent) and an ionic substance. The ionic substance is dissolved in the solvent and contains cations and anions. The ionic substance may also include, for example, a low-melting-point compound (ionic liquid) that can exist in liquid form near room temperature. The concentration of the ionic substance in the electrolyte is, for example, 0.5 mol / L or more and 2.0 mol / L or less.

[0061] As the solvent, a high-boiling-point solvent is preferred. Examples of the solvent include lactones such as γ-butyrolactone; carbonates such as propylene carbonate; polyols such as ethylene glycol and propylene glycol; cyclic sulfones such as sulfolane; amides such as N-methylacetamide, N,N-dimethylformamide, and N-methyl-2-pyrrolidone; esters such as methyl acetate; ethers such as 1,4-dioxane; ketones such as methyl ethyl ketone; and formaldehyde.

[0062] Ionic substances include, for example, organic salts. Organic salts refer to salts in which at least one of the anion and the cation contains an organic substance. Examples of organic salts in which the cation contains an organic substance include quaternary ammonium salts. Examples of organic salts in which the anion (or zwitterion) contains an organic substance include trimethylamine maleate, triethylamine borodisalicylate, ethyldimethylamine phthalate, mono-1,2,3,4-tetramethylimidazolinium phthalate, and mono-1,3-dimethyl-2-ethylimidazolinium phthalate.

[0063] From the viewpoint of improving the withstand voltage characteristics, the anion preferably includes an anion of a fluorine-containing acid. Examples of the anion of a fluorine-containing acid include BF4 - and / or PF6 - The organic salt preferably contains, for example, a tetraalkylammonium cation and a fluorine-containing acid anion. Specific examples include diethyldimethylammonium tetrafluoroborate (DEDMABF4) and triethylmethylammonium tetrafluoroborate (TEMABF4).

[0064] A separator is preferably placed between the pair of electrodes. The separator is ion-permeable and serves to physically separate the pair of electrodes to prevent short circuits. Examples of the separator include non-woven fabrics primarily composed of cellulose, glass fiber mats, and microporous films made of polyolefins such as polyethylene.

[0065] here, Figure 3 This is a partially cutaway perspective view of an electrochemical device obtained by the method for manufacturing an electrochemical device according to an embodiment of the present disclosure. Figure 3 An example of an electrochemical device obtained by using the method for manufacturing an electrochemical device according to an embodiment of the present disclosure is shown.

[0066] Figure 3 The electrochemical device 10 is an electric double-layer capacitor having a wound capacitor element 1. The capacitor element 1 is formed by winding a sheet-like first electrode 2 and a second electrode 3, respectively, with a separator 4 interposed therebetween. The first electrode 2 and the second electrode 3 each have a first metal current collector and a second metal current collector, and a first active layer and a second active layer supported on their surfaces, and exhibit capacitance by adsorbing and desorbing ions.

[0067] The collector foil is, for example, an etched aluminum foil. The separator 4 is, for example, a non-woven fabric with cellulose as the main component. The first lead member 5a and the second lead member 5b are connected to the first electrode 2 and the second electrode 3, respectively. The capacitor element 1 is housed in a cylindrical housing 6 together with an electrolyte (not shown). The material of the housing 6 can be, for example, aluminum, stainless steel, copper, iron, brass or other metal. The opening of the housing 6 is sealed by a sealing member 7. The leads 5a and 5b are led out to the outside in a manner that passes through the sealing member 7. The sealing member 7 is made of a rubber material such as butyl rubber.

[0068] Hereinafter, the present disclosure will be described in more detail based on examples, but the present disclosure is not limited to the examples.

[0069] Example 1

[0070] As an electrochemical device, a wound electric double layer capacitor was produced with a rated voltage of 2.7 V. A specific method for producing the electrochemical device will be described below.

[0071] (Electrode Preparation)

[0072] Water is added to the electrode material to prepare a slurry. The electrode material uses a mixture of 88.25 parts by mass of activated carbon particles, 1.75 parts by mass of styrene-butadiene rubber (SBR) as a binder, 4 parts by mass of carboxymethyl cellulose (CMC) as a thickener, and 6 parts by mass of acetylene black (AB) as a conductive agent. The content of SBR in the electrode material is 1.75 mass % relative to the entire electrode material. The content of water in the slurry is 75 mass % relative to the entire slurry. The TI value of the slurry obtained by the above method is 2.5.

[0073] The resulting slurry was applied to both sides of a strip-shaped collector foil. The coating was vacuum-dried at 110°C and rolled to form an active layer (40 μm thick per side), resulting in an electrode (500 mm long, 59 mm wide). The collector foil used was an etched Al foil (20 μm thick, 0.89 μm arithmetic mean roughness Ra).

[0074] In the above process, the slurry was applied to the collector foil intermittently, forming coated and uncoated areas in the same pattern on both sides of the collector foil. A slot die was used as the coating apparatus. This procedure produced an electrode a1 comprising a collector foil, an active layer formed on both sides of the collector foil, and an exposed portion of the collector foil formed by an uncoated area (electrode lengthwise dimension: 6 mm).

[0075] (Connection between electrodes and lead parts)

[0076] A lead assembly comprising a lead, a connecting portion, and a tab was prepared. The tab of the lead assembly was placed on one surface of the exposed collector foil portion of the electrode. Riveting was performed on the overlapping portion between the exposed collector foil portion and the tab. In this manner, the tab was attached to the exposed collector foil portion, yielding an electrode a1 with a lead assembly.

[0077] (Preparation of Electrolyte)

[0078] An electrolyte solution was prepared by dissolving diethyldimethylammonium tetrafluoroborate (DEDMABF4) in γ-butyrolactone (GBL). The concentration of DEDMABF4 in the electrolyte solution was set to 1.0 mol / L.

[0079] (Fabrication of Electrochemical Device)

[0080] Two electrodes with lead members obtained above were prepared and wound with a cellulose nonwoven fabric separator interposed therebetween to form a capacitor element. This was then housed in a predetermined casing along with an electrolyte solution and sealed with a sealing member to complete electrochemical device A1. An aging treatment was then performed at 60°C for 16 hours while applying a rated voltage.

[0081] The electrode a1 with a lead member and the electrochemical device A1 obtained above were evaluated as follows.

[0082] [evaluate]

[0083] (Peel strength of active layer)

[0084] Cut the electrode into 15 mm wide pieces to obtain a sample. Secure the sample to a specified table with 20 mm wide double-sided tape (Nichiban, NW-20). Apply 12 mm wide masking tape (Nitto Denko, No. 7239) to the sample. Use a dynamometer to stretch one end of the masking tape in the longitudinal direction to measure the force required to peel off the active layer (peel strength). At this time, calculate the average value of the peel strength maintained stably for 15 seconds.

[0085] (Rivet resistance between electrode and lead part)

[0086] Measured using a digital multimeter Figure 1 The position indicated by the arrow in P1 is Figure 1 The resistor (riveting resistor) between the positions indicated by the arrows in P2. Figure 1 The position indicated by the arrow P1 in FIG. 1 is the end portion of the lead 33 on the side of the tab portion 31 . Figure 1 The position indicated by the arrow P2 in FIG. 1 is near the end of the tab portion 31 on the opposite side to the lead 33 in the collector foil exposed portion 23 .

[0087] (Capacity of electrochemical device)

[0088] At -30°C, constant current charging was performed at 1.35A until the voltage reached 2.35V, and the voltage of 2.35V was maintained for 10 minutes. Then, constant current discharge was performed at 1A until the voltage reached 0V at -30°C.

[0089] During the discharge, the time t (seconds) required for the voltage to drop from 2.0 V to 1.6 V was measured. Using the measured time t, the capacity C1 (F) of the electrochemical device was calculated from the following formula (1).

[0090] Capacity C1=Id×t / V(1)

[0091] In the formula (1), Id is the current value during discharge (1.0 A), and V is the value obtained by subtracting 1.6 V from 2.0 V (0.4 V).

[0092] (DC resistance (DCR) of electrochemical devices)

[0093] At -30°C, constant current charging was performed at 1.35A until the voltage reached 2.35V, and the voltage of 2.35V was maintained for 10 minutes. Then, constant current discharge was performed at 1.35A until the voltage reached 0V at -30°C.

[0094] Using the discharge curve obtained by the above discharge (vertical axis: discharge voltage, horizontal axis: discharge time), a linear approximation line was calculated for the interval 0.5 seconds to 2 seconds from the start of discharge on the discharge curve. The intercept of this approximation line, voltage VS, was determined. ΔV was calculated by subtracting voltage VS from voltage V0 at the start of discharge (0 seconds from the start of discharge) (V0 - VS). Using ΔV (V) and the current value Id (1.35 A) during discharge, the internal resistance (DCR) R1 (Ω) of the electrochemical device was calculated using the following equation (2).

[0095] Internal resistance R1 = ΔV / Id (2)

[0096] (Remaining capacity of electrochemical device)

[0097] At 25°C, constant current charging was performed at 1.35A until the voltage reached 2.5V, followed by constant voltage charging at 2.5V for 5 hours. The electrochemical device was then left at 60°C for 24 hours. After 24 hours, the voltage of the electrochemical device was measured at 25°C. If the voltage of the electrochemical device after 24 hours was 2.3V or higher, it was determined that micro-short circuits were suppressed and the remaining capacity was high.

[0098] Comparative Example 1

[0099] An electrode b1 with a lead member was produced in the same manner as in Example 1 except that polytetrafluoroethylene (PTFE) was used instead of SBR as the binder, and an electrochemical device B1 was produced and evaluated.

[0100] Comparative Example 2

[0101] Polytetrafluoroethylene (PTFE) was used as a binder instead of SBR.

[0102] In the process of applying the slurry to the collector foil, the slurry is applied to the entire surface of both sides of the collector foil to form an active layer. Afterwards, a portion of the active layer is heat-pressed at 250-280°C for 3 seconds and then removed with a brush. This process creates exposed portions of the collector foil at designated locations on the electrodes.

[0103] Except for this, the same operation as in Example 1 was carried out to produce an electrode b2 with a lead member, and an electrochemical device B2 was produced and evaluated.

[0104] Comparative Example 3

[0105] During the slurry coating process, the slurry is applied to both surfaces of the collector foil to form an active layer. Afterwards, a portion of the active layer is heat-pressed. Subsequently, attempts to remove the active layer with a brush are made. However, due to the thin thickness of the collector foil and the strong adhesion of the active layer, the active layer adheres tightly to the collector foil, making removal of the active layer difficult and preventing the collector foil from being exposed.

[0106] Comparative Example 4

[0107] The thickness of the etched aluminum foil used for the collector foil was set to 30 μm. During the slurry coating process, the slurry was applied to both surfaces of the collector foil to form an active layer. Afterwards, a portion of the active layer was heat-pressed and then removed with a brush. This process created exposed portions of the collector foil at the specified locations on the electrodes.

[0108] Except for this, the same operation as in Example 1 was carried out to produce an electrode b4 with a lead member, and an electrochemical device B4 was produced and evaluated.

[0109] The evaluation results are shown in Table 1. In addition, Tables 1 and 2 show the TI values ​​of the slurries obtained by the above-mentioned methods. The ○ in the "Tail of Coating" column in Tables 1 and 2 indicates that no tailing of the coating was visually observed when the slurry was intermittently coated on the collector foil. On the other hand, the × in the "Tail of Coating" column indicates that the tailing of the coating was visually observed when the slurry was intermittently coated on the collector foil. The ○ in the "Residual Capacity" column in Tables 1 and 2 indicates that the voltage of the electrochemical device after being placed for 24 hours was 2.3 V or more, and a high residual capacity was obtained. On the other hand, the × in the "Residual Capacity" column indicates that the voltage of the electrochemical device after being placed for 24 hours was less than 2.3 V, and a low residual capacity was obtained.

[0110]

[0111] In Example 1, the use of SBR as a binder enhanced the bonding strength of the active layer in Electrode a1, resulting in high peel strength. Furthermore, the intermittent coating process formed an exposed portion of the collector foil, reducing the caulking resistance between Electrode a1 and the lead member. Electrochemical device A1 achieved high capacity, low DCR, and a high residual capacity.

[0112] In Comparative Examples 1 and 2, since PTFE was used as the binder, the active layer bonding strength of electrodes b1 and b2 decreased, resulting in reduced peel strength. Micro short circuits occurred in electrochemical devices B1 and B2, resulting in reduced residual capacity.

[0113] Furthermore, in Comparative Example 2, the collector foil exposed portion was formed by removing part of the active layer with a brush. This increased the surface roughness of the collector foil exposed portion, increasing the caulking resistance between electrode b2 and the lead member. Electrochemical device B2 exhibited a higher DCR than electrochemical device B1.

[0114] In Comparative Example 4, the brush removal of a portion of the active layer exposed the collector foil, increasing the caulking resistance between electrode B4 and the lead member. Furthermore, in Comparative Example 4, increasing the thickness of the A1 etched foil, the collector foil, to 30 μm reduced the active layer loading, resulting in a decrease in the capacity of electrochemical device B4.

[0115] Examples 2 to 3 and Comparative Examples 5 to 7

[0116] Water was added to the electrode material to prepare a slurry. The electrode material used was a mixture of 88.25 parts by mass of activated carbon particles and 11.75 parts by mass of SBR, CMC, and AB combined. The SBR content in the electrode material relative to the total electrode material was set to the values ​​shown in Table 2. The mass ratio of SBR to CMC to AB was set to 1.75:4:6.

[0117] In Examples 2 to 3 and Comparative Examples 6 to 7, electrodes a2 to a3 and b6 to b7 with lead members were produced in the same manner as in Example 1 except that the above-mentioned slurry was used in the electrode production process, and electrochemical devices A2 to A3 and B6 to B7 were produced and evaluated.

[0118] In Comparative Example 5, since the SBR content in the electrode material was 0.25 mass %, an active layer was formed in the same manner as in Example 1. However, the adhesion between the active layer and the collector foil was low, and an electrode could not be produced. The peel strength of the active layer could not be measured.

[0119] The evaluation results are shown in Table 2. Table 2 also shows the evaluation results of Example 1.

[0120]

[0121] In Examples 1 to 3 in which the SBR content in the active layer (electrode material) was greater than 0.5% by mass and less than 2.5% by mass, no tailing occurred during intermittent coating, and the collector foil exposed portion was stably formed. As for electrodes a2 to a3, as in the case of electrode a1, the adhesion of the active layer was improved by SBR, and high peel strength was obtained. In addition, since the collector foil exposed portion was formed by intermittent coating, the riveting resistance between electrodes a2 to a3 and the lead component was reduced. As for electrochemical devices A2 to A3, as in the case of electrochemical device A1, high capacity and low DCR were obtained, and high residual capacity was also obtained.

[0122] In Comparative Examples 6 and 7, where the SBR content in the active layer (electrode material) was 3% by mass or greater, the slurry viscosity increased, causing coating tailing during intermittent coating, and the collector foil exposed portion was not stably formed. Electrochemical devices B6 and B7 exhibited increased DCR.

[0123] Industrial applicability

[0124] The electrode with a lead component obtained using the method for manufacturing an electrode for an electrochemical device with a lead component disclosed herein is suitable for use in electrochemical devices requiring low internal resistance. Although the present invention has been described in conjunction with the present preferred embodiments, such disclosure should not be construed restrictively. Upon reading the above disclosure, various modifications and variations will become apparent to those skilled in the art to which the present invention pertains. Therefore, the appended claims should be interpreted as encompassing all modifications and variations to the extent possible without departing from the true spirit and scope of the present invention.

[0125] Explanation of symbols

[0126] 1: Capacitor element, 2: First electrode, 3: Second electrode, 4: Diaphragm, 5a: First lead member, 5b: Second lead member, 6: Case, 7: Sealing member, 10: Electrochemical device, 20: Electrode, 21: Collector foil, 22: Active layer, 23: Exposed portion of collector foil, 30: Lead member, 31: Tab, 32: Connecting portion, 33: Lead, 40: Riveted portion, 41: Through hole, 42: Riveted tab.

Claims

1. A method for producing an electrode for an electrochemical device with a lead component, comprising the following steps: In the first step, a slurry containing activated carbon and a binder and a collector foil with a roughened surface are prepared; The second step is to apply the slurry on the surface of the collector foil and dry it to form an active layer, thereby obtaining an electrode; as well as The third step is to connect the electrode and the lead component; In the second step, the slurry is intermittently applied to the collector foil to form an uncoated area on a portion of the electrode where the surface of the collector foil is exposed. In the third step, the lead component is mounted on the uncoated area. The binder contains an elastomer, The content of the elastomer in the active layer exceeds 0.25 mass % and is less than 3 mass %.

2. The method for producing an electrode for an electrochemical device with a lead member according to claim 1, wherein: The elastomer is styrene-butadiene rubber.

3. The method for producing an electrode for an electrochemical device with a lead member according to claim 2, wherein: The content of the styrene-butadiene rubber in the active layer is 0.5 mass % or more and 2.5 mass % or less.

4. The method for producing an electrode for an electrochemical device with a lead member according to claim 2 or 3, wherein: The TI value of the slurry is 2 or more and 4 or less.

5. The method for producing an electrode for an electrochemical device with a lead member according to any one of claims 1 to 4, wherein: The arithmetic mean roughness Ra of the surface of the uncoated region is 0.5 μm or more and 1.0 μm or less.

6. The method for producing an electrode for an electrochemical device with a lead member according to any one of claims 1 to 5, wherein: The current collector foil is aluminum foil.

7. The method for producing an electrode for an electrochemical device with a lead member according to any one of claims 1 to 6, wherein: The thickness of the collector foil is 20 μm or less.

8. A method for manufacturing an electrochemical device, comprising the following steps: Step A, preparing a first electrode with a first lead member and a second electrode with a second lead member; Step B, winding the first electrode and the second electrode with a separator interposed therebetween to obtain a wound body; and Step C, making the electrolyte contained in the wound body; In the step A, at least one of the first electrode with the first lead member and the second electrode with the second lead member is obtained using the method for producing an electrode for an electrochemical device with a lead member according to any one of claims 1 to 7.