Current collector for rechargeable battery

By designing reinforced metal foils with fine and uniform functional porosity, the problems of high resistance, small surface area, and high cost of current collectors in lithium-ion batteries have been solved, achieving efficient electron and lithium-ion transport, reducing resistance and cost, and making it suitable for a variety of power devices.

CN118946989APending Publication Date: 2024-11-12ADDIONICS IL LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380031709.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-02-03
Filing Date
2023-02-02
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Existing lithium-ion battery current collectors face problems such as high resistance, small surface area, high cost, incompatibility with industrial manufacturing, and complex synthesis under high performance requirements, making it difficult to meet the demands for high energy density, high power density, and high stability.

Method used

Employing reinforced metal foil with fine and uniform functional porosity, and using a seamless repeating pattern of through-hole and non-perforated structural elements, it increases surface area and reduces resistance. Suitable for roll-to-roll manufacturing, materials include copper, aluminum, etc., and suitable for current collectors in lithium-ion batteries.

Benefits of technology

It improves the electrochemical performance of batteries, enhances electron and lithium-ion transport efficiency, reduces resistance, lowers costs, and is compatible with industrial manufacturing, making it suitable for a variety of power devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118946989A_ABST
    Figure CN118946989A_ABST
Patent Text Reader

Abstract

The present invention provides a foil having a fine and uniform functional porosity that can be inexpensively produced in a roll-to-roll configuration, while the porosity originates from wrinkling and / or perforation of the foil. The reinforced metal foils of the present disclosure may be used in many applications, including but not limited to use as current collectors in lithium ion batteries.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] Related Applications

[0002] This application claims the benefit of priority to U.S. Provisional Patent Application No. 63 / 267,543, filed on February 3, 2022, the contents of which are incorporated herein by reference in their entirety. Technical Field

[0003] The present invention, in some embodiments thereof, relates to electrochemical cells and, more particularly, but not exclusively, to current collectors suitable for use in primary and secondary cells. Background Art

[0004] Recently, a major century-long change from engine to battery has occurred in the automotive and renewable energy industries. Lithium-ion batteries (LIBs) have played a central role as a power source, and post-LIBs have attracted great interest as an alternative to LIBs. There is a strong demand for the rapid development of LIBs and post-LIBs with high performance parameters such as high charge and discharge cyclability, high energy density, high rate performance, and high safety of batteries. Efforts to meet the needs of high-performance LIBs have led to the development of many materials involving anodes, cathodes, separators, and solid electrolytes, which play an important role in improving battery performance. On the other hand, in order to improve battery performance, binders for binding anode and cathode active material particles, conductive additives mixed in the anode and cathode layers, additives added to the electrolyte solution, and current collectors (CCs) are also required. Binders, additives, and CCs with improved compatibility with high-performance anode, cathode, separator, and electrolyte materials can enable high-performance anodes, cathodes, separators, and electrolytes to be achieved.

[0005] CC plays an important role in the charge and discharge process of the battery. CC supports the active material layers of the anode and cathode, and they collect and distribute electrons to / from the supported active layers. In order to accelerate the transfer of electrons to / from the active layers, the contact between CC and the active layers should be maintained for thousands of cycles during the charge / discharge process. The active layer should have a path where fast electron transport is spread throughout the active layer, and Li + The CC structure should be designed to maintain the function of the active layer structure. Currently, in commercially available LIBs, the CC has a thickness of 10-12 μm and is planar. Copper (Cu) and aluminum (Al) foils are used as CCs for the anode and cathode, respectively. In the anode and cathode, Li + Ions and electrons should quickly move to and from the anode and cathode particle surfaces to charge and discharge the battery at high current density, respectively. Therefore, in the anode and cathode layers, Li +In the present LIB preparation process, a slurry consisting of anode or cathode active material particles, a binder, a conductive additive and a solvent is cast on a planar CC surface, and then the solvent in the slurry is evaporated to dry the anode and cathode layers formed on the CC. Anode and cathode material particles are filled into the prepared anode and cathode layers. Binders and conductive additives are located in the spaces between active material particles to bind the particles and form electrical contacts between active material particles. Li + An electrolyte solution of ions permeates through the space. + Ions pass through the space permeated by the electrolyte solution and reach the surface of the anode and cathode active material particles. In order to improve battery performance, Li + and improved paths for electrons. In addition, CCs should have high mechanical strength, chemical and electrochemical stability, and adhesion between the active material layer and the CC surface. In order to achieve these requirements, optimization of materials for CCs, structural modification of CCs, and formation of surface layers on CCs have been conducted. Improvements in battery performance such as charge / discharge capacity, energy density, and capacity retention at high current density and its stability can be obtained through the contribution of these factors.

[0006] Three-dimensional (3D) current collectors have been shown to be promising by enabling high energy density and high power density batteries. The utilization of 3D current collectors in lithium-based batteries benefits from the conductivity of the interconnected 3D structure, which ensures that electrons and lithium ions can be quickly transported / diffused throughout the network, and from the mechanical strength and chemical stability obtained through the microstructure, preventing delamination of active materials and collapse or corrosion of the skeleton, while maintaining flexibility and large pore volume, which can ensure sufficient space to accommodate the volume expansion of active materials. Despite the many advantages of 3D current collectors, there are still some concerns that need to be addressed: 1) The large surface area usually leads to a high electrode / electrolyte interface area, resulting in a large consumption of electrolyte and lithium materials, thereby leading to low Coulombic efficiency; 2) 3D porous current collectors still retain a considerable volume due to their disordered microstructure and low packing density, and their volumetric capacity is incomparable to those densely packed materials; 3) The high stability requirements of battery systems require strict control of the structure of 3D current collectors; and 4) Due to the complexity of 3D current collector synthesis, large-scale 3D current collectors for practical applications are still economically out of reach; 5) Since in industry the active materials are coated on metal foils through a roll-to-roll process and the current collectors need to be welded to metal leads, small or monolithic 3D current collectors are incompatible with downstream manufacturing processes.

[0007] Nakamura, T. et al. ["Electrochemical performance of cathodes prepared on current collector with different surface morphologies", J. Power Sources, 2013, 244, 532-537] reported cathode electrodes prepared on aluminum current collectors with different surface morphologies by conventional scraper technology, and their electrochemical performance, especially at high current rates, which was affected by the surface morphology of the current collector.

[0008] Wang, GQ et al. [“Investigation of the hole-formation process during double-sided through-maske electrochemical machining”, J. Mat. Processing Technology, 2016, 234, 95-101] reported a through-mask electrochemical machining technology developed for making hole arrays in titanium alloys that are difficult to cut using traditional machining.

[0009] Jeong, CU et al. [“Embossed aluminum as a current collector for high-rate lithium cathode performance,” J. Power Sources, 2018, 398, 193–200] reported an aluminum foil prepared by an anodization process followed by chromate phosphate treatment, which was evaluated as a current collector for cathode powders prepared by conventional electrode coating methods.

[0010] Shan, W. et al. [“Three-dimensional Porous Current Collector for Lithium Storage Enhancement of NiO Electrode”, Acta Chim. Sinica, 2019, 77(6), 551-558] reported the preparation of 3D porous metals, which have been used as current collectors to improve the cycle stability and high rate capacity of lithium-ion batteries.

[0011] Loghavi, MM et al. [“Improvement of the cyclability of Li-ion battery cathode using a chemical-modified current collector”, J. Electroanal. Chem., 2019, 841, 107–110] reported an aluminum current collector treated by a simple reaction of aluminum foil with a solution containing three acids, and studied the physical effects of this modification on the current collector surface by scanning electron microscopy (SEM) and contact angle testing.

[0012] Choi H. et al. ["Fabrication of a Porous Copper Current Collector Using a FacileChemical Etching to Alleviate Degradation of a Silicon-Dominant Li-ionBattery Anode", Corrosion Science and Technology, 2021, 20(5), 249-255] reported a simple method for preparing a three-dimensional porous copper current collector (3D Cu CC) for silicon-dominated anodes in lithium-ion batteries (LiB). The 3D Cu CC is prepared by combining chemical etching and thermal reduction from a planar copper foil.

[0013] JP2002216775A teaches a method of forming a current collector foil for secondary battery electrodes in which a large number of through holes are formed, wherein a non-elongated embossed roll having a large number of protrusions and a flat roll having no unevenness are provided.

[0014] WO2010011509A3 teaches an electrode material comprising: a first electrode; and a current collector disposed adjacent to and bonded to the first electrode, wherein the current collector comprises a plurality of conductive protrusions extending from the current collector into the first electrode along the z-direction.

[0015] WO2010116872A1 teaches a method for manufacturing an electrode for an electricity storage device, which prevents electrode particles from breaking and current collectors from bending, and forms a plurality of grooves in one direction on the surface of the current collector.

[0016] WO2013157806A1 relates to a method for manufacturing an electrode for a secondary battery, the method comprising a step of surface treating a current collector so as to provide a morphology having a surface roughness (Ra) between 0.001 μm and 10 μm on the entire surface and to improve adhesion between an electrode active material and the current collector, and an electrode for a secondary battery manufactured by using the method.

[0017] US20160197353A1 provides a perforated plate-like material having at least one through hole extending from a first main surface to a second main surface opposite thereto, and in its cross-sectional shape, it has a minimum width portion on the hole surface, and has a first main surface portion where the hole surface terminates at the first main surface, and includes a first protruding curve portion between the first main surface portion and the minimum width portion, and at least a portion of the first protruding curve portion has the surface properties / shape of a non-hole surface on the first main surface.

[0018] CN206250289U is a utility model that proposes a current collector, which is formed with a surface embossed portion in the thickness direction, wherein the embossed portion is distributed with a plurality of embossments, and inside each embossed periphery, a groove extending from the current collector surface to the current collector along the thickness direction of the current collector is formed in the peripheral area along the thickness direction of the current collector. Summary of the invention

[0019] The present invention provides a foil having fine uniform functional porosity that can be produced inexpensively in a roll-to-roll configuration, and the porosity originates from the corrugation and / or perforation of the foil. The enhanced metal foils of the present disclosure can be used in many applications, including but not limited to use as current collectors in lithium-ion batteries. The present invention provides enhanced metal foils that benefit from the advantages of carefully produced 3D metal structures, but are not limited by the cost, time and production size associated with state-of-the-art metal processing methods. The functional porosity of thin metal foils is increased to levels that challenge 3D structures (such as metal foams) through unique corrugation and perforation criteria and methods described below, while maintaining and benefiting from the speed, cost and roll readiness of thin foil production methods.

[0020] Modern current collector design faces several challenges, including:

[0021] The resistance of the current collector is reduced to improve the efficiency of the device; this is achieved by the present invention teaching the approach of using materials with low resistance such as copper, aluminum or nickel, and by designing the current collector to have a low resistance path for the current to flow.

[0022] The surface area of ​​the current collector is increased to improve its ability to collect electrical current; this is accomplished by the present invention, for example, by adding surface features such as vias, protrusions, and / or ridges.

[0023] Minimize the cost of the current collector; the present invention achieves this by teaching the use of low cost materials and by simplifying the production and design of the current collector to reduce manufacturing costs.

[0024] Ensuring that the current collector is compatible with other materials and techniques commonly used in an industrial setting; this is achieved through the inventive approach by teaching a continuous production method that provides a current collector that is not limited in size (length) and therefore facilitates a roll-to-roll coating process.

[0025] The present invention relates to an object comprising a metal component characterized by a seamless repeating pattern of through-hole textural elements and at least one of: (a) a seamless repeating pattern of non-perforated textural elements; (b) a local thickness in the range of 3-100 μm; and (c) a functional porosity (P) of at least 10%. f ), wherein the metal member is at least 0.1 m wide and at least 0.5 m long. The metal member can be composed of various metals, including aluminum, copper, nickel, gold, cobalt, iron, titanium, steel, stainless steel and any alloys and combinations thereof. The object can be used as a current collector in a battery electrode. The present invention also relates to a roll comprising a cylindrical core and an object wound around the core, and the object wound into a roll can have any length up to several thousand meters.

[0026] Thus, according to an aspect of some embodiments of the present invention, there is provided an object comprising a metal component characterized by a seamless repeating pattern of through-hole structural elements and at least one of:

[0027] (a) Seamless repeating pattern of non-perforated structural elements;

[0028] (b) a local thickness in the range of 3-100 μm; and

[0029] (c) a functional porosity (Pf) of at least 10%,

[0030] The metal component has a width of at least 0.1 m (at least 0.1 m wide) and a length of at least 0.5 m (at least 0.5 m long).

[0031] In some embodiments, the metal component is characterized by (a).

[0032] In some embodiments, the metal component is characterized by (b).

[0033] In some embodiments, the metal component is characterized by (c).

[0034] In some embodiments, the metal component is characterized by (a) and (b).

[0035] In some embodiments, the metal component is characterized by (a) and (c).

[0036] In some embodiments, the metal component is characterized by (b) and (c).

[0037] In some embodiments, the metal component is characterized by (a), (b), and (c).

[0038] In some embodiments, the metal component comprises or consists of a metal selected from the group consisting of aluminum, copper, nickel, gold, cobalt, iron, titanium, steel, stainless steel, and any alloys and combinations thereof.

[0039] In some embodiments, the local thickness of the object is in the range of 3-20 μm.

[0040] In some embodiments, the functional porosity is at least 50%.

[0041] In some embodiments, the through-hole structural elements in the seamless repeating pattern have an average opening size in the range of 10-200 μm.

[0042] In some embodiments, the seamless repeating pattern has 30-200 holes / mm 2 range of pore density.

[0043] In some embodiments, the seamless repeating pattern is characterized by a uniformity of at least 5%.

[0044] In some embodiments, the object is characterized by a tensile strength of at least 20-45 MPa.

[0045] In some embodiments involving objects provided herein:

[0046] The metal member comprises copper,

[0047] The seamlessly repeating pattern of the through-hole structural element comprises a motif of circular holes with a diameter less than 100 μm and a horizontal distance less than 500 μm,

[0048] The seamless repeating pattern of the non-perforated structural elements comprises primitives of circular depressions and / or circular protrusions each having a diameter of less than 500 μm and a horizontal distance of less than 1000 μm,

[0049] The local thickness is less than 50 μm,

[0050] The functional porosity is at least 50%,

[0051] The width is at least 0.1-5 m, and

[0052] The length is at least 50 m.

[0053] In some embodiments involving objects provided herein:

[0054] The metal member comprises aluminum,

[0055] The seamlessly repeating pattern of the through-hole structural element comprises primitives of circular holes with a diameter less than 120 μm and a horizontal distance less than 1000 μm,

[0056] The seamless repeating pattern of the non-perforated structural elements comprises primitives of circular depressions and circular protrusions each having a diameter of less than 500 μm and a horizontal distance of less than 1000 μm,

[0057] The local thickness is less than 100 μm,

[0058] The functional porosity is at least 50%,

[0059] The metal member is at least 0.1-5 m wide, and

[0060] The metal component is at least 50m long.

[0061] According to an aspect of some embodiments of the present invention, there is provided a roll comprising a cylindrical core and an object provided herein wound around the core.

[0062] In some embodiments, the width of the objects in the roll is in the range of at least 0.1-5 m.

[0063] In some embodiments, the length of the objects in the roll ranges from at least 0.5-10,000 m, and up to tens of kilometers.

[0064] According to an aspect of some embodiments of the present invention, there is provided a current collector comprising at least one object provided herein.

[0065] According to another aspect of some embodiments of the present invention, there is provided an electrode comprising the current collector provided herein.

[0066] According to another aspect of some embodiments of the present invention, there is provided a battery comprising at least one electrode provided herein.

[0067] According to another aspect of some embodiments of the present invention, there is provided an electric device comprising at least one battery provided herein.

[0068] In some embodiments, the electric device is selected from an electric vehicle for transportation in air, land, water, and / or space, a smartphone, a laptop computer, a media player, a power tool, a toy, a heating device, a cooling device, and a lighting device.

[0069] According to some embodiments of the present invention, the enhanced metal foil is manufactured by electroforming. This foil has a pattern of through holes that are seamlessly repeated throughout the foil. In order to manufacture this enhanced metal foil, a metal deposition substrate with small non-conductive gaps (referred to as lacunae) on the surface is used. The metal foil is then formed on this substrate, and the lacunae serve as a template for the through holes in the foil so that they are seamlessly repeated throughout the foil. In some embodiments, this enhanced metal foil is further subjected to wrinkling enhancement.

[0070] In some embodiments of the present invention, a special type of foil, referred to as "enhanced metal foil," is manufactured that exhibits a pattern of small through-holes that repeat seamlessly throughout the foil. The method of manufacturing this foil involves using a mask with openings, referred to as voids, through which to etch the metal foil. The voids act as a template for the through-holes, causing them to repeat seamlessly throughout the foil. In some embodiments, this enhanced metal foil is further subjected to wrinkling enhancement.

[0071] As used herein, the term "about" refers to ±10%. For example, "about 100 μm" includes 100 μm and 90 μm, 91 μm, 92 μm, 93 μm, 94 μm, 95 μm, 96 μm, 97 μm, 98 μm, 98 μm, 99 μm, 100 μm, 101 μm, 102 μm, 103 μm, 104 μm, 105 μm, 106 μm, 107 μm, 108 μm, 109 μm and 110 μm.

[0072] The terms "including", "comprising", "having" and their conjugations mean "including but not limited to".

[0073] The term "consisting of" means "including and limited to."

[0074] The term "consisting essentially of" means that the composition, method or structure may include additional ingredients, steps and / or parts, but only if the additional ingredients, steps or parts do not materially change the basic and novel characteristics of the claimed composition, method or structure.

[0075] As used herein, the phrase "selected from" includes all members of the recited group, each member of the recited group, and all possible combinations. For example, selected from A, B, and C includes only A, and only B, and only C, and A and B, and A and C, and B and C, and A, B, and C.

[0076] As used herein, the phrases "substantially free" and / or "essentially free" in the context of a substance refer to a composition that is completely free of such a substance or contains less than about 5%, 1%, 0.5% or 0.1% of the substance by total weight or volume of the composition. Alternatively, in the context of a process, method, property or feature, the phrases "substantially free" and / or "essentially free" refer to a process, composition, structure or article that is completely free of a process / method step or a property or a feature, or a process / method in which a process or method step is performed at less than about 5%, 1%, 0.5% or 0.1% compared to a given standard process / method, or a property or feature characterized by less than about 5%, 1%, 0.5 or 0.1% of a property or feature compared to a given standard.

[0077] As used herein, the term "substantially maintain" when applied to an original, desired, or provided property of an object or composition means that the property does not change by more than 20%, 10%, or 5% in the processed object or composition.

[0078] The term “exemplary” is used herein to mean “serving as an example, instance, or illustration.” Any implementation described as “exemplary” is not necessarily to be construed as preferred or advantageous over other implementations and / or to exclude the incorporation of features from other implementations.

[0079] The words “optionally” or “optionally” are used herein to mean “provided in some embodiments and not provided in other embodiments.” Unless such features are in conflict, any particular embodiment of the present invention may include a number of “optional” features.

[0080] When used herein, references without a specific number include plural referents unless the context clearly dictates otherwise. For example, the term "compound" or "at least one compound" may include a plurality of compounds, including mixtures thereof.

[0081] Throughout this application, various embodiments of the present invention may be presented in a range format. It should be understood that the description of the range format is only for convenience and brevity and should not be interpreted as a hard limit to the scope of the present invention. Therefore, the description of the range should be considered to have specifically disclosed all possible sub-ranges and individual numerical values ​​within the range. For example, the description of a range such as 1 to 6 should be considered to have specifically disclosed sub-ranges such as 1 to 3, 1 to 4, 1 to 5, 2 to 4, 2 to 6, 3 to 6, etc., and individual numbers such as 1, 2, 3, 4, 5 and 6 within the range. This applies regardless of the breadth of the range.

[0082] Whenever a numerical range is indicated herein, it is meant to include any cited numeral (fractional or integer) within the indicated range. The phrases "range between a first indicated numeral and a second indicated numeral" and "range from a first indicated numeral to a second indicated numeral" are used interchangeably herein and are meant to include the first and second indicated numerals and all fractions and integers therebetween.

[0083] The terms "process" and "method" as used herein refer to ways, means, techniques and procedures for accomplishing a given task, including but not limited to those ways, means, techniques and procedures that are known or readily developable from known ways, means, techniques and procedures by practitioners in the chemical, material, mechanical, computing and digital fields.

[0084] Unless otherwise defined, all technical and / or scientific terms used herein have the same meaning as commonly understood by those of ordinary skill in the art to which the invention belongs. Although methods and materials similar or equivalent to those described herein can be used in the practice or testing of embodiments of the present invention, exemplary methods and / or materials are described below. In the event of a conflict, the present patent specification, including definitions, shall prevail. In addition, the materials, methods, and examples are illustrative only and are not necessarily limiting. BRIEF DESCRIPTION OF THE DRAWINGS

[0085] Some embodiments of the present invention are described herein with reference to the accompanying drawings by way of example only. With specific and detailed reference now to the drawings, it should be emphasized that the details shown are merely examples and are used for illustrative discussion of embodiments of the present invention. In this regard, the description in conjunction with the drawings makes it clear to those skilled in the art how embodiments of the present invention can be practiced.

[0086] In said drawings:

[0087] Figure 1A -E shows an exemplary primitive (tile) and its corresponding seamless repeating pattern;

[0088] Figure 2 A simplified illustration showing the concepts of local thickness, minimum bounding box (MBB) thickness, and functional porosity;

[0089] Figure 3 A schematic diagram showing two tapered through holes in a foil, showing that the diameter of the holes at the top side of the foil (d1) is smaller than the diameter of the holes at the bottom side of the foil (d2);

[0090] Figure 4A -E shows various non-limiting examples of components or current collectors according to some embodiments of the present invention, each of which exhibits a different type of perforation enhancement of the metal foil;

[0091] Figure 5 Nine non-limiting examples of seamless repeating patterns provided by wrinkle enhancement according to some embodiments of the present invention are shown;

[0092] Figure 6 shows a schematic diagram of an exemplary component exhibiting SRP of circular depressions and protrusions provided by corrugation reinforcement using separate non-perforated structural elements, and showing the local thickness and bounding box thickness of the exemplary component, according to some embodiments of the present invention;

[0093] Fig. 7A -C shows a schematic diagram of a coating scheme for a reinforced metal foil according to some embodiments of the present invention, wherein the top cross-sectional view ( Fig. 7A ) shows an electrode which exhibits the same thickness as the total thickness of the corrugated foil member (MBB thickness), similar to the middle figure ( Figure 7B ), bottom graph( Figure 7C ) shows an electrode exhibiting a greater thickness compared to the total thickness of the corrugated member (MBB thickness);

[0094] Fig. 8A -B shows a micrograph taken using an optical microscope, taking a photo of a 12 μm thick copper foil ( Fig. 8A ) and 60μm thick aluminum foil ( Figure 8B ) each foil having undergone corrugation reinforcement in the form of hexagonally arranged circular depressions spaced about 500 μm horizontally from one another;

[0095] Fig. 9 shows a photograph taken with a Leica DVM6 optical microscope of a 60 μm thick aluminum foil subjected to perforation and wrinkling enhancements in the form of hexagonally arranged circular holes and depressions, respectively, spaced approximately 500 μm horizontally from each other;

[0096] Fig.10 shows a photograph taken with a Leica DVM6 optical microscope of a dried layer of a slurry applied to a corrugated aluminum foil or component after aluminum removal by acid etching, showing five raised structural elements and four recessed structural elements pointing to opposite sides, according to some embodiments of the present invention;

[0097] Fig.11 shows a photograph taken with a Leica DVM6 optical microscope of a dried layer of a slurry applied to a perforated member made of aluminum after the aluminum was removed by acid etching, showing several circular protrusions made of active material formed in the voids in the member where pores would normally be located, according to some embodiments of the present invention;

[0098] Fig. 12A -B shows battery cycling results obtained for a lithium-ion battery including a wrinkled current collector according to some embodiments of the present invention, wherein Fig. 12A Shown are the measurements of the retained capacity (capacity scale is a percentage of the initial capacity) of cells using the corrugated CC configuration provided herein, Fig. 12B The measured values ​​of the internal resistance of the battery at various states of charge are shown, while the results are compared with those obtained for similar batteries containing conventional (flat, non-porous) current collectors;

[0099] Fig.13A -B shows a 0.53 cm section of a perforated and flat (non-corrugated) reinforced foil made using one of the continuous manufacturing processes described herein. 2 Optical scanning of the sample, where Fig.13A shows an aluminum object with a local thickness of 20 μm having an SRP consisting of circular via primitives with a mean radius of 55.1 μm and a standard deviation of 2.4 μm (uniformity of the SRP is 4.4% SD), Fig. 13B shows a copper object with a local thickness of 22 μm having an SRP consisting of circular via primitives with a mean radius of 58.9 μm and a standard deviation of 1.4 μm (uniformity of the SRP is 2.4% SD);

[0100] Fig.14A -B shows an SEM micrograph of a wrinkled and perforated object showing a top view of a copper current collector coated with active material on one side for demonstration purposes ( Fig.14A ), and the cross section of the SRP perforated aluminum current collector ( Fig. 14B );

[0101] Fig.15 shows a graph of capacity retention versus cycle number measured in lithium-ion batteries produced with perforated and corrugated CCs according to some embodiments of the present invention, with an initial capacity of 35 mAh as 100%;

[0102] Fig.16 is a comparative graph showing the variation of DCIR with cycle life between two constructions, one being a cell constructed with a conventional (original foil) CC and the other being a cell constructed with an enhanced metal foil as provided herein;

[0103] Fig.17A -B shows a photograph of a reinforced metal foil (metal member) according to some embodiments of the present invention, the foil comprising aluminum and exhibiting corrugation reinforcement, wherein the local thickness is about 20 μm, the vertical distance (height) of the circular protrusions (non-perforated structural elements) is about 72 μm (which is also the MBB thickness), and the horizontal distance between the structural elements is about 500 μm, wherein Fig.17Aand a close-up inset showing the entire roll of reinforced metal foil, Fig. 17B A microscopic image showing corrugated structural elements is shown in FIG; and

[0104] Fig.18A -C shows a photograph of a reinforced copper foil according to some embodiments of the present invention, which exhibits wrinkling reinforcement, wherein the local thickness is about 12 μm, the MBB thickness is about 100 μm, and the horizontal distance between structural elements is about 500 μm, wherein Fig.18A The entire roll of reinforced metal foil is shown in Fig.18B A close-up inset is shown in FIG. Fig. 18C A microscopic image showing corrugated structural elements is shown in . DETAILED DESCRIPTION

[0105] The present invention, in some embodiments thereof, relates to electrochemical cells and, more particularly, but not exclusively, to current collectors suitable for use in primary and secondary cells.

[0106] Before explaining at least one embodiment of the invention in detail, it should be understood that the invention is not necessarily limited in its application to the details set forth in the following description or exemplified by the examples. The disclosure is intended to encompass other embodiments or to be practiced or carried out in various ways.

[0107] As discussed above, the current collector is responsible for making electrical contact with the anode and cathode in a rechargeable battery so that electrons can be transferred to the battery in the form of charge-balancing ions or lithium ions (Li + ) (especially in the case of lithium and lithium-ion batteries) enter and leave the battery. + When entering the cathode, electrons must also enter the cathode to balance the charge of the cathode. + The electrons are conducted through an electrolyte that does not conduct electrons, so they need another way to get to and from the cathode and anode. The current collector (CC) provides this path. An external circuit (the "load", such as a light bulb or an electric vehicle) is connected to the rechargeable battery through terminals that are in electrical contact with the CC.

[0108] Commercially available primary and secondary batteries traditionally use planar, flat metal foils, woven metals or meshes attached to the back of the cathode and anode as their CCs. These CCs are limited in their ability to support large amounts of active materials, and their ability to uniformly transfer charge from the active material mass and extract useful energy from large active material loads is also limited. Lack of uniformity and other spatial inconsistencies are the main causes of battery malfunctions, failures and even dangerous outcomes, mostly due to delamination of active materials from the CC, formation of hot spots, cracks and expansion.

[0109] In conceiving the present invention, the inventors envisioned a CC for battery electrodes that can be manufactured according to industry requirements, standards, practices and machines, i.e., coated and integrated into battery production lines, and unlike other 3D CCs, it can be manufactured quickly and in any length (tens, hundreds and thousands of meters long rolls) at a cost comparable to standard metal foils of similar size / quality. The inventors have envisioned that corrugation can increase the surface area of ​​thin metal foils because the corrugated foil presents a wavy / uneven structure with a series of ridges and grooves, which increases the total surface area of ​​the foil compared to a flat foil of the same size because the wavy / uneven structure creates more surface area for contact with active materials. It has also been envisioned that the increased surface area in the structural material will be beneficial because it can increase the bonding surface area between the foil and other materials. The inventors have also envisioned perforation to increase the surface area of ​​thin metal foils, which is achieved by creating a series of small holes or openings in the foil. Perforating the foil creates additional surface area by exposing the edges of the holes, which can be beneficial to improve the electrical pathways in the current collector and increase the efficiency of the electrochemical processes occurring in the battery electrodes. The perforations allow the top and bottom active material layers applied on the CC to contact through the holes, thereby also increasing the adhesion between the active materials and the current collector.

[0110] While putting the present invention into practice, the inventors demonstrated an enhanced metal foil having structural elements that increase its surface area and minimum bounding box voids (see below, functional porosity), such that the amount of active material that can be loaded thereon is much greater than a flat featureless metal foil of similar size / mass. The structural elements of the enhanced metal foil also shorten the electrical paths within the active material layer deposited thereon, thereby improving the contact and charge transfer parameters of using such enhanced metal foil as an electrode of a CC.

[0111] Thus, described herein are reinforced metal foils useful as current collectors that overcome the above-mentioned disadvantages and solve some of the problems in the related art to which the present disclosure pertains, as well as methods of making and using the same.

[0112] Thus, according to some embodiments of the present invention, there is provided a component referred to herein as a reinforced metal foil, characterized by a combination of some or all of the following properties:

[0113] Made of conductive material (preferably metal);

[0114] exhibiting seamless repeating patterns of non-perforated structural elements;

[0115] exhibiting a seamless repeating pattern of through-hole structural elements;

[0116] exhibiting a local thickness of less than 100 μm or a local thickness in the range of 3-100 μm;

[0117] Functional porosity of at least 10% or greater than 50%,

[0118] The reinforced metal foil or object is at least 0.1 m wide and at least 0.5-200 m long, or at least its width or length is greater than 0.5 m.

[0119] Reinforced Metal Foil:

[0120] As used herein, the terms "enhanced" and "enhancement" refer to improvements in certain properties of a foil-like object as compared to those properties in a comparable original metal foil or unreinforced foil, wherein the original foil and the enhanced foil are each related to the context of an object used as a current collector in an electrode, regardless of the process by which they are obtained. Depending on the embodiment, the term "enhancement" encompasses the terms "extend", "extend", "expand", "stretch", "enlarge", "swell", "enlarge", "enlarge", "broaden", "enlarge", "expand", "stretch", "refine", "lengthen", "unfold", "stretch", "widen", and "inflate".

[0121] One of the objects of the present invention is to provide a reinforced metal foil which can be effectively used in an industrial environment, in particular as a current collector forming an electrode for the battery industry. The phrase "reinforced metal foil" is used interchangeably with the term "member" and the term "object" and refers to the final product, regardless of the process by which it is obtained, i.e. the term "reinforced" is used as a pronoun rather than a verb and does not necessarily mean that the original foil is a precursor to the final product.

[0122] In the context of embodiments of the present invention, a raw metal foil is a very thin sheet of metal, typically made by rolling, hammering and / or electrochemical deposition. Here and throughout, the term "raw" is used to refer to an unreinforced foil, or, according to some embodiments of the present invention, to a precursor substrate for a component provided herein, or, according to some embodiments of the present invention, to a step in a process for making the component. In some embodiments, the term "raw metal foil" refers to a flat, smooth and planar metal foil or a non-reinforced metal foil.

[0123] In some embodiments, the reinforced metal foil (object; member) is made of a conductive metal. In some embodiments, the object comprises or consists of aluminum, copper, nickel, magnesium, cobalt, iron, titanium, platinum, tungsten and gold and any alloys thereof (including steel, stainless steel, carbide / nitride steel, bronze, silver-gold alloy, tin wax, brass and pig iron). In some embodiments, the alloy comprises magnesium, manganese, chromium, molybdenum and vanadium, as well as semi-metallic and / or non-metallic elements.

[0124] As used herein, the term "thickness" refers to the local thickness of the original foil or the thickness of a non-corrugated member, or the thickness achieved by reinforcement of the foil according to some embodiments of the present invention.

[0125] In some embodiments, the object (member) is a corrugated foil, and its local thickness refers to the property of the flat original foil that has undergone corrugation, rather than the thickness of the corrugated foil. Unless otherwise explicitly stated, the thickness of the corrugated object is the thickness of the smallest bounding box corresponding to the reinforced object as described below.

[0126] In some embodiments of the present invention, the local thickness of the components provided herein is as thin as about 3 micrometers (μm), and typically the local thickness of the components is less than about 100 μm, less than 90 μm, less than 80 μm, less than 70 μm, less than 60 μm, less than 50 μm, less than 40 μm, less than 30 μm, less than 20 μm, less than 15 μm, less than 10 μm, less than 9 μm, less than 8 μm, less than 7 μm, less than 6 μm, less than 5 μm or less than 4 μm. In some embodiments, the local thickness of the member is about 3 micrometers (μm), 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, about 10 μm, 15 μm, 20 μm, 30 μm, 40 μm, 50 μm, 60 μm, 70 μm, 80 μm, 90 μm, about 100 μm, 110 μm, 120 μm, 130 μm, 140 μm, 150 μm, 160 μm, 170 μm, about 180 μm, about 200 μm, about 250 μm, about 260 μm, about 270 μm, about 280 μm, about 290 μm, about 300 μm, about 350 μm, about 360 μm, about 370 μm, about 380 μm, about 390 μm, about 400 μm, about 450 μm, about 460 μm, about 470 μm In some embodiments of the present invention, the thickness of the metal foil forming the substrate of the member is within a certain range. In some embodiments of the invention, the local thickness of the member is in the range of 3-100 μm, 4-50 μm, 4-40 μm, 4-30 μm, 4-20 μm, or 4-10 μm 10-50 μm, 40-100 μm, 90-200 μm, 190-300 μm or 290-400 μm.

[0127] In some embodiments, the reinforced metal foil is a perforated reinforced metal foil. In some embodiments, the reinforced metal foil is a corrugated reinforced metal foil. In some embodiments, the reinforced metal foil is a metal foil reinforced by both perforation and corrugation.

[0128] In some embodiments, the metal is aluminum and the local thickness of the object is in the range of about 3-250 μm, 3-100 μm, 3-50 μm, 4-500 μm, 10-50 μm, 50-100 μm, or in the range of about 100-250 μm. According to some embodiments of the present invention, the thickness of a smooth (planar, non-corrugated) member made of aluminum, or the local thickness of a member made of aluminum corrugated but not perforated by a seamless repeating pattern (SRP) of non-perforated structural elements, or the local thickness of a member made of aluminum corrugated by SRP and perforated by SRP as defined herein, is less than 100 μm, less than 50 μm, less than 40 μm, less than 30 μm, less than 20 μm, less than 15 μm, less than 10 μm, less than 8 μm, or less than 6 μm.

[0129] In some embodiments, the metal is copper and the local thickness of the object is in the range of about 4-250 μm, 4-50 μm, 6-50 μm, or in the range of about 10-100 μm. According to some embodiments of the present invention, the thickness of a smooth (planar, non-corrugated) member made of copper, or the local thickness of a member made of copper corrugated by SRP but not perforated, or the local thickness of a member made of copper corrugated by SRP and perforated by SRP as defined herein, is less than 100 μm, less than 50 μm, less than 40 μm, less than 30 μm, less than 20 μm, less than 15 μm, less than 10 μm, less than 8 μm, less than 6 μm, or less than 5 μm.

[0130] As described below, the components provided herein are enhanced to increase their functional porosity. The enhanced object may be thicker than its precursor original foil, so in some embodiments including any of the above embodiments, the thickness of the component (see below, MBB thickness) is about 10 μm, about 20 μm, about 30 μm, about 40 μm, about 50 μm, about 60 μm, about 70 μm, about 80 μm, about 90 μm, about 100 μm, about 150 μm, 200 μm, 300 μm, 400 μm, 500 μm, 600 μm, 700 μm, 800 μm, 900 μm or about 1 mm.

[0131] Unless otherwise stated, the local thickness of a component or object provided herein can be measured using microscopy techniques such as scanning electron microscopy (SEM), optical microscopy, a micrometer, or other methods.

[0132] In some embodiments, the metal foil is in the form of a long sheet with a fixed width and an unlimited length, subject only to practical limitations. In some embodiments, the metal foil has a width in the range of 10 cm to 5 meters and a length of at least 0.5 meters, or at least 1 meter, or at least 2 meters, or at least 5 meters, or at least 10 meters.

[0133] In some embodiments of the present invention, the enhanced metal foil provided herein is produced as a single piece or continuous roll using a manual or automatic process. The substrate here can be a metal mesh (i.e., a perforated material), a dense metal layer, a metal foil, etc. The process for enhancing the metal substrate can be carried out at room temperature, or the deformation process can be assisted by heating. The process using heating can be carried out in a standard atmosphere or in an atmosphere with a vacuum or an inert gas.

[0134] After the metal foil substrate is enhanced, the enhanced metal foil (component) can be stacked on top of other components. In some embodiments, the enhanced metal foil is stacked to form a layered structure, and in some embodiments, the stacked components are bonded together. In some embodiments, the bonding is achieved by diffusion bonding. In other embodiments, the bonding is achieved by ultrasonic welding. In other embodiments, the bonding is achieved by welding. In some embodiments, the stacked components are laminated to provide thicker objects. In some embodiments, the thickness of the layer is 1 μm, 5 μm, 10 μm, 25 μm, 50 μm or 100 μm. WO2022064483A1 of the assignee of the present invention teaches a method of liquid cold welding (LCW), comprising: (a) combining two or more porous conductive substrate layers between perforated non-conductive frames so that the substrate layers are in contact with each other; (b) immersing the substrate layers in an electrolyte solution; and (c) applying current and / or voltage and / or electricity to the electrolyte solution. WO2022064483A1 also discloses a device suitable for performing some embodiments of the method.

[0135] In some embodiments, the components can be stacked on top of other metal substrates that have not been reinforced. In some embodiments, the non-reinforced metal substrates are stacked. In some embodiments, the non-reinforced metal substrates are stacked and bonded together. In some embodiments, the bonding is achieved by diffusion bonding, thermal welding, ultrasonic welding, or electrochemical welding.

[0136] In some embodiments, the member is produced as a single sheet with or without heating. In some embodiments, the member is produced as a continuous sheet with or without heating.

[0137] In some embodiments, the metal component provided herein is manufactured by a continuous process discussed below and wound into a roll. In some embodiments, the component is rolled into a cylindrical roll with a width in the range of 10 cm to 3 meters and a length of at least 10 meters or at least 100 m long.

[0138] The reinforced metal foil provided herein is designed for continuous manufacture, which generally produces a roll of the object, and is further designed to be used in the form of a roll in an industrial environment. Therefore, the object provided herein is characterized by mechanical properties that make it producible and usable in an industrial environment. One of these properties is tensile strength, which is sufficient to withstand the forces and stresses of drawing, winding, stretching and other operations used in the manufacturing process. The tensile strength required for a typical foil used to make a current collector for a battery in a typical industrial environment will vary according to the specific application and the type of foil, coating material and battery. For example, a foil for a lithium ion battery generally has a tensile strength of about 45MPa (about 4.6KgF / mm 2 , in kgf / mm2). The enhanced metal foils provided herein differ from the original foils in that the enhanced properties should also withstand the forces and stresses used in industrial environments, and the objects should not tear and their structural elements should be protected. In the context of some embodiments of the present invention, the objects provided herein are characterized by a tensile strength of at least 20-45 MPa or at least 60 MPa, at least 55 MPa, at least 50 MPa, at least 45 MPa, at least 40 MPa, at least 35 MPa, at least 30 MPa, at least 25 MPa, or at least 20 MPa.

[0139] Seamless Repeating Pattern:

[0140] An object of the present invention is to provide a reinforced metal foil characterized by a high uniformity of its structural elements and properties substantially over its entire area, whereby it is also desirable that the properties of the reinforcement are substantially the same over the entire area of ​​the foil. It is to be noted here that the term "structural elements" refers to the surface quality or feel of a material, such as its roughness, smoothness or pattern. Structural elements are visual aspects of a surface that give it a sense of depth and dimension. In the context of the present invention, the term "structural elements" encompasses both perforated elements (through holes) and non-perforated elements (protrusions; depressions).

[0141] The uniform distribution of fine structural elements (through-holes and / or non-perforated elements) can increase the conductivity and reduce the resistance of the reinforced metal foil provided herein. In order to show uniform reinforcement, the reinforced metal foil provided herein is characterized in particular by a non-random and specially designed seamless repeating pattern (SRP) of the structural elements, which conceptually spans the entire area of ​​the metal foil, with no visible boundaries or irregular / arbitrary / random transitions between or within the repeating pattern primitives. In the context of the present invention, the reinforced metal foil is regarded as an infinite planar area, limited only by practical limits.

[0142] As used herein, the term "patterned" when referring to foil refers to a non-random, specially designed and engineered metal foil having regularly spaced and oriented structural elements on its surface in some embodiments of the present invention. The features may be, but are not limited to, holes, peaks, valleys, defects, bends, twists, undulations, holes, or combinations thereof.

[0143] The phrase "seamless repeating pattern" (abbreviated herein as SRP) as used herein refers to a pattern that spans an undefined and unrestricted surface without visible transitions or boundaries. An SRP is an endlessly repeating pattern of structural elements, consisting of repeating elements such as geometric shapes or decorative designs arranged in a two-dimensional format. An SRP extends infinitely in all directions, creating a seamless visual effect. This pattern type is commonly used in textiles, wallpapers, flooring and other decorative materials, as well as graphic design, packaging and branding. As discussed herein, an SRP can be defined by a repeating pattern unit, and placing multiple such units in close proximity (juxtaposition) to each other will provide the SRP. The repeating unit is referred to herein as a tile or primitive.

[0144] The primitives are defined by one or more structural elements, and each primitive is integrated into adjacent primitives to achieve the SRP. In the context of the present invention, the primitives include structural elements in the form of holes (i.e., perforations, pores, through-windows) or protrusions / indentations (i.e., protrusions / depressions, bulges / creases, valleys / ridges), and the entire SRP can be defined by the primitives. As explained below, in contrast to the random distribution of similar structural elements over similar areas, the arrangement of any given structural element in the seamless repeating pattern that characterizes the metal components provided herein is not random; therefore, the SRP that characterizes the metal foils provided herein is non-random by definition.

[0145] Covering a planar metal foil surface with the above-described SRP follows essentially any standard tessellation or tiling method using one or more geometric shapes (tiles; primitives) with no overlaps and gaps. Although some embodiments of the present invention are drawn to metal foils (which are essentially two-dimensional entities if thickness is ignored), it is worth noting that tessellation can be generalized to higher dimensions and various geometric shapes. In some embodiments, the SRP is provided by periodic tiling, while some embodiments include regular tiling using regular polygonal tiles, all of which have the same shape, and some embodiments include semi-regular tiling using more than one shape and regular tiles with the same arrangement at each corner.

[0146] The term "element" or "tile" as used herein refers to the smallest and simplest single structural element or a non-repeating group of structural elements, which are repeated to form and define the SRP. In the context of the present invention, the element is closely related to the unit cell in a 3D lattice (crystal / lattice), and the SRP is formed by repeating the element in a plane in any direction on the plane. There may be one structural element or more than one structural element in an element. In some embodiments, the element includes more than one structural element related to each other by symmetry operations (such as translation, rotation and reflection transformation operations) in a 2D plane. In some embodiments, the element includes more than one structural element arranged asymmetrically relative to each other, or more than one structural element with different sizes / shapes. A plane or SRP can be completely tiled (covered) with triangular, rectangular and hexagonal polygons (tiles), each of which has one or more structural elements arranged inside. Rectangular and hexagonal tiles can be placed using the same tile orientation (translation only, no rotation), while triangular tiles are placed with a 60° rotation (translation and rotation).

[0147] An example of a simple primitive is a dot, which may appear as a hole (perforation reinforcement) and / or a protrusion / depression (wrinkle reinforcement), and its SRP may be a circle packing of squares or hexagons, where the circles are evenly spaced and, in the case of through holes, do not touch each other to allow for continuous foil material in between. Further exemplary and non-limiting embodiments of primitives and their corresponding SRPs, according to some embodiments of the present invention, are presented in Figure 1A -E.

[0148] Figure 1A -E shows an exemplary primitive (tile) and its corresponding seamless repeating pattern, where Figure 1A A square primitive (left) is presented, which shows rounded rectangular structural elements of various sizes arranged asymmetrically within a tile, and their corresponding SRPs generated by endlessly repeating the primitive on a plane; Figure 1B Three variations of the square primitive are shown, two with asymmetric arrangements of structural elements and one with a symmetric arrangement (lower left, 4-fold rotation), leading to the same SRP; Figure 1C Three variations of tile shapes are shown, along with the same SRP produced by endlessly repeating the primitive on a plane through a translation operation; Figure 1D Four variations of tiles are shown, and the same SRP produced by endlessly repeating the primitive on a plane through rotation and translation operations; Figure 1E Shown are tiles and their corresponding SRPs resulting from endless repetition of the primitive on a plane through reflection, rotation, and translation operations.

[0149] It is worth noting that the terms "structural element", "primitive" / "tile" and "seamless repeating pattern" (SRP) apply to any type of foil reinforcement, as these terms will be discussed below. In other words, the component is required to present a seamless repeating pattern for any of its structural elements (including through-holes, recesses / protrusions and / or creases).

[0150] In fact, in some embodiments, the reinforced metal foil exhibits SRP over its entire area from one side to the other; in some embodiments, due to technical / practical requirements of industrial processing machinery, the SRP spans the main area of ​​the foil, leaving narrow boundaries along its edges. By boundaries is meant that the foil does not exhibit SRP in the area considered as the boundaries, wherein the foil can be original or have a pattern different from SRP. In some embodiments, the boundaries extend over each edge of the metal foil, and in some embodiments where the foil is a long piece with a length more than 10 times longer than the width, the boundaries span less than 1%, less than 2%, less than 5%, or less than 10% of the total width of the metal foil. In some embodiments, one or more non-patterned strips are present near or at the center along the long axis of the member, which are designed for practical and industrial purposes, such as cutting the member into narrower strips. In such embodiments, the majority of the member contains SRP, and the narrow strips of the original foil separate the wide strips of SRP.

[0151] According to an embodiment of the present invention, the seamless repeating pattern is defined or constructed by mathematical methods. In some embodiments, the SRP is generated by machine learning.

[0152] roll:

[0153] The object provided herein is very thin, has a high surface area to volume ratio, and is highly flexible, meaning it can be easily bent, folded, and shaped without breaking, and can withstand a variety of stresses and forces. Therefore, due to these characteristics and the requirements of the manufacturing and utilization industries, one of the best formats for handling the object provided herein is in the form of a roll.

[0154] The long-travel roll of the member provided herein can be described as a cylindrical product, which is composed of a thin metal object wound around an axle. The roll has a fixed width generally and can have a length of tens of meters, hundreds of meters, or even several kilometers. The roll can be packaged with protective material to avoid any damage during transportation and storage.

[0155] The coil of foil is also characterized by winding density. The winding density of the coil of foil refers to the compactness of the foil when it is wound on the coil. It is a measure of the tightness of the foil wound on the coil core. The winding density is usually expressed as the ratio of the width of the foil to the diameter of the coil, and is usually measured in units of width per unit diameter (such as millimeters per millimeter or inches per inch). The winding density may be affected by various factors, such as the width of the foil, the thickness of the foil, the diameter of the core, and the tension applied during the winding process. A higher winding density results in a smaller diameter of the coil, and a higher packing density of the foil, while a lower winding density results in a larger diameter of the coil, and a lower packing density of the foil. The winding density is an important parameter in the manufacture of the coil of foil, because it affects the amount of foil that can be wound on the coil and the overall size of the coil. It also affects the handling and storage of the foil coil, and the performance of the foil in the intended application. Since the winding density is related to the MBB thickness of the object provided herein, the winding density of a fixed number of coils can be determined according to the MBB thickness, wherein the coil corresponds to a complete winding of the foil around the coil. Thus, according to some embodiments of the present invention, the winding density of the roll is in a range from at least 101 times the object MBB thickness per 100 roll layers to at least 150 times the object MBB thickness per 100 roll layers.

[0156] The reinforced metal foils provided herein can be wound onto a core tube or hollow cylinder, the inner and outer diameters of which can be selected to suit the manufacturing and utilization setting.

[0157] Therefore, according to one aspect of the present invention, a roll is provided, which comprises a cylindrical core and a reinforced metal foil wound around the core. The roll consists of a central cylindrical support, which is usually made of cardboard, plastic or metal, and a member provided herein is wound around the core. The core is usually hollow and provides the necessary support for the roll, while the member is a material for producing, for example, an electrode for a battery. Depending on the specific application, the roll can have different sizes and the member can have different thicknesses.

[0158] In some embodiments, a single continuous member provided in roll form has any fixed width, such as 0.1-5 meters wide, and any length, such as at least 0.5m, 1m, 10m, 30m, 50m, at least 100m long, at least 500m long, at least 1,000m long, or at least 0.5-100m long, at least 50-500m long, or at least 100-1,000m long, and in some embodiments, at least 1-5 kilometers long.

[0159] A coil of exemplary corrugated aluminium with a local thickness of 20 μm and a MBB of 70 μm would have the following dimensions: width 193 mm, length 350 m ± 10 m, coil inner diameter 80 mm, coil outer diameter 180 mm.

[0160] Foil reinforcement:

[0161] The reinforced metal foil (component) provided herein can be viewed as a metal foil that has been reinforced by perforating into a mesh and / or corrugating into a patterned plate to uniformly increase the surface area; these two forms of foil reinforcement are referred to herein as perforated reinforcement and corrugated reinforcement, respectively, and the property affected is referred to as "functional porosity," as that term is defined below.

[0162] In some embodiments, the member is corrugated, folded, protruding, curved, twisted, undulating, or a combination thereof (corrugated enhancement). In some embodiments, the member is perforated, pierced, punched, perforated, meshed, or a combination thereof (perforated enhancement). According to embodiments of the present invention, the member exhibits corrugated enhancement, perforated enhancement, or both perforated and corrugated enhancement.

[0163] In embodiments where the foil exhibits more than one type of enhancement simultaneously, each type of enhancement needs to be substantially uniform over the entire area of ​​the foil. In some embodiments, the uniformity of each type of enhancement is required to correspond to the size of its structural elements, such as the standard deviation of the structural elements in size and shape estimated by the similarity between primitives (tile similarity).

[0164] The term "size" as used herein refers to the characteristic dimension of an object or structural element. When referring to the size of multiple objects, it refers to the average value obtained by measuring the size of a representative set of objects. The size of a circular object can refer to the diameter of the object. In the case where the object is non-circular, the size of the non-circular object can refer to the diameter of the corresponding circular object, wherein the corresponding circular object exhibits or has a set of specific derivable or measurable features, which are substantially the same as the features of the non-circular object. Alternatively or jointly, the size of a non-circular object can refer to the average value of various orthogonal dimensions of the object. Therefore, for example, the size of an elliptical object can refer to the average value of the major axis and minor axis of the object. When referring to a group of objects having a specific size, it is envisioned that the object can have a size distribution around the specific size. Therefore, when used in this article, the size of a group of objects can refer to the typical size of the size distribution, such as the average size, median size or peak size.

[0165] Functional Porosity:

[0166] In the context of the present invention, a reinforced metal foil is referred to as having a non-zero functional porosity. The phrase "functional porosity" as used refers to a structural property of an object that defines and quantifies the available volume within a minimum bounding box (MBB) of said object. A minimum bounding box is the smallest bounding cuboid of an object, as this geometric concept is known in the art. In the context of a foil defined as being unlimited in width and length, the concept of MBB refers to an arbitrarily selected portion, section or fragment of said foil, or to a thickness dimension, such as Figure 6 as shown in .

[0167] The usable volume is considered to be all the volume within the MBB that is not occupied by the material of the object. For solid (non-perforated) foils, the functional porosity (P f ) is calculated as defined in Equation 1:

[0168] P f =(T b –T l ) / T b Eq.1.

[0169] Where T l is the thickness or local thickness of the original (smooth) foil, T b is the thickness of the corrugated member or the MBB thickness.

[0170] For a more general example, such as a perforated and corrugated member according to an embodiment of the present invention, the functional porosity (P or P) of the member is f ) is the volume fraction of the MBB not occupied by the building material, as defined in Equation 2:

[0171] P f =1–V m / V b Eq.2

[0172] Where V m is the volume occupied by the building block material, V b is the volume of the MBB including the building block material and voids. Functional porosity can also be expressed as a percentage of thickness or volume. The volume of a building block provided herein can be determined by dividing its mass by its density (m / cm 3). Herein, the density of the foil material is given in units of mass per unit volume. Thus, by recording the density of the component material, measuring the mass of the component, and determining the volume of the MBB, the functional porosity of the component can be calculated. For example, a foil that is wrinkled to exhibit peaks and valleys has a higher functional porosity than a flat / smooth foil made of the same material. In other words, a wrinkled foil will have a higher functional porosity than a flat / smooth foil because a completely flat foil occupying 100% of the MBB would have a functional porosity of zero.

[0173] Functional porosity as used herein relates to corrugated components (i.e., ridges, ridges / depressions, bulges / creases, valleys / ridges) and / or perforated components (i.e., mesh-like through-holes). For example, to calculate the functional porosity of a flat and uncorrugated foil or flat web, it should be considered that the thickness of the foil is much smaller than its width or length, however, the holes "expose" the inner wall, allowing access to a larger surface area of ​​the foil, and in terms of volume, the holes free up space that would otherwise be occupied by the substrate of the foil. Therefore, the functional porosity of a web with a finite thickness is higher than that of the original (non-perforated) foil. It is clear that the density, shape, and size of the holes (hole geometry) affect the functional porosity of the perforated component, and the thicker the foil, the more profound the effect of the hole geometry on the functional porosity. Similar to perforation, corrugation also increases the functional porosity of the component.

[0174] Figure 2 A simplified illustration of the concepts of local thickness, bounding box thickness and functional porosity is shown, where a straight horizontal dark black band (top) represents a longitudinal cross-section of a pristine foil with a given local thickness (shown to the right of the cross-section), and shows the minimum bounding box (dashed rectangle) of a foil with perforation reinforcement (left), the MBB of a foil with corrugation reinforcement (right), and the MBB and its thickness associated with a foil with both perforation and corrugation reinforcement (bottom).

[0175] As can be seen in Figure 2 As can be seen in Fig. 1, each reinforcement increases the free volume within the MBB, where perforation reinforcement increases the surface area within the MBB and corrugation reinforcement also increases the volume of the MBB; as can be further seen, when the foil is regarded as the substrate of the component, the simultaneous perforation and corrugation reinforcement increases the functional porosity to a maximum value.

[0176] In some embodiments, the constructs provided herein are characterized by a functional porosity of at least 5%, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70%, 75%, 80%, 85%, 90%, 95%, 100%, 105%, 110%, 115%, 120%, 125%, 130%, 135%, 140%, 145%, 150%, 155%, 160%, 165%, 170%, 175%, 180%, 185%, 190%, 195%, or at least 200% and more. In some embodiments, the functional porosity of the component is in the range of 5-100%, or 10-100%, or 50-150%, or 50-200%, or 100-150%, or 100-200%.

[0177] Perforation Enhancement:

[0178] Metal mesh can be produced in a variety of thicknesses depending on the intended application and the manufacturing method used. In general, metal mesh can be manufactured very thin, however, thinner mesh may tear or break more easily and may be less suitable for certain applications. There are several methods that can be used to produce thin metal mesh, including electroforming, electroplating, rolling, weaving, stamping, and cutting and stretching. Each of these methods has its own advantages and limitations, and the best method depends on the specific requirements of the application. Thin metal mesh can also be produced by etching or laser cutting metal sheets, which allows very fine, precise patterns to be produced in the mesh, however, these methods are very expensive and time consuming and are therefore suitable for relatively small sheets, which are generally not suitable for industrial environments.

[0179] In some embodiments, the perforated reinforced structural element is a small hole, i.e., a small through hole. The terms "hole", "hole", "through hole" (TH), through hole (TH), "interstitial hole" and "hole-type structural element" are used interchangeably herein. According to embodiments of the present invention, the hole can take any shape and direction, including circular, rectangular, triangular, hexagonal, elliptical, diamond or a variety of shapes.

[0180] The optional definition of SRP describes the member as a foil with a patterned surface, wherein the patterned surface is a porous surface with a designed hole position distribution (PLD). In some embodiments, the holes are located on the member at regular intervals. In some embodiments, the member has holes of different sizes at different locations on the member. In some embodiments, the member has holes of different types at different locations on the member. In some embodiments, the member has holes of different shapes at different locations on the member. In some embodiments, the member has holes arranged in a straight line. In some embodiments, the member has holes arranged in rows, and the rows are tilted at a certain angle relative to the side of the member.

[0181] As discussed above, the reinforcement of the metal foil follows a seamless repeating pattern or SRP, which can be defined by a tangent tile or pattern in which the hole is a structural element and is located. The SRP is formed by filling a plane with the tiles. A tile can include a portion of a (symmetrical) hole, a single hole or any shape, or more than one hole of the same or different shape (mixture of shapes) and / or its portion.

[0182] A metal foil reinforced by perforations following a seamless repeating pattern is also referred to herein as an SRP perforated member.

[0183] In some embodiments, the through holes may have parallel walls that are perpendicular to the plane of the foil. In some embodiments, the through holes may have inclined walls so that the size and shape of one opening of the through hole is different from the opposite opening of the same hole. For example, the space (aperture) defining a circular hole may have the conical shape of a trimmed cone, and the space defining a rectangular hole may have the conical shape of a trimmed pyramid.

[0184] Figure 3 A schematic diagram showing two conical holes in a foil with a certain local thickness shows that the diameter of the holes at the top side of the foil (d1) is smaller than the diameter of the holes at their bottom side (d2).

[0185] In some embodiments, the holes in the component with perforated reinforcement are characterized by tapered holes, or in other words, the holes narrow from one surface side of the foil plane to the other surface. It is noteworthy that this through-hole morphology is typical for methods of providing reinforced metal foils by electroforming the foil on a conductive substrate patterned with non-conductive voids as the SRP template surface. In some embodiments, the component with perforated reinforcement has a bottom side and a top side, and all holes in the component are wider at the bottom side of the component than at the top side, i.e., all holes taper to the same side of the component (see Figure 3). According to some embodiments, the taper of the pores is about 1-100% size reduction, or 1-50%, or 1-30%, or 1-20%, or 1-10% taper (pore size reduction) in terms of the decrease in diameter (or estimated size) of the pores from bottom to top. A 50% taper (pore diameter / size reduction) means that the surface of the bottom pore is 50% larger than the top pore. A 100% taper means that the pores are closed on the top side of the foil and the formation is a non-perforated structural element.

[0186] According to some embodiments, the hole opening diameter (opening size) of the member with the seamless repeating pattern of the through-hole structural element provided herein can be as small as 10-200 μm. In some embodiments, the opening size of the through-hole is in the range of 10 μm to 5000 μm, or about 10-2000 μm, or about 10-1000 μm, or about 10-100 μm, or about 10-50 μm, or 20-100 μm, 30-100 μm, 40-100 μm, 50-100 μm, 60-100 μm, 70-100 μm, 80-100 μm, 90-200 μm, 90-300 μm, 90-400 μm or about 90-500 μm. In some embodiments, the opening size of the through-hole structural element (hole, hole) is less than about 1,000 μm, less than about 750 μm, less than about 500 μm, less than about 250 μm, less than about 100 μm, less than 90 μm, less than 80 μm, less than 70 μm, less than 60 μm, less than 50 μm, less than 40 μm, less than 30 μm, less than 20 μm, less than 15 μm, less than 10 μm, less than 9 μm, less than 8 μm, less than 7 μm, less than 6 μm, less than 5 μm or less than 4 μm.

[0187] In some embodiments, including any of the above embodiments, the pores have opening (pore; opening size) dimensions of about 1-100 μm x about 1-100 μm, or about 40 μm x 50 μm, or about 52 μm x 52 μm.

[0188] In some embodiments, the horizontal distance between the centers of two adjacent through-hole structure elements is in the range of 1-1000 μm, or about 10-100 μm, or 20-100 μm, 30-100 μm, 40-100 μm, 50-100 μm, 60-100 μm, 70-100 μm, 80-100 μm, or about 90-100 μm. In some embodiments, the horizontal distance between the centers of two through holes (holes) in the perforated reinforcement member is about 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, 10 μm, 20 μm, 30 μm, 40 μm, 50 μm, 60 μm, 70 μm, 80 μm, 90 μm, or about 100 μm, 110 μm, 120 μm, 130 μm, 140 μm, 150 μm, 160 μm, 170 μm, 180 μm, 190 μm, or about 200 μm, 210 μm, 220 μm, 2 30μm, 240μm, 250μm, 260μm, 270μm, 280μm, 290μm, 300μm, 310μm, 320μm, 330μm, 340μm, 350μm, 360μm, 370μm, 380 μm, 390 μm or about 400 μm, 450 μm, 500 μm, 550 μm, 600 μm, 650 μm, 700 μm, 750 μm, 800 μm, 850 μm, about 900 μm, 950 μm or about 1,000 μm.

[0189] The hole density depends on the size of the holes and the horizontal distance between adjacent holes. In the context of the present invention, the hole density of a perforated member (or foil) is related to the number of through holes per unit area. In some embodiments, the hole density is related to the ratio between the area of ​​the substrate (metal) and the area of ​​the voids (holes) per unit area. According to some embodiments, the hole density is 1 mm2 / s. 2 (square millimeter) 30 holes to 200 holes / mm 2 In the Examples section below, non-limiting examples of perforation enhancement are provided based on pore size, density, and uniformity.

[0190] The uniformity of the perforated enhanced SRP is determined by any experimental method, such as taking photos of different parts of the component, scanning predetermined areas within a photo or different photos, identifying and digitizing the primitives in the scanned image, and measuring the size and horizontal distance of a predetermined number of primitives in each scanned portion, and calculating the standard deviation of the primitives across the portion. In embodiments where the primitive / tile contains a single hole, the SRP uniformity is related to the standard deviation between the individual holes. In embodiments where the primitive / tile contains more than one hole, the SRP uniformity is related to the standard deviation between the primitives / tiles. In some embodiments, the standard deviation of primitive overlap is in the range of 0-15%. In some embodiments, the standard deviation of primitive overlap is less than 15%, less than 10%, or less than 5%.

[0191] Figure 4A -E shows various non-limiting examples of components or current collectors according to some embodiments of the present invention, each example showing a different type of perforation enhancement of the metal foil.

[0192] According to some embodiments of the present invention, a reinforced metal foil comprising a seamless repeating pattern of vias is produced by electroforming a metal foil onto a metal deposition substrate having voids on its conductive surface, wherein the voids serve as a template for the seamless repeating pattern of vias in the deposited metal foil.

[0193] According to some embodiments of the present invention, a reinforced metal foil comprising a seamless repeating pattern of vias is produced by electro-etching a metal foil through a mask having voids (openings) therein, wherein the voids serve as a template for the seamless repeating pattern of vias in the etched metal foil.

[0194] Wrinkle Enhancement:

[0195] Corrugated metal foils are used in a variety of applications, including packaging materials, structural materials, and electrical and thermal insulation. Corrugation in thin metal foils refers to the process of creating ridges or grooves in the foil in order to increase its surface adhesion and surface area, strength and stiffness. This is usually achieved by subjecting the foil to high pressure, which causes it to deform and take on a wavy or bumpy structure. The resulting corrugated foil is stronger, more resistant to bending and deformation, and has a larger surface area than a flat foil of the same initial thickness.

[0196] In some embodiments, including any of the above embodiments, the raw foil or perforated metal foil exhibits a non-planar patterned member (a non-smooth embossed structure protruding from the general plane of the foil), that is, the foil is corrugated, folded, protruding, bent, twisted, undulating, or a combination thereof, collectively referred to herein as a non-planar patterned foil or a corrugated foil. The term "non-planar" as used herein refers to a substrate that is not flat, not smooth, not planar, not located or capable of being confined within a single plane, has a three-dimensional quality, or has an angle less than 180° or greater than 180° on its surface.

[0197] The term "corrugation" as used herein refers to a plurality of convex and concave embossed structural elements that impart a patterned structure, a regular surface roughness, and / or a regular surface waviness. The term "corrugation" as used herein combines and encompasses protrusions and depressions, "dual-face convex embossing" and / or "dual-face concave embossing", and refers to structural elements that produce protrusions and depressions within the same design on a material. In some embodiments, the size, shape, spacing, and relative orientation of the corrugated structural elements are regular. According to an embodiment of the present invention, corrugation is defined as a plurality of non-perforated structural elements arranged in a seamless repeating pattern (SRP), wherein the term "non-perforated" refers to a discernible structural feature on the surface of the foil that is not a hole and does not disrupt the surface to allow a substance to pass through.

[0198] Metal foils reinforced by corrugation following a seamless repeating pattern are also referred to herein as SRP corrugated members.

[0199] Unlike through-holes, non-perforated structural elements, such as creases, can span any length relative to the dimensions of the component, i.e., a crease can extend from one side to the other while forming part of a SRP parallel to the crease. Furthermore, unlike through-holes, non-perforated structural elements can disturb the surface on one side thereof and can be either protruding (e.g., a peak) or concave (e.g., a valley), depending on the definition of the "top side" and "bottom side" of the component. Thus, non-perforated structural elements can be divided into a set of individual elements, which can form a single localized protrusion, and a set of extended elements, which can form a ridge spanning the foil, terminating at the edge of the foil.

[0200] The non-limiting examples of non-perforated structural elements include projections, ridges, folds, depressions, peaks, protrusions, ridges and valleys. The shape of non-perforated individual structural elements can be defined by the "footprint" of the element on the foil surface, such as how it looks from above. The shape of non-perforated extended structural elements can be defined by the cross section of the foil perpendicular to the overall direction of the element. For example, simple circular projections / depressions are examples of individual non-perforated structural elements with circular (circle) shapes, and parallel ridges / valleys or parallel waves of undulations taking sinusoidal (sine wave) shapes are examples of extended non-perforated structural elements. Extended non-perforated structural elements can be perpendicular to the longitudinal axis of the member or span the width of the member at any angle relative to the longitudinal axis, and are parallel to the longitudinal axis of the member.

[0201] Figure 5 Nine non-limiting examples of seamless repeating patterns provided by corrugation enhancements according to some embodiments of the present invention are shown.

[0202] Figure 6 Schematic diagrams of exemplary components showing rounded concave and convex SRP provided by corrugation reinforcement using separate non-perforated structural elements are shown, along with the local thickness and bounding box thickness of the exemplary components according to some embodiments of the present invention.

[0203] Compared to the perforated reinforcement of the metal foil provided herein, the structural elements of the corrugated reinforcement may be smaller, similar, or larger, and may be defined by height as well as planar dimensions and shapes. The height of the corrugated structural element refers to the vertical distance from the bottom side to the top side of the member, in other words, the thickness of the MBB. For example, a valley refers to a depression in a surface, and a peak refers to the midpoint of two adjacent valleys extending above a portion of the surface. The peak-to-valley vertical distance or peak-to-valley distance is the distance between the top of a peak and the bottom of an adjacent valley, and is also the thickness of the MBB.

[0204] The horizontal distance between structural elements (non-perforated or through-hole) ("horizontal spacing") is essentially the distance between the centers of two adjacent structural elements (see Figures 4 and Figure 5). In some embodiments, in the wrinkling enhancement, the horizontal distance between the centers of two adjacent individual or extended non-perforated structural elements is in the range of 1-1000 μm, or about 10-100 μm, or 20-100 μm, 30-100 μm, 40-100 μm, 50-100 μm, 60-100 μm, 70-100 μm, 80-100 μm, or about 90-100 μm. In some embodiments, the horizontal distance between the centers of two non-perforated structural elements is less than about 1,000 μm, less than about 750 μm, less than about 500 μm, less than about 250 μm, less than about 100 μm, less than 90 μm, less than 80 μm, less than 70 μm, less than 60 μm, less than 50 μm, less than 40 μm, less than 30 μm, less than 20 μm, less than 15 μm, less than 10 μm, less than 9 μm, less than 8 μm, less than 7 μm, less than 6 μm, less than 5 μm, or less than 4 μm. In some embodiments, the horizontal distance between the centers of two non-perforated structural elements is at least about 10 μm, 50 μm, 100 μm, 150 μm, 200 μm, 300 μm, 400 μm, 500 μm, 600 μm, 700 μm, 800 μm, 900 μm, or at least about 1,000 μm.

[0205] It is to be noted here that in some corrugation methods where a thin foil is pressed against a flat or circular corrugated template (or vice versa) in order to imprint the SRP of the template onto the foil, the thickness of the foil may vary depending on the type of corrugation employed. In some embodiments, corrugation is achieved by mechanical expansion of the perforated member. For example, if the perforated member is characterized by a functional porosity of 55% (45% of the volume is occupied by metal), a thickness of 20 μm, and the perforated member (mesh) is pressed to present a corrugated structural element, during which it is stretched to a local thickness of 100 μm (5 times stretching), which will reduce the metal portion in the member by 5 times, from 45% to 9%. This also increases the functional porosity from 55% to 91%. In some embodiments, the stretching is achieved using embossing technology. In some instances, the stretched member is long and is rolled up for factory assembly lines.

[0206] The above can be described numerically as follows:

[0207] P (0) is the functional porosity of the original foil or planar perforated component;

[0208] P (1) is the functional porosity after wrinkling (stretching);

[0209] M (0) is the fraction of metal in the original foil or planar perforated member;

[0210] M(1) It is the fraction of metal in the reinforced metal component;

[0211] T (0) is the local thickness of the original foil or planar perforated member; and

[0212] T (1) is the local thickness after wrinkling (stretching),

[0213] Therefore, M (0) =1-P (0) .

[0214] Since no material is added or removed during the corrugation process:

[0215] M (1) =M (0) ·(T (0) / T (1) ),and

[0216] P (1) =1-M (1) .

[0217] Therefore, from 50% of P (0) Start and stretch 4 times to get P (1) =1-M (1) =1-50% / 4=87.5%. (0) =80% to get P (1) =95%.

[0218] In some embodiments, the stretching (local thinning) occurs primarily where the angles of the structural elements are sharpest or where the flatness changes sharply. This thinning or stretching of the foil may result in tears in the foil, which may be intentional, thereby forming through holes; otherwise, tears in the foil should be avoided. Therefore, the size of the corrugated structural elements also depends on the thickness of the foil, and in some embodiments on the perforations of the foil, which affect the tendency of the foil to tear under the corrugated stretching.

[0219] In some embodiments, the ratio of the thickness of the MBB to the local thickness (thickness of the original foil) is at least 1.1:1, at least 1.2:1, at least 1.3:1, at least 1.4:1, at least 1.5:1, at least 1.6:1, at least 1.7:1, at least 1.8:1, at least 1.9:1, at least 2:1, at least 2.2:1, at least 2.3:1, at least 2.4:1, at least 2.5:1, at least 2.6:1, at least 2.7:1, at least 2.8:1, at least 2.9:1, or at least 3: 1. In some embodiments, the ratio of the thickness of the MBB to the local thickness is in the range of 1.1:1-2:1, or 1.1:1-3:1, or 1.1:1-4:1, or 1.1:1-5:1. In some embodiments, the MBB thickness is 5-10 times greater than the local thickness. The ratio of the MBB thickness to the local thickness is also an indicator of the functional porosity on the non-perforated member with corrugated reinforced SRP, ie, a ratio of 1.1:1 corresponds to a functional porosity of 10% and a ratio of 3:1 corresponds to a functional porosity of 200%.

[0220] In some embodiments, the thickness of the MBB of the component with corrugation reinforcement is in the range of 6 μm to 5,000 μm. In some embodiments, the thickness or vertical distance of the MBB of the component with corrugation reinforcement is less than about 1,000 μm, less than about 750 μm, less than about 500 μm, less than about 250 μm, less than about 100 μm, less than 90 μm, less than 80 μm, less than 70 μm, less than 60 μm, less than 50 μm, less than 40 μm, less than 30 μm, less than 20 μm, less than 15 μm, less than 10 μm, less than 9 μm, less than 8 μm, less than 7 μm, less than 6 μm, less than 5 μm or less than 4 μm. In some embodiments, the MBB thickness of the component with corrugation reinforcement is at least about 5μm, 10μm, 20μm, 30μm, 40μm, 50μm, 60μm, 70μm, 80μm, 90μm, about 100μm, 150μm, 200μm, 300μm, 400μm, 500μm, 600μm, 700μm, 800μm, 900μm, 1,000μm, 1,200μm, 1,400μm, or at least about 1,500μm (about 1.5mm).

[0221] In some embodiments, the size of an individual non-perforated structural element (diameter, footprint, or widest horizontal span at the bottom of the structural element) is in the range of 10 μm to 5,000 μm. In some embodiments, the size of an individual non-perforated structural element is less than about 400 μm, less than 350 μm, less than 300 μm, less than 250 μm, less than 200 μm, less than 150 μm, less than 100 μm, less than 90 μm, less than 90 μm, less than 80 μm, less than 70 μm, less than 60 μm, less than 50 μm, less than 40 μm, less than 30 μm, less than 20 μm, less than 15 μm, less than 10 μm, less than 9 μm, less than 8 μm, less than 7 μm, less than 6 μm, less than 5 μm, or less than 4 μm.

[0222] In some embodiments, the corrugated SRP comprises extended structural elements, such as folds or undulations extending perpendicular to the longitudinal axis of the member, which is one long, continuous sheet. In some embodiments, the extended structural elements span the longitudinal axis diagonally.

[0223] In some embodiments, the corrugated SRP comprises individual structural elements, such as protrusions (convex) and depressions (concave), protrusions on one side of the member (protrusions only) or protrusions on both sides of the member (protrusions and depressions). In some embodiments, the individual structural elements are arranged in a straight line. In some embodiments, the individual structural elements are aligned in an inclined line, which is inclined relative to the longitudinal axis of the member or one of its sides. In some embodiments, as described above and Figure 5 As illustrated in , the individual structural elements are arranged in tiles / primitives.

[0224] In some embodiments, the structural elements of the perforation reinforcement are much smaller and more densely arranged (10-100 times smaller) than the structural elements of the corrugation reinforcement. As a non-limiting example, the circular through holes as the structural elements of the mesh foil subjected to perforation reinforcement are 10-100 times smaller than the protrusions / depressions as the structural elements of the foil subjected to corrugation reinforcement; the member as described above will have the appearance of a rugged fine mesh / screen.

[0225] In some embodiments, the perforated reinforced structural elements are substantially similar in size to the corrugated reinforced structural elements, and in some embodiments are also similarly arranged. In some embodiments, the perforated reinforced SRPs are aligned with the corrugated reinforced SRPs, in which case the two SRPs are referred to as sharing frequencies.

[0226] The post-production uniformity of the corrugated reinforcement SRP can be determined by any experimental statistical method, similar to that used for perforation reinforcement or a different method. In some embodiments, the standard deviation of the corrugated element overlap is less than 15%, less than 10%, or less than 5%.

[0227] Continuous manufacturing process:

[0228] The method of making the components provided herein facilitates the production of a continuous SRP on or in a continuous metal foil (also referred to herein as a metal substrate) and includes a continuous additive manufacturing method, a continuous subtractive manufacturing method, a bonding method, and in some embodiments, also includes a continuous post-manufacturing reinforcement step. The present invention provides a technique for cheaply and quickly producing long reinforced metal foils with high and uniform porosity, which involves enhancing the functional porosity of thin foils so that these reinforced foils provide the benefits of 3D structures (e.g., metal foams) while maintaining the benefits of uniformity (non-random SRP), production speed, production cost, and roll readiness obtained from thin foil production methods.

[0229] The preparation of the present invention includes forming very thin and highly perforated foils in a single additive manufacturing step, that is, the metal components provided herein can be provided in any length (up to several thousand meters) in a single process step, and some characteristics of the objects provided herein have been shown to define, such as local thickness and perforation enhancement and uniformity requirements under SRP conditions. In some embodiments, the additive manufacturing technology is electroforming, wherein the metal is deposited on a surface, the surface serves as a substrate for metal deposition and foil formation, and is simultaneously used to provide perforation enhancement under SRP conditions, as discussed below. For example, copper can be deposited on a cylindrical surface with orderly arranged voids or small gaps, the voids are evenly spaced on the surface, and are made of non-conductive material. In the context of the present invention, this orderly arrangement is a template for SRP, and a cylinder with a conductive surface and small non-conductive voids can be used to form a thin metal perforated foil with fine pores by an electroforming process. The voids serve as a template for forming holes in the metal component. The non-conductive material prevents metal from being deposited in those areas, and produces holes in the metal mesh that are approximately the same size and shape as the voids. This produces a seamless repeating pattern of fine through-holes in the metal component, reflecting the arrangement of the voids on the surface. According to some embodiments of the present invention, as proposed herein, the perforated metal component can also undergo corrugation enhancement to further increase its functional porosity, wherein the corrugation enhancement is achieved through a continuous roll-to-roll setup or as a step in the manufacture of other products (such as electrodes) using the metal component.

[0230] The preparation of the present invention includes enhancing a preformed thin metal foil in a single subtractive manufacturing step to exhibit perforation enhancement, that is, by introducing perforations into a foil that already exhibits some characteristics (such as local thickness) that define the object provided herein, the metal component provided herein can be provided at any length (up to several thousand meters). The perforation enhancement step is performed under SRP conditions and uniformity requirements. In some embodiments, the subtractive manufacturing technique is electro-etching, in which the metal is subjected to metal etching conditions through a mask that exhibits pores arranged under SRP conditions, resulting in the selective removal of metal (by mask or mask electro-etching) through the pores as discussed below. For example, a thin aluminum foil can be masked electro-etched through a mask having orderly arranged voids or small gaps, and the voids are evenly spaced in the mask. In the context of the present invention, this orderly arrangement is a template for SRP, and the voids act as a template for forming holes in the metal component. This step produces a seamless repeating pattern of fine through holes in the metal component, reflecting the arrangement of the voids in the mask. According to some embodiments of the present invention, as proposed herein, the perforated metal component may also undergo corrugation enhancement to further increase its functional porosity, wherein the corrugation enhancement is achieved through a continuous roll-to-roll setup or as a step in the manufacture of other products (e.g., electrodes) using the metal component.

[0231] In some embodiments, including any of the above embodiments, reinforcing the metal foil, substrate, or surface includes increasing the usable volume relative to the total volume of the bounding box, or in other words, increasing its functional porosity.

[0232] In some additive manufacturing embodiments, the metal foil is electroformed. In some embodiments, the metal foil is electroformed on a mandrel, which can be flat or have other shapes, such as a cylindrical barrel (cylinder). The terms "barrel", "cylinder" and "mandrel" are used interchangeably herein and refer to curved surfaces on which the metal foil can be formed, processed and / or enhanced as described herein. In some embodiments, the metal foil is electroformed on a mold and portions of the mold are completely or partially filled with a dielectric material. In some embodiments, such a mold can produce non-planar materials. In some embodiments, such non-planar materials can be dense / flat or have functional pores (dense means lacking pores).

[0233] In some subtractive manufacturing embodiments, the metal substrate is chemically etched. In some embodiments, the metal substrate is electro-etched. In some examples, the metal substrate is electro-etched on a cylindrical barrel or any other non-planar shape.

[0234] In some embodiments, the metal substrate is bonded to other metal substrates by diffusion bonding, ultrasonic welding, arc welding, electrochemical welding. In some embodiments, the metal substrate is deformed. In some instances, the substrate is a metal foil. In some instances, the substrate is a metal mesh.

[0235] In some embodiments, the metal substrate is rolled to further reduce its thickness. In some embodiments, after the metal substrate is electroformed or etched (chemical or electrical etching), the metal substrate further undergoes wrinkling enhancement to increase its functional porosity.

[0236] In some embodiments, described herein is a method of making a component, wherein the method includes electroforming a metal structure on a mandrel, which may be planar or have another shape, such as a cylindrical barrel.

[0237] In some embodiments, including any of the above embodiments, the method includes using a mandrel on which the structure is electroformed. In some embodiments, the mandrel has a flat surface or a patterned surface.

[0238] In some embodiments, patterning of the mandrel surface is achieved by machining, such as machining, etching, milling, laser machining, or any combination thereof.

[0239] In some embodiments, the method includes using forward and reverse current / voltage / power pulses and modifying the amplitude, shape, duration and rate / frequency of the pulses by modifying the pulse source during the electroforming process to control the lateral growth of the metal and produce a structure. In some embodiments, the method includes using direct current during the electroforming process.

[0240] In some embodiments, the shape of the pulse is not symmetrical. In some embodiments, the shape, amplitude, or duration of the pulse can be varied during the electroforming process to specifically control lateral growth at any stage of metal deposition.

[0241] In some embodiments, including any of the above embodiments, the method includes producing a perforated member by electroforming, wherein some portions of the working electrode are exposed and some portions of the working electrode are covered by a dielectric material, and the dielectric material is non-conductive, and the working electrode is a conductive surface where metal electrodeposition (plating) occurs. The non-conductive portions on the working electrode surface are also referred to herein as voids. The dielectric material may include various types of plastics, polymers, glues, epoxies, and other non-conductive materials.

[0242] In some embodiments, pockets are machined by mechanical, laser, controlled chemical process, or any other means and then filled with dielectric material. This results in electrochemical deposition of metal (electroforming) on ​​the conductive mandrel surface, but not on the non-conductive dielectric material, where holes are formed that typically have a tapered void shape that narrows from the bottom to the top of the formed foil (see Figure 3 ).

[0243] In some embodiments, pockets are machined by mechanical, laser, controlled chemical process or any other means and then partially filled with dielectric material. This results in electrochemical deposition (electroforming) on ​​the mandrel surface not covered by the dielectric material, including on the exposed portion of the inner wall of the pocket, producing a rimmed hole with a tapered void shape, as shown in FIG. Figure 3 In this embodiment of the invention and others, a continuous electroforming process is used to produce structural elements that simultaneously perforate the surface and protrude from the surface, or in other words, perforation and corrugation reinforcement are simultaneously performed by the same structural element.

[0244] In some embodiments, described herein is a method of making a component provided herein, wherein the method includes providing a metal foil having a patterned surface; and reinforcing the metal foil so that the metal is non-planar and has a functional porosity of 5-98% (wrinkle enhancement).

[0245] In some embodiments, including any of the above embodiments, the method includes providing a metal foil having a patterned surface, wherein the metal is initially planar but is transformed into a non-planar metal by corrugation enhancement. The transformation can be achieved using electrical, mechanical, magnetic or other forces or combinations thereof.

[0246] In some embodiments including any of the above embodiments, the method includes providing a substrate in the form of a metal foil, a perforated metal foil (net) or a member with perforation enhancement as provided herein, including applying a local mechanical force to the substrate. In other embodiments, the wrinkling enhancement includes using a metal tool (plane or cylinder) to press on the metal foil, thereby forming a non-perforated structural element in the metal foil. In certain other embodiments, the method includes using a metal structure (e.g., a template or substrate) to press on the metal foil, thereby producing a non-planar non-perforated structural element in the metal foil.

[0247] In certain other embodiments, the metal foil is modified using a stretching process. In certain other embodiments, the metal foil is modified using a stamping process. In certain other embodiments, the metal foil is modified using a twisting process. In certain other embodiments, the metal foil is modified using a wrinkling process. In certain other embodiments, the metal foil is modified using a bending process. In certain other embodiments, the metal foil is modified at room temperature. In certain other embodiments, the metal foil is modified at an elevated temperature.

[0248] In some embodiments, including any of the above embodiments, the method includes providing a member provided herein by deforming a metal substrate. In some embodiments, including any of the above embodiments, the method includes strengthening the metal foil, including applying mechanical force to a metal substrate such as an original thin metal foil or a perforated thin metal foil (SRP perforated member). In certain embodiments, the method includes strengthening the metal by stretching a metal substrate. Here, deformation includes changing the shape of a metal substrate, changing the porosity of a metal substrate, changing the pore size of a porous metal substrate, changing the pore shape of a porous material, or a combination of both or more of the above. Here, strengthening the substrate includes increasing some of the outer dimensions of the metal surface, such as its thickness and / or functional porosity. For example, strengthening the substrate may include increasing the size of pores in a porous metal surface. For example, strengthening the substrate may include increasing the surface area of ​​the metal surface. Strengthening may include increasing the length or width of the metal surface. In other embodiments, strengthening the substrate includes stretching the metal to make it longer or wider, but also thinner.

[0249] According to some embodiments of the present invention, the components provided herein can be manufactured by continuous electroforming (additive manufacturing) of components (e.g., meshes) having perforated reinforcements. In some embodiments, including any of the above embodiments, the continuous method includes providing a raw metal foil by electroforming, and further enhancing the foil to include the corrugated reinforcements described herein. In some embodiments, including any of the above embodiments, the method includes providing a perforated component by electroforming on a patterned barrel / mandrel, and further enhancing the perforated component to include the corrugated reinforcements described herein, thereby providing the perforated and corrugated components described herein.

[0250] Electroforming herein includes the process of forming a mesh or solid using electricity (specifically current, voltage or power). Electroforming includes electrodeposition, wherein metal ions are reduced to metal, wherein the metal has the shape of a mesh or foil, thereby forming a mesh or foil. Electroforming can include the use of a template on which the reduced metal is formed, wherein the template can be patterned or unpatterned. In some embodiments, the template is planar. In some embodiments, the template is curved, such as a cylinder / mandrel.

[0251] In some embodiments, the method for electroforming a mesh or foil comprises electroforming a mesh or foil comprising or consisting of copper, nickel, or zinc.

[0252] In some embodiments, the method for etching (chemically or electrochemically) a mesh or foil comprises etching a mesh comprising or consisting of copper, aluminum, titanium, or steel / stainless steel, and generally any metal that is conducive to etching.

[0253] Electroforming copper on a cylinder is a standard production method used by suppliers of copper foil, such as for battery current collectors. In some embodiments, including any of the above embodiments, the equipment used to electroform the metal foil is similar to equipment used to make screens for screen printing, screens for electric shavers, and nickel meshes as filters mainly used in the sugar industry. In some embodiments, the tool or mandrel for electroforming the components provided herein is reusable and facilitates continuous additive manufacturing. In certain other examples, the tool or mandrel for electroforming is not reusable.

[0254] In some embodiments, including any of the above embodiments, the method further comprises stretching the solid foil or mesh; wherein the stretching also increases the pore size of the mesh. In other examples, this type of reinforcement increases the length or width of the mesh. In other examples, this type of reinforcement increases the length or width of the mesh and also reduces the thickness of the mesh. In some embodiments, a combination of the above types of reinforcement steps are implemented.

[0255] In some embodiments, the methods herein include a first step of manufacturing a metal mesh or a member with perforated reinforcement by continuous additive manufacturing or continuous subtractive manufacturing as described above.

[0256] In some embodiments, the methods herein include a second step of increasing the functional porosity of the metal mesh or member by corrugation reinforcement. In some embodiments, the metal foil or perforated member formed by a continuous electroforming and / or continuous etching process is subjected to a mechanical force, which introduces non-perforated (corrugated) structural elements into the foil or mesh in a continuous manner.

[0257] In some embodiments, including any of the above embodiments, the method includes enhancing a metal surface, which includes etching a pattern on the metal surface. In some embodiments, the etching is completed using a neutral, acidic or alkaline etching solution. In some embodiments, the etching is completed using electricity to oxidize the metal surface. In some embodiments, the etching is a combination of electrical etching and chemical etching. In some embodiments, the etched pattern includes perforated (holes) and non-perforated (depression) structural elements.

[0258] For aluminum electrochemical etching, an aqueous solution with 0.5-3 M NaCl and a pH range between 0 and 5 may be used. Then, a constant or pulsed positive voltage in the range of 3-20 V on Al may be applied to the aluminum substrate for 5-600 sec.

[0259] In some embodiments, etching a pattern on a metal surface includes using a mask so as to etch a pattern through an opening in the mask. The openings in the mask are also referred to herein as gaps. In some embodiments, the mask is applied to a substrate to be etched. In some embodiments, the mask is inserted between two electrodes, one of which is a foil, but does not contact either electrode. In some embodiments, the mask is inserted between two electrodes, but does not contact the substrate to be etched. In some embodiments, the mask is attached to a counter electrode. In some embodiments, the etching is chemical etching. In some embodiments, the etching is electrochemical etching.

[0260] In some embodiments, including any of the above embodiments, manufacturing the metal substrate comprises electroforming or electroetching on a drum. In some of these embodiments, the drum is made of Al, Ni, Cu, Mg, Ti, steel, stainless steel, chrome-coated steel or other suitable metals, and in some embodiments, the drum is made of a dielectric material.

[0261] In some embodiments, the diameter of the barrel / cylinder / mandrel used for electroforming the metal foil or member according to some embodiments of the present invention, or the diameter of the barrel used for electroetching, is each independently about 100mm, 200mm, 300mm, 400mm, 500mm, 600mm, 700mm, 800mm, 900mm, 1,000mm, 200cm, 300cm, 400cm, 500cm, 600cm, 700cm, 800cm, 900cm, or a diameter of about 1-4m, about 2m, 3m, 4m, or about 5m.

[0262] In some embodiments, including any of the above embodiments, the barrel / cylinder / mandrel has a patterned structure arranged in SRP around its circumference on its curved surface, wherein the elements of the patterned structure on the curved surface can have any shape and size depending on the designed primitive. In some embodiments, the elements of the patterned structure on the curved surface are approximately circular and have a diameter in the range of 1-500 μm. In some embodiments, the diameter of the elements of the patterned structure on the curved surface is about 1 μm, or the diameter is about 1-10 μm, 10-20 μm, 20-30 μm, 30-40 μm, 40-50 μm, 50-60 μm, 60-70 μm, 70-80 μm, 80-90 μm, 90-100 μm, 100-110 μm, 110-120 μm, 120-130 μm, 130-140 μm, 140 -150μm, 150-160μm, 160-170μm, 170-180μm, 180-190μm, 190-200μm, 200-220μm, 220-240μm, 240-260μm, 260-280μm, 280-300μm, 300-220μm, 300-350μm, 350-400μm, 400-450μm, or about 450-500μm in diameter.

[0263] In some embodiments, including any of the above embodiments, the elements of the patterned structure are present in the curved surface of the tube / cylinder / mandrel in the form of holes that are at least 10-100 μm deep, at least 20-100 μm deep, or at least 30-100 μm deep, at least 40-100 μm deep, or at least 50-100 μm deep. In some embodiments, including any of the above embodiments, the hole in the barrel / cylinder / mandrel is at least 10 μm deep, or at least 20 μm, 30 μm, 40 μm, 50 μm, 60 μm, 70 μm, 80 μm, 90 μm or at least 100 μm deep, at least 110 μm deep, or at least 120 μm, 130 μm, 140 μm, 150 μm, 160 μm, 170 μm, 180 μm, 190 μm or at least 200 μm deep, or at least 210 μm deep, at least 220 μm, 230 μm, 240 μm, 250 μm, 260 μm, 270 μm, 280 μm, 290 μm or at least 300 μm deep.

[0264] Currently known subtractive manufacturing methods for perforating metal foils (e.g. aluminum foils) with a thickness of less than 100 μm are unable to provide the fine structure elements currently provided by the present invention, i.e., the state-of-the-art technology is unable to consistently and efficiently form uniform holes of less than 50 μm in thin aluminum foils with a thickness of less than 100 μm in a roll-to-roll mode. At best, the state-of-the-art technology provides a metal foil sheet of finite size (rather than a roll of infinite length) with relatively large holes of more than 150 μm, which are non-uniform (hole size varies more than 30%) and have jagged edges.

[0265] State-of-the-art techniques involve chemical etching through a photoresist mask applied to one or both sides of the foil, and etching is performed on one or both sides thereof, respectively. State-of-the-art techniques also include perforating the metal foil by electron beam emission or laser. These and other subtractive manufacturing methods of foil perforation do not produce highly uniform patterns, and / or are slow and expensive at best, are limited to the manufacture of relatively small sheets, and are therefore not conducive to the production and use of unlimited length roll-to-roll formats.

[0266] The perforated metal foil provided is achieved by electrochemical etching, using an electric current under certain chemical conditions, using a mask to dissolve certain locations in the metal foil atom by atom from one side of the foil. By choosing to use electrochemical etching instead of chemical etching to perforate the metal foil, the inventors have achieved control over the process parameters, thereby achieving a uniform perforation pattern.

[0267] In short, electrochemical etching is realized especially by fixing a metal foil on at least a portion of the circumference of the curved surface of a conductive cylinder, the cylinder acting as an anode during the electro-etching process, so as to form a conductive contact between the foil and the cylinder. In some embodiments, the anode is a flat surface, and in other embodiments, the anode is a curved conductive surface. A mask is placed on the exposed surface of the foil, substantially above the area where the foil contacts the anode, and the cathode bent to match the anode curvature is very close to the mask (about 0.1-10mm), preferably 3mm according to some embodiments, thereby forming a closed working space. Once the working space is sealed to act as a flow cell, the electrolyte flows continuously therein, and an electric current is continuously applied between the anode and the cathode, thereby continuously etching the foil through the holes of the mask while the foil continuously advances through the flow cell.

[0268] The challenge of seamless and endlessly repeating patterning is achieved by using a mask that is constructed for continuous production mode based on a roll-to-roll architecture. This architecture and the use of an SRP conductive mask enable the production of an "endless" perforated foil, overcoming the limitations of state-of-the-art technology. In some embodiments, the mask takes the form of a closed tape, stretched directly on a narrow roll of aluminum foil. In some other embodiments, a transient mask is created directly on the surface of the metal foil, for example by continuously printing an SRP conductive mask on a narrow roll of foil.

[0269] Current collector:

[0270] The current collector (CC) has the following general roles in a battery system: (i) since typical electrodes are made by casting a slurry (a mixture of active materials, polymer binder, and carbon additives) on the CC, the CC supports the electrode layers, and (ii) the CC provides an electrical path to transfer electrons between the electrode material and the external circuit. By controlling the properties of the CC, the following effects can be obtained: (i) the lower the thickness and the higher the strength, the more active materials can be stacked in a limited space, resulting in a high volumetric energy density; (ii) by strengthening the connection between the active material and the CC with a wide contact area, additional electron paths can be achieved, thereby reducing the internal resistance of the battery. Typically, Cu and Al are used as CCs for the anode (0-1.5 V relative to Li / Li+) and the cathode (3-4.7 V relative to Li / Li+), respectively, due to their electrochemical stability and active material compatibility in each reaction potential range.

[0271] The present invention provides a reinforced metal foil that exhibits high functional porosity and uniformity, thereby allowing a larger amount of active material slurry to be loaded thereon, increasing the contact surface area between the active material and the CC, and exhibiting uniformity over the entire area of ​​the CC, thereby reducing delamination of the active material, cracking, swelling, unfavorable formation of "hot spots", and other mechanical failures that lead to battery failure.

[0272] Compared to solid flat and smooth foil current collectors, current collectors with large surface area and low density (low weight) can have several advantages in electrodes of lithium-ion batteries. Improved active material utilization: Larger surface area allows more active materials such as lithium ions to be deposited on the current collector, thereby increasing the overall energy density of the electrode. Improved conductivity: High surface area current collectors can have greater conductivity, which can improve the overall performance of the battery. Reduced weight: Low weight current collectors can reduce the overall weight of the battery, making it more portable and convenient for use in applications such as electric vehicles and portable electronic devices. Better mechanical stability: High surface area current collectors can have greater mechanical stability, which can improve the overall durability and life of the battery. Better rate performance: High surface area current collectors can have greater rate performance, which means that the battery can be charged and discharged faster without reducing its performance. Overall, current collectors with large surface area and low density can improve the overall performance and efficiency of lithium-ion batteries.

[0273] In some embodiments of the present invention, the reinforced metal foil acting as a current collector with large surface area and low density (high functional porosity) provides the following advantages:

[0274] (i) The lower the thickness and the higher the strength, the more active materials can be packed in a limited space, resulting in high volumetric energy density;

[0275] (ii) by strengthening the connection between the active material and CC with a wide contact area, additional and shorter electron pathways can be achieved, thereby reducing the internal resistance of the battery; and

[0276] (iii) Low-cost, rapid and continuous manufacturing and provision of industrial-sized coils facilitates machinery and processes used in contemporary and advanced electrode and battery industries.

[0277] Thus, according to one aspect of some embodiments of the present invention, there is provided a current collector, in the sense of being a part of an electrode, which collects electrons from an electrode material and transfers them to an external circuit, wherein the CC consists of or comprises the reinforced metal foil (member) provided herein.

[0278] As used herein, the term "current collector" refers to a substrate that conducts electrons in a manner sufficient for use in a battery or electrochemical cell to complete an electrical circuit at the cathode and anode. The CC is typically made of a metal such as copper, aluminum, or nickel. Other metals such as magnesium, tungsten, cobalt, iron, titanium, platinum, tungsten, and gold, and any alloys thereof, as well as alloys or combinations of metals such as steel, may also be used. In the context of a secondary battery, the CC in the cathode conducts electrons into the cathode during discharge and conducts electrons out of the cathode during charge, while in the anode, the CC conducts electrons into the anode during charge and conducts electrons out of the anode during discharge.

[0279] The current collector may also include contacts and contact leads, terminals, and other features that are common and / or required as part of a current collector, or other features required for its assembly and implementation in an electrical device, and these additional features (all or any selection thereof) are encompassed in the definition of current collector used herein.

[0280] In some embodiments, the current collector comprises or consists of a member (eg, a mesh) that undergoes perforation reinforcement as defined and exemplified herein.

[0281] In some embodiments, the current collector comprises or consists of a member that undergoes corrugation reinforcement as defined and exemplified herein.

[0282] In some embodiments, the current collector comprises or consists of a member undergoing perforation and corrugation reinforcement as defined and exemplified herein.

[0283] In some embodiments, including any of the above embodiments, the current collector is provided in the form of a roll, as that term is defined above.

[0284] In some embodiments, the current collector provided herein comprises a significantly different metal layer (layer). Here, significantly different layers are defined as multiple metal layers that can be distinguished from each other under microscope imaging conditions. If the layers are melted, bonded, welded, brazed or diffused together or to each other so that the boundaries between them cannot be observed under microscope imaging, then the layers are not significantly different. However, if the layers are bonded together in a manner that the boundaries between them can be distinguished under microscope imaging, then the layers are referred to as being significantly different.

[0285] In the context of the present invention, particularly in the context of multilayer current collectors, a layer comprises or consists of a reinforced metal foil as provided herein. For example, the CC may have a total thickness of 100 μm and include five discernible layers, each 20 μm thick, and when stacked on top of each layer, the five layers add up to a total thickness of 100 μm. In some embodiments, the metal layers may be porous or non-porous, and each may be independently corrugated, perforated, or perforated and corrugated.

[0286] In some embodiments, including any of the above, the CC comprises distinct layers, each layer independently characterized by a total thickness (MBB thickness) in the range of about 4-20 μm, or 5-20 μm, or about 10-50 μm.

[0287] In some embodiments of the invention, CCs are made by stacking individual building blocks provided herein into metallic layers and are further characterized by indistinguishable layers (the layers are not distinct from each other).

[0288] In some embodiments, including any of the above embodiments, the SRP of the CC comprises pores with a diameter of 20-200 μm. In some embodiments, the SRP of the CC comprises pores with a diameter of 15-500 μm. In some embodiments, including any of the above embodiments, the SRP of the CC comprises circular pores with a diameter of 50 μm; the functional porosity is 90%; and wherein the CC is 100 μm thick (MBB thickness).

[0289] In some embodiments, including any of the above embodiments, the pores have rectangular or polygonal openings. In some embodiments, the opening size of the pores is about 40 μm x 50 μm. In some embodiments, the opening size of the pores is about 52 μm x 52 μm. In some embodiments, including any of the above embodiments, the CC comprises square pores of 50 μm x 50 μm; the functional porosity is 90%; and wherein the CC is 100 μm thick.

[0290] According to an aspect of some embodiments of the present invention, there is provided a current collector suitable for an electrode (e.g. a battery), comprising at least one reinforced metal foil as proposed herein, wherein the reinforced metal foil is produced by a continuous manufacturing process such that it can be produced with a width of at least 0.1 m and an unlimited length of at least 0.5 m, and is characterized by at least some of the following features:

[0291] seamless repeating pattern of non-perforated structural elements;

[0292] seamless repeating pattern of through-hole structural elements;

[0293] Local thickness in the range of 4-100 μm; and

[0294] Functional porosity of at least 10%.

[0295] Wrinkled current collector:

[0296] According to an aspect of some embodiments of the present invention, there is provided a current collector suitable for an electrode (e.g. a battery), comprising at least one reinforced metal foil as proposed herein, wherein the reinforced metal foil is produced by a continuous corrugation process such that it can be produced with a width of at least 0.1 m and an unlimited length of at least 0.5 m, and characterized in that:

[0297] seamless repeating pattern of non-perforated structural elements (corrugated SRP);

[0298] Local thickness in the range of 4-100 μm; and

[0299] Functional porosity of at least 10%.

[0300] In some embodiments, the current collector comprises or consists of a reinforced metal foil (member) produced by any continuous manufacturing technique known in the art and including a continuous corrugation process step (which imparts corrugation reinforcement to the member), these terms and characteristics being described above.

[0301] Unless otherwise specified, the member is corrugated but not perforated, i.e., it is not a mesh. In such embodiments, the corrugated SRP may include individual non-perforated structural elements and / or expanded non-perforated structural elements as defined above, such that the functional porosity of the corrugated member exceeds 10% as described herein.

[0302] In some embodiments, the size (diameter, widest span at bottom) of individual non-perforated structural elements in the SRP of the corrugated member is in the range of 10 μm to 5,000 μm or 10-500 μm. In some embodiments, the horizontal distance between non-perforated structural elements in the SRP of the corrugated member is in the range of 100-5000 μm or 100-500 μm.

[0303] In some embodiments, the horizontal distance between two adjacent non-perforated structural elements in the corrugated reinforcement is in the range of 1-2000 μm or about 10-100 μm.

[0304] In such embodiments, the height of the corrugated structural elements characterizing the component can be expressed as a ratio between local thickness and MBB thickness, where the MBB of the non-corrugated foil is equal to the local thickness of its initial thickness before corrugation. In such embodiments, the ratio of the MBB thickness to the local thickness (thickness of the original foil) is at least 1.1:1-2:1. In some embodiments, the ratio of the MBB thickness to the local thickness is at least 3:1, 4:1, 5:1, 10:1 or at least 20:1. For example, an original foil having a local thickness of 10 μm can be enhanced by corrugation to present an MBB thickness of 200 μm.

[0305] In some embodiments, the MBB having corrugated reinforcement has a thickness in the range of 6 μm to 5,000 μm.

[0306] In some embodiments, including any of the above embodiments, the reinforced metal foil produced by the continuous corrugation process is provided in the form of a roll of the foil, wherein the width of the foil or the width of the roll is at least 0.1m, at least 0.5m, at least 1m, at least 2m, at least 3m, at least 4m, or at least 5m wide and the length is at least 0.5m, 1m, 10m, 100m, 200m, 300m, or 400m long.

[0307] Perforated Current Collector:

[0308] In some embodiments, the current collector comprises or consists of a reinforced metal foil characterized by perforation reinforcement, the metal foil being produced by a continuous electroforming process. In some embodiments, the CC produced by a continuous electroforming process comprises or consists of copper. In some embodiments, the reinforced metal foil produced by a continuous electroforming process is perforated by electroforming it on the curved surface of a conductive cylinder, the conductive cylinder having an SRP of a non-conductive material engraved or provided in its surface. In some embodiments, the reinforced metal foil produced by a continuous electroforming process exhibits the SRP of the perforated structural elements proposed herein, and is optionally corrugated to exhibit the SRP of the corrugated structural elements proposed herein.

[0309] In some embodiments, the current collector produced by the continuous electro-etching process comprises aluminum or consists of aluminum. In some embodiments, the current collector produced by the continuous electro-etching process comprises copper or consists of copper. In some embodiments, the reinforced metal foil produced by the continuous electro-etching process is perforated by electro-etching it using a mask having an SRP. In some embodiments, the reinforced metal foil produced by the continuous electro-etching process is further corrugated to exhibit the SRP of the corrugated structural element proposed herein.

[0310] In some embodiments, the perforated member forming part of or constituting the current collector is also corrugated.

[0311] In some embodiments, including any of the above embodiments, the reinforced metal foil produced by a continuous electro-etching or continuous electro-forming process as described above and exhibiting perforation reinforcement only or perforation and corrugation reinforcement is provided in the form of a roll of an object, wherein the width of the object or the width of the roll is at least 0.1m, at least 0.5m, at least 1m, at least 2m, at least 3m, at least 4m or at least 5m wide and the length is at least 0.5m, at least 1m, at least 10m, at least 100m, at least 1000m or at least 10,000m long.

[0312] electrode:

[0313] As discussed above, the advantages obtained by the enhanced metal foil provided herein include reducing the mass of the electrode, increasing the amount of active material that can be loaded per unit area, increasing the contact surface area with the active material, improving the electrical pathway within the active material, and all of this while maintaining low production costs and compatibility with large-scale production machinery and processes, compared to the original solid (non-porous) and flat (planar, smooth) metal foils currently used.

[0314] The components and CCs provided herein help to significantly reduce the local current density by expanding the surface area of ​​the CC. Since reducing the current density at the electrode can delay the onset of dendritic growth and slow down the growth rate, the CCs provided herein effectively mitigate dendritic growth. In addition, since the CC acts as a matrix for the Li metal, the CCs provided herein block the randomly generated Li metal-electrolyte interface and the internal pressure changes caused by the volume change of the Li metal during the cycle.

[0315] Compared to other 3D porous metal sheets that have been proposed and demonstrated in the art, the present invention provides a solution to the extremely high costs, long manufacturing times and, most importantly, the very limited production capacity of all other 3D porous structures, which cannot be mass-produced into rolls of tens and hundreds of meters in length, which are required for contemporary electrode coating production in large-scale production plant facilities. The components provided herein and the current collectors comprising or consisting of the same can be implemented in electrode production in the form of a continuous roll of feed foil that is fed into an active material coating device and cut into individual electrodes at a later time.

[0316] Thus, according to some embodiments of the present invention, there is provided an electrode, for example in the context of a battery or capacitor, comprising at least one current collector and an active electrode material (also referred to as a coating material) constructed on the CC, wherein the current collector comprises or consists of at least one reinforced metal foil (member) provided herein. Unless otherwise expressly stated, throughout the present invention, the term "electrode" refers to both anodes and cathodes.

[0317] Electrode coating is an important part of the battery manufacturing process, contributing greatly to the final microstructure and therefore related to the functionality of the resulting electrode. According to embodiments of the present invention, the coating of the reinforced metal foil provided herein can be carried out by various routes, and the coater device can be a pull-down coater commonly used in research laboratories to produce small coatings, or for larger industrial applications, a roll-to-roll (i.e., R2R or reel-to-reel) coater, and the components disclosed herein are most suitable for such coaters. In a roll-to-roll setting, the geometry of the coater used to coat the components according to some embodiments of the present invention can be a doctor blade (a fine blade set at a fixed gap from the CC), a comma rod (a comma-shaped geometry with a curved leading edge), a slot die (the coating material is extruded from the slot onto the CC), a "knife-to-roll" (the coating material is distributed onto the CC and then passed through a knife and a roller), a "reverse roller", a "Meyer rod" (where the roller applies the coating material to the CC, and then the Meyer rod meters the correct amount), and these methods and devices are known in the art. The coating can be applied while the CC is supported by a roller. Alternatively it can also be applied to an unsupported CC under tension, which is known as tension web coating.Other electrode coating methods known in the art can be used to coat the current collectors described herein.

[0318] The coating material is introduced directly onto the CC without causing additional morphological deformation of the CC, and can be introduced onto one or both sides of the member according to the design requirements of the battery. For example, the wrinkled member provided herein has been used in an industrial electrode coater to successfully produce electrodes for LiBs, demonstrating the feasibility of large-scale production and applicability to practical industry. This simple manufacturing process can also be associated with its cost-effective characteristics.

[0319] Thus, according to some embodiments of the present invention, the electrode is produced by any known R2R process using a roll of the reinforced metal foil provided herein.

[0320] In some embodiments, the thickness of the electrode including the coating material is greater than the total thickness of the current collector (MBB thickness) due to the added layer of coating material constructed on the current collector. In some embodiments, the thickness of the electrode including the coating material is similar to the total thickness of the current collector including the added layer of coating material constructed on the current collector (MBB thickness).

[0321] Fig. 7A -C shows a schematic diagram of a coating scheme for a reinforced metal foil according to some embodiments of the present invention, wherein the top cross-sectional view ( Fig. 7A ) shows an electrode exhibiting the same thickness as the total thickness of the corrugated foil member (MBB thickness), similar to the middle figure ( Figure 7B ), and the bottom graph ( Figure 7C ) shows an electrode that exhibits a greater thickness compared to the total thickness of the corrugated member (MBB thickness).

[0322] In some non-limiting embodiments where the thickness of the electrode is similar to that of the current collector, the CC has a thickness of 9-12 μm or up to 100 μm. In some non-limiting embodiments where the thickness of the electrode is thicker than that of the current collector, the current collector has 50 μm pores on its surface and a porosity greater than 90%, provided by corrugation and / or perforation.

[0323] As discussed herein, a current collector can include more than one metal layer, wherein at least one or all of the layers are a reinforced metal foil as provided herein.

[0324] Coating Material:

[0325] Since the reinforced metal foils provided herein are designed to be suitable for contemporary industrial electrode production, all known and commonly used processes, methods and techniques for producing active coating materials and applying them to current collectors are applicable hereto.

[0326] In some embodiments, the process includes coating a current collector with a wet or fluid active material composition in the form of a slurry, paste, liquid, etc. In some embodiments, the coating is provided by a dry (solvent-free) coating, wherein the active material is deposited on the current collector, using little or no solvent to carry the active material.

[0327] Electrode comprising a wrinkled current collector:

[0328] According to some embodiments of the present invention, there is provided an electrode comprising at least one current collector and an active electrode material constructed on the CC, wherein the current collector comprises or consists of at least one reinforcing metal foil (member) in the form of a corrugated metal foil as proposed above. In some embodiments, the member has no perforations.

[0329] Electrode comprising a perforated and optionally wrinkled current collector:

[0330] According to some embodiments of the present invention, there is provided an electrode comprising at least one current collector and an active electrode material constructed on the CC, wherein the current collector comprises at least one reinforcing metal foil (member) in the form of a perforated metal foil as proposed above, or consists of it. In some embodiments, the perforated member is also corrugated as described above.

[0331] Batteries and Power Equipment:

[0332] In view of the above, a battery or battery pack is provided, which comprises at least one electrode, wherein the electrode comprises at least one reinforced metal foil provided herein, or wherein the electrode comprises a current collector, and the current collector comprises at least one reinforced metal foil provided herein (member; object), or consists of it. It should be noted here that although a battery is a single unit of a device that converts chemical energy into electrical energy, and a battery pack is a collection of batteries that convert chemical energy into electrical energy, the terms "battery" and "battery pack" are used interchangeably herein.

[0333] Accordingly, an electric power device is provided, which includes the battery, battery array, battery pack or battery pack array provided herein.

[0334] In some embodiments, the cell or battery comprises at least one electrode comprising at least one current collector, wherein the CC is a corrugated metal foil or a corrugated reinforced metal foil as described herein.

[0335] In some embodiments, the cell or battery comprises at least one electrode comprising at least one current collector, wherein the CC is a perforated reinforced metal foil or a perforated reinforced metal foil described herein.

[0336] In some embodiments, the cell or battery comprises at least one electrode comprising at least one current collector, wherein the CC is a perforated and corrugated metal foil or a metal foil reinforced by both perforation and corrugation as described herein.

[0337] The power devices contemplated within the scope of the present invention include any power device that can use a battery or battery pack as a primary, auxiliary or secondary energy source. Alternatively, the power device is a power device that includes at least one battery pack, wherein the device uses the power stored in the battery pack as its power source.

[0338] Examples of electric devices include, but are not limited to, electric vehicles for transportation in air, land, water, and / or space, smart phones, laptop computers, portable media players, power tools, toys, heating devices, cooling devices, lighting products (e.g., flashlights), etc.

[0339] In some embodiments, the power device is a device that requires a high power density battery pack, such as a vehicle (e.g., an electric car). In terms of a battery pack, power density refers to the amount of electricity that can be stored or delivered by a battery pack per unit volume or unit mass. High power density means that a battery pack can store or deliver a relatively large amount of electricity in a relatively small space or weight. This is one of the features of a battery pack using an enhanced metal foil provided herein, which is designed for portable electronic devices and electric vehicles, where size and weight are key factors. High power density batteries can also have a higher energy density, which means that they can store more energy per unit weight or volume.

[0340] It is anticipated that many related enhanced metal foils will be developed during the life of the patent expiring on this application, and the scope of the phrase "enhanced metal foil" is intended a priori to include all such new technologies.

[0341] It should be understood that certain features of the invention described in the context of separate embodiments for the sake of clarity may also be provided in combination in a single embodiment. Conversely, various features of the invention described in the context of a single embodiment for the sake of brevity may also be provided separately or in any suitable sub-combination, or in any other described embodiment of the invention where appropriate. Certain features described in the context of various embodiments should not be considered essential features of those embodiments unless the embodiments do not work without those elements.

[0342] Various embodiments and aspects of the present invention as delineated hereinabove and as claimed in the claims section below find experimental support in the following examples.

[0343] Example

[0344] Reference is now made to the following examples, which together with the above descriptions illustrate some embodiments of the invention in a non-limiting fashion.

[0345] Example 1

[0346] Wrinkle Enhancement

[0347] Copper and aluminum foils with local thicknesses of 12 μm and 60 μm, respectively, and at least 125 m in length were subjected to a roll-to-roll corrugation enhancement process as described herein. The SRP of the non-perforated structural elements consisted of circular depressions spaced about 500 μm apart horizontally and arranged in a hexagonal array, resulting in a total corrugated thickness (MBB thickness) of 60 μm in copper and 190 μm in aluminum.

[0348] Fig. 8A-B shows a micrograph taken using a Nikon eclipse LV100ND optical microscope, capturing a 12 μm thick copper foil ( Fig. 8A ) and 60 μm thick aluminum foil ( Figure 8B ), each foil having undergone corrugation reinforcement in the form of hexagonally arranged circular depressions spaced approximately 500 μm apart horizontally from each other.

[0349] Example 2

[0350] Effect of perforation and wrinkling on functional porosity

[0351] To demonstrate the effect of perforation and corrugation of the original metal foil, the same aluminum foil used in Example 1 was perforated by electro-etching and corrugated as described in Example 1. The perforation was performed in the form of a hexagonal array of circular through holes, each through hole being located at the center between four adjacent depressions, thereby constituting a SRP of circular through holes.

[0352] Fig. 9 Shown are photographs taken using a Leica DVM6 optical microscope of a 60 μm thick aluminum foil which has undergone perforation and wrinkling enhancements, respectively, in the form of hexagonally arranged circular holes and depressions spaced approximately 500 μm horizontally from each other.

[0353] The resulting total (MBB) thickness of the reinforced metal foil was increased from 60 μm to 100 μm, resulting in a functional porosity greater than or equal to 90%, calculated according to the bounding box.

[0354] Example 3

[0355] Active material coating

[0356] To demonstrate the ability of the enhanced metal foils provided herein to load electrode active materials, the corrugated aluminum foil presented in Example 1 above was used as a current collector and coated with a cathode active material slurry comprising 95 wt.% NMC811 (LiNi 2O3) suspended in NMP (N-methyl-2-pyrrolidone slurry carrier). 0.8 Mn 0.1 Co 0.1 O2), 3wt.% polyvinylidene fluoride (PVDF), C65 (nano carbon black conductive additive; 2wt.%).

[0357] According to some embodiments of the present invention, the slurry is applied to an aluminum current collector member using a draw-down coater and dried to form an exemplary cathode. Thereafter, aluminum is chemically etched from the cathode to obtain a Fig.10 The morphology of the dry active material residual layer is shown in FIG.

[0358] Fig.10 A photograph taken using a Leica DVM6 optical microscope is shown of a dried layer of a slurry applied to a corrugated aluminum foil or component after aluminum removal by acid etching according to some embodiments of the present invention, showing five protruding protrusions and four depressions pointing to opposite sides.

[0359] Similar experiments were performed with different slurries containing LiFePO4, where the slurries were coated on similar corrugated aluminum foil and dried.

[0360] Fig.11 A photograph taken using a Leica DVM6 optical microscope is shown of a dried layer of a slurry applied to a perforated member made of aluminum after the aluminum was removed by acid etching according to some embodiments of the present invention, showing several circular protrusions made of active material formed in the voids where the pores in the member would normally be located.

[0361] As can be seen in Fig.11 As seen in the SRP, a columnar structure is formed due to the holes of the perforated aluminum components.

[0362] Example 4

[0363] Lithium-ion battery with wrinkled current collector

[0364] According to some embodiments of the present invention, multilayer lithium ion pouch cells with a capacity ranging from 1-1.5 Ah are prepared using corrugated copper foil and aluminum foil as current collectors, wherein according to some embodiments of the present invention, the anode is prepared using corrugated copper foil and the cathode is prepared using corrugated aluminum foil.

[0365] The battery includes a graphite anode and a nickel manganese cobalt (NMC622) cathode known in the art, the cathode active material composition is 94wt.% NMC622, 2wt.% PVDF, 2wt.% C65 (carbon black conductive additive), the slurry carrier is N-methylpyrrolidone (NMP), and a standard electrolyte of 1M LiPF6, EC / DEC 1: 1 is used. The active material is coated on the current collector using a standard roll-to-roll machine, and the battery is assembled using standard battery assembly practices.

[0366] The copper current collector for the anode has a local thickness of 12 μm, an MBB thickness of 43.5 μm, and a hexagonal array of circular depressions separated by a horizontal distance of 500 μm. The aluminum current collector for the cathode has a local thickness of 20 μm, an MBB thickness of 63.2 μm, and a hexagonal array of circular depressions separated by a horizontal distance of 500 μm.

[0367] Cathode active area 6 x 10 cm 2Prior to the cycle test, the pouch cells were first subjected to a forming step at a C rate of C / 20. After forming, the cells were subjected to 1C charge-discharge cycles at room temperature (with regular capacity checks at C / 3).

[0368] The result of the cycle is as follows Fig. 12A As shown in , where the capacity retention of the battery is plotted against the number of cycles, with the initial capacity of 1.1 Ah being 100%. The battery can be cycled at a high rate of 1C for more than 450 cycles with 85% of the initial capacity remaining.

[0369] To compare the direct current internal resistance (DCIR) of the pouch cell with wrinkled current collectors relative to the pouch cell with conventional electrodes, as shown in the previous example, the GITT method was used. The internal resistance of the cell was measured at three different SOCs during cell discharge. Fig. 12B A comparison of DCIR as a function of SOC between the two configurations is shown.

[0370] Fig. 12A -B shows battery cycling results obtained for a lithium-ion battery comprising a wrinkled current collector according to some embodiments of the present invention, wherein Fig. 12A The measured values ​​of the retained capacity (capacity scale is a percentage of the initial capacity) of the cells using the corrugated CC configuration provided herein are shown, and Fig. 12B The internal resistance measurements of the cells at various states of charge are shown, and the results are compared with those obtained for similar cells containing conventional (flat, non-porous) current collectors.

[0371] Reducing the internal resistance of a battery pack cell has a significant impact on overall battery performance because it allows faster charging and discharging, and charging and discharging with less loss in overall capacity retention. Fig. 12A The performance of cells constructed according to some embodiments of the present invention outperforms that of cells using conventional foils for the CC, as seen in Figure 1-B. As can be seen, the cells with the wrinkled CC in the electrode exhibit lower DCIR (more than two times) than the cells with the conventional electrode.

[0372] Example 5

[0373] Perforation Enhancement

[0374] Fig.13A -B shows a 0.53 cm section of a perforated and flat (non-corrugated) reinforced foil made using one of the continuous manufacturing processes described herein. 2 Optical scanning of the sample, where Fig.13Ashows an aluminum object with a local thickness of 20 μm and an SRP consisting of circular via primitives with an average radius of 55.1 μm and a standard deviation of 2.4 μm (the uniformity of the SRP is 4.4% SD), Fig. 13B A copper object with a local thickness of 22 μm and a SRP consisting of circular via primitives with a mean radius of 58.9 μm and a standard deviation of 1.4 μm (SRP uniformity 2.4% SD) is shown. In the copper object, the number of holes found in the sample area is 930, accounting for 35% of the total sample area.

[0375] The perforated copper metal member exhibited a tensile strength of approximately 50 MPa, and the perforated aluminum metal member exhibited a tensile strength of approximately 45 MPa.

[0376] The objects were dimensionally analyzed using an Epson Perfection V850 Pro scanner and Image Expert software to calculate key metrics related to SRP.

[0377] Table 1 represents the data collected to measure the uniformity of the SRP, where Area Average refers to the average of the sample area, Radius Average refers to the average of the pore radius, and Roundness refers to the average measurement of the pore roundness.

[0378] Table 1

[0379]

[0380] Example 6

[0381] Lithium-ion batteries with porous and wrinkled current collectors

[0382] A single-layer pouch cell with an anode and cathode produced according to some embodiments of the present invention was prepared. The local thickness of the copper CC for the anode was 18 μm, the MBB thickness was 100 μm, and the SRP element was a square through hole with a size of 50 μm (see Fig.17A The local thickness of the aluminum CC used for the cathode is 100 μm, the MBB thickness is 200 μm, and the SRP element is a circular through hole with a radius of 90 μm (see Fig. 17B ).

[0383] Fig.14A -B shows a SEM micrograph of a wrinkled and perforated object, showing a top view of a copper current collector coated with active material on one side (for demonstration purposes) ( Fig.14A ) and the cross section of the aluminum current collector ( Fig. 14B ).

[0384] The battery includes a graphite anode and a LiFePO4 (LFP) cathode, the cathode active material composition is 90wt.% LFP, 5wt.% PVDF, 5wt.% C45 (carbon black conductive additive), and the slurry carrier is N-methylpyrrolidone (NMP). The cathode active area is 4x 4cm 2 The pouch cell formation step includes the first charge-discharge cycle. A standard electrolyte of 1M LiPF6, EC / DEC 1:1 is used.

[0385] Prior to the cycling test, the pouch cells were first subjected to a forming step at a C rate of C / 30. After forming, the cells were subjected to more than 50 charge and discharge cycles at C / 3 (with regular capacity checks at C / 10) at room temperature. The results of the cycles are presented in Fig.15 middle.

[0386] Fig.15 A graph of capacity retention versus cycle number measured in lithium-ion cells produced using a perforated and corrugated CC according to some embodiments of the present invention is shown, with the initial capacity of 35 mAh being 100%.

[0387] To compare the direct current internal resistance (DCIR) of pouch cells using perforated and wrinkled CCs with those built using conventional (pristine foil) current collectors, a galvanostatic intermittent titration technique (GITT) was employed.

[0388] GITT is a common procedure for measuring the internal resistance of a battery using current pulses. In short, GITT involves gradually discharging (or charging) a battery at a known state of charge (SOC) and running a current pulse to estimate the battery resistance based on the difference between the initial voltage (before the pulse) and the voltage measured at the end of the pulse on the applied current.

[0389] During battery discharge, the internal resistance of the battery is measured at four different SOCs, and the average of these measurements is taken as the battery DC internal resistance. The results are presented in Fig.16 middle.

[0390] Fig.16 is a comparative graph showing the variation of DCIR with cycle life between two constructions, one for a cell built with a conventional (pristine foil) CC and the other for a cell built with the enhanced metal foils provided herein.

[0391] As can be seen in Fig.16 As seen in Figure 5, the cells with perforated and wrinkled CCs in the electrodes maintain lower DCIR (by more than four times) at all cycles compared to the performance of conventional CCs.

[0392] In addition to showing reduced internal resistance compared to cells with conventional foils, cells with perforated and corrugated CCs also exhibited enhanced capacity retention during battery cycling. As summarized in Table 2, the degradation rate (capacity loss during cycling) of cells with perforated and corrugated current collectors was significantly lower than that of cells with conventional current collectors, as indicated by the higher capacity retention.

[0393] Table 2

[0394]

[0395] As can be seen in Table 2, the batteries constructed using CCs designed and obtained according to some embodiments of the present invention exhibit higher capacity retention than batteries constructed using pristine foil CCs. Having higher capacity retention after battery cycling indicates improved overall cycle life by reducing degradation rates. This improvement can lead to longer battery life and better performance.

[0396] Example 7

[0397] Exemplary Structural Elements and Corresponding SRPs

[0398] Table 3 shows the combinations of various SRP parameters for perforation enhancement.

[0399] Table 3

[0400]

[0401] Table 4 shows the combination of various SRP parameters for wrinkling enhancement.

[0402] Table 4

[0403] Metal Local thickness MBB thickness Horizontal distance copper 8μm 4-30μm 320-1000μm copper 10-12μm 20-60μm 300-200μm copper 20μm 20-120μm 200-100μm copper 50μm 90-120μm 100-50μm aluminum 20μm 30-60μm 320-1000μm aluminum 30μm 30-90μm 320-1000μm aluminum 60μm 90-180μm 500-1000μm aluminum 125μm 130-500μm 500-2000μm

[0404] Example 8

[0405] Reinforced metal foil rolls

[0406] Fig.17A -B shows a photograph of a reinforced metal foil (metal member) according to some embodiments of the present invention, the foil comprising aluminum and exhibiting corrugation reinforcement, wherein the local thickness is about 20 μm, the vertical distance (height) of the circular protrusions (non-perforated structural elements) (which is also the MBB thickness) is about 72 μm, and the horizontal distance between the structural elements is about 500 μm, wherein Fig.17A The entire roll and close-up insert of the reinforced metal foil are shown in Fig. 17B is a microscopic image showing a corrugated structural element.

[0407] Fig.18A-C shows a photograph of a reinforced copper foil according to some embodiments of the present invention, which exhibits wrinkling reinforcement, wherein the local thickness is about 12 μm, the MBB thickness is about 100 μm, and the horizontal distance between structural elements is about 500 μm, wherein Fig.18A The entire roll of reinforced metal foil is shown in Fig.18B A close-up inset is shown in Fig. 18C is a microscopic image showing a corrugated structural element.

[0408] Although the present invention has been described in conjunction with its specific embodiments, it is apparent that many alternatives, modifications and variations will be apparent to those skilled in the art. Therefore, the present invention is intended to cover all such alternatives, modifications and variations that fall within the spirit and broad scope of the appended claims.

[0409] All publications, patents and patent applications mentioned in this specification are incorporated herein by reference in their entirety, to the same extent as if each individual publication, patent or patent application was specifically and individually indicated to be incorporated herein by reference. In addition, the citation or identification of any reference in this application should not be construed as an admission that the reference can serve as prior art to the present invention. Where section headings are used, they should not be construed as necessarily limiting.

[0410] Furthermore, any priority documents of this application are incorporated herein by reference in their entirety.

Claims

1. An object comprising a metal component characterized by a seamless repeating pattern of through-hole structural elements and at least one of the following: (a) Seamless repeating pattern of non-perforated structural elements; (b) a local thickness in the range of 3-100 μm; and (c) a functional porosity (Pf) of at least 10%. The metal component has a width of at least 0.1 m and a length of at least 0.5 m.

2. The object of claim 1, wherein the metal component is characterized by (a).

3. The object of claim 1, wherein the metal component is characterized by (b).

4. The object of claim 1, wherein the metal component is characterized by (c).

5. The object of claim 1, wherein the metal component is characterized by (a) and (b).

6. The object of claim 1, wherein the metal component is characterized by (a) and (c).

7. The object of claim 1, wherein the metal component is characterized by (b) and (c).

8. The object of claim 1, wherein the metal component is characterized by (a), (b), and (c).

9. The object of any of the preceding claims, wherein the metal component comprises a metal selected from the group consisting of aluminum, copper, nickel, gold, cobalt, iron, titanium, steel, stainless steel, and any alloys and combinations thereof.

10. The object according to any of the preceding claims, wherein the local thickness is in the range of 3-20 μm.

11. An object according to any one of the preceding claims, wherein the functional porosity is at least 50%.

12. An object according to any one of the preceding claims, wherein the through-hole structural elements in the seamless repeating pattern have an opening size in the range of 10-200 μm.

13. An object according to any one of the preceding claims, wherein the seamless repeating pattern has 30-200 holes / mm 2 range of pore density.

14. An object according to any one of the preceding claims, wherein the seamless repeating pattern is characterized by a uniformity of at least 5%.

15. An object according to any one of the preceding claims, characterised in that Tensile strength of at least 20-45MPa.

16. An object according to any one of the preceding claims, wherein: The metal member comprises copper, The seamlessly repeating pattern of the through-hole structural element comprises primitives of circular holes with a diameter less than 100 μm and a horizontal distance less than 500 μm, The seamless repeating pattern of the non-perforated structural elements comprises primitives of circular depressions and / or circular protrusions each having a diameter of less than 500 μm and a horizontal distance of less than 1000 μm, The local thickness is less than 50 μm, The functional porosity (P f ) is at least 50%, The width of the metal member is at least 0.1-5 m, and The length of the metal member is at least 50 m.

17. An object according to any one of the preceding claims, wherein: The metal member comprises aluminum, The seamlessly repeating pattern of the through-hole structural element comprises primitives of circular holes with a diameter less than 120 μm and a horizontal distance less than 1000 μm, The seamless repeating pattern of the non-perforated structural elements comprises primitives of circular depressions and circular protrusions each having a diameter of less than 500 μm and a horizontal distance of less than 1000 μm, The local thickness is less than 100 μm, The functional porosity (P f ) is at least 50%, The width of the metal member is at least 0.1-5 m, and The length of the metal member is at least 50 m.

18. A roll comprising a cylindrical core and an object according to any one of the preceding claims wound around the core.

19. The roll according to claim 18, wherein the width of the objects is in the range of at least 0.1-5 m.

20. The roll of claim 18, wherein the length of the objects in the roll is in the range of at least 0.5-10,000 m.

21. A current collector comprising at least one object according to any one of claims 1 to 17.

22. An electrode comprising the current collector according to claim 21.

23. A battery comprising at least one electrode according to claim 22.

24. An electric device comprising at least one battery according to claim 23.

25. The electric device of claim 24, selected from an electric vehicle for transportation in air, land, water and / or space, a smartphone, a laptop computer, a media player, a power tool, a toy, a heating device, a cooling device and a lighting device.