Low-color-difference zirconia false tooth and preparation process thereof
By adding a specific proportion of colorants and antibacterial agents to the zirconia dentures, combined with isostatic molding and high-temperature sintering processes, the problems of large color difference between zirconia dentures and teeth and insufficient antibacterial performance are solved, and color matching and antibacterial effect are improved. , improves the aesthetics and oral health of dentures.
Patent Information
- Application Number
- CN202411142793.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-20
- Publication Date
- 2024-11-15
AI Technical Summary
The existing zirconia dentures have a large color difference between teeth, which affects aesthetics and confidence, and lacks antibacterial properties.
Using the preparation process of low-color difference zirconia dentures, chlorine is added by mixing zirconia, ceramic powder, alumina, yttrium oxide, cellulose powder, colorant and auxiliary agent in a specific proportion, isostatic molding and high-temperature sintering, and adding chlorine Colorants such as iron, praseodymium chloride, erbium chloride, manganese chloride, neodymium chloride, and antibacterial agents such as honeysuckle extract and green tea extract to regulate color and antibacterial properties.
Reduce the chromatic difference between dentures and teeth, improve beauty and confidence, while improving the antibacterial effect of dentures and enhancing oral health.
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of dentures, and in particular to a low-color-difference zirconia denture and a preparation process thereof. Background Art
[0002] Since the surface of teeth is covered with a layer of enamel, which is transparent or translucent, and the deeper part is dentin, the teeth are light yellow. When a denture is needed due to disease or loss of teeth, the color of zirconia dentures is very white due to the problem of raw materials. When installed in the mouth, the denture will appear particularly protruding compared with other teeth in the mouth, giving people a fake feeling, which not only affects the appearance, but also causes embarrassment and is not conducive to improving people's self-confidence. Therefore, a low-color-difference zirconia denture and its preparation process are needed to meet the demand. Summary of the invention
[0003] The purpose of the present invention is to solve the disadvantage of large color difference between zirconia dentures and teeth in the prior art, and to propose a low-color difference zirconia denture and a preparation process thereof.
[0004] In order to achieve the above object, the present invention adopts the following technical solutions: A low-color-difference zirconia denture is designed, and the raw materials thereof are formulated as follows in parts by weight: 65-85 parts of zirconium oxide, 30-50 parts of ceramic powder, 20-30 parts of aluminum oxide, 10-15 parts of yttrium oxide, 8-12 parts of cellulose powder, 0.5-1 parts of colorant, and 0.3-0.7 parts of auxiliary agent.
[0005] Preferably, the colorant includes ferric chloride, praseodymium chloride, erbium chloride, manganese chloride and neodymium chloride.
[0006] Preferably, the mass ratio of ferric chloride, praseodymium chloride, erbium chloride, manganese chloride and neodymium chloride is 3:1:3:1:1.
[0007] Preferably, the auxiliary agent is a dispersant, a light stabilizer, a photoinitiator, a toughening agent, a bonding agent, a defoaming agent, a silane coupling agent and an antibacterial agent.
[0008] Preferably, the mass ratio of the dispersant, light stabilizer, photoinitiator, toughening agent, bonding agent, defoaming agent, silane coupling agent and antibacterial agent is 1:1:1:2:3:1:1:5.
[0009] Preferably, the antibacterial agent is honeysuckle extract and green tea extract, and the mass ratio of the honeysuckle extract to the green tea extract is 1:1.
[0010] The present invention also provides a preparation process of a low-color-difference zirconia denture, comprising the following steps: S1. Mixing zirconium oxide, ceramic powder, aluminum oxide, yttrium oxide, cellulose powder, colorant and auxiliary agent together with a mixer to prepare a mixture A; S2, preparing an embryo mold, and injecting the mixture A in step S1 into the embryo mold; S3, placing the embryo mold in an isostatic press for isostatic pressing to obtain a denture tooth blank; S4, pre-sintering the denture tooth blank first, and then sintering at high temperature; S5. Grind and polish the denture after high-temperature sintering.
[0011] Preferably, in step S4, the denture tooth blank is preheated in a sintering furnace at 280-320 degrees for 30-40 minutes, then the temperature of the sintering furnace is increased to 1200-1450 degrees for sintering for 10-30 hours, and finally kept at 900-1000 degrees for 5-10 hours.
[0012] Preferably, after the insulation is completed, the sintering furnace is closed and the furnace body is allowed to cool naturally to room temperature.
[0013] The low-color-difference zirconia denture and its preparation process proposed in the present invention have the beneficial effects of improving the color of the zirconia denture by adding a colorant, making the zirconia denture closer to the color of the teeth after processing, which not only makes the denture better hidden and improves the appearance, but also enhances people's self-confidence. In addition, the addition of honeysuckle extract and green tea extract in the auxiliary agent enhances the antibacterial effect of the zirconia denture, making it healthier for people's oral cavity. DETAILED DESCRIPTION
[0014] The present invention is further described below in conjunction with specific embodiments. Obviously, the described embodiments are only a part of the embodiments of the present invention, rather than all the embodiments.
[0015] Example 1: A low-color-difference zirconia denture, the raw materials of which are formulated in parts by weight as follows: 65 parts of zirconium oxide, 30 parts of ceramic powder, 20 parts of aluminum oxide, 10 parts of yttrium oxide, 8 parts of cellulose powder, 0.5 parts of colorant, and 0.3 parts of auxiliary agent.
[0016] Colorants include ferric chloride, praseodymium chloride, erbium chloride, manganese chloride and neodymium chloride. The mass ratio of ferric chloride, praseodymium chloride, erbium chloride, manganese chloride and neodymium chloride is 3:1:3:1:1. Colorants are used to improve the color of zirconia dentures and make them closer to the color of teeth after processing. This not only makes the dentures better hidden and improves their appearance, but also increases people's confidence.
[0017] The auxiliary agents are dispersant, light stabilizer, photoinitiator, toughening agent, binding agent, defoaming agent, silane coupling agent and antibacterial agent. The mass ratio of dispersant, light stabilizer, photoinitiator, toughening agent, binding agent, defoaming agent, silane coupling agent and antibacterial agent is 1:1:1:2:3:1:1:5.
[0018] The antibacterial agents are honeysuckle extract and green tea extract, and the mass ratio of the honeysuckle extract and the green tea extract is 1:1. By adding the honeysuckle extract and the green tea extract, the antibacterial effect of the zirconia denture is enhanced, which is healthier for people's oral cavity.
[0019] The present invention also provides a preparation process of a low-color-difference zirconia denture, comprising the following steps: S1. Mix zirconium oxide, ceramic powder, aluminum oxide, yttrium oxide, cellulose powder, colorant and auxiliary agent together with a mixer to prepare a mixture A. The mixer uses a V-type mixer. The V-type mixer is easy to operate and has a good mixing effect when mixing zirconium oxide, ceramic powder, aluminum oxide, yttrium oxide, cellulose powder, colorant and auxiliary agent. S2, preparing an embryo mold, and injecting the mixture A in step S1 into the embryo mold; S3, placing the embryo mold in an isostatic press for isostatic pressing to obtain a denture blank; the denture blank processed by the isostatic press has a high density and is more uniform. At this time, the size of the denture blank is larger than the size of the denture to be manufactured, providing shrinkage space for subsequent sintering; S4, pre-sintering the denture blank first, and then sintering at high temperature; the denture blank is preheated in a sintering furnace at 280 degrees for 30 minutes. During the preheating, the volatiles in the denture blank can be removed. Then the temperature of the sintering furnace is increased to 1200 degrees for sintering for 10 hours. The high-temperature sintering takes a long time, which can allow the denture blank to undergo a chemical reaction and form a hard structure. Finally, it is kept warm at 900 degrees for 5 hours. The heat preservation after sintering can ensure the stability of the material of the denture after sintering, which not only ensures the hardness of the denture, but also ensures the coloring effect of the denture. When in use, the color difference between the denture and the teeth is reduced. After the heat preservation is completed, the sintering furnace is closed and the furnace body is allowed to cool naturally to room temperature. In this process, the denture gradually solidifies and becomes hard; S5. Grind and polish the denture after high-temperature sintering.
[0020] Example 2: A low-color-difference zirconia denture, the raw materials of which are formulated as follows in parts by weight: 78 parts of zirconium oxide, 38 parts of ceramic powder, 24 parts of aluminum oxide, 12 parts of yttrium oxide, 9 parts of cellulose powder, 0.6 parts of colorant, and 0.4 parts of auxiliary agent.
[0021] Colorants include ferric chloride, praseodymium chloride, erbium chloride, manganese chloride and neodymium chloride. The mass ratio of ferric chloride, praseodymium chloride, erbium chloride, manganese chloride and neodymium chloride is 3:1:3:1:1. Colorants are used to improve the color of zirconia dentures and make them closer to the color of teeth after processing. This not only makes the dentures better hidden and improves their appearance, but also increases people's confidence.
[0022] The auxiliary agents are dispersant, light stabilizer, photoinitiator, toughening agent, binding agent, defoaming agent, silane coupling agent and antibacterial agent. The mass ratio of dispersant, light stabilizer, photoinitiator, toughening agent, binding agent, defoaming agent, silane coupling agent and antibacterial agent is 1:1:1:2:3:1:1:5.
[0023] The antibacterial agents are honeysuckle extract and green tea extract, and the mass ratio of the honeysuckle extract and the green tea extract is 1:1. By adding the honeysuckle extract and the green tea extract, the antibacterial effect of the zirconia denture is enhanced, which is healthier for people's oral cavity.
[0024] The present invention also provides a preparation process of a low-color-difference zirconia denture, comprising the following steps: S1. Mix zirconium oxide, ceramic powder, aluminum oxide, yttrium oxide, cellulose powder, colorant and auxiliary agent together with a mixer to prepare a mixture A. The mixer uses a V-type mixer. The V-type mixer is easy to operate and has a good mixing effect when mixing zirconium oxide, ceramic powder, aluminum oxide, yttrium oxide, cellulose powder, colorant and auxiliary agent. S2, preparing an embryo mold, and injecting the mixture A in step S1 into the embryo mold; S3, placing the embryo mold in an isostatic press for isostatic pressing to obtain a denture blank; the denture blank processed by the isostatic press has a high density and is more uniform. At this time, the size of the denture blank is larger than the size of the denture to be manufactured, providing shrinkage space for subsequent sintering; S4, pre-sintering the denture blank first, and then sintering at high temperature; the denture blank is preheated in a sintering furnace at 290 degrees for 34 minutes. During the preheating, the volatiles in the denture blank can be removed. Then the temperature of the sintering furnace is increased to 1300 degrees for sintering for 18 hours. The high-temperature sintering takes a long time, which can allow the denture blank to undergo a chemical reaction and form a hard structure. Finally, it is kept warm at 930 degrees for 8 hours. The heat preservation after sintering can ensure the stability of the material of the denture after sintering, which not only ensures the hardness of the denture, but also ensures the coloring effect of the denture. When in use, the color difference between the denture and the teeth is reduced. After the heat preservation is completed, the sintering furnace is closed and the furnace body is allowed to cool naturally to room temperature. In this process, the denture gradually solidifies and becomes hard; S5. Grind and polish the denture after high-temperature sintering.
[0025] Example 3: A low-color-difference zirconia denture, the raw materials of which are formulated as follows in parts by weight: 80 parts of zirconium oxide, 45 parts of ceramic powder, 28 parts of aluminum oxide, 14 parts of yttrium oxide, 11 parts of cellulose powder, 0.9 parts of colorant, and 0.6 parts of auxiliary agent.
[0026] Colorants include ferric chloride, praseodymium chloride, erbium chloride, manganese chloride and neodymium chloride. The mass ratio of ferric chloride, praseodymium chloride, erbium chloride, manganese chloride and neodymium chloride is 3:1:3:1:1. Colorants are used to improve the color of zirconia dentures and make them closer to the color of teeth after processing. This not only makes the dentures better hidden and improves their appearance, but also increases people's confidence.
[0027] The auxiliary agents are dispersant, light stabilizer, photoinitiator, toughening agent, binding agent, defoaming agent, silane coupling agent and antibacterial agent. The mass ratio of dispersant, light stabilizer, photoinitiator, toughening agent, binding agent, defoaming agent, silane coupling agent and antibacterial agent is 1:1:1:2:3:1:1:5.
[0028] The antibacterial agents are honeysuckle extract and green tea extract, and the mass ratio of the honeysuckle extract and the green tea extract is 1:1. By adding the honeysuckle extract and the green tea extract, the antibacterial effect of the zirconia denture is enhanced, which is healthier for people's oral cavity.
[0029] The present invention also provides a preparation process of a low-color-difference zirconia denture, comprising the following steps: S1. Mix zirconium oxide, ceramic powder, aluminum oxide, yttrium oxide, cellulose powder, colorant and auxiliary agent together with a mixer to prepare a mixture A. The mixer uses a V-type mixer. The V-type mixer is easy to operate and has a good mixing effect when mixing zirconium oxide, ceramic powder, aluminum oxide, yttrium oxide, cellulose powder, colorant and auxiliary agent. S2, preparing an embryo mold, and injecting the mixture A in step S1 into the embryo mold; S3, placing the embryo mold in an isostatic press for isostatic pressing to obtain a denture blank; the denture blank processed by the isostatic press has a high density and is more uniform. At this time, the size of the denture blank is larger than the size of the denture to be manufactured, providing shrinkage space for subsequent sintering; S4, pre-sintering the denture blank first, and then sintering at high temperature; the denture blank is preheated in a sintering furnace at 310 degrees for 38 minutes. During the preheating, the volatiles in the denture blank can be removed. Then the temperature of the sintering furnace is increased to 1400 degrees for sintering for 28 hours. The high-temperature sintering takes a long time, which can allow the denture blank to undergo a chemical reaction and form a hard structure. Finally, it is kept warm at 980 degrees for 9 hours. The heat preservation after sintering can ensure the stability of the material of the denture after sintering, which not only ensures the hardness of the denture, but also ensures the coloring effect of the denture. When in use, the color difference between the denture and the teeth is reduced. After the heat preservation is completed, the sintering furnace is closed and the furnace body is allowed to cool naturally to room temperature. In this process, the denture gradually solidifies and becomes hard; S5. Grind and polish the denture after high-temperature sintering.
[0030] Example 4: A low-color-difference zirconia denture, the raw materials of which are formulated as follows in parts by weight: 85 parts of zirconium oxide, 50 parts of ceramic powder, 30 parts of aluminum oxide, 15 parts of yttrium oxide, 12 parts of cellulose powder, 1 part of colorant, and 0.7 parts of auxiliary agent.
[0031] Colorants include ferric chloride, praseodymium chloride, erbium chloride, manganese chloride and neodymium chloride. The mass ratio of ferric chloride, praseodymium chloride, erbium chloride, manganese chloride and neodymium chloride is 3:1:3:1:1. Colorants are used to improve the color of zirconia dentures and make them closer to the color of teeth after processing. This not only makes the dentures better hidden and improves their appearance, but also increases people's confidence.
[0032] The auxiliary agents are dispersant, light stabilizer, photoinitiator, toughening agent, binding agent, defoaming agent, silane coupling agent and antibacterial agent. The mass ratio of dispersant, light stabilizer, photoinitiator, toughening agent, binding agent, defoaming agent, silane coupling agent and antibacterial agent is 1:1:1:2:3:1:1:5.
[0033] The antibacterial agents are honeysuckle extract and green tea extract, and the mass ratio of the honeysuckle extract and the green tea extract is 1:1. By adding the honeysuckle extract and the green tea extract, the antibacterial effect of the zirconia denture is enhanced, which is healthier for people's oral cavity.
[0034] The present invention also provides a preparation process of a low-color-difference zirconia denture, comprising the following steps: S1. Mix zirconium oxide, ceramic powder, aluminum oxide, yttrium oxide, cellulose powder, colorant and auxiliary agent together with a mixer to prepare a mixture A. The mixer uses a V-type mixer. The V-type mixer is easy to operate and has a good mixing effect when mixing zirconium oxide, ceramic powder, aluminum oxide, yttrium oxide, cellulose powder, colorant and auxiliary agent. S2, preparing an embryo mold, and injecting the mixture A in step S1 into the embryo mold; S3, placing the embryo mold in an isostatic press for isostatic pressing to obtain a denture blank; the denture blank processed by the isostatic press has a high density and is more uniform. At this time, the size of the denture blank is larger than the size of the denture to be manufactured, providing shrinkage space for subsequent sintering; S4, pre-sintering the denture blank first, and then sintering at high temperature; the denture blank is preheated in a sintering furnace at 320 degrees for 40 minutes. During the preheating, the volatiles in the denture blank can be removed. Then the temperature of the sintering furnace is increased to 1450 degrees for sintering for 30 hours. The high-temperature sintering takes a long time, which can allow the denture blank to undergo a chemical reaction and form a hard structure. Finally, it is kept warm at 1000 degrees for 10 hours. The heat preservation after sintering can ensure the stability of the material of the denture after sintering, which not only ensures the hardness of the denture, but also ensures the coloring effect of the denture. When in use, the color difference between the denture and the teeth is reduced. After the heat preservation is completed, the sintering furnace is closed and the furnace body is allowed to cool naturally to room temperature. In this process, the denture gradually solidifies and becomes hard; S5. Grind and polish the denture after high-temperature sintering.
[0035] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A low color difference zirconia denture, It is characterized in that The raw materials are formulated as follows according to weight parts: 65-85 parts of zirconium oxide, 30-50 parts of ceramic powder, 20-30 parts of aluminum oxide, 10-15 parts of yttrium oxide, 8-12 parts of cellulose powder, 0.5-1 parts of colorant, and 0.3-0.7 parts of auxiliary agent.
2. The low-color-difference zirconia denture according to claim 1, It is characterized in that The colorants include ferric chloride, praseodymium chloride, erbium chloride, manganese chloride and neodymium chloride.
3. The low-color-difference zirconia denture according to claim 2, It is characterized in that The mass ratio of the ferric chloride, praseodymium chloride, erbium chloride, manganese chloride and neodymium chloride is 3:1:3:1:
1.
4. The low-color-difference zirconia denture according to claim 1, It is characterized in that The auxiliary agents are dispersants, light stabilizers, light initiators, toughening agents, bonding aids, defoaming agents, silane coupling agents and antibacterial agents.
5. The low-color-difference zirconia denture according to claim 4, It is characterized in that The mass ratio of the dispersant, the light stabilizer, the photoinitiator, the toughening agent, the bonding aid, the defoaming agent, the silane coupling agent and the antibacterial agent is 1:1:1:2:3:1:1:
5.
6. The low-color-difference zirconia denture according to claim 5, It is characterized in that The antibacterial agents are honeysuckle extract and green tea extract, and the mass ratio of the honeysuckle extract to the green tea extract is 1:
1.
7. A process for preparing the low-color-difference zirconia denture according to claim 1, It is characterized in that The steps include: S1. Mixing zirconium oxide, ceramic powder, aluminum oxide, yttrium oxide, cellulose powder, colorant and auxiliary agent together with a mixer to prepare a mixture A; S2, preparing an embryo mold, and injecting the mixture A in step S1 into the embryo mold; S3, placing the embryo mold in an isostatic press for isostatic pressing to obtain a denture tooth blank; S4, pre-sintering the denture tooth blank first, and then sintering at high temperature; S5. Grind and polish the denture after high-temperature sintering.
8. The low-color-difference zirconia denture and its preparation process according to claim 7, It is characterized in that In step S4, the denture tooth blank is preheated in a sintering furnace at 280-320 degrees for 30-40 minutes, and then the temperature of the sintering furnace is increased to 1200-1450 degrees for sintering for 10-30 hours, and finally kept at 900-1000 degrees for 5-10 hours.
9. The preparation process of the low-color-difference zirconia denture according to claim 8, It is characterized in that After the insulation is completed, the sintering furnace is closed and the furnace body is allowed to cool naturally to room temperature.